A-site doped modified germanate high-temperature radar stealth material and preparation method thereof
By introducing A-site doping elements into germanate materials and controlling the lattice structure and oxygen vacancy concentration, the problems of structural stability and insufficient electromagnetic loss of materials under high temperature conditions were solved, and the excellent radar stealth performance of materials under high temperature conditions was achieved.
Patent Information
- Application Number
- CN202511492993.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-20
- Publication Date
- 2026-01-06
AI Technical Summary
In existing high-temperature environments, traditional radar-absorbing materials are prone to performance degradation in oxidizing atmospheres, making it difficult to meet the requirements for long-term stable service under ultra-high temperature conditions. Furthermore, existing germanate materials lack structural stability and electromagnetic loss performance at high temperatures, making it difficult to achieve effective radar stealth.
By introducing A-site doping elements into germanate materials, the lattice structure and oxygen vacancy concentration are controlled to form a multipolarization mechanism, thereby enhancing dielectric loss performance and preparing RE10-xSrxGe6O27-x/2 materials.
The structure stability and dielectric loss performance of the material were optimized under high temperature conditions, which improved the radar wave absorption capability and made it suitable for stealth coatings and radar absorbing elements in high temperature and complex environments.
Smart Images

Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-temperature electromagnetic protection preparation technology, and in particular to an A-site doped modified germanate high-temperature radar stealth material and its preparation method. Background Technology
[0002] With the development of advanced flight platforms such as hypersonic vehicles and reentry capsules, the outer shell materials not only need to possess excellent high-temperature thermal stability and thermal shock resistance, but also need to have good electromagnetic wave absorption capabilities to achieve radar stealth in high-temperature environments. Traditional high-performance absorbing materials, such as carbon-based materials and magnetic metal oxides, have certain electromagnetic loss capabilities, but they are prone to performance degradation under high-temperature oxidizing atmospheres, making it difficult to meet the requirements for long-term stable service under ultra-high temperature (>1000°C) conditions.
[0003] by Layered germanates, represented by [specific example], exhibit excellent thermal stability under high-temperature conditions, with a coefficient of thermal expansion of approximately [specific value]. It can withstand continuous high-temperature ablation tests up to 1200°C without significant structural changes; doped with Sr 2+ Once it enters the A site, the oxygen vacancy concentration is adjustable.
[0004] Therefore, the primary task of this invention is to develop a stealth material based on germanate structure that possesses high-temperature stability, tunable dielectric properties, and strong radar wave absorption capability. Through reasonable doping and structural control, a high-temperature radar stealth material with dual advantages of "thermal stability and electromagnetic loss" is constructed, providing a theoretical basis for the research and application of its high-temperature oxide stealth materials. Summary of the Invention
[0005] The purpose of this invention is to provide an A-site doped modified germanate high-temperature radar stealth material and its preparation method, so as to solve the above-mentioned problems in the prior art. Compared with the radar stealth materials currently being studied, this material has good high-temperature stability, strong oxidation resistance, adjustable dielectric properties and oxygen vacancies, and strong environmental adaptability, which can effectively cope with the high-temperature heat load and radar detection problems faced by aerospace hot-end components.
[0006] To achieve the above objectives, this invention provides an A-site doped modified germanate high-temperature radar stealth material and its preparation method, comprising the following steps: (1) Weigh appropriate amounts of RE2O3, SrCO3 and GeO2 powders according to the molar ratio; (2) Add the three raw materials weighed in step (1) into the ball mill jar in sequence, add an appropriate amount of anhydrous ethanol, and mix them in the ball mill to obtain a mixture containing anhydrous ethanol. (3) The mixture solution containing anhydrous ethanol obtained in step (2) is dried; (4) Sift the dried mixed powder from step (3); (5) Place the sieved powder from step (4) into an alumina ceramic boat and perform high-temperature pre-sintering; (6) Repeat the high-temperature pre-sintering process of step (5); (7) The powder after pre-sintering in step (6) is uniaxially pressed to obtain a green body; (8) The green body from step (7) is sintered at high temperature to form the required RE. 10-x Sr x Ge6O 27-x / 2 Material.
