Oil well cement fluid loss agent suitable for preventing thickening time from being upside down at medium-temperature section of 80-90 DEG C and preparation method of oil well cement fluid loss agent
By using a combination of components such as potassium 2-acrylamido-2-methylpropanesulfonate solution, the problem of inverted thickening time in the temperature range of 80~90℃ for traditional sodium salt-type water loss reducing agents was solved, thereby improving the stability and safety of the cement hydration process.
Patent Information
- Application Number
- CN202511997141.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-27
- Publication Date
- 2026-02-24
AI Technical Summary
Traditional sodium salt-based fluid loss reducers are prone to thickening time reversal in the 80-90℃ temperature range, which seriously threatens cementing safety.
Using potassium 2-acrylamido-2-methylpropanesulfonate solution, cyclic monomers, carboxylic acid monomers, and amide monomers, stable weak complexes and electrostatic shielding are formed to suppress fluctuations in aluminate concentration and calcium sulfonate precipitation, thereby improving the stability of ettringite and preventing thickening time inversion.
It effectively shortens the hydration induction period, reduces secondary retardation, improves the thermal stability of ettringite, prevents thickening time inversion, and ensures cementing safety.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical formulation technology. Specifically, it relates to an oil well cement fluid loss reducing agent suitable for preventing thickening and time inversion in the 80-90℃ medium-temperature range, and its preparation method. Background Technology
[0002] 80–90℃ is the most common bottom hole circulation temperature range for shallow and medium-depth oil and gas wells and shale gas horizontal wells in my country, particularly during the second and third stages of development. In this temperature range, traditional sodium-based fluid loss reducers are prone to thickening time inversion (thickening time actually increases by 30–100 minutes after the temperature rises). The fundamental reason for this is:
[0003] ① At 80-90℃, the dissolution rate of the aluminate phase in cement accelerates, leading to a surge in the concentration of liquid aluminate. Aluminate poisons the C3S (tricalcium silicate) surface and significantly prolongs the silicate hydration induction period, resulting in an abnormally slow hydration reaction rate. Meanwhile, Na… + Although it has strong polarization ability, the Na-Al complex formed with aluminate ions is unstable and easily dissociates, making it impossible to effectively control the aluminate release rate. Instead, it exacerbates the fluctuation of aluminate concentration and the efficiency of poisoning the C3S surface, ultimately inducing the "inverted" thickening time phenomenon unique to sodium salt systems; ②Na + It has strong polarization ability, and its -SO3Na group is easily converted by Ca. 2+ The substitution process (replacement rate reaching 35–45%) generates insoluble calcium sulfonate precipitate, causing the polymer adsorption layer to collapse and releasing a large number of free carboxyl groups. This release of carboxyl groups leads to secondary retardation, resulting in a reversed thickening time. Simultaneously, the formation of a relatively tight ion pair between Na⁺ and calcium ions on the calcium silicate surface exposes some of the negative charge on the calcium silicate surface, increasing the negative value of the Zeta potential. This, in turn, makes the calcium silicate surface more susceptible to the influence of Ca²⁺. 2+ Strong electrostatic repulsion is generated, further prolonging the hydration induction period. ③ Ettringite is a calcium aluminum sulfate mineral with the chemical formula 3CaO·Al2O3·3CaSO4·32H2O. It is prone to transformation to the monosulfide type, resulting in a loose slurry. Due to the relatively small radius of Na⁺ ions, the hydrated shell is more robust and difficult to dehydrate. Even if forced dehydration is performed, the bare ions are too small and do not match the channel size, so they are not easy to embed into the lattice of ettringite and cannot improve the stability of ettringite at 80~90℃.
