Ultra-thick tabular tungsten oxide and preparation method thereof
By controlling the dissolution and calcination conditions of ammonium tungstate, ultra-coarse plate-shaped tungsten oxide was prepared, solving the problems of easy agglomeration and disordered morphology of tungsten oxide, improving dielectric and breakdown properties, making it suitable for high-end applications, and reducing production costs.
Patent Information
- Application Number
- CN202511961317.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-24
- Publication Date
- 2026-01-23
- Estimated Expiration
- 2045-12-24
AI Technical Summary
Existing tungsten oxide materials are prone to agglomeration at the nanoscale, are costly, and pose significant safety risks. Bulk or ordinary particulate tungsten oxide has many grain boundary defects, small specific surface area, and poor processing compatibility, resulting in fluctuations in the dielectric properties of functional ceramics, short battery cycle life, decreased sensor sensitivity, insufficient catalytic activity, and weak coating protection, making it difficult to meet the needs of high-end applications.
Using ammonium tungstate as raw material, ultra-coarse plate-shaped tungsten oxide was prepared by controlling the dissolution temperature, cooling rate, and calcination temperature and time, ensuring a purity ≥99%, crystallinity ≥90%, aspect ratio ≥5:1, and average width ≥180μm. A high-purity alumina ceramic boat was used to avoid material reaction and form a complete plate-shaped structure.
It achieves tungsten oxide with uniform particle size and complete plate shape, improves dielectric and breakdown properties, is suitable for multiple high-end scenarios, reduces production costs, is green and safe, and is easy to operate.
Smart Images

Figure CN121377119A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of functional materials, and particularly relates to super coarse plate-shaped tungsten oxide and a preparation method thereof. BACKGROUND
[0002] In the current field of functional materials, tungsten oxide is widely used in functional ceramics, energy storage, photocatalysis, sensing and protection and other important fields due to its unique physical and chemical properties, and has become one of the key materials for promoting the development of related industries.
[0003] The current tungsten oxide has obvious limitations: nano-tungsten oxide is prone to agglomeration, has high cost and safety risks, resulting in fluctuations in the dielectric properties of functional ceramics, short battery cycle life, and decreased sensitivity of sensors; block or ordinary particle tungsten oxide has many grain boundary defects, small specific surface area and poor processing compatibility, resulting in low ceramic breakdown field strength, insufficient catalytic activity, weak coating protection, and overall imbalance between form and performance, poor long-term reliability, and difficulty in meeting the needs of high-end applications.
[0004] The development of super coarse plate-shaped tungsten oxide can solve the above problems, and through unique structural design, it can realize the synergistic optimization of performance and practicability, promote the technological upgrading of strategic industries such as functional ceramics and energy storage, enrich the theoretical system of functional materials, meet the needs of multiple fields for material performance and reliability, reduce production costs, and has broad application prospects and significant economic and social benefits. SUMMARY
[0005] To solve the above technical problems, the application provides a preparation method of super coarse plate-shaped tungsten oxide, comprising the following steps: S1, ammonium tungstate is added to deionized water, stirred and dissolved at a temperature of 70-90 DEG C to obtain a clear ammonium tungstate solution; S2, the clear ammonium tungstate solution is cooled to room temperature at a cooling rate of 0.5-2 DEG C / h, and then filtered to obtain plate-shaped ammonium tungstate crystals; S3, the plate-shaped ammonium tungstate crystals are calcined to obtain super coarse plate-shaped tungsten oxide.
[0006] Further, ammonium tungstate is added to deionized water, and the temperature for stirring and dissolving is any one or a range between any two of 70 DEG C, 80 DEG C and 90 DEG C. Further, the cooling rate of the clear ammonium tungstate solution to room temperature is any one or a range between any two of 0.5 DEG C / h, 1.0 DEG C / h, 1.5 DEG C / h and 2.0 DEG C / h.
[0007] In the step S1, the concentration of the clear ammonium tungstate solution is 300-450 g / L in terms of WO3.
