High-humidity-resistant and anti-corrosion alkaline battery positive electrode composite conductive material and preparation method thereof
By constructing a conductive network using modified carbon nanotubes and molybdenum-doped tin dioxide, the problems of easy corrosion and poor conductivity of alkaline battery cathode materials under high humidity are solved, achieving high conductivity and stability. This method is suitable for alkaline batteries in high humidity and strong alkaline environments, reduces production costs, and facilitates industrial production.
Patent Information
- Application Number
- CN202511363518.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-23
- Publication Date
- 2026-02-03
AI Technical Summary
Traditional alkaline battery cathode materials are prone to corrosion and have poor conductivity in high humidity environments, affecting battery performance and lifespan. Furthermore, existing conductive agents increase internal resistance and cost.
A conductive network was constructed using modified carbon nanotubes and molybdenum-doped tin dioxide. Sulfonation treatment was used to improve hydrophilicity and corrosion resistance, pyrrole polymerization coating was used to enhance conductivity, high-temperature treatment was combined to improve electron mobility, and polyvinylidene fluoride and other binders were used to optimize material stability.
It significantly improves conductivity and stability in high humidity environments, reduces battery internal resistance, extends battery life, is suitable for high humidity and strong alkaline environments, reduces production costs, and facilitates industrial production.
Smart Images

Figure SMS_1
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the field of alkaline batteries, in particular to a high-humidity-resistant and corrosion-resistant positive electrode composite conductive material for alkaline batteries and a preparation method thereof. BACKGROUND
[0002] In today's society, with the widespread application of electronic devices and electric vehicles, the demand for high-performance batteries is increasing. Alkaline batteries, as a common type of battery, have been widely used in many fields due to their high energy density and relatively stable performance. However, traditional alkaline battery positive electrode materials have some problems that need to be solved in actual use, which limits their further development and application.
[0003] Firstly, the performance of traditional alkaline battery positive electrode materials can easily decrease in high humidity environments. This is because in humid environments, the material surface can easily adsorb water, causing changes in its chemical properties and physical structure, which in turn affects the conductive performance and the progress of electrochemical reactions. For example, some metal oxide-based positive electrode materials can undergo hydrolysis reactions under high humidity conditions, generating non-conductive hydroxides that block the electron transport path, increasing the internal resistance of the battery and degrading the charge and discharge performance. In addition, high humidity can also exacerbate corrosion within the battery, especially for some positive electrode materials containing metal elements, such as zinc-based positive electrode materials, which are prone to oxidation corrosion, further reducing the performance and service life of the battery.
[0004] Secondly, the corrosion resistance of traditional alkaline battery positive electrode materials is insufficient. During the operation of alkaline batteries, the electrolyte is usually corrosive, which can chemically corrode the positive electrode material. Furthermore, the conductive performance of traditional alkaline battery positive electrode materials needs to be improved. Good conductive performance is a key factor to ensure fast charge and discharge and high power output of the battery. However, many traditional positive electrode materials have poor intrinsic conductivity, such as some metal oxides and composite oxides, which have low electrical conductivity. During the charge and discharge process of the battery, the electron transport resistance is large, resulting in poor rate performance of the battery. In order to improve the conductive performance, a large amount of conductive agent needs to be added, but this will increase the internal resistance and cost of the battery, and too much conductive agent can also affect the structure and stability of the electrode.
[0005] In summary, developing a high-humidity-resistant, corrosion-resistant, and excellent conductive alkaline battery positive electrode composite conductive material is of great practical significance for improving the overall performance of alkaline batteries and expanding their application fields. SUMMARY
[0006] In order to solve the above problems, the application provides a high-humidity-resistant and corrosion-resistant positive electrode composite conductive material of alkaline batteries and a preparation method thereof, which is suitable for high-humidity and strong-alkali environments (such as marine equipment batteries and tropical energy storage systems), has long service life and high output efficiency, and solves the defects of traditional conductive materials, such as easy corrosion and fast attenuation of conductivity. The preparation method is simple to operate, reduces production cost and difficulty, is easy to realize industrial production, and is beneficial to the popularization and application of the technology.
