Efficient asphalt vulcanization cross-linking agent for replacing elemental sulfur and method for preparing cross-linked modified asphalt by using efficient asphalt vulcanization cross-linking agent

The highly efficient asphalt vulcanization crosslinking agent prepared by using a mixture of sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole solves the problems of long mixing time, high energy consumption and environmental pollution in the existing technology, and realizes efficient and environmentally friendly modified asphalt production.

CN121609970APending Publication Date: 2026-03-06NORTHEAST FORESTRY UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610020304.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-08
Publication Date
2026-03-06

AI Technical Summary

Technical Problem

While existing vulcanization crosslinking systems have some effect on improving the anti-segregation stability of modified asphalt, the long mixing time of stabilizers with other components results in high energy consumption, low production efficiency, and environmental pollution.

Method used

A high-efficiency asphalt vulcanization crosslinking agent prepared by mixing sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole is formed by high-speed shear dispersion followed by low-speed stirring to shorten the mixing time and form a stable three-dimensional network crosslinking structure.

Benefits of technology

It significantly shortens reaction time, reduces energy consumption, reduces environmental pollution, improves production efficiency, and enhances the anti-segregation stability and road performance of modified asphalt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121609970A_ABST
    Figure CN121609970A_ABST
Patent Text Reader

Abstract

The invention discloses a high-efficiency asphalt vulcanization cross-linking agent for replacing elemental sulfur and a method for preparing cross-linked modified asphalt by using the high-efficiency asphalt vulcanization cross-linking agent, and belongs to the technical field of asphalt additives. The invention aims to solve the problems of high energy consumption, low production efficiency, environmental pollution and the like caused by overlong mixing and dissolving time of a stabilizer and other components although the existing vulcanization cross-linking system has a certain effect on improving the segregation-resistant stability of the modified asphalt. The invention provides an efficient asphalt cross-linking agent for replacing elemental sulfur. The efficient asphalt cross-linking agent is prepared by compounding sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole. The specific mode for preparing the cross-linked modified asphalt by using the efficient asphalt vulcanization cross-linking agent replacing elemental sulfur is that the efficient asphalt vulcanization cross-linking agent is added 5-15 minutes before swelling development processing is finished. When the efficient asphalt cross-linking agent provided by the invention is used for preparing cross-linked modified asphalt, the processing and preparation time is obviously shortened, the process is obviously simplified, and the energy consumption is effectively reduced, the production efficiency is improved and the pollution is reduced while the excellent segregation resistance is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of asphalt additive technology. Background Technology

[0002] SBS-modified asphalt or rubber powder-modified asphalt is widely used in modern road engineering. However, due to the significant molecular weight difference between the polymer or rubber powder used as the modifier and the modified base asphalt, poor compatibility leads to segregation during storage after preparation. To suppress segregation after preparation, elemental sulfur is commonly incorporated into SBS / rubber powder-modified asphalt as an anti-segregation stabilizing component.

[0003] The main technical mechanism of sulfur as an anti-segregation stabilizing component is to utilize the vulcanization and cross-linking reaction between sulfur and SBS / rubber powder modified asphalt to form a wide molecular cross-linking network in the asphalt, thereby improving the colloidal stability of the modified product and inhibiting its segregation. The asphalt vulcanization and cross-linking reaction involves introducing active sulfur (such as sulfur free radicals ·S·) into the asphalt. Active sulfur attacks the unsaturated bonds or polar groups in the asphalt molecules (especially aromatics and resins), causing the molecular chains to generate active ends. These active ends are then connected through CS and SS bonds, constructing a stable three-dimensional network structure. When modified asphalt contains rubber polymers (such as SBS), the polybutadiene segments in the molecules are also unsaturated and will generate stable covalent bonds under the action of active sulfur, thus forming a stable SBS-asphalt network cross-linked structure. A higher degree of cross-linking in SBS / rubber powder modified asphalt implies better stability; however, from a chemical reaction perspective, sulfur in sulfur-containing asphalt always exists in two forms: reacted sulfur and unreacted sulfur (dissolved or crystalline). The proportion of sulfur used as an anti-segregation stabilizer is usually no more than 0.5%. If a higher proportion of sulfur is desired to participate in the cross-linking reaction to improve its effect as an anti-segregation stabilizer, a longer reaction time and higher reaction temperature are required. This processing operation will reduce production efficiency, increase production energy consumption, and cause more serious environmental pollution.