[0008] The temperature of the calcination in the step S3 is 500-700 DEG C, and the time is 1-3 hours.
[0009] The step S3 is specifically placing the plate-shaped ammonium tungstate crystal in a ceramic boat, and then placing the ceramic boat in a muffle furnace to perform aerobic calcination to obtain the super coarse plate-shaped tungsten oxide.
[0010] The ceramic boat is an alumina ceramic boat, and the purity of the alumina ceramic boat is greater than or equal to 99%.
[0011] To solve the above technical problems, the application further provides a super coarse plate-shaped tungsten oxide prepared by the preparation method of the super coarse plate-shaped tungsten oxide.
[0012] The purity of the super coarse plate-shaped tungsten oxide is greater than or equal to 99%.
[0013] The crystallinity of the super coarse plate-shaped tungsten oxide is greater than or equal to 90% in terms of WO3.
[0014] The aspect ratio of the super coarse plate-shaped tungsten oxide is greater than or equal to 5:1.
[0015] The average width of the super coarse plate-shaped tungsten oxide is greater than or equal to 180 microns.
[0016] The application uses ammonium tungstate as a raw material, has high controllability, and obtains tungsten oxide with uniform particle size and complete plate shape through optimized crystallization and calcination, has a purity of greater than or equal to 99%, solves the problems of traditional tungsten oxide agglomeration and chaotic morphology, has strong functional adaptability, the plate-shaped structure can be oriented, improves the dielectric, breakdown and other performances, is suitable for many high-end scenes, and is easy to control and simple to operate. BRIEF DESCRIPTION OF DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the application or the prior art, the following will briefly introduce the drawings needed to be used in the embodiments or the prior art description. Obviously, the drawings in the following description only some embodiments of the application, and for those skilled in the art, without creative labor, other drawings can also be obtained from the structure shown in the drawings.
[0018] Figure 1 The SEM graph of the super coarse plate-shaped tungsten oxide prepared in Example 1 is shown in the following figure. Figure 2 The XRD graph of the super coarse plate-shaped tungsten oxide prepared in Example 1 is shown in the following figure. Figure 3 The SEM graph of the super coarse plate-shaped tungsten oxide prepared in Example 2 is shown in the following figure. Figure 4 The SEM graph of the super coarse plate-shaped tungsten oxide prepared in Example 3 is shown in the following figure. Figure 5 SEM image of the ultra coarse plate-like tungsten oxide prepared in Comparative Example 1; Figure 6 SEM image of the ultra fine tungsten oxide prepared in Comparative Example 2; Figure 7 SEM image of the polygonal tungsten oxide prepared in Comparative Example 4.
[0019] The implementation, functional features and advantages of the present application will be further described with reference to the embodiments and the accompanying drawings. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments will be described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all the other embodiments obtained by a person of ordinary skill in the art without creative work fall within the protection scope of the present application.
[0021] The present application provides a preparation method of ultra coarse plate-like tungsten oxide, comprising the following steps: S1, adding ammonium tungstate into deionized water, stirring and dissolving at a temperature of 70-90℃ to obtain a clear ammonium tungstate solution; In the present application, the concentration of the clear ammonium tungstate solution is 300-450g / L in terms of WO3. Too low concentration is easy to result in low crystallization efficiency and fine crystal particles. Too high concentration is easy to result in large solution viscosity and local supersaturation and caking. In the present application, the temperature for dissolving ammonium tungstate is 70-90℃. Too high temperature will increase energy consumption, and too low temperature will possibly result in insufficient dissolution and residual unsolved solids.
[0022] S2, cooling the clear ammonium tungstate solution to normal temperature at a cooling rate of 0.5-2℃ / h, and then performing suction filtration to obtain plate-like ammonium tungstate crystals; In the present application, the cooling rate of the clear ammonium tungstate solution is 0.5-2℃ / h. Slow cooling can promote ordered growth of the crystals, forming crystals with uniform particles and high purity. Too fast cooling rate is easy to produce a large number of fine crystal nuclei, and the crystals are easy to agglomerate. Too slow cooling rate will result in too long cooling time.