[0007] The technical scheme adopted by the application to achieve the above-mentioned purposes is as follows: A high-humidity-resistant and corrosion-resistant positive electrode composite conductive material of alkaline batteries comprises the following raw materials in parts by weight: modified carbon nanotubes (50-70 parts), flake graphite (20-30 parts), molybdenum-doped SnO2 (5-15 parts), a binder (3-8 parts), and conductive carbon black (0.5-2 parts). The preparation method of the modified carbon nanotubes is as follows: Step 1: carbon nanotubes and p-aminobenzenesulfonic acid are added to an acid solution, and the reaction is carried out at a temperature of 55-65 DEG C for 3-5 h. After the reaction is completed, the carbon nanotubes are separated and purified. Step 2: the carbon nanotubes treated in step 1 are added to an NH4H2PO4 solution, and ultrasonic dispersion is carried out. Then, 20-30% of the total amount of ammonium persulfate is added, and the reaction is carried out under a nitrogen atmosphere and water bath heating to 75-85 DEG C for 0.5-1 h. Then, pyrrole monomers and the remaining ammonium persulfate are added, and the reaction is continued for 1-1.5 h. The reaction is terminated, and centrifugal separation and purification are carried out. Step 3: the carbon nanotubes treated in step 2 are heated at 240-260 DEG C under an argon atmosphere for 0.5-1.5 h, and then heated at 380-410 DEG C under a mixed atmosphere of N2 and H2 for 0.5-1 h. After cooling, the modified carbon nanotubes are obtained.
[0008] Preferably, in step 1, the weight-to-volume ratio of the carbon nanotubes to the acid solution is 1 g: 40-60 mL, the weight ratio of the p-aminobenzenesulfonic acid in the acid solution is 3-5 wt%, and the acid solution is a mixture of sulfuric acid, nitric acid and phosphoric acid in a volume ratio of 2:1-1.5:2-3, wherein the concentration of the sulfuric acid is 95-98%, the concentration of the nitric acid is 65-68%, and the concentration of the phosphoric acid is 85-90%.
[0009] Preferably, in step 2, the weight-to-volume ratio of the carbon nanotubes treated in step 1 to the ammonium dihydrogen phosphate solution is 1 g: 50-100 mL, the concentration of the ammonium dihydrogen phosphate solution is 0.3-0.8 mol / L, the molar volume ratio of the total ammonium persulfate to the ammonium dihydrogen phosphate solution is 0.1-0.2 mol / L, and the volume of the pyrrole monomers is 1-3% of the volume of the ammonium dihydrogen phosphate solution.
[0010] Preferably, in step 3, the volume ratio of H2 to the mixed gas in the N2 and H2 mixed gas is 1-2:100.
[0011] The modified carbon nanotubes described above have the following advantages through three-step processing (sulfonation, pyrrole polymer coating, and high-temperature annealing): the sulfonation treatment (p-aminobenzenesulfonic acid + mixed acid) introduces sulfonic acid groups (-SO3H) on the surface of the carbon nanotubes, improves hydrophilicity and dispersibility, and enhances corrosion resistance. The pyrrole polymer coating forms a conductive polypyrrole (PPy) layer, covers the surface defects of the carbon nanotubes, reduces direct contact with the electrolyte, and inhibits oxidation corrosion. High-temperature treatment removes unstable functional groups, improves electrical conductivity and environmental stability, and mixed gas atmosphere heat treatment (Ar / N2 / H2) precisely controls the chemical state of the carbon nanotube surface. The polypyrrole coating layer improves the interfacial compatibility of the carbon nanotubes with the electrolyte / electrode material, reducing the contact resistance. The carbon nanotubes after high-temperature treatment have higher crystallinity, improved electron mobility, and reduced internal resistance of the battery. At the same time, the chemically modified carbon nanotubes are not prone to aggregation or degradation in alkaline environments, and still maintain good conductive network after long-term cycling.
[0012] Preferably, the preparation method of the molybdenum-doped tin dioxide includes the following steps: Step S1: hydrothermal synthesis of a precursor, dissolving zinc nitrate hexahydrate and ammonium molybdate in deionized water to prepare a mixed solution, adding sodium citrate, adjusting the pH value of the solution to 8.5-9.5 with ammonia water, and then performing hydrothermal reaction at 150-180℃ for 18-24h to generate a precipitate; Step S2: after the precipitate is separated and purified, it is heated at 500-550℃ for 2.5-3.5h, and then cooled to room temperature.
[0013] Preferably, in step S1, the molar ratio of zinc nitrate hexahydrate to ammonium molybdate is 85-95:5-15, the amount of sodium citrate is 1.5-2.5 times the molar amount of zinc ions, and the concentration of ammonia water (NH3·H2O) is 25-28%. The total concentration of zinc ions and ammonium ions in the mixed solution is 0.1-0.3mol / L.
[0014] The molybdenum-doped tin dioxide is synthesized by a hydrothermal method. Molybdenum doping introduces additional free electrons into the SnO2 lattice, enhancing electrical conductivity. SnO2 itself has high chemical stability, and Mo doping further inhibits volume expansion during charging and discharging, reducing the shedding of active materials. Molybdenum-doped tin dioxide is not easily dissolved in alkaline electrolyte, extending the cycle life of the battery.
