Plastic package device chip bonding layer layering judgment method fusing multi-mode ultrasonic scanning and high-power microscopic examination
By integrating multi-mode ultrasonic scanning with high-magnification microscopy, and combining the propagation characteristics of materials with different acoustic impedances with high-magnification microscopy, the problem of inaccurate detection of delamination of the bonding layer of molded device chips in existing technologies has been solved, achieving a more comprehensive and reliable defect determination.
Patent Information
- Application Number
- CN202511948094.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-23
- Publication Date
- 2026-01-20
AI Technical Summary
In existing technologies, relying solely on C-scan and A-scan cannot accurately and intuitively detect delamination defects in the bonding layer of molded device chips.
This method integrates multi-mode ultrasound scanning (C-scan, T-scan, B-scan, and A-scan) with high-magnification microscopy. By combining frontal and back scans, along with analysis of the propagation characteristics of ultrasound waves between materials with different acoustic impedances and high-magnification microscopy for sample preparation and examination, multi-dimensional detection and verification are achieved.
It enables accurate identification of delamination defects in the adhesive layer of molded devices, improving the comprehensiveness and reliability of the detection, and is applicable to the identification of other types of defects.
Smart Images

Figure CN121364245A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of plastic package device defect detection, in particular to a plastic package device chip adhesive layer delamination determination method fusing multi-mode ultrasonic scanning and high-power microscopy. BACKGROUND
[0002] In the field of plastic package device detection, ultrasonic detection is widely used due to its sensitivity to internal defects of the measured object. When ultrasonic waves interact with the measured object and its defects, reflection, transmission, diffraction and scattering occur, resulting in changes in the direction and characteristics of the waves. By processing and analyzing the reflected and transmitted ultrasonic waves, an acoustic image of the measured object can be obtained, and a theoretical determination can be made as to whether there are internal defects in the measured object.
[0003] However, for a general plastic package device composed of plastic packaging material, chip, adhesive layer, substrate (back surface exposed), and lead frame, the chip adhesive layer is located between the chip and the substrate. The substances before and after this position are not single, and the ultrasonic waveform is complex when it passes through this position. In the prior art, only based on C-scan (plane scan) and A-scan (amplitude scan), whether scanning from the front or the back, the situation between the adhesive layer and the chip cannot be accurately, intuitively and single detected, and it is difficult to accurately determine the delamination defects existing at this position. SUMMARY
[0004] In view of the deficiencies of the prior art, the present application provides a plastic package device chip adhesive layer delamination determination method fusing multi-mode ultrasonic scanning and high-power microscopy to solve the problem that the prior art cannot accurately determine the delamination defects of the plastic package device chip adhesive layer only relying on C-scan and A-scan.
[0005] To achieve the above purpose, the present application realizes the following technical scheme: a plastic package device chip adhesive layer delamination determination method fusing multi-mode ultrasonic scanning and high-power microscopy, comprising the following specific steps:
[0006] S1, front C-scan detection and analysis, using a scanning acoustic microscope to perform C-scan on the front of the plastic package device, focusing on the substrate to detect whether there are delamination or cavities between the upper surface of the chip and the plastic packaging material, the C-scan parameters are set as: scanning frequency 50-100MHz, scanning step 5-10um, GatePosition 286ns, Length 796ns, C-scan mode image and corresponding A-scan waveform graph are obtained;
[0007] If the A-scan waveform appears strong reflection after the waveform of the plastic packaging material and the chip interface, it is determined that there may be delamination under the chip; if the waveform appears attenuation after the waveform, it is determined that there is no obvious delamination;