[0023] S3, calcining the plate-like ammonium tungstate crystals to obtain ultra coarse plate-like tungsten oxide.
[0024] In the present application, the calcination temperature is 500-700℃, and if the temperature is too low, the ammonium tungstate is not completely decomposed, and the crystal cannot be fully converted into WO3, it is difficult to form a complete plate-like structure, and loose porous irregular particles are prone to occur; if the temperature is too high, the WO3 crystal grains are prone to excessive growth and sintering agglomeration, the plate-like structure is destroyed, and massive or molten tungsten oxide is formed, losing the morphological characteristics of "ultra coarse plate-like". In the present application, the calcination time is 1-3h, and if the calcination time is too short, the ammonium tungstate is not completely decomposed, and the tungsten oxide is mixed with undecomposed products, and the plate-like structure is not fully developed; if the time is too long, although complete decomposition can be ensured, energy consumption will be increased, and the edges of the WO3 plate-like crystal grains may be excessively sintered, making the plate-like structure thicker and more brittle, and affecting the processing performance in subsequent applications.
[0025] In the present application, high-purity alumina ceramic boats (purity greater than or equal to 99%) are used for calcination, which avoids the reaction between the boat material and WO3 at high temperature, and ensures the purity and morphology stability of the ultra coarse plate-like tungsten oxide.
[0026] Example 1 Ammonium tungstate is taken and added to deionized water to prepare a clear ammonium tungstate solution with a concentration of 300g / L (calculated as WO3), and the solution is dissolved by stirring at 70℃; the ammonium tungstate solution is cooled to room temperature at a rate of 0.5℃ / h by standing in a crystallization container; the cooled ammonium tungstate solution is filtered to obtain plate-like ammonium tungstate crystals; the plate-like ammonium tungstate crystals are placed in a ceramic boat, and then placed in a muffle furnace for calcination, the calcination temperature is 500℃, and the calcination time is 1h, to obtain ultra coarse plate-like tungsten oxide; Please refer to Figure 1 , Figure 1 The SEM image of the ultra coarse plate-like tungsten oxide prepared in Example 1 is shown in Figure 1 , from which it can be seen that the crystal has a complete ultra coarse plate-like morphology, the particles are uniformly dispersed, there is no obvious agglomeration, the plate-like edges are regular, the surface is smooth, and the size uniformity is good; please further refer to Figure 2 , Figure 2 The XRD pattern of the ultra coarse plate-like tungsten oxide prepared in Example 1 is shown in Figure 2 , from which it can be seen that the characteristic diffraction peaks of WO3 in the pattern are sharp and have high intensity, and no impurity peaks are present, indicating that the internal structure of the crystal is regular, the crystal lattice is ordered, and there is no impurity phase interference.
[0027] The ultra coarse plate-like tungsten oxide is detected, and the purity is 99.99%, the crystallization rate is 91.43% (calculated as WO3), the length-width ratio is greater than 5:1, and the average width is 220μm.
[0028] Example 2 Ammonium tungstate was taken and added to deionized water to prepare a clear ammonium tungstate solution with a concentration of 450 g / L (calculated as WO3), which was dissolved by stirring at 90℃; the ammonium tungstate solution was left to stand in a crystallization container and cooled at a rate of 2℃ / h to room temperature; the cooled ammonium tungstate solution was subjected to suction filtration to obtain plate-shaped ammonium tungstate crystals; the plate-shaped ammonium tungstate crystals were placed in a ceramic boat, which was then placed in a muffle furnace for calcination at a temperature of 700℃ for 3h to obtain super-coarse plate-shaped tungsten oxide; See Figure 3 , Figure 3 The SEM image of the super-coarse plate-shaped tungsten oxide prepared in Example 2 is shown in Figure 3 It can be seen from the SEM image that the plate-shaped tungsten oxide crystals have significantly increased in size, are thick and have complete edges, and have excellent dispersibility without sintering agglomeration.