[0004] Currently, almost all commercially available medium-temperature dehydration agents are sodium salt systems, leading to frequent inversion accidents and seriously threatening cementing safety. Summary of the Invention
[0005] Therefore, the technical problem to be solved by the present invention is to provide an oil well cement dehydration agent suitable for preventing thickening time inversion in the medium temperature range of 80~90℃ and its preparation method, so as to solve the thickening time inversion phenomenon in the 80~90℃ range.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0007] A cement fluid loss reducing agent for oil wells suitable for preventing thickening and time inversion in the medium temperature range of 80~90℃ comprises the following components: potassium 2-acrylamido-2-methylpropanesulfonate solution, cyclic monomers, carboxylic acid monomers, amide monomers, and chain transfer agents.
[0008] The potassium 2-acrylamido-2-methylpropanesulfonate (K⁺) used in this application has weak polarization, a large ionic radius, and low dehydration energy. Due to these characteristics, firstly, K⁺ readily forms more stable weak complexes with aluminate ions, effectively reducing the concentration of free aluminate in the liquid phase and suppressing the 'aluminum peak' (a sudden increase in aluminate concentration). Secondly, K⁺ exerts a weak physical effect (van der Waals forces, electrostatic attraction) to cover a large area of the calcium silicate particle surface, forming a loose, positively charged hydrated ion layer, which provides efficient electrostatic shielding, significantly reducing the Zeta potential and Ca... 2+ Nucleation on the CSH surface occurs almost without resistance, shortening the hydration induction period by 20–30%. Then, due to the "weak complexation" or "surface shielding" effect of potassium ions in cement hydration, the nucleation and growth of calcium sulfonate precipitates are significantly inhibited. Specifically, the -SO3K groups are almost not replaced by Ca²⁺ at 80–90℃ (replacement rate <5%), maintaining the stability of the polymer adsorption layer and thus greatly reducing the secondary carboxyl retarding phenomenon. In other words, the use of potassium 2-acrylamido-2-methylpropanesulfonate disrupts the conditions for simultaneous aluminate bursting and secondary carboxyl retarding at 80–90℃, eliminating the thickening time inversion phenomenon unique to sodium salt systems. Finally, due to the low hydration energy and radius-channel matching of K⁺, K⁺ readily embeds into the ettringite lattice, improving the thermal stability of ettringite at 90℃ and inhibiting the transformation of ettringite to the monosulfide form.
[0009] The above-mentioned oil well cement dehydration agent, which is suitable for preventing thickening and time inversion in the medium temperature range of 80~90℃, has the following weight ratio of each component: 180~200 parts of potassium 2-acrylamido-2-methylpropanesulfonate solution, 10~15 parts of cyclic monomer, 8~12 parts of carboxylic acid monomer, 6~10 parts of amide monomer, and 2.5~4.5 parts of chain transfer agent.
[0010] The aforementioned oil well cement dehydration agent, suitable for preventing thickening and time inversion in the medium-temperature range of 80-90℃, has a potassium 2-acrylamido-2-methylpropanesulfonate solution with a concentration of 54-55 wt%. Too low a concentration will affect the subsequent polymerization reaction, while too high a concentration is also detrimental to the polymerization reaction.
[0011] The above-mentioned oil well cement dehydration agent suitable for preventing thickening time inversion in the medium temperature range of 80~90℃, the preparation method of the potassium 2-acrylamido-2-methylpropanesulfonic acid solution is as follows: add 2-acrylamido-2-methylpropanesulfonic acid to potassium hydroxide aqueous solution, stir evenly and react fully, and filter to obtain potassium 2-acrylamido-2-methylpropanesulfonic acid solution.
[0012] The concentration of potassium hydroxide in the potassium hydroxide aqueous solution is 17~18 wt%; the molar ratio of 2-acrylamido-2-methylpropanesulfonic acid to potassium hydroxide is (1.2~1.3):1, and excess AMPS is used to control the pH value of the reaction.
