Sliding bearing surface modification method

By employing cold metal transition arc additive manufacturing technology on the surface of sliding bearings, first cladding a nickel-based alloy intermediate layer and then a copper-based alloy wear-resistant layer, the problems of high performance and low cost of wind turbine sliding bearings have been solved, and the process stability and material utilization rate have been improved.

CN121423760APending Publication Date: 2026-01-30RICO ADDITIVE IND TECHNOLOGY (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511600348.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-04
Publication Date
2026-01-30

AI Technical Summary

Technical Problem

Existing technologies struggle to balance high performance, low cost, and process stability in wind turbine sliding bearings, particularly due to issues such as low material utilization, numerous internal defects, poor bonding strength, and a wide heat-affected zone in the manufacturing process.

Method used

Using cold metal transition arc additive manufacturing technology, a nickel-based alloy intermediate layer is first fused onto the surface of the sliding bearing substrate, and then a copper-based alloy wear-resistant layer is fused onto it. By controlling the welding parameters and vibration aging treatment, a dense metallurgical bond is formed and residual stress is eliminated.

Benefits of technology

It improves the wear resistance, fatigue strength and load-bearing capacity of bearings, extends their service life, and reduces production costs and cycle time, while avoiding internal defects and matrix deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121423760A_ABST
    Figure CN121423760A_ABST
Patent Text Reader

Abstract

The invention discloses a sliding bearing surface modification method which comprises the following steps: pretreating a sliding bearing matrix to obtain a clean and dehumidified surface; the pretreated base body is fixed to a rotating tool so as to ensure the stability and concentricity in the cladding process; cladding a nickel-based alloy middle layer on the surface of the matrix by adopting a cold metal transition electric arc additive manufacturing technology; machining the nickel-based alloy intermediate layer to remove surface oxide skin and formed ripples so as to obtain a flat substrate; cladding a copper-based alloy wear-resistant layer on the machined middle layer by adopting a cold metal transition electric arc additive manufacturing technology; and carrying out stress relief treatment on the clad workpiece. Through the gradient design that the nickel-based alloy is firstly cladded to serve as the middle layer and then the tin bronze is cladded to serve as the wear-resistant layer, the problem that direct combination is difficult due to large physical property difference between the steel substrate and the copper alloy is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of additive manufacturing technology, specifically to a method for modifying the surface of a sliding bearing. Background Technology

[0002] Sliding bearings are core components in wind turbine gearboxes and other major equipment, and their performance directly determines the transmission efficiency, reliability, and service life of the equipment. These operating conditions are typically characterized by low speed, heavy load, impact load, and difficulty in ensuring absolutely ideal lubrication conditions, which places extremely high demands on the wear resistance, fatigue resistance, and bonding strength of the bearing surface.

[0003] The wear-resistant layer preparation process of heavy-duty sliding bearings in wind turbines has several inherent defects: Centrifugal casting: The process route is long, with many steps from smelting to machining; the material utilization rate is low and the machining allowance is large; the casting layer is prone to internal defects such as shrinkage cavities and segregation, which affect fatigue strength.

[0004] Powder sintering method: Although the inherent porosity of the wear-resistant layer can store oil, it reduces the load-bearing strength and crush resistance; the bonding strength between the layer and the substrate is low, mostly mechanically interlocked, and has poor impact resistance.

[0005] Traditional surfacing welding method: high heat input, resulting in large workpiece deformation and wide heat-affected zone; severe dilution of the substrate, contaminating the wear-resistant layer composition; poor forming quality, easy to produce porosity and slag inclusions, and large amount of subsequent processing.

[0006] Laser cladding: The equipment and powder materials are expensive; the deposition efficiency is low, and it is not economical for large-size bearings, making it difficult to apply on a large scale.

[0007] Therefore, existing technologies struggle to balance high performance, low cost, and process stability, necessitating a new solution. Summary of the Invention

[0008] To address the existing problems, this invention provides a method for modifying the surface of a sliding bearing to solve the aforementioned issues.

[0009] A method for modifying the surface of a sliding bearing, comprising: The sliding bearing substrate is pretreated by heating to remove moisture and contaminants, and then laser cleaning technology is used to obtain an active clean surface. The pre-treated sliding bearing base is precisely clamped onto a rotating fixture to ensure that the runout after clamping is less than 0.1 mm; A nickel-based alloy intermediate layer is fused onto the surface of the sliding bearing substrate using cold metal transition arc additive manufacturing technology. By controlling welding parameters such as current, voltage and wire feed speed, the nickel-based alloy intermediate layer forms a dense metallurgical bond with the sliding bearing substrate, and plays a role in gradient transition of thermal expansion coefficient and blocking element diffusion. The nickel-based alloy intermediate layer is machined and turned to remove surface oxide scale and ripples, resulting in a flat substrate with uniform thickness. The cold metal transition arc additive manufacturing technology was used again to clad a copper-based alloy wear-resistant layer onto the machined nickel-based alloy intermediate layer. By adjusting the process parameters, it was ensured that the copper-based alloy wear-resistant layer was free of pores and cracks and exhibited a dense structure. After cladding, the workpiece is subjected to vibration aging treatment, vibrating at the resonant frequency for 15 to 25 minutes to eliminate residual stress and stabilize dimensions.