[0029] The super-coarse plate-shaped tungsten oxide was detected to have a purity of 99.99%, a crystallization rate of 95.64% (calculated as WO3), a length-width ratio of greater than 5:1, and an average width of 241μm.
[0030] Example 3 Ammonium tungstate was taken and added to deionized water to prepare a clear ammonium tungstate solution with a concentration of 400 g / L (calculated as WO3), which was dissolved by stirring at 80℃; the ammonium tungstate solution was left to stand in a crystallization container and cooled at a rate of 1℃ / h to room temperature; the cooled ammonium tungstate solution was subjected to suction filtration to obtain plate-shaped ammonium tungstate crystals; the plate-shaped ammonium tungstate crystals were placed in a ceramic boat, which was then placed in a muffle furnace for calcination at a temperature of 600℃ for 2h to obtain super-coarse plate-shaped tungsten oxide; See Figure 4 , Figure 4 The SEM image of the super-coarse plate-shaped tungsten oxide prepared in Example 3 is shown in Figure 4 It can be seen from the SEM image that the plate-shaped surface is smooth and the particles are uniform, and the size and morphology are between those of Example 1 and Example 2.
[0031] The super-coarse plate-shaped tungsten oxide was detected to have a purity of 99.99%, a crystallization rate of 93.25% (calculated as WO3), a length-width ratio of greater than 5:1, and an average width of 190μm.
[0032] Comparative Example 1 Unlike Example 1, the solution was stirred at 60℃, and there were undissolved ammonium tungstate crystals in the ammonium tungstate solution; See Figure 5 , Figure 5 The SEM image of the super-coarse plate-shaped tungsten oxide prepared in Comparative Example 1 is shown in Figure 5It can be seen from the SEM image in FIG. 1 that the crystal has retained some plate-like features, but there are a small amount of fine particle agglomerates, and some of the plate-like crystals are small in size and have rough edges. The low dissolution temperature resulted in incomplete dissolution of the ammonium tungstate, and the residual raw material affected the uniformity of the crystal growth.
[0033] The ultra-coarse plate-like tungsten oxide was detected to have a purity of 99.99% and a crystallization rate of 92.71% (calculated based on WO3). The length-width ratio was greater than 5:1, and the average width was 131 μm.
[0034] Comparative Example 2 Unlike Example 1, the ammonium tungstate solution was left to stand in the crystallization vessel, and was cooled at a rate of 5°C / h to room temperature. Ultra-fine tungsten oxide was obtained. See FIG. 2, Figure 6 , Figure 6 FIG. 2 is a SEM image of the ultra-fine tungsten oxide obtained in Comparative Example 2, Figure 6 It can be seen from the SEM image in FIG. 2 that there is no plate-like structure, and only a large number of nanoscale fine particle agglomerates are present. The particle size is small, and the rapid cooling rate produced too many crystal nuclei, so the crystals could not grow in an orderly manner.
[0035] The ultra-fine tungsten oxide was detected to have a purity of 99.99% and a crystallization rate of 90.89% (calculated based on WO3).
[0036] Comparative Example 3 Unlike Example 1, a clear ammonium tungstate solution was prepared, and the concentration was 100 g / L (calculated based on WO3). The ultra-coarse plate-like tungsten oxide was detected to have a purity of 99.99% and a crystallization rate of 66.87% (calculated based on WO3). The length-width ratio was greater than 5:1, and the average width was 201 μm.
[0037] Comparative Example 4 Unlike Example 1, the plate-like ammonium tungstate crystals were placed in a ceramic boat, and then were placed in a muffle furnace for calcination. The calcination temperature was 800°C, and the calcination time was 1 h. This resulted in polyhedral tungsten oxide. See FIG. 4, Figure 7 , Figure 7 FIG. 4 is a SEM image of the polyhedral tungsten oxide obtained in Comparative Example 4, Figure 7 It can be seen from the SEM image in FIG. 4 that the plate-like structure was destroyed, and the crystals appeared as irregular polyhedral blocks. The WO3 grains grew excessively and agglomerated due to the high calcination temperature.