[0013] The above-mentioned oil well cement dehydration agent suitable for preventing thickening time inversion in the medium temperature range of 80~90℃, wherein the cyclic monomer is one or more of N-vinylpyrrolidone, N-vinylcaprolactam and N-vinylformamide;
[0014] The carboxylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid;
[0015] The amide monomer is one or more of N,N-dimethylacrylamide, acrylamide, and N-hydroxymethylacrylamide;
[0016] The chain transfer agent is one or more of isopropanol, mercaptoethanol, and sodium hypophosphite.
[0017] Cyclic monomers such as N-vinylpyrrolidone possess strongly adsorbing lactam rings, which can slowly hydrolyze at high temperatures to release small amounts of carboxylic acid, providing secondary dispersion, preventing high-temperature particle aggregation, and improving the polymer's temperature and salt resistance. Carboxylic acid monomers such as acrylic acid serve as the main anchoring groups and provide a negative charge, enhancing particle dispersibility. Amide monomers such as N,N-dimethylacrylamide possess salt- and temperature-resistant amide groups, ensuring molecular weight integrity; improving the polymer's resistance to calcium buildup; refining the thickening curve shape; and reducing molecular chain rigidity.
[0018] A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range includes the following steps:
[0019] Step 1: Under a nitrogen atmosphere, add deionized water to the reaction vessel and start stirring;
[0020] Step 2: Add potassium 2-acrylamido-2-methylpropanesulfonate solution, cyclic monomer, carboxylic acid monomer and amide monomer sequentially to the reaction vessel, stir under heating conditions, and mix evenly to obtain a monomer mixture;
[0021] Step 3: Add chain transfer agent and metal ion chelating agent to the monomer mixture, mix well to obtain a mixed solution;
[0022] Step 4: After heating to the first reaction temperature, add the initiator to the mixture and let it stand. After heating to the second reaction temperature, restart the stirring and mature the mixture to obtain the above-mentioned oil well cement dehydration reducer.
[0023] This application introduces nitrogen gas during the reaction to isolate oxygen from the air and prevent it from inhibiting polymerization. Nitrogen gas introduction is stopped after a mixed solution is obtained in step three. The addition of materials during the preparation of the fluid loss reducer follows a specific order to ensure the stability of the reaction system: First, deionized water is mixed with a potassium 2-acrylamido-2-methylpropanesulfonate solution to prepare a premix as the reaction medium, providing an initial dissolution environment and adjusting the pH to avoid excessively high local monomer concentrations later. Next, cyclic monomers are added, and after complete dissolution, carboxylic acid monomers are added to prevent the cyclic monomers from agglomerating upon contact with water, which would then cause violent exothermic reactions upon contact with acrylic acid, leading to spraying. Finally, amide monomers are added, as they are easily dispersed in the system, and even if a small amount of agglomerate is present, it is easily dissolved by stirring. Then, a chain transfer agent is added to adjust the molecular length of the polymer, and a metal ion chelating agent is added to bind iron, copper, manganese, and other metal ions in the system, preventing them from catalytically decomposing the added initiator, leading to explosive polymerization and a decrease in polymer molecular weight. Finally, an initiator is added to react and obtain the oil well cement fluid loss reducer.
[0024] The above-mentioned method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the medium temperature range of 80~90℃ involves weighing the following components according to the following weight ratio: 180~200 parts of potassium 2-acrylamido-2-methylpropanesulfonate solution, 10~15 parts of cyclic monomer, 8~12 parts of carboxylic acid monomer, 6~10 parts of amide monomer, 2.5~4.5 parts of chain transfer agent, 0.01~0.03 parts of metal ion chelating agent, 0.5~1.5 parts of initiator, and 230–250 parts of deionized water, for later use.
[0025] The above-mentioned method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the medium temperature range of 80~90℃, wherein the cyclic monomer is one or more of N-vinylpyrrolidone, N-vinylcaprolactam and N-vinylformamide;
[0026] The carboxylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid;
[0027] The amide monomer is one or more of N,N-dimethylacrylamide, acrylamide, and N-hydroxymethylacrylamide;
[0028] The chain transfer agent is one or more of isopropanol, mercaptoethanol, and sodium hypophosphite;
[0029] The metal ion chelating agent is EDTA-2Na.