[0010] In one possible implementation, the removal of moisture and contaminants by heating is carried out using flame heating, with the temperature controlled between 58°C and 62°C; the process parameters for laser cleaning include: laser power of 400–800W, cleaning speed of 200–450 mm / min, and surface roughness Ra after cleaning not exceeding 3.2 μm.

[0011] In one possible implementation, when cladding the nickel-based alloy intermediate layer and the copper-based alloy wear-resistant layer, the welding torch is at an angle of 85° to 95° to the central axis of the sliding bearing substrate, and is oscillating with an oscillation width of 5 to 8 mm and a frequency of 1.5 to 2.5 Hz.

[0012] In one possible implementation, the nickel-based alloy intermediate layer is a nickel-chromium alloy or a nickel-based high-temperature alloy with a thickness of 0.2 to 2.5 mm; the copper-based alloy wear-resistant layer is a tin bronze alloy with a thickness of 1.2 to 2.2 mm, used to form a gradient functional structure to improve load-bearing capacity and wear resistance. In one possible implementation, the process parameters for cladding the nickel-based alloy intermediate layer are: welding current 160-220A, arc voltage 17.5-19.5V, wire feed speed 6.5-7.5m / min, shielding gas is argon, flow rate 17-22L / min; The process parameters for cladding the copper-based alloy wear-resistant layer are as follows: welding current 160-200A, arc voltage 16.0-18.0V, wire feed speed 5.5-6.5m / min, shielding gas is argon, flow rate 17-22L / min.

[0013] In one possible implementation, during the vibration aging process, an accelerometer is used to monitor the vibration curve. When the vibration curve changes from steep to flat, the vibration is stopped to ensure that the residual stress changes from tensile stress to compressive stress, and the stress value is reduced to below 65 MPa. In one possible implementation, the penetration depth between the copper-based alloy wear-resistant layer and the nickel-based alloy intermediate layer is less than 0.1 mm, and the penetration depth between the nickel-based alloy intermediate layer and the sliding bearing substrate is less than 0.5 mm.

[0014] In one possible implementation, the metallographic structure of the copper-based alloy wear-resistant layer is a dense morphology of mixed grains of different sizes, with a porosity of less than 0.5%.

[0015] Compared with the prior art, the present invention has the following advantages: 1. By employing a gradient design—first cladding a nickel-based alloy as an intermediate layer, then cladding a tin bronze layer as a wear-resistant layer—the problem of direct bonding between the steel substrate and the copper alloy due to significant differences in physical properties is effectively solved. The intermediate layer serves a dual purpose: buffering stress and preventing the diffusion of iron elements from the substrate into the wear-resistant layer, thus ensuring the stability of the wear-resistant layer's composition and performance.

[0016] 2. By using the cold metal transition arc additive manufacturing process, a dense metallurgical bonding layer is obtained, which eliminates inherent defects such as shrinkage cavities and segregation compared with traditional casting; compared with sintering, a cladding layer with no pores and high bonding strength is achieved; compared with traditional welding, the extremely low heat input avoids matrix deformation and microstructure deterioration, thereby significantly improving the wear resistance, fatigue strength and load-bearing capacity of the bearing and extending its service life.

[0017] 3. Using wire as raw material, the cost is much lower than that of metal powder used in laser cladding, and the material utilization rate is high. At the same time, the high deposition efficiency of cold metal transfer technology makes the process have a shorter production cycle when cladding large areas, overcoming the problems of expensive and relatively low efficiency of laser cladding equipment. Attached Figure Description

[0018] Figure 1 This is a flowchart of a sliding bearing surface modification method according to the present invention; Figure 2 This is a schematic diagram of the cross-sectional shape of the sliding bearing of the present invention; Figure 3 This is a schematic diagram of the metallographic image of the copper-tin coating of the present invention. Detailed Implementation

[0019] The embodiments of this disclosure will now be described in detail with reference to the accompanying drawings.

[0020] The following specific examples illustrate the implementation of this disclosure. Those skilled in the art can easily understand other advantages and effects of this disclosure from the content disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of this disclosure, and not all of them. This disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of this disclosure. It should be noted that, in the absence of conflict, the following embodiments and features in the embodiments can be combined with each other. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this disclosure.