[0008] S2, T-scan corroborative detection and analysis, synchronously perform T-scan, the scanning parameters are consistent with those of C-scan, obtain T-scan mode images and corresponding A-scan waveform graphs;
[0009] If the chip part in the T-scan perspective is black abnormally, and there is no waveform in the A-scan waveform graph corresponding to the chip position, it is corroborated that there is delamination under the chip; if there is no black abnormality at the chip position and there is a waveform in the A-scan waveform graph, it is determined that there is no delamination;
[0010] S3, back C-scan detection and analysis, perform C-scan on the back of the plastic package device, the scanning parameters are set as: scanning frequency 50-100 MHz, scanning step 5-10 pm, GatePosition 116 ns, Length 100 ns, obtain C-scan mode images and corresponding A-scan waveform graphs;
[0011] If the reflection amplitude of a certain sample is greater than that of other samples, it is determined that the chip adhesive layer of the sample has delamination; otherwise, it is determined that there is no delamination;
[0012] S4, B-scan depth verification and analysis, perform B-scan on the back of the plastic package device, the scanning parameters are consistent with those of the back C-scan, obtain B-scan mode images;
[0013] If the chip under the B-scan image is bright, it is verified that the chip adhesive layer has delamination; if it is dark, it is verified that there is no delamination;
[0014] S5, high-power microscope sample preparation and microscopic verification, specifically as follows:
[0015] S501, sample preparation for delaminated devices: precisely cut the delaminated part, grind and polish to obtain a detection section;
[0016] S502, place the section under a high-power microscope, observe at 10000 times magnification under the condition of an accelerating voltage of 10.00 kV, a working distance of 10.0 mm and an SE mode;
[0017] If delamination defects are observed, delamination is finally confirmed; otherwise, delamination is excluded.
[0018] Optionally, in step S1, when focusing on the substrate by C-scan, the focal length of the scanning acoustic microscope is adjusted to ensure that the ultrasonic signal accurately acts on the corresponding area of the substrate and the chip adhesive layer, and the interference of the plastic package material on the signal is reduced.
[0019] Optionally, when steps S2 and S1 are performed synchronously, the multi-mode cooperative control module of the scanning acoustic microscope is used to realize synchronous triggering of C-scan and T-scan, synchronous data acquisition, and ensure the consistency of the detection conditions.
[0020] Optionally, in step S3, when the back surface C scanning, an ultrasonic coupling agent is applied on the back surface of the substrate, the coupling agent is a water-soluble ultrasonic coupling agent, and the thickness is controlled to be 0.1-0.2 mm, so as to ensure efficient transmission of ultrasonic waves.
[0021] Optionally, in step S4, the thickness resolution of the B scanning tomography is ≤1 μm, and the depth sampling interval of the scanning acoustic microscope is adjusted to realize accurate imaging of the thickness direction of the chip bonding layer.
[0022] Optionally, in step S5, a diamond cutting piece is used for precise cutting during sample preparation, and the cutting speed is controlled to be 1-2 mm / s, so as to avoid secondary damage to the chip bonding layer during cutting.
[0023] Optionally, the method is also applicable to the determination of defects such as cavities or impurities between plastic sealing materials, delamination between a substrate and plastic sealing materials, and delamination between a lead frame and plastic sealing materials, and only the acoustic interface reference for focusing area and waveform analysis in each scanning step needs to be adjusted.
[0024] The application provides a plastic-sealed device chip bonding layer delamination determination method combining multi-mode ultrasonic scanning and high-power microscopy.
[0025] The plastic-sealed device chip bonding layer delamination determination method combining multi-mode ultrasonic scanning and high-power microscopy combines C scanning, T scanning, B scanning and A scanning, and optimizes the order and parameters of each scanning mode, preliminarily determines through front surface C scanning, uses T scanning as evidence, and then verifies through back surface C scanning and B scanning, so that the chip bonding layer of the plastic-sealed device is detected and analyzed from different dimensions.