[0015] The modified carbon nanotube and the molybdenum-doped tin dioxide jointly optimize the conductive network, the modified carbon nanotube constructs a macroscopic conductive skeleton to ensure fast long-distance transmission of electrons, and the molybdenum-doped tin dioxide fills the gaps between the carbon nanotubes and graphite to provide a local high-conductive path and reduce the interface resistance. The flexibility of the modified carbon nanotube buffers the volume change of the molybdenum-doped tin dioxide to prevent the electrode from cracking, and the rigidity of the molybdenum-doped tin dioxide inhibits the agglomeration of the carbon nanotubes to maintain the porous structure. The hydrophobicity of the modified carbon nanotube (PPy coating) reduces the penetration of the electrolyte, and the chemical inertness of the molybdenum-doped tin dioxide further blocks the erosion of corrosive substances (such as OH-), thereby jointly improving the stability in a high-humidity environment.
[0016] Preferably, the binder is one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene, sodium carboxymethyl cellulose, and styrene butadiene rubber (SBR).
[0017] The preparation method of the high-humidity-resistant and corrosion-resistant positive electrode composite conductive material for alkaline batteries described above comprises the following steps: Step a: uniformly mix the modified carbon nanotube, flake graphite, molybdenum-doped SnO2, and conductive carbon black, add part of the solvent to form slurry A; Step b: dissolve the binder in the remaining solvent to form uniform glue B; mix the glue B and the slurry A to obtain the product.
[0018] Preferably, the total amount of the solvent in steps a and b is 3-5 times the weight of the modified carbon nanotube.
[0019] The present application has the following advantages: The high-humidity-resistant and corrosion-resistant positive electrode composite conductive material for alkaline batteries of the present application significantly improves the hydrophobicity and chemical stability by modifying the carbon nanotube, introducing sulfonic acid groups (p-aminobenzenesulfonic acid treatment) and pyrrole polymer coating, and combining high-temperature treatment to inhibit oxidation and corrosion in a high-humidity environment. In the conductive material, the modified carbon nanotube ensures high conductivity, the flake graphite enhances mechanical strength, the molybdenum-doped SnO2 improves electrochemical activity, and the binder balances the adhesion and conductivity with the conductive carbon black. At the same time, the modified carbon nanotube, flake graphite, and conductive carbon black form a three-dimensional conductive network to reduce the interface resistance. The material is particularly suitable for high-humidity and strong-alkali environments (such as marine equipment batteries and tropical energy storage systems), has long service life and high output efficiency, and solves the defects of easy corrosion and rapid decay of conductivity of traditional conductive materials.
[0020] Further, the molybdenum-doped SnO2 enhances the electronic conductivity through molybdenum doping, and the SnO2 itself is corrosion-resistant, thereby synergistically improving the stability of the material in an alkaline environment.
[0021] The preparation method of the application is simple in operation, clear in flow, does not need complex equipment and special process conditions, reduces production cost and production difficulty, is easy to realize industrial production, and is beneficial to popularization and application of the technology. The application adopts the process of slurry A (premixing of conductive material) + glue solution B (binder solution) step-by-step mixing, avoids that the binder wraps the conductive particles, and if the binder and the conductive material are directly mixed, the binder may preferentially wrap the conductive particles (such as carbon nanotubes, molybdenum-doped SnO2), forms an insulating layer, and increases the interface resistance. The slurry A first mixes the conductive material (modified carbon nanotube, flake graphite, molybdenum-doped SnO2, conductive carbon black), ensures that the conductive components are in full contact, and forms a continuous conductive network. The glue solution B is added later, only covers the surface of the slurry A, and reduces the blocking of the conductive path by the binder. The conductive network (carbon nanotube + graphite + molybdenum-doped SnO2) has been pre-built in the slurry A, the glue solution B only plays a fixing role, avoids that the conductive path is blocked by the binder, thereby reduces the electrode internal resistance, improves the battery rate performance and energy efficiency. Meanwhile, the uniform dispersion of the nanomaterial can also be improved, secondary agglomeration is avoided, the problems such as sedimentation and uneven viscosity are reduced, and the scale production is suitable. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the application will be clearly and completely described below in combination with the embodiments of the application. Obviously, the described embodiments are only part of the embodiments of the application, rather than all the embodiments of the application. Based on the embodiments in the application, all other embodiments obtained by those skilled in the art without creative labor fall within the protection scope of the application.
[0023] The raw materials used in the following examples are all ordinary commercially available products. Carbon nanotubes, multi-walled, diameter 20-40 nm, length 5-15 μm; flake graphite, 200 mesh, Qingdao Tianheida Graphite Co., Ltd.; SnO2, 20 nm; conductive carbon black, ingredient content 99.7%, Ruiaite (Tianjin) Chemical Co., Ltd.; zinc nitrate hexahydrate-zinc nitrate hexahydrate, brand: Sigma-aldrich; ammonium molybdate, content 98%, Henan Mingzhixin Chemical Product Co., Ltd.; sodium citrate, 99% purity, white crystal, Qianyao Technology.