[0030] The above-mentioned method for preparing an oil well cement dehydration agent suitable for preventing thickening and time inversion in the medium temperature range of 80~90℃, in step one: the stirring rate is 150~250r / min. Too low a stirring rate will lead to uneven stirring, and too high a stirring rate will lead to mechanical degradation.
[0031] The preparation method of the oil well cement fluid loss reducing agent applicable to the medium temperature range of 80~90℃ for preventing thickening and time inversion includes a heating temperature of 45~55℃ in step two. Cyclic monomers such as N-vinylpyrrolidone dissolve slowly below 40℃, and AMPS-K salt does not easily crystallize above 45℃, requiring a certain heat capacity buffer to accommodate the exothermic reaction during acrylic acid droplet addition. If the temperature is too low, cyclic monomers such as N-vinylpyrrolidone will float to the surface and agglomerate, leading to localized overheating after the subsequent droplet addition of carboxylic acid monomers such as acrylic acid; if the temperature is too high, acrylic acid will volatilize, causing localized self-polymerization and affecting polymer properties.
[0032] The above-mentioned method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the medium-temperature range of 80~90℃ includes the following steps in step four: The first reaction temperature is 60~65℃; if the temperature is too low, initiation is slow and the residual monomer content is high; if the temperature is too high, the reaction is violent. The initiator is an aqueous solution of potassium persulfate, and the concentration of potassium persulfate in the aqueous solution is 4.5~5wt%; if the concentration is too high, it will lead to excessively high local initiator concentration and violent local reaction; if the concentration is too low, the reaction will be too slow. The second reaction temperature is 80℃, and the curing time is 2~4 hours. The temperature is further increased to ensure thorough curing. If the temperature is too low, polymerization will be incomplete and there will be more free monomers; if the temperature is too high, the reaction will be violent.
[0033] The technical solution of the present invention achieves the following beneficial technical effects:
[0034] The potassium 2-acrylamido-2-methylpropanesulfonate used in this application has weak K⁺ polarization ability, large ionic radius, and low dehydration energy, which has the following effects:
[0035] (1) K⁺ readily forms a more stable weak complex with aluminate ions, which can effectively reduce the concentration of free aluminate in the liquid phase and suppress the 'aluminate peak' (a sudden increase in aluminate concentration).
[0036] (2) In this application, K⁺ forms a loose, positively charged hydrated ion layer on the surface of calcium silicate particles through relatively weak physical forces (van der Waals forces, electrostatic attraction), which provides efficient electrostatic shielding, significantly reducing the Zeta potential and Ca 2+ Nucleation occurs on CSH surfaces with almost no resistance, resulting in a 20–30% reduction in the hydration induction period;
[0037] (3) Due to the “weak complexation” or “surface shielding” effect of potassium ions in cement hydration, the nucleation and growth of calcium sulfonate precipitate are significantly inhibited. That is, the -SO3K group is hardly replaced by Ca²⁺ at 80–90℃ (replacement rate <5%), and the polymer adsorption layer remains stable, thereby greatly reducing the secondary carboxyl retarding phenomenon. Therefore, the use of potassium 2-acrylamido-2-methylpropanesulfonate disrupts the conditions for the simultaneous occurrence of aluminate ion burst and secondary carboxyl retarding in the 80–90℃ temperature range, eliminating the thickening time inversion phenomenon unique to sodium salt systems.
[0038] (4) Due to the low hydration energy of K⁺ and the matching radius with the channel, K⁺ is easy to embed into the ettringite lattice, which improves the thermal stability of ettringite at 90℃ and inhibits the transformation of ettringite to monosulfide.