[0004] In existing technology, CN112300586A discloses an SBS-modified asphalt stabilizer and SBS-modified asphalt. The SBS-modified asphalt stabilizer is prepared using sulfur (S content > 99.0%) obtained from the treatment of acidic gases from catalytic cracking in a refinery, thiuram-based accelerators, zinc oxide, antioxidants, and recycled carbon black. This stabilizer is then added to a system of base asphalt and SBS at 0.15%~0.3% by weight of the base asphalt. This patent improves the formation rate of sulfidation products through the use of thiuram-based accelerators.

[0005] CN106751947A discloses an SBS asphalt stabilizer and its application. The SBS asphalt stabilizer is prepared using activated calcium carbonate, sulfur powder, SBS, styrene-butadiene rubber, octadecylamine polyoxyethylene ether, stearyltrimethylammonium chloride, polyoxyethylene nonylphenyl ether, polyethylene resin, and nano-zinc oxide. This patent primarily utilizes surface-treated activated calcium carbonate to increase the compatibility and dispersibility of asphalt, thereby increasing the reaction rate between sulfur and asphalt and enhancing the stabilizer's anti-segregation effect.

[0006] CN118185328A discloses an SBS-modified asphalt stabilizer, SBS-modified asphalt, and their preparation process. The stabilizer is prepared using sulfur, asbestos ash, zinc oxide, and rock asphalt powder, and then combined with base asphalt, linear SBS modifier, and furfural extract to prepare SBS-modified asphalt. Theoretically, the various powders, such as asbestos ash and zinc oxide, in this patent have a synergistic stabilizing effect with sulfur.

[0007] CN107556764A discloses an SBS-modified asphalt stabilizer, its preparation method, and its application. The stabilizer is prepared using sulfur, phosphate ester, activator, and dispersant. It is then added to an asphalt and SBS system at a ratio of asphalt:SBS:stabilizer = (400-600):(20-30):(0.5-2.0) to prepare modified asphalt. The activator and dispersant can promote the dispersion of asphalt molecules and, theoretically, also enhance the reaction between sulfur and asphalt.

[0008] The SBS-modified asphalt stabilizers proposed in the aforementioned patents all use sulfur as a key functional component, while employing vulcanization reaction accelerators, powdered additives, and surfactants to enhance the stabilizing effect, aiming to overcome the limitations of using sulfur alone as a stabilizer. These patented products generally incorporate a sulfur-based stabilizer into the SBS-base asphalt miscible (intermediate stage product) prepared by high-speed shearing, and then participate in its high-temperature and long-term low-speed stirring process. The processing conditions are summarized in Table 1. Although this incorporation method does not conflict with the swelling and development requirements of SBS / rubber powder in the base asphalt, the long-term high-temperature stirring involving sulfur will generate a large amount of hydrogen sulfide (H2S) and sulfur dioxide (SO2), leading to significant environmental pollution.

[0009] Table 1. Process conditions for preparing SBS / rubber powder modified asphalt using relevant patented products.

[0010] Summary of the Invention

[0011] This invention aims to address the problems of existing sulfur crosslinking systems, which, while effective in improving the anti-segregation stability of modified asphalt, suffer from excessively long mixing times between the stabilizer and other components, resulting in high energy consumption, low production efficiency, and environmental pollution. The invention provides a highly efficient asphalt sulfur crosslinking agent to replace elemental sulfur and a method for preparing crosslinked modified asphalt using this agent.

[0012] A highly efficient asphalt vulcanization crosslinking agent that can replace elemental sulfur is composed of sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole.

[0013] A method for preparing crosslinked modified asphalt using a highly efficient asphalt vulcanization crosslinking agent that replaces elemental sulfur is carried out according to the following steps:

[0014] The base asphalt is heated and melted, and then SBS or rubber powder is added. It is first dispersed and mixed by high-speed shearing, and then swelled and developed under low-speed stirring. 5 to 15 minutes before the end of the swelling and development process, a high-efficiency asphalt vulcanization crosslinking agent to replace elemental sulfur is added, and low-speed stirring continues until the swelling and development process is completed, thus completing the preparation of crosslinked modified asphalt.