[0021] It should be noted that the following description covers various aspects of embodiments within the scope of the appended claims. It will be apparent that the aspects described herein can be embodied in a wide variety of forms, and any particular structure and / or function described herein is merely illustrative. Based on this disclosure, those skilled in the art will understand that one aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. It should also be noted that the illustrations provided in the following embodiments are merely schematic representations of the basic concept of this disclosure. The illustrations only show structures relevant to this disclosure and are not drawn according to the actual number, shape, and size of structures in implementation. In actual implementation, the form, number, and proportion of each structure can be arbitrarily changed, and its structural layout may also be more complex.

[0022] Furthermore, specific details are provided in the following description to facilitate a thorough understanding of the examples. However, those skilled in the art will understand that the described aspects can be practiced without these specific details.

[0023] A method for modifying the surface of a sliding bearing includes the following steps: S1. Pretreatment: The sliding bearing substrate is pretreated by heating to remove moisture and contaminants, and then laser cleaning technology is used to obtain an active clean surface. The process involves removing moisture and contaminants through heating using a flame heating method, with the temperature controlled between 58°C and 62°C. The laser cleaning process parameters include: laser power of 400–800W, cleaning speed of 200–450 mm / min, and a post-cleaning surface roughness Ra not exceeding 3.2 μm. Flame heating thoroughly removes moisture and low-boiling-point contaminants from the substrate material surface and any adsorbed substances, preventing porosity (especially hydrogen porosity) during subsequent welding. Laser cleaning removes oxide scale, oil, and trace residues from the area to be clad, resulting in an active, clean surface that ensures high-quality metallurgical bonding.

[0024] S2. Clamping: Precisely clamp the pre-treated sliding bearing base onto the rotating fixture to ensure that the runout after clamping is less than 0.1 mm; Specifically, the pre-treated sliding bearing substrate is mounted on a CNC machine tool or a dedicated positioner. One end is held by a three-jaw chuck, and the other end is secured to the center process hole of the substrate using a rotary center. Achieving precise and stable rotation of the bearing during additive manufacturing is fundamental to ensuring the uniformity and roundness of the cladding layer.

[0025] S3. Preparation of intermediate layer: Using cold metal transition arc additive manufacturing technology, a nickel-based alloy intermediate layer is fused onto the surface of the sliding bearing substrate; by controlling welding parameters such as current, voltage and wire feed speed, the nickel-based alloy intermediate layer and the sliding bearing substrate form a dense metallurgical bond, and play the role of gradient transition of thermal expansion coefficient and blocking element diffusion. The specific process parameters are as follows: welding current 160–220A, arc voltage 17.5–19.5V, wire feed speed 6.5–7.5m / min, shielding gas is argon, flow rate 17–22L / min. A spiral path is used for multi-pass overlapping cladding, with a single layer thickness of approximately 2.0–2.5mm.

[0026] S4. Machining: The nickel-based alloy intermediate layer is machined to remove surface oxide scale and ripples, and a flat base with uniform thickness is obtained; the final nickel-based alloy intermediate layer has a uniform thickness of 1 mm.

[0027] S5. Preparation of wear-resistant layer: The cold metal transition arc additive manufacturing technology is used again to clad a copper-based alloy wear-resistant layer on the intermediate layer of the machined nickel-based alloy. By adjusting the process parameters, it is ensured that the copper-based alloy wear-resistant layer is free of pores and cracks and has a dense structure. The copper-based alloy wear-resistant layer is a tin bronze alloy with a thickness of 1.2–2.2 mm. The welding current is 160–200 A, the arc voltage is 16.0–18.0 V, the wire feed speed is 5.5–6.5 m / min, and the shielding gas is argon with a flow rate of 17–22 L / min.

[0028] S6. Stress Relief: Vibration aging treatment is performed on the cladding workpiece, vibrating at the resonant frequency for 15 to 25 minutes to eliminate residual stress and stabilize dimensions.

[0029] During the vibration aging process, an accelerometer is used to monitor the vibration curve. When the vibration curve changes from steep to flat, the vibration is stopped to ensure that the residual stress changes from tensile stress to compressive stress and the stress value is reduced to below 65 MPa. In the products prepared using the present invention, such as Figure 1 and Figure 2As shown, the penetration depth between the copper-based alloy wear-resistant layer and the nickel-based alloy intermediate layer is less than 0.1 mm, and the penetration depth between the nickel-based alloy intermediate layer and the sliding bearing substrate is less than 0.5 mm. The metallographic structure of the copper-based alloy wear-resistant layer is a dense morphology of mixed grains of different sizes, with a porosity of less than 0.5%.