[0039] In summary, this application, by simply replacing sodium 2-acrylamido-2-methylpropanesulfonate, commonly used in water loss reducers, with potassium 2-acrylamido-2-methylpropanesulfonate, can accelerate early hydration in the 80–90℃ temperature range, thereby inhibiting the aluminate burst in cement, locking the polymer adsorption layer to prevent the release of carboxyl groups and secondary retardation, and stabilizing the ettringite crystal phase to inhibit the conversion of ettringite to monosulfide, thus preventing the thickening time inversion phenomenon in the 80–90℃ temperature range. Detailed Implementation
[0040] Example 1
[0041] A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range includes the following steps:
[0042] (1) Add 240g of deionized water to a 1000mL three-necked flask equipped with a stirrer, thermometer and nitrogen delivery tube, turn on the stirrer (stirring speed is 200r / min) and purge with nitrogen for 15min.
[0043] (2) Add 180g of potassium 2-acrylamido-2-methylpropanesulfonate (AMPS-K) solution, 12g of N-vinylpyrrolidone (NVP), 10g of acrylic acid (AA), and 8g of N,N-dimethylacrylamide (DMAA) to the three-necked flask in sequence, heat to 50°C and stir until completely dissolved to obtain a monomer mixture.
[0044] The preparation method of potassium 2-acrylamido-2-methylpropanesulfonate solution is as follows: 96g of potassium hydroxide is dissolved in 454g of water to prepare potassium hydroxide solution, 450g of AMPS is added, stirred evenly, cooled to room temperature, and filtered to obtain the solution.
[0045] (3) Add 3.5g isopropanol and 0.1g EDTA-2Na to the monomer mixture, continue to purge with nitrogen for 30min, and mix evenly to obtain the mixture.
[0046] (4) Heat the mixture to 62°C and add 1g of potassium persulfate aqueous solution (potassium persulfate concentration is 4.76%) to the mixture. Stir evenly and let stand to obtain a reaction solution. After the reaction solution is heated to 80°C, start stirring and mature for 3 hours to obtain a light yellow transparent viscous liquid, which is the oil well cement dehydration reducer.
[0047] Example 2
[0048] Except for increasing the amount of isopropanol to 5.0g, the other raw materials and operating steps are exactly the same as in Example 1.
[0049] Comparative Example
[0050] Except for replacing AMPS-K with an equal amount of sodium 2-acrylamido-2-methylpropanesulfonate, the types and quality of other raw materials and all operating steps are exactly the same as in Example 1.
[0051] The oil well cement fluid loss reducing agent prepared in the above examples and comparative examples was then added to cement (Jiahua G-grade cement) to prepare cement slurry. The density of the prepared cement slurry was 1.90 g / cm³. 3 The addition amount of the oil well cement fluid loss reducing agent prepared in the above embodiments and comparative examples was 4%. The prepared cement slurry was tested, as shown in Table 1 below.
[0052] Table 1
[0053]
[0054] As can be seen from the table above, the comparative example only replaced the potassium salt with the sodium salt, and the other conditions were completely the same, that is, the typical thickening and inversion occurred at 80–90 ℃. However, no thickening and inversion occurred in Example 1 and Example 2, which proves the role of potassium ions in preventing thickening and inversion in this temperature range.
[0055] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of the claims of this patent application.
Claims
1. A cement fluid loss reducing agent for oil wells suitable for preventing thickening time inversion in the medium-temperature range of 80~90℃, characterized in that, It includes the following components: potassium 2-acrylamido-2-methylpropanesulfonate solution, cyclic monomers, carboxylic acid monomers, amide monomers, and chain transfer agents.
2. The oil well cement fluid loss reducing agent according to claim 1, suitable for preventing thickening time inversion in the 80-90℃ medium temperature range, is characterized in that, The weight ratios of each component are as follows: 180-200 parts of potassium 2-acrylamido-2-methylpropanesulfonate solution, 10-15 parts of cyclic monomers, 8-12 parts of carboxylic acid monomers, 6-10 parts of amide monomers, and 2.5-4.5 parts of chain transfer agent.