[0026] The method first analyzes the phenomena and waveforms in each scanning mode based on the propagation characteristics of ultrasonic waves between different acoustic impedance materials from the principle level, obtains a theoretical determination conclusion, and then directly verifies the conclusion through sample preparation microscopy, so that the theory and the practice are combined, the misjudgment caused by the non-obvious ultrasonic scanning waveform is avoided, and the reliability of the chip bonding layer delamination determination is significantly improved. BRIEF DESCRIPTION OF DRAWINGS
[0027] Figure 1 FIG. 1 is a schematic diagram of a back surface structure of a plastic-sealed device;
[0028] Figure 2 FIG. 4 is a front surface C scanning mode (top view) image of a plastic-sealed device;
[0029] Figure 3 For Figure 2 A-scan waveform diagram of the corresponding position of sample No. 1 in the middle;
[0030] Figure 4 For Figure 2 A-scan waveform diagram of the corresponding position of sample No. 2 in the middle;
[0031] Figure 5 For Figure 2 A-scan waveform diagram of the corresponding position of sample No. 3 in the middle;
[0032] Figure 6 T-scan mode (top view) image of a plastic package device;
[0033] Figure 7 For Figure 6 A-scan waveform diagram of the corresponding position of sample No. 1 in the middle;
[0034] Figure 8 For Figure 6 A-scan waveform diagram of the corresponding position of sample No. 2 in the middle;
[0035] Figure 9 For Figure 6 A-scan waveform diagram of the corresponding position of sample No. 3 in the middle;
[0036] Figure 10 C-scan mode (rear view) image of the back of a plastic package device;
[0037] Figure 11 For Figure 10 A-scan waveform diagram of the corresponding position of sample No. 1 in the middle;
[0038] Figure 12 For Figure 10 A-scan waveform diagram of the corresponding position of sample No. 2 in the middle;
[0039] Figure 13 For Figure 10 A-scan waveform diagram of the corresponding position of sample No. 3 in the middle;
[0040] Figure 14 1-3 Sample sound scan B-scan mode position diagram (rear view);
[0041] Figure 15 1-3 Sample No. 1 sound scan B-scan mode (rear view) image;
[0042] Figure 16 1-3 Sample No. 2 sound scan B-scan mode (rear view) image;
[0043] Figure 17 High-power microscope sample preparation microscopy of sample No. 1 position 1 cross-section local magnification (10000 times). Detailed Implementation
[0044] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0045] In the description of this invention, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," "outer," "front end," "rear end," "head," "tail," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0046] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0047] Please see Figures 1 to 17 A method for determining the delamination of the adhesive layer of a molded device chip by integrating multi-mode ultrasonic scanning and high-magnification microscopy, wherein the molded device includes molding material, chip, adhesive layer, exposed substrate on the back and lead frame;
[0048] The determination method includes the following steps:
[0049] Step 1: Front C-scan detection and analysis. A scanning acoustic microscope is used to perform a C-scan on the front of the molded device, focusing on the substrate, to detect whether there are problems such as delamination or voids between the chip surface and the molding compound, and to obtain the C-scan mode (top view) image and the corresponding A-scan waveform.
[0050] The C-scan parameters are set as follows: scan frequency 50-100MHz, scan step size 5-10μm, gate position 286ns, and gate length 796ns.
[0051] The interface between two materials with different acoustic impedance is an acoustic interface, and the acoustic interface of the plastic package device includes the interface between the plastic package material and the chip, the interface between the chip and the substrate, and the interface between the plastic package material and the lead frame. If the A-scan waveform of a sample (such as sample No. 1) appears strong reflection behind the waveform of the interface between the plastic package material and the chip, it indicates that the ultrasonic wave is reflected because it cannot completely penetrate the air, and it is preliminarily judged that delamination may occur under the chip of the sample. If the A-scan waveform of a sample (such as sample No. 2 or No. 3) appears attenuation behind the waveform of the interface between the plastic package material and the chip, it is because the waveform is diffracted, scattered and absorbed, and it is preliminarily judged that no obvious delamination occurs under the chip.
[0052] Step two: T-scan detection and analysis, while the front C-scan is performed in step one, the plastic package device is subjected to T-scan (transmission scan), and the T-scan mode (top view) image and the A-scan waveform graph of the corresponding position are obtained.
[0053] The T-scan parameters are consistent with the C-scan parameters, ensuring that the detection conditions are unified.