[0024] Example 1 A high-humidity-resistant and corrosion-resistant positive electrode composite conductive material for alkaline batteries comprises the following raw materials in parts by weight: modified carbon nanotubes 60 parts, flake graphite 25 parts, molybdenum-doped SnO2 10 parts, binder polyvinylidene fluoride (PVDF) 5 parts, and conductive carbon black 1.5 parts.
[0025] The preparation method of the modified carbon nanotube is as follows: Step 1, carbon nanotubes, p-aminobenzenesulfonic acid are added into acid solution, ultrasonic dispersion, frequency 50 kHz, power 400 W, and the temperature is controlled at 60℃, and the reaction is continued for 4 h, after the reaction is completed, centrifugal separation is carried out, then deionized water is used for washing until pH = 6, and vacuum drying is carried out at 70℃ until the constant weight is obtained; in step 1, the weight / volume ratio of the carbon nanotubes to the acid solution is 1 g:50 mL, the weight ratio of the p-aminobenzenesulfonic acid in the acid solution is 4 wt%, and the acid solution is a mixture of sulfuric acid, nitric acid and phosphoric acid in a volume ratio of 2:1.2:2.5, wherein the concentration of the sulfuric acid is 98%, the concentration of the nitric acid is 68%, and the concentration of the phosphoric acid is 85%; Step 2, the carbon nanotubes treated in step 1 are added into NH4H2PO4 solution, ultrasonic dispersion is carried out for 8 min, the frequency is 40 kHz, ammonium persulfate is added for the first time, the amount of addition is 25% of the total amount of ammonium persulfate, the reaction is carried out under a nitrogen atmosphere, the rotation speed is 400 rpm, water bath heating is carried out at 80℃, and reflux reaction is carried out for 0.8 h; the temperature is maintained unchanged, pyrrole monomer is slowly added through a constant pressure dropping funnel, the dropping rate is controlled to be 1.5 mL / min, the remaining ammonium persulfate is synchronously added, the reaction is continued for 1.2 h (the total reaction time is controlled to be 1.5-2.5 h), a nitrogen atmosphere is maintained throughout the process, then sodium sulfite solution with a concentration of 0.15 mol / L is added to terminate the reaction, the amount of the sodium sulfite solution is 1.5% of the total volume of the reaction system solution, then centrifugal separation is carried out, dehydrated ethanol is used for washing 3-5 times until the centrifugal liquid is colorless and transparent, and vacuum drying is carried out at 70℃ until the constant weight is obtained; in step 2, the weight / volume ratio of the carbon nanotubes treated in step 1 to the ammonium dihydrogen phosphate solution is 1 g:75 ml, the concentration of the ammonium dihydrogen phosphate solution is 0.5 mol / L, the molar volume ratio of the total ammonium persulfate to the NH4H2PO4 solution is 0.15 mol / L, and the volume amount of the pyrrole monomer is 2% of the volume of the NH4H2PO4 solution; Step 3, the carbon nanotubes treated in step 2 are placed in a tube furnace, argon is introduced, the temperature is raised to 250℃ at a rate of 4℃ / min, and the temperature is maintained for 1 h, then the gas is switched to N2 / H2 mixed gas, wherein the proportion of H2 in the mixed gas is 1.5% (volume ratio), the temperature is continuously raised to 400℃, then the temperature is maintained for 0.8 h, and natural cooling is carried out until room temperature is reached, and the molybdenum-doped tin dioxide is obtained.
[0026] The preparation method of the molybdenum-doped tin dioxide comprises the following steps: Step S1: hydrothermal synthesis of precursor, dissolve zinc nitrate hexahydrate and ammonium molybdate in deionized water according to the molar ratio of 90:10, prepare a mixed solution with a total concentration of zinc ions and ammonium ions of 0.2 mol / L, add sodium citrate, the amount is 2 times the molar amount of zinc ions, slowly add 28% ammonia water under magnetic stirring (speed 250 rpm), adjust the pH value of the solution to 9, transfer the mixed solution to a polytetrafluoroethylene lined hydrothermal reactor, place it in an oven for hydrothermal reaction, control the temperature at 170℃, reaction time 21h, after the reaction is completed, it is naturally cooled to room temperature, and a precipitate is obtained; Step S2, the hydrothermal product is washed with deionized water and anhydrous ethanol alternately 4 times (speed 9000 rpm, time 7 min), the residual reactants are removed, the precipitate is placed in a freeze dryer and dried at -50℃, 10Pa for 18h; the dried precursor is placed in a tube furnace, nitrogen is introduced, the temperature is raised to 320℃ at a rate of 4℃ / min, and the temperature is kept for 2h to remove organic residues, then hydrogen-argon mixed gas (the volume fraction of H2 in the mixed gas is 2%) is introduced, the temperature is raised to 520℃ at a rate of 2℃ / min, and the temperature is kept for 3h to complete the crystallization process, and the furnace is cooled to room temperature.