[0007] Oxide ceramic materials have become a new direction in high-temperature microwave absorbing material research due to their excellent thermal stability, oxidation resistance, and tunable dielectric properties. In particular, perovskite and layered ceramic materials can maintain structural integrity at high temperatures while also possessing a certain dielectric loss capability. Germanate materials, due to their unique layered or chain-like crystal structure, exhibit good polarization response and thermal stability. Germanates show good dielectric response to electromagnetic waves in the X-band frequency range (8~12GHz). Introducing appropriate doping elements can further induce lattice distortion, generate oxygen vacancies, enhance carrier transitions and space charge polarization behavior, and significantly improve their dielectric loss capability.
[0008] Under high-temperature thermal activation conditions, oxygen vacancies migrate, leading to an increase in the material's electrical conductivity. This allows for effective regulation of its dielectric loss performance and optimization of its electromagnetic loss performance at high temperatures.
[0009] Further, in step (1), RE is one or any combination of multiple elements from La, Ce, Pr, Nd, Sm, Eu, Gd, Te, Dy, Ho, Er, Tm, Yb, and Lu in equal proportions, where RE:Sr:Ge = 10-x:x:6, and x≤0.5.
[0010] Furthermore, in step (2), the ball-to-material ratio in ball milling is 4-10:1; the mass ratio of anhydrous ethanol to the raw material powder is 2-6:1; the ball milling speed is 300-400 rpm; and the ball milling time is 12-14 hours.
[0011] Furthermore, the drying temperature in step (3) is 80-100℃ and the drying time is 10-14h.
[0012] Furthermore, in step (4), the sieving is performed through a 100-300 mesh sieve.
[0013] Furthermore, in step (5), the high-temperature pre-sintering temperature is 900-1300℃ and the sintering time is 10-25h.
[0014] Furthermore, the high-temperature pre-sintering process in step (6) is repeated 3-5 times.
[0015] Furthermore, in step (7), the pressure of uniaxial pressing is 5-50 MPa, and the holding time is 5-15 min.
[0016] Furthermore, in step (8), the high-temperature sintering temperature is 1300-1700℃ and the sintering time is 10-25h.
[0017] This invention also provides a RE with high-temperature radar stealth performance prepared by the above-described method. 10- x Sr x Ge6O 27-x / 2 Novel germanate materials.
[0018] The advantages or beneficial effects of the above technical solutions include at least the following: (1) The present invention can effectively adjust the lattice constant and symmetry of germanates, so that the material can maintain excellent structural stability at high temperatures. This lattice control capability helps to optimize the dielectric constant distribution and improve the stealth performance at high temperatures.
[0019] (2) The increased oxygen vacancy concentration caused by doping in this invention can enhance polarization relaxation loss and conductivity loss, forming a synergistic effect of multiple electromagnetic loss mechanisms. Oxygen vacancies can also act as charge traps, inhibiting the migration of free electrons and improving the dielectric loss efficiency of the material.
[0020] (3) The lattice distortion and electron cloud distribution changes caused by A-site doping in this invention promote the coexistence of multiple polarization mechanisms such as electronic polarization, ion polarization and interface polarization, which makes the material have higher complex dielectric constant and dielectric loss factor, which is beneficial to radar wave absorption in a wide frequency band. Detailed Implementation
[0021] The embodiments of the present invention are described in detail below. Throughout these embodiments, the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions. The following embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the invention. In the description of the present invention, "a plurality of" means two or more, unless otherwise explicitly specified. Example 1
[0022] This embodiment provides an A-site doped modified germanate high-temperature radar stealth material, La. 9.6 Sr 0.4 Ge6O 26.8 The preparation method thereof includes the following steps: (1) Using La2O3, SrCO3 and GeO2 powders as raw materials, weigh the powder raw materials according to the molar ratio La2O3:SrCO3:GeO2=9.6:0.4:6; (2) Place the weighed three raw materials in a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 4:1. The mass ratio of anhydrous ethanol to mixed powder is 6:1. The ball mill speed is maintained at 300 rpm and the ball milling time is 12 hours. (3) The mixed powder anhydrous ethanol solution was placed in an 80℃ forced-air drying oven for 12 hours for drying treatment; (4) The dried powder is sieved using a 300-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 1100℃ for 10 hours. After sintering, it is ground and sieved using a 300-mesh sieve. This high-temperature pre-sintering heat treatment is repeated three times. (6) After the pre-sintered powder is sieved through a 300-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 30 MPa and a holding time of 10 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1500℃ for 25 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0023] The La prepared in this embodiment 9.6 Sr 0.4 Ge6O 26.8 The radar reflection loss performance of the material in the 2-18GHz frequency band at 1000℃ is shown in Table 1.