[0054] The imaging principle of the T-scan perspective view is that the ultrasonic wave is transmitted between different acoustic impedance materials, and when there is air in a certain part, the ultrasonic wave is totally reflected from the material to the air, and no ultrasonic wave is transmitted, which appears as total black in the perspective view.
[0055] If the chip part of a sample (such as sample No. 1) appears black abnormality in the T-scan perspective view, and there is no waveform in the A-scan waveform graph corresponding to the chip position, it further proves that there is delamination under the chip of the sample (because the wave is totally reflected from the chip or the plastic package material with large acoustic impedance to the air with small acoustic impedance, and no waveform is generated); if the chip position of a sample (such as sample No. 2 or No. 3) has no black abnormality in the T-scan perspective view, and there is a waveform in the corresponding A-scan waveform graph, it indicates that there is no delamination in the chip position (part of the wave is reflected, and a waveform is generated).
[0056] Step three: back C-scan detection and analysis, because the ultrasonic wave needs to penetrate the plastic package material and the chip to reach the adhesive layer in the front C-scan, it has a certain influence on imaging and waveform, and the substrate is exposed on the back, so the ultrasonic wave can directly enter the adhesive layer from the substrate, therefore, the back of the plastic package device is subjected to C-scan, and the C-scan mode (rear view) image and the A-scan waveform graph of the corresponding position are obtained.
[0057] The back C-scan parameters are set as follows: scanning frequency 50-100 MHz, scanning step 5-10 μm, GatePosition 116 ns, and Length 100 ns.
[0058] The obtained back C-scan image and A-scan waveform graph are analyzed: when the wave is from the metal outer layer with large acoustic impedance to the adhesive layer with small acoustic impedance, a negative wave is generated; if the amplitude of the reflected wave of a sample (such as sample No. 1) is much larger than that of other samples (such as sample Nos. 2 and 3), it indicates that the wave from the metal outer layer with large acoustic impedance to the air with smaller acoustic impedance is totally reflected, and it is further confirmed that the sample chip adhesive layer has a delamination phenomenon;
[0059] Step four: B-scan depth verification and analysis, B-scan (tomography) is performed on the back of the plastic package device to obtain a B-scan mode (rear view) image, and the condition of the chip adhesive layer in the depth direction is determined;
[0060] The B-scan parameters are consistent with the back C-scan parameters;
[0061] The B-scan image analysis principle is as follows: when the wave is from a material with large acoustic impedance to a material with small acoustic impedance, the reflection condition is different; if a sample (such as sample No. 1) presents a bright color under the chip in the B-scan image, it indicates that the wave from the substrate with large acoustic impedance to the air with small acoustic impedance is totally reflected, and the chip adhesive layer of the sample is verified to have a delamination again; if a sample (such as sample Nos. 2 and 3) presents a dark color under the chip in the B-scan image, it indicates that the wave from the heat sink with large acoustic impedance to the adhesive layer with small acoustic impedance is partially reflected, and the chip adhesive layer is verified to have no delamination;
[0062] Step five: high-power microscope sample preparation and microscopic verification: for the plastic package device (such as sample No. 1) determined to have a chip adhesive layer delamination in steps one to four, sample preparation is performed: a precision cutting device is used to cut the delamination part, and then grinding and polishing are performed to obtain a smooth detection section;
[0063] The prepared sample section is placed under a high-power microscope, and observation is performed under 10,000 times magnification; the high-power microscope parameter settings are as follows: acceleration voltage 10.00 kV, working distance 10.0 mm, and detection mode SE (secondary electron) mode;
[0064] If the chip adhesive layer of the sample is observed to have a delamination defect under the high-power microscope, it is finally confirmed that the chip adhesive layer of the plastic package device has a delamination; if no delamination defect is observed, the delamination condition is excluded, and the determination result of the previous ultrasonic scanning is corrected.
[0065] The above merely describes a preferred specific embodiment of the present application, but the protection scope of the present application is not limited thereto, and any person skilled in the art can make equivalent replacements or changes to the technical solution and the inventive concept of the present application within the technical range disclosed by the present application, which should be covered within the protection scope of the present application.