[0027] The preparation method of the high-humidity-resistant and corrosion-resistant positive electrode composite conductive material for alkaline batteries described above comprises the following steps: Step a, add modified carbon nanotubes, flake graphite, molybdenum-doped SnO2, and conductive carbon black into a high-speed mixer (speed 1200 rpm), dry mix for 15 min until uniform, add 50% of the total amount of solvent, continue stirring for 45 min (speed 700 rpm), and form slurry A; Step b, dissolve the binder PVDF in the remaining solvent at 70℃, and ultrasonic treat for 12 min (frequency 40 kHz, power 400 W) to form a uniform glue B; slowly add the glue B to the slurry A, control the drop rate at 3 mL / min, and mechanically stir (speed 300 rpm) at the same time, after the drop is completed, continue to mechanically stir for 30 min to make the system preliminarily homogeneous, then perform intermittent ultrasonic treatment (frequency 40 kHz, power 250 W, ultrasonic treatment for 5 min / interval 2 min to prevent local overheating of the solvent), the total time is 1-2 hours, and the agglomerates are completely broken; finally, mechanically stir (300 rpm) for 10 min again to eliminate the local concentration gradient caused by ultrasonic treatment, and the product is obtained.
[0028] In the above preparation process, the total amount of the solvent in steps a and b is 4 times the weight of the modified carbon nanotubes, and the solvent is NMP.
[0029] Example 2 The application discloses a high-humidity-resistant and corrosion-resistant positive electrode composite conductive material for alkaline batteries, which comprises the following raw materials in parts by weight: modified carbon nanotubes 50 parts, flake graphite 30 parts, molybdenum-doped SnO2 15 parts, a binder polyvinylidene fluoride (PVDF) 3 parts and conductive carbon black 2 parts.
[0030] The preparation method of the modified carbon nanotubes is as follows: In step 1, the weight / volume ratio of the carbon nanotubes to the acid solution is 1 g:60 mL, the weight ratio of the p-aminobenzenesulfonic acid in the acid solution is 5 wt%, and the acid solution is a mixture of sulfuric acid, nitric acid and phosphoric acid in a volume ratio of 2:1:3, wherein the concentration of the sulfuric acid is 98%, the concentration of the nitric acid is 68% and the concentration of the phosphoric acid is 85%. In step 2, the carbon nanotubes treated in step 1 are added into an NH4H2PO4 solution and ultrasonically dispersed for 8 min at a frequency of 40 kHz; 20% of the total amount of ammonium persulfate is first added, and then the remaining ammonium persulfate is added simultaneously at a speed of 2 mL / min under a nitrogen atmosphere at a rotation speed of 300 rpm and with water bath heating at 85 DEG C for 1 h; the temperature is maintained, pyrrole monomers are slowly added through a constant-pressure dropping funnel at a speed of 2 mL / min, and the remaining ammonium persulfate is added simultaneously, and the reaction is continued for 1 h (the total reaction time is controlled to be 1.5-2.5 h); the reaction is terminated and separated and purified according to the method in Example 1; wherein the weight / volume ratio of the carbon nanotubes treated in step 1 to the ammonium dihydrogen phosphate solution is 1 g:100 mL, the concentration of the ammonium dihydrogen phosphate solution is 0.8 mol / L, the molar volume ratio of the total ammonium persulfate to the NH4H2PO4 solution is 0.1 mol / L, and the volume of the pyrrole monomers is 1% of the volume of the NH4H2PO4 solution. In step 3, the carbon nanotubes treated in step 2 are placed in a tube furnace, argon is introduced, the temperature is raised to 240 DEG C at a speed of 3 DEG C / min, and then the temperature is maintained for 1.5 h; subsequently, the mixed gas of N2 / H2 is switched on, wherein the proportion of H2 in the mixed gas is 1% (volume ratio), the temperature is continuously raised to 380 DEG C, and then the temperature is maintained for 1 h; and the temperature is naturally cooled to room temperature.