[0030] After the above processing steps are completed, the prepared product undergoes finishing and testing: 1. Finishing: The workpiece is clamped again, and a precision CNC machine tool is used to perform final finishing turning and boring on the tin bronze wear-resistant layer to achieve the dimensional tolerances required by the drawing.

[0031] 2. Non-destructive testing: The entire cladding layer is inspected 100% using dye penetrant testing (PT) or ultrasonic testing (UT) to ensure that there are no welding defects exceeding the standard.

[0032] 3. Dimensional inspection: Use a coordinate measuring machine (CMM) to perform final inspection on the bearing's inner diameter, roundness, cylindricity, and other key dimensions to ensure compliance with design standards.

[0033] The test results are shown in Table 1: Table 1 The bonding strength of the cladding layer was tested according to the GB / T 7314 standard.

[0034] The contents not described in detail in this specification are existing technologies known to those skilled in the art.

[0035] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method of modifying a sliding bearing surface, characterized by, The application relates to a method for manufacturing a sliding bearing, which comprises the following steps: Pre-treating the sliding bearing base, removing moisture and pollutants by heating, and obtaining an active clean surface by laser cleaning; Accurately clamping the pre-treated sliding bearing base on a rotating tool, and ensuring that the run-out after clamping is less than 0.1 mm; Using cold metal transfer arc additive manufacturing technology to melt and clad a nickel-based alloy intermediate layer on the surface of the sliding bearing base; by controlling welding parameters such as current, voltage and wire feeding speed, the nickel-based alloy intermediate layer is formed into a dense metallurgical bond with the sliding bearing base, and plays the role of gradient transition of the thermal expansion coefficient and barrier to element diffusion; Machining and turning the nickel-based alloy intermediate layer to remove surface oxide scales and ripples, and obtaining a uniform and smooth base; Using cold metal transfer arc additive manufacturing technology again to melt and clad a copper-based alloy wear-resistant layer on the machined nickel-based alloy intermediate layer, and adjusting the process parameters to ensure that the copper-based alloy wear-resistant layer is free of pores and cracks and has a dense structure; Performing vibration aging treatment on the cladded workpiece, and vibrating for 15 to 25 minutes at the resonance frequency to eliminate residual stress and stabilize the size.

2. A method of modifying a sliding bearing surface according to claim 1, characterised in that, The moisture and pollutants are removed by flame heating, and the temperature is controlled at 58 DEG C to 62 DEG C; the process parameters of the laser cleaning include that the laser power is 400-800 W, the cleaning speed is 200-450 mm / min, and the surface roughness Ra after cleaning is not greater than 3.2 mu m.

3. A method of modifying a sliding bearing surface according to claim 1, wherein, When the nickel-based alloy intermediate layer and the copper-based alloy wear-resistant layer are cladded, the welding torch is at an angle of 85 DEG to 95 DEG with the central axis of the sliding bearing base, and oscillation is applied, the oscillation width is 5-8 mm, and the frequency is 1.5-2.5 Hz.

4. A method of modifying a sliding bearing surface according to claim 1, wherein, The nickel-based alloy intermediate layer is a nickel-chromium alloy or a nickel-based high-temperature alloy, and the thickness is 0.2-2.5 mm; the copper-based alloy wear-resistant layer is a tin bronze alloy, and the thickness is 1.2-2.2 mm, which is used for forming a gradient functional structure to improve the carrying capacity and wear resistance.

5. A method of modifying a sliding bearing surface according to claim 1, wherein, The process parameters for cladding the nickel-based alloy intermediate layer are as follows: welding current 160-220 A, arc voltage 17.5-19.5 V, wire feeding speed 6.5-7.5 m / min, and the protective gas is argon with a flow rate of 17-22 L / min; The process parameters for cladding the copper-based alloy wear-resistant layer are as follows: welding current 160-200 A, arc voltage 16.0-18.0 V, wire feeding speed 5.5-6.5 m / min, and the protective gas is argon with a flow rate of 17-22 L / min.

6. A method of modifying a sliding bearing surface according to claim 1, wherein, During the vibration aging treatment, an acceleration sensor is used to monitor the vibration curve, and the vibration is stopped when the vibration curve changes from steep to gentle, so that the residual stress is changed from tensile stress to compressive stress, and the stress value is reduced to below 65 MPa.

7. A method of modifying a sliding bearing surface according to claim 1, wherein The penetration between the copper-based alloy wear-resistant layer and the nickel-based alloy intermediate layer is less than 0.1 mm, and the penetration between the nickel-based alloy intermediate layer and the sliding bearing base is less than 0.5 mm.

8. A method of modifying a sliding bearing surface according to claim 7, characterised in that, The metallographic structure of the copper-based alloy wear-resistant layer is a dense mixed grain structure with different sizes, and the porosity is less than 0.5%.