Claims
1. A method for determining the delamination of the adhesive layer of a molded device chip by integrating multi-mode ultrasonic scanning and high-magnification microscopy, characterized in that, The specific steps include the following: S1. Front C-scan detection and analysis: A scanning acoustic microscope is used to perform C-scan on the front of the molded device. The substrate is focused to detect whether there is delamination or voids between the chip surface and the molding material. C-scan mode images and corresponding A-scan waveforms are obtained. If the A scan waveform shows a strong reflection behind the waveform at the interface between the molding compound and the chip, it is determined that there may be delamination under the chip. If attenuation occurs after the waveform, it is determined that no obvious stratification has yet occurred; S2 and T scans are used for corroborative detection and analysis. T scans are performed simultaneously with the same scanning parameters as C scans to obtain T scan mode images and corresponding A scan waveforms. If the chip portion appears abnormally black in the T-scan perspective image, and there is no waveform at the corresponding chip location in the A-scan waveform image, it corroborates the existence of layering beneath the chip. If there is no black abnormality at the chip location and the A-scan waveform shows a waveform, it is determined that there is no layering; S3. Backside C-scan detection and analysis: Perform C-scan on the backside of the plastic-encapsulated device to obtain C-scan mode images and corresponding A-scan waveforms. If the amplitude of the reflected wave of a certain sample is greater than that of other samples, it is determined that the chip bonding layer of that sample is delaminated. Conversely, if no layering is found, it is determined that there is no layering. S4 and B scan depth verification and analysis: B scan is performed on the back side of the plastic-encapsulated device. The scanning parameters are the same as those for the back side C scan to obtain the B scan mode image. If the chip appears bright in the B scan image, it verifies that the chip adhesive layer is delaminated; if it appears dark, it verifies that there is no delamination. S5. Sample preparation and microscopic examination under a high-power microscope, as detailed below: S501. Sample preparation for layered devices: Precision cutting of the layered areas, followed by grinding and polishing to obtain the test profile; S502. Place the cross-section under a high-power microscope and observe it at 10,000x magnification with an accelerating voltage of 10.00kV, a working distance of 10.0mm, and SE mode. If a layering defect is observed, layering is confirmed; otherwise, layering is ruled out.
2. The method according to claim 1, characterized in that, In step S1, when C scans and focuses on the substrate, the focal length of the scanning acoustic microscope is adjusted to ensure that the ultrasonic signal is accurately applied to the corresponding area of the substrate and the chip bonding layer, thereby reducing the interference of the molding compound on the signal.
3. The method according to claim 1, characterized in that, When step S2 is performed simultaneously with step S1, the multi-mode collaborative control module of the scanning acoustic microscope enables synchronous triggering of C-scan and T-scan and synchronous data acquisition, ensuring the consistency of detection conditions.
4. The method according to claim 1, characterized in that, In step S3, during the backside C-scan, an ultrasonic coupling agent is applied to the backside of the substrate. The coupling agent is a water-soluble ultrasonic coupling agent, and the thickness is controlled at 0.1-0.2 mm to ensure efficient transmission of ultrasonic waves.
5. The method according to claim 1, characterized in that, In step S4, the thickness resolution of the tomographic imaging of the B scan is ≤1μm. By adjusting the depth sampling interval of the scanning acoustic microscope, accurate imaging of the thickness direction of the chip adhesive layer is achieved.
6. The method according to claim 1, characterized in that, In step S5, a diamond cutting disc is used for precision cutting during the sample preparation process. The cutting speed is controlled at 1-2 mm / s to avoid secondary damage to the chip bonding layer during the cutting process.
7. The method according to claim 1, characterized in that, The method is also applicable to the determination of voids or impurities between molding compounds, delamination between the substrate and molding compound, and delamination defects between the lead frame and molding compound. When making the determination, only the focusing area and the acoustic interface reference of the waveform analysis in each scanning step need to be adjusted.
Citation Information
Patent Citations
Method for judging defects of flash memory plastic packaging device based on acoustic scanning