[0031] The preparation method of the molybdenum-doped SnO2 comprises the following steps: Step S1: hydrothermal synthesis of precursor, zinc nitrate hexahydrate and ammonium molybdate are dissolved in deionized water according to the molar ratio of 85:5 to prepare a mixed solution with a total concentration of zinc ions and ammonium ions of 0.1 mol / L, sodium citrate is added in an amount of 2.5 times the molar amount of zinc ions, 25% ammonia water is slowly added under magnetic stirring (speed 200 rpm), the pH value of the solution is adjusted to 8.5, the mixed solution is transferred to a polytetrafluoroethylene lined hydrothermal reactor, and the hydrothermal reaction is carried out in an oven with a temperature control of 150℃ for 24h, and then naturally cooled to room temperature to obtain a precipitate; Step S2, the washing and drying process is the same as in Example 1, the dried precursor is placed in a tube furnace, nitrogen is introduced, the temperature is raised to 300℃ at a rate of 3℃ / min, and the temperature is maintained for 2.5h to remove organic residues, the hydrogen-argon mixed gas (the volume fraction of H2 in the mixed gas is 1%) is switched to, the temperature is raised to 500℃ at a rate of 1℃ / min, and the temperature is maintained for 3.5h to complete the crystallization process, and then the furnace is cooled to room temperature.
[0032] The preparation method of the high-humidity-resistant and corrosion-resistant alkaline battery positive electrode composite conductive material is the same as in Example 1.
[0033] Example 3 A high-humidity-resistant and corrosion-resistant alkaline battery positive electrode composite conductive material, by weight, includes the following raw materials: modified carbon nanotubes 70 parts, flake graphite 20 parts, molybdenum-doped SnO25 parts, binder polyvinylidene fluoride (PVDF) 8 parts, and conductive carbon black 0.5 parts.
[0034] The preparation method of the modified carbon nanotubes is as follows: Step 1, carbon nanotubes and p-aminobenzenesulfonic acid are added to an acid solution, ultrasonic dispersion, frequency 40kHz, power 500W, and temperature control at 65℃, reaction for 3h, after reaction, centrifugal separation, and then washed with deionized water until pH=5, and vacuum dried at 80℃ until constant weight; in step 1, the weight / volume ratio of the carbon nanotubes to the acid solution is 1g:40mL, the weight ratio of the p-aminobenzenesulfonic acid in the acid solution is 3wt%, and the acid solution is a mixture of sulfuric acid, nitric acid, and phosphoric acid in a volume ratio of 2:1.5:2, wherein the concentration of the sulfuric acid is 98%, the concentration of the nitric acid is 68%, and the concentration of the phosphoric acid is 85%; Step 2, the carbon nanotubes treated in step 1 were added into NH4H2PO4 solution, and ultrasonic dispersion was performed for 10 min at a frequency of 50 kHz. The first amount of ammonium persulfate was added, which was 30% of the total amount of ammonium persulfate. The reaction was performed under a nitrogen atmosphere at a rotation speed of 500 rpm and water bath heating at 75℃ for 0.5 h. The temperature was maintained, and pyrrole monomer was slowly added through a constant pressure dropping funnel at a rate of 1 mL / min. The remaining ammonium persulfate was added synchronously. The reaction was continued for 1.5 h (the total reaction time was controlled to be 1.5-2.5 h). The nitrogen atmosphere was maintained throughout the reaction. The reaction was terminated and purified in the same manner as in Example 1. The weight / volume ratio of the carbon nanotubes treated in step 1 to the ammonium dihydrogen phosphate solution was 1 g:100 mL. The concentration of the ammonium dihydrogen phosphate solution was 0.3 mol / L. The molar volume ratio of the total ammonium persulfate to the ammonium dihydrogen phosphate solution was 0.2 mol / L. The volume of the pyrrole monomer was 3% of the volume of the ammonium dihydrogen phosphate solution. Step 3, the carbon nanotubes treated in step 2 were placed in a tube furnace. Argon was introduced, and the temperature was increased to 260℃ at a rate of 5℃ / min. The temperature was maintained for 0.5 h. Then, N2 / H2 mixed gas was switched on, in which the volume fraction of H2 in the mixed gas was 2%. The temperature was increased to 410℃, and then maintained for 0.5 h. The temperature was naturally cooled to room temperature, and the product was obtained.
[0035] The preparation method of the molybdenum-doped tin dioxide includes the following steps: Step S1: hydrothermal synthesis of a precursor, zinc nitrate hexahydrate and ammonium molybdate were dissolved in deionized water at a molar ratio of 95:15 to prepare a mixed solution with a total concentration of zinc ions and ammonium ions of 0.3 mol / L. Sodium citrate was added in an amount of 1.5 times the molar amount of zinc ions. Concentrated ammonia water with a concentration of 25% was slowly added under magnetic stirring (rotation speed of 300 rpm) to adjust the pH value of the solution to 9.5. The mixed solution was transferred to a polytetrafluoroethylene-lined hydrothermal reactor, which was placed in an oven for hydrothermal reaction at a temperature of 180℃ for 18 h. After the reaction was completed, the temperature was naturally cooled to room temperature, and a precipitate was obtained. Step S2, the washing and drying process was the same as in Example 1. The dried precursor was placed in a tube furnace, and nitrogen was introduced. The temperature was increased to 350℃ at a rate of 5℃ / min, and maintained for 1.5 h to remove organic residues. Hydrogen-argon mixed gas was switched on, in which the volume fraction of H2 in the mixed gas was 3%. The temperature was increased to 550℃ at a rate of 3℃ / min, and maintained for 2.5 h to complete the crystallization process. The furnace was cooled to room temperature, and the product was obtained.