[0024]
[0025] Comparative Example 1 La 10 Ge6O 27 The materials and their preparation method, specifically the following steps: (1) Using La2O3 and GeO2 powders as raw materials, weigh the powders according to the molar ratio of La2O3:GeO2=5:6; (2) Place the weighed raw materials into a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 4:1. The mass ratio of anhydrous ethanol to mixed powder is 6:1. The ball mill speed is maintained at 300 rpm and the mixing time is 12 hours. (3) The mixed powder anhydrous ethanol solution was placed in an 80℃ forced-air drying oven for 10 hours for drying treatment; (4) The dried powder is sieved using a 300-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 1100℃ for 10 hours. After sintering, it is ground and sieved using a 300-mesh sieve. This high-temperature pre-sintering heat treatment is repeated three times. (6) After the pre-sintered powder is sieved through a 300-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 30 MPa and a holding time of 10 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1500℃ for 25 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0026] The La prepared in this embodiment 10 Ge6O 27 The radar reflection loss performance of the material in the 2-18GHz frequency band at 1000℃ is shown in Table 2.
[0027]
[0028] A comparison of Tables 1 and 2 reveals that introducing specific A-site doping elements into the germanate crystal structure effectively modulates the lattice structure and electronic environment, promotes the formation of oxygen vacancies, and enhances the dielectric polarization behavior and microwave loss mechanism of the material. The lattice distortion and defect states induced by doping improve the material's dielectric response to radar waves, achieving broadband electromagnetic wave absorption and radar stealth performance in high-temperature environments. This material is suitable for stealth coatings, radar-absorbing elements, and advanced protection systems in high-temperature and complex environments, demonstrating promising application prospects and engineering value. Example 2
[0029] This embodiment provides Ce, an A-site doped modified germanate high-temperature radar stealth material. 9.5 Sr 0.5 Ge6O 26.75 The preparation method thereof includes the following steps: (1) Using Ce2O3, SrCO3 and GeO2 powders as raw materials, weigh the powder raw materials according to the molar ratio Ce2O3:SrCO3:GeO2=9.5:0.5:6; (2) Place the weighed three raw materials in a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 8:1. The mass ratio of anhydrous ethanol to mixed powder is 4:1. The ball mill speed is maintained at 400 rpm and the ball milling time is 13 hours. (3) The mixed powder anhydrous ethanol solution was placed in a 100℃ forced-air drying oven for 12 hours for drying treatment; (4) The dried powder is sieved using a 200-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 1300℃ for 15 hours. After sintering, it is ground and sieved using a 200-mesh sieve. This high-temperature pre-sintering heat treatment is repeated four times. (6) After the pre-sintered powder is sieved through a 200-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 50 MPa and a holding time of 15 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1700℃ for 10 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0030] After Ce 9.5 Sr 0.5 Ge6O 26.75 After testing and evaluation, the material was found to have good high-temperature stability, strong dielectric loss, and good radar absorption performance, which are characteristics of high-temperature radar stealth. Example 3
[0031] This embodiment provides Pr, an A-site doped modified germanate high-temperature radar stealth material. 9.7 Sr 0.3 Ge6O 26.85 The preparation method thereof includes the following steps: (1) Using Pr2O3, SrCO3 and GeO2 powders as raw materials, weigh the powder raw materials according to the molar ratio Pr2O3:SrCO3:GeO2=9.7:0.3:6; (2) Place the weighed three raw materials in a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 10:1. The mass ratio of anhydrous ethanol to mixed powder is 2:1. The ball mill speed is maintained at 350 rpm and the ball milling time is 12 hours. (3) The mixed powder anhydrous ethanol solution was placed in a 90℃ forced-air drying oven for 14 hours for drying treatment; (4) The dried powder is sieved using a 300-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 1300℃ for 15 hours. After sintering, it is ground and sieved using a 100-mesh sieve. This high-temperature pre-sintering heat treatment is repeated five times. (6) After the pre-sintered powder is sieved through a 100-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 5 MPa and a holding time of 5 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1300℃ for 20 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0032] After examining Pr 9.7 Sr 0.3 Ge6O 26.85 After testing and evaluation, the material was found to have good high-temperature stability, strong dielectric loss, and good radar absorption performance, which are characteristics of high-temperature radar stealth. Example 4