3. A cement fluid loss reducing agent for oil wells suitable for preventing thickening and time inversion in the 80-90℃ medium-temperature range, as described in claim 1 or 2, characterized in that... The concentration of potassium 2-acrylamido-2-methylpropanesulfonate in the potassium 2-acrylamido-2-methylpropanesulfonate solution is 54~55 wt%.
4. The oil well cement fluid loss reducing agent according to claim 3, suitable for preventing thickening time inversion in the 80-90℃ medium temperature range, is characterized in that, The method for preparing the potassium 2-acrylamido-2-methylpropanesulfonic acid solution is as follows: 2-acrylamido-2-methylpropanesulfonic acid is added to an aqueous solution of potassium hydroxide, stirred until homogeneous and reacted completely, and then filtered to obtain a potassium 2-acrylamido-2-methylpropanesulfonic acid solution. The concentration of potassium hydroxide in the potassium hydroxide aqueous solution is 17~18 wt%; the molar ratio of 2-acrylamido-2-methylpropanesulfonic acid to potassium hydroxide is (1.2~1.3):
1.
5. A cement fluid loss reducing agent for oil wells suitable for preventing thickening and time inversion in the 80-90℃ medium-temperature range, as described in claim 1 or 2, characterized in that, The cyclic monomer is one or more of N-vinylpyrrolidone, N-vinylcaprolactam, and N-vinylformamide; The carboxylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid; The amide monomer is one or more of N,N-dimethylacrylamide, acrylamide, and N-hydroxymethylacrylamide; The chain transfer agent is one or more of isopropanol, mercaptoethanol, and sodium hypophosphite.
6. A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range, characterized in that, Includes the following steps: Step 1: Under a nitrogen atmosphere, add deionized water to the reaction vessel and start stirring; Step 2: Add potassium 2-acrylamido-2-methylpropanesulfonate solution, cyclic monomer, carboxylic acid monomer and amide monomer sequentially to the reaction vessel, stir under heating conditions, and mix evenly to obtain a monomer mixture; Step 3: Add chain transfer agent and metal ion chelating agent to the monomer mixture, mix well to obtain a mixed solution; Step 4: After heating to the first reaction temperature, add the initiator to the mixture and let it stand. After heating to the second reaction temperature, restart the stirring and mature the mixture to obtain the oil well cement dehydration reducer as described in any one of claims 1 to 5.
7. A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range, as described in claim 6, characterized in that, Weigh the following components according to the following weight ratio: 180-200 parts of potassium 2-acrylamido-2-methylpropanesulfonate solution, 10-15 parts of cyclic monomer, 8-12 parts of carboxylic acid monomer, 6-10 parts of amide monomer, 2.5-4.5 parts of chain transfer agent, 0.01-0.03 parts of metal ion chelating agent, 0.5-1.5 parts of initiator, and 230-250 parts of deionized water, and set aside.
8. A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range, as described in claim 6 or 7, characterized in that, The cyclic monomer is one or more of N-vinylpyrrolidone, N-vinylcaprolactam, and N-vinylformamide; The carboxylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid; The amide monomer is one or more of N,N-dimethylacrylamide, acrylamide, and N-hydroxymethylacrylamide; The chain transfer agent is one or more of isopropanol, mercaptoethanol, and sodium hypophosphite; the metal ion chelating agent is EDTA-2Na.
9. A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range, as described in claim 6, characterized in that, In step two: the heating temperature is 45~55℃.
10. A method for preparing an oil well cement fluid loss reducing agent suitable for preventing thickening time inversion in the 80-90℃ medium-temperature range, as described in claim 6, characterized in that, In step four: the first reaction temperature is 60~65℃; the initiator is an aqueous solution of potassium persulfate, and the concentration of potassium persulfate in the aqueous solution is 4.5~5wt%; the second reaction temperature is 80℃, and the aging time is 2~4h.