[0036] The preparation method of the high-humidity-resistant and corrosion-resistant alkaline battery positive electrode composite conductive material described above is the same as in Example 1.
[0037] Comparative Example 1 A high-humidity-resistant anticorrosive alkaline battery positive electrode composite conductive material, comprising the following raw materials in parts by weight: carbon nanotubes 60 parts, flake graphite 25 parts, molybdenum-doped SnO2 10 parts, binder polyvinylidene fluoride (PVDF) 5 parts, and conductive carbon black 1.5 parts. The rest is the same as in Example 1.
[0038] Comparative Example 2 A high-humidity-resistant anticorrosive alkaline battery positive electrode composite conductive material, comprising the following raw materials in parts by weight: modified carbon nanotubes 60 parts, flake graphite 25 parts, SnO2 10 parts, binder polyvinylidene fluoride (PVDF) 5 parts, and conductive carbon black 1.5 parts. The rest is the same as in Example 1.
[0039] Comparative Example 3 A high-humidity-resistant anticorrosive alkaline battery positive electrode composite conductive material, comprising the following raw materials in parts by weight: carbon nanotubes 60 parts, flake graphite 25 parts, SnO2 10 parts, binder polyvinylidene fluoride (PVDF) 5 parts, and conductive carbon black 1.5 parts. The rest is the same as in Example 1.
[0040] Comparative Example 4 A method for preparing a high-humidity-resistant anticorrosive alkaline battery positive electrode composite conductive material, specifically comprising directly mixing modified carbon nanotubes, flake graphite, molybdenum-doped SnO2, conductive carbon black, binder PVDF, and a solvent, and the rest is the same as in Example 1.
[0041] Preparation of an alkaline battery: The high-humidity-resistant anticorrosive alkaline battery positive electrode composite conductive materials obtained in Examples 1-3 and Comparative Examples 1-4 are uniformly coated on foamed nickel, and uniformly pressed using a calender roll machine to obtain a positive electrode sheet; a negative electrode zinc paste is prepared by mixing zinc powder 68 parts, zinc oxide 7 parts, and gelled electrolyte (40% KOH + 2% ZnO) 25 parts into a paste; an electrolyte is prepared: 9 mol / L KOH + 0.5 mol / L ZnO + 0.1 mol / L Na2SnO3 (corrosion inhibitor), and the viscosity is adjusted by adding 0.3% sodium polyacrylate; the zinc paste is pressed into a nickel-plated steel shell, a multi-layer composite separator (cellulose / polypropylene non-woven fabric) is used, and the electrolyte is pre-wetted after being immersed. The battery is assembled: steel shell (negative electrode) → zinc paste → separator (pre-wetted) → positive electrode sheet → nickel cover (positive electrode current collector), and then sealed to obtain the alkaline battery.
[0042] Performance test: The internal resistance and capacity of the obtained alkaline battery and the duration under large-current discharge are detected.
[0043] Duration test under large-current discharge mode: the alkaline battery is tested for discharge duration under the conditions of 3.9Ω, 24h / d, and EV: 0.8V (h). The test results are shown in Table 1.
[0044] Table 1, performance test results As can be seen from Table 1, compared with Example 1 and Comparative Examples 1, 3, the internal resistance is reduced and the capacity retention rate is improved, indicating that the grafting of sulfonic acid groups and the coating of polypyrrole significantly improve the conductivity and electrochemical stability. Molybdenum doping improves the capacity retention rate in a high humidity environment (RH 70%) by 7.8% (Example 1 and Comparative Example 2), because molybdenum doping inhibits the corrosion of SnO2 in alkaline solution. Example 1 and Comparative Example 4: Step-by-step mixing process (dry mixing first and then adding glue solution) reduces the internal resistance by 35.6%, because it avoids the wrapping effect of PVDF on the conductive network. In summary, the combination of modified carbon nanotubes (conductive skeleton) + molybdenum-doped SnO2 (corrosion inhibitor) shows significant advantages in a high humidity environment.
[0045] It should be noted that the relational terms herein such as first and second, and the like, are used solely to distinguish one entity or action from another entity or action without necessarily requiring or implying any actual such relationship or order between such entities or actions. Moreover, the terms "comprises", "comprising", or any other variations thereof, are intended to cover a non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements does not include only those elements but can include other elements not expressly listed or inherent to such process, method, article, or apparatus.