[0033] This embodiment provides an A-site doped modified germanate high-temperature radar stealth material Nd 9.8 Sr 0.2 Ge6O 26.9 The preparation method thereof includes the following steps: (1) Using Nd2O3, SrCO3 and GeO2 powders as raw materials, weigh the powder raw materials according to the molar ratio Nd2O3:SrCO3:GeO2=9.8:0.2:6; (2) Place the weighed three raw materials in a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 5:1. The mass ratio of anhydrous ethanol to mixed powder is 3:1. The ball mill speed is maintained at 400 rpm and the ball milling time is 14 hours. (3) The mixed powder anhydrous ethanol solution was placed in a 100℃ forced-air drying oven for 10 hours to dry; (4) The dried powder is sieved using a 200-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 1000℃ for 20 hours. After sintering, it is ground and sieved using a 200-mesh sieve. This high-temperature pre-sintering heat treatment is repeated three times. (6) After the pre-sintered powder is sieved through a 200-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 10 MPa and a holding time of 8 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1600℃ for 22 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0034] After Nd 9.8 Sr 0.2 Ge6O 26.9 After testing and evaluation, the material was found to have good high-temperature stability, strong dielectric loss, and good radar absorption performance, which are characteristics of high-temperature radar stealth. Example 5
[0035] This embodiment provides an A-site doped modified germanate high-temperature radar stealth material Sm 9.9 Sr 0.1 Ge6O 26.95 The preparation method thereof includes the following steps: (1) Using Sm2O3, SrCO3 and GeO2 powders as raw materials, weigh the powder raw materials according to the molar ratio Sm2O3:SrCO3:GeO2=9.9:0.1:6; (2) Place the weighed three raw materials in a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 9:1. The mass ratio of anhydrous ethanol to mixed powder is 5:1. The ball milling speed is maintained at 350 rpm and the ball milling time is 13 hours. (3) The mixed powder anhydrous ethanol solution was placed in a 90℃ forced-air drying oven for 12 hours for drying treatment; (4) The dried powder is sieved using a 100-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 1200℃ for 15 hours. After sintering, it is ground and sieved using a 100-mesh sieve. This high-temperature pre-sintering heat treatment is repeated three times. (6) After the pre-sintered powder is sieved through a 100-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 20 MPa and a holding time of 10 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1500℃ for 20 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0036] After Sm 9.9 Sr 0.1 Ge6O26.95 After testing and evaluation, the material was found to have good high-temperature stability, strong dielectric loss, and good radar absorption performance, which are characteristics of high-temperature radar stealth. Example 6
[0037] This embodiment provides an A-site doped modified germanate high-temperature radar stealth material, Eu. 9.6 Sr 0.4 Ge6O 26.8 The preparation method thereof includes the following steps: (1) Using Eu2O3, SrCO3 and GeO2 powders as raw materials, weigh the powder raw materials according to the molar ratio Eu2O3:SrCO3:GeO2=9.6:0.4:6; (2) Place the weighed three raw materials in a ball mill jar and add anhydrous ethanol. To ensure uniform ball milling, the ball-to-material ratio is controlled at 7:1. The mass ratio of anhydrous ethanol to mixed powder is 2:1. The ball milling speed is maintained at 300 rpm and the ball milling time is 12 hours. (3) The mixed powder anhydrous ethanol solution was placed in an 80℃ forced-air drying oven for 12 hours for drying treatment; (4) The dried powder is sieved using a 100-mesh sieve; (5) The sieved powder is placed evenly in an alumina ceramic boat and pre-sintered at a high temperature of 900℃ for 40 hours. After sintering, it is ground and sieved using a 100-mesh sieve. This high-temperature pre-sintering heat treatment is repeated four times. (6) After the pre-sintered powder is sieved through a 100-mesh sieve, it is subjected to uniaxial compression. Under a uniaxial pressure of 20 MPa and a holding time of 10 min, it is pressed into a blank with a diameter of 30 mm and a thickness of 2 mm. (7) The pressed preform is placed in a muffle furnace for high-temperature sintering at a temperature of 1700℃ for 10 hours. (8) The radar stealth performance of the sintered and machined bulk material was tested and evaluated using a high-temperature electromagnetic parameter testing system.