[0038] The polyhedral tungsten oxide was detected to have a purity of 99.99% and a crystallization rate of 91.76% (calculated based on WO3).
[0039] The application adopts ammonium tungstate as raw material, has high controllability, and obtains uniform particle size, complete plate-shaped tungsten oxide with purity of 99% or more by optimized crystallization and calcination, solves the problems of traditional tungsten oxide agglomeration and chaotic form. The function adaptability is strong, the plate-shaped structure can be oriented, the dielectric, breakdown and other performances are improved, and the product is suitable for multiple high-end scenes; the parameters are easy to control, the operation is simple, and the product is green and safe.
[0040] The above only describes the preferred embodiments of the application, and does not limit the patent range of the application, and any equivalent structural transformation, direct / indirect application in other related technical fields made by using the content of the application specification under the inventive concept of the application are included in the patent protection range of the application.
Claims
1. A method for producing ultra-coarse plate-like tungsten oxide, characterized by, The method comprises the following steps: S1, adding ammonium tungstate into deionized water, stirring and dissolving at a temperature of 70-90℃ to obtain a clear ammonium tungstate solution; S2, cooling the clear ammonium tungstate solution to normal temperature at a cooling rate of 0.5-2℃ / h, and then performing suction filtration to obtain plate-shaped ammonium tungstate crystals; S3, calcining the plate-shaped ammonium tungstate crystals to obtain ultra-coarse plate-shaped tungsten oxide.
2. The method of claim 1, wherein the method is characterized by: In the step S1, the concentration of the clear ammonium tungstate solution is 300-450g / L in terms of WO3.
3. The method of claim 1, wherein the method is characterized by: In the step S3, the calcination temperature is 500-700℃, and the time is 1-3h.
4. The method of claim 1, wherein the method is characterized by: In the step S3, the plate-shaped ammonium tungstate crystals are placed in a ceramic boat, and then put into a muffle furnace for aerobic calcination to obtain the ultra-coarse plate-shaped tungsten oxide.
5. The method for preparing ultra-coarse plate-shaped tungsten oxide according to claim 4, characterized in that, The ceramic boat is an alumina ceramic boat, and the purity of the alumina ceramic boat is greater than or equal to 99%.
6. An ultra-coarse platelet-shaped tungsten oxide, characterized by, The ultra-coarse plate-shaped tungsten oxide is prepared by the preparation method of the ultra-coarse plate-shaped tungsten oxide according to any one of claims 1-5.
7. The ultra coarse plate-like tungsten oxide according to claim 6, wherein The purity of the ultra-coarse plate-shaped tungsten oxide is greater than or equal to 99%.
8. The ultra coarse plate-like tungsten oxide according to claim 6, wherein The crystallinity of the ultra-coarse plate-shaped tungsten oxide is greater than or equal to 90% in terms of WO3.
9. The ultra coarse plate-like tungsten oxide according to claim 6, wherein The aspect ratio of the ultra-coarse plate-shaped tungsten oxide is greater than or equal to 5:
1.
10. The ultra coarse plate-like tungsten oxide according to claim 6, wherein The average width of the ultra-coarse plate-shaped tungsten oxide is greater than or equal to 180μm.
Citation Information
Patent Citations
High-purity nano tungsten oxide, preparation method thereof, electrode material and battery
CN115947374A
Uniform nano tungsten oxide and preparation method thereof, electrode material and battery
CN116216782A
Preparation method of high-purity nano tungsten oxide
CN120774466A
Rapid preparation method of tungsten trioxide
CN121181030A
Method for producing tungsten trioxide
JP2019142760A
Cited By
Spherical-like nano tungsten oxide and preparation method thereof
CN121894707A