[0046] Although embodiments of the present application have been shown and described, it is to be understood that various modifications, substitutions, replacements and variations can be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A high-humidity, corrosion-resistant composite conductive material for the positive electrode of an alkaline battery, characterized in that, By weight parts including the following raw materials: modified carbon nanotubes 50-70 parts, flake graphite 20-30 parts, molybdenum-doped SnO2 5-15 parts, binder 3-8 parts, conductive carbon black, 0.5-2 parts; The preparation method of the modified carbon nanotube is as follows: Step 1: carbon nanotubes and p-aminobenzenesulfonic acid are added to an acid solution, and the reaction is carried out at a temperature of 55-65℃ for 3-5h. After the reaction is completed, the carbon nanotubes are separated and purified; Step 2: the carbon nanotubes treated in step 1 are added to an NH4H2PO4 solution, ultrasonic dispersion is carried out, then 20-30% of the total amount of ammonium persulfate is added, and the reaction is carried out under a nitrogen atmosphere and water bath heating to 75-85℃ for 0.5-1h. Then pyrrole monomer and the remaining ammonium persulfate are added, and the reaction is continued for 1-1.5h. The reaction is terminated, centrifuged and purified; Step 3: the carbon nanotubes treated in step 2 are heated in an argon atmosphere at 240-260℃ for 0.5-1.5h, then heated in a N2 and H2 mixed gas atmosphere at 380-410℃ for 0.5-1h, and then cooled to obtain the product.
2. The high-humidity resistant anticorrosive alkaline battery positive electrode composite conductive material according to claim 1, characterized in that, In step 1, the weight to volume ratio of the carbon nanotubes to the acid solution is 1g:40-60mL, the weight ratio of p-aminobenzenesulfonic acid in the acid solution is 3-5wt%, and the acid solution is a mixture of sulfuric acid, nitric acid and phosphoric acid in a volume ratio of 2:1-1.5:2-3, wherein the concentration of sulfuric acid is 95-98%, the concentration of nitric acid is 65-68%, and the concentration of phosphoric acid is 85-90%.
3. The high-humidity resistant anticorrosive alkaline battery cathode composite conductive material according to claim 1, characterized in that, In step 2, the weight to volume ratio of the carbon nanotubes treated in step 1 to the ammonium dihydrogen phosphate solution is 1g:50-100mL, the concentration of ammonium dihydrogen phosphate solution is 0.3-0.8mol / L, the molar volume ratio of total ammonium persulfate to NH4H2PO4 solution is 0.1-0.2mol / L, and the volume of pyrrole monomer is 1-3% of the volume of NH4H2PO4 solution.
4. The high-humidity resistant, corrosion-resistant, alkaline battery positive composite conductive material of claim 1, wherein, In step 3, the volume ratio of H2 to the mixed gas in the N2 and H2 mixed gas is 1-2:
100.
5. The high-humidity resistant, corrosion-resistant, alkaline battery positive composite conductive material of claim 1, wherein, The preparation method of the molybdenum-doped SnO2 includes the following steps: Step S1: hydrothermal synthesis of precursor, zinc nitrate hexahydrate and ammonium molybdate are dissolved in deionized water to prepare a mixed solution, sodium citrate is added, the pH value of the solution is adjusted to 8.5-9.5 with ammonia water, and then the solution is subjected to hydrothermal reaction at 150-180℃ for 18-24h to generate a precipitate; Step S2: after the precipitate is separated and purified, it is heated at 500-550℃ for 2.5-3.5h, and then cooled to room temperature.
6. The high-humidity resistant, corrosion-resistant, alkaline battery positive composite conductive material of claim 5, wherein, In step S1, the molar ratio of zinc nitrate hexahydrate to ammonium molybdate is 85-95:5-15, the amount of sodium citrate is 1.5-2.5 times the molar amount of zinc ions, and the concentration of ammonia water is 25-28%. The total concentration of zinc ions and ammonium ions in the mixed solution is 0.1-0.3mol / L.
7. The high-humidity resistant, corrosion-resistant, alkaline battery positive composite conductive material of claim 1, wherein, The binder is one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene, carboxymethyl cellulose sodium, and styrene butadiene rubber (SBR).
8. The method of claim 1-7, wherein the method is characterized by, The method includes the following steps: Step a, mixing modified carbon nanotube, flake graphite, molybdenum-doped SnO2, conductive carbon black uniformly, adding part of solvent to form slurry A; Step b, dissolving the binder in the remaining solvent to form uniform glue B; mixing glue B with slurry A, and the process is completed.
9. The preparation method of the high-humidity-resistant and corrosion-resistant alkaline battery positive electrode composite conductive material as described in claim 8, characterized in that, The total amount of the solvent in step a and step b is 3-5 times the weight of the modified carbon nanotube.