[0038] After Eu 9.6 Sr 0.4 Ge6O 26.8 After testing and evaluation, the material was found to have good high-temperature stability, strong dielectric loss, and good radar absorption performance, which are characteristics of high-temperature radar stealth.
[0039] In summary, the material prepared by this invention has better high-temperature stability, stronger oxidation resistance, adjustable dielectric properties and oxygen vacancies, and stronger environmental adaptability compared to radar stealth materials currently under research. It can effectively address the high-temperature heat load and radar detection problems faced by aerospace hot-end components.
[0040] The above-disclosed embodiments are merely some examples of the present invention and should not be construed as limiting the scope of the invention. Those skilled in the art will understand that implementing all or part of the above embodiments and making equivalent changes in accordance with the claims of the present invention are still within the scope of the invention.
Claims
1. A kind of A-site doped modified germanate high temperature radar stealth material and its preparation method, characterized by: The method comprises the following steps: (1) weighing a proper amount of RE2O3, SrCO3 and GeO2 powders according to the molar ratio; (2) adding the three kinds of raw materials weighed in step (1) into a ball mill tank in sequence, adding a proper amount of anhydrous ethanol, and mixing in a ball mill to obtain a mixture containing anhydrous ethanol; (3) drying the mixture solution containing anhydrous ethanol obtained in step (2); (4) sieving the mixed powder dried in step (3); (5) placing the sieved powder in step (4) in an alumina ceramic boat and performing high-temperature pre-sintering; (6) repeating the high-temperature pre-sintering in step (5); (7) performing uniaxial pressing on the pre-sintered powder in step (6) to obtain a green body; (8) high temperature sintering of the body in step (7) to form the desired RE 10-x Sr x Ge6O 27-x / 2 material.
2. The A-site doped modified germanate high-temperature radar stealth material and its preparation method as described in claim 1, characterized in that: In step (1), RE is one or any multiple elements of La, Ce, Pr, Nd, Sm and Eu in equal proportions, wherein RE: Sr: Ge = 10-x: x: 6, and x ≤ 0.
5.
3. The A-site doped modified germanate high-temperature radar-stealth material and the preparation method thereof according to claim 1, characterized in that: In step (2), the ball-to-material ratio of ball milling is 4-10:1; the mass ratio of anhydrous ethanol to raw material mixed powder is 2-6:1; the ball milling speed is 300-400 rpm, and the ball milling time is 12-14 hours.
4. The A-site doped modified germanate high-temperature radar-stealth material and the preparation method thereof according to claim 1, characterized in that: In step (3), the drying temperature is 80-100℃, and the drying time is 10-14h.
5. The A-site doped modified germanate high-temperature radar-stealth material and the preparation method thereof according to claim 1, characterized in that: In step (4), the sieving is through 100-300 mesh sieves.
6. The A-site doped modified germanate high-temperature radar stealth material and its preparation method as described in claim 1, characterized in that: In step (5), the high-temperature pre-sintering temperature is 900-1300℃, and the sintering time is 10-25h.
7. The A-site doped modified germanate high-temperature radar stealth material and its preparation method as described in claim 1, characterized in that: In step (6), the number of repeated high-temperature pre-sintering is 3-5 times.
8. The A-site doped modified germanate high-temperature radar stealth material and its preparation method as described in claim 1, characterized in that: In step (7), the uniaxial pressing pressure is 5-50Mpa, and the pressure holding time is 5-15min.
9. The A-site doped modified germanate high-temperature radar stealth material and its preparation method as described in claim 1, characterized in that: In step (8), the high-temperature sintering temperature is 1300-1700℃, and the sintering time is 10-25h.
10. A RE 10- x Sr x Ge6O 27-x / 2 germanate material prepared by the method of any one of claims 1 to 9.