[0015] The beneficial effects of this invention are:

[0016] This invention provides a highly efficient asphalt vulcanization crosslinking agent that can replace elemental sulfur. While ensuring the anti-segregation stability of modified asphalt, it can significantly shorten the mixing time of the stabilizer and other components, which has practical application value for reducing energy consumption, improving production efficiency, and reducing environmental pollution.

[0017] 1. When the high-efficiency asphalt vulcanization crosslinking agent of this invention, which replaces elemental sulfur, is used for SBS / rubber powder modified asphalt vulcanization crosslinking, the reaction time can be shortened to 5 min to 15 min, and the efficiency of achieving the technical goal is significantly improved.

[0018] 2. The raw materials used in the high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur in this invention are two inexpensive chemical products, which can be pre-mixed uniformly under normal temperature and pressure. Moreover, the mass of the high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur is 0.1% to 0.3% of the mass of the base asphalt, and the cost is relatively low.

[0019] 3. The high-efficiency asphalt vulcanization crosslinking agent of this invention, which replaces elemental sulfur, can form a stable three-dimensional network crosslinking structure in SBS / rubber powder modified asphalt, thereby improving the segregation stability of SBS / rubber powder modified asphalt and enhancing its road performance such as rutting resistance and fatigue resistance. Attached Figure Description

[0020] Figure 1 This is a comparison chart showing the measured penetration, softening point, and 48-hour segregation softening point difference parameters of the final samples of different SBS modified asphalt from the examples and comparative experiments. Detailed Implementation

[0021] Specific Implementation Method 1: This implementation method is a high-efficiency asphalt vulcanization crosslinking agent that can replace elemental sulfur. It is composed of sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole.

[0022] Principle: In this specific embodiment, sodium dimethyl dithiocarbamate (SDD) and 2-mercaptobenzothiazole (M) are two commonly used sulfur-containing organic compounds in industry. SDD, a dithiocarbamate, can generate highly reactive free radicals (dimethyl dithiocarbamoyl radical (CH3)2N-CS· and sulfur radical ·S, etc.) through CS bond cleavage under thermal activation. These radicals can undergo free radical addition reactions with unsaturated components in modified asphalt, acting as initiators for vulcanization crosslinking reactions. The M molecule contains highly reactive thiol groups (-SH), which can react with the highly reactive free radicals generated by the thermal activation of SDD to produce activated intermediates (such as polysulfides). These intermediates mainly act on the active sites of unsaturated chemical bonds in modified asphalt. Aromatic rings, cycloalkane rings, and heteroatom functional groups in asphaltenes and resins are the main reaction sites, preferentially undergoing crosslinking reactions with the CC double bonds of polybutadiene segments in SBS. This system eliminates the need for elemental sulfur (sulfur) because the highly reactive sulfur-containing free radicals and intermediates are released upon heating, allowing the vulcanization and crosslinking reaction of modified asphalt to occur more rapidly. Compared to the traditional method of incorporating elemental sulfur, this specific embodiment uses a compound formulation of SDD and M as the vulcanization and crosslinking agent for SBS / rubber powder modified asphalt, which significantly improves the efficiency of the vulcanization and crosslinking reaction, thereby overcoming the problems of long reaction time, high energy consumption, and severe environmental pollution associated with incorporating elemental sulfur. It offers significant technical, economic, and social benefits.

[0023] The beneficial effects of this embodiment are:

[0024] This embodiment provides a highly efficient asphalt vulcanization crosslinking agent that can replace elemental sulfur. While ensuring the anti-segregation stability of modified asphalt, it can significantly shorten the mixing time of the stabilizer and other components, which has practical application value for reducing energy consumption, improving production efficiency, and reducing environmental pollution.

[0025] 1. When the high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur is used for SBS / rubber powder modified asphalt vulcanization crosslinking, the reaction time can be shortened to 5 min to 15 min, and the efficiency of achieving the technical goal is significantly improved.

[0026] 2. The raw materials used in the high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur in this embodiment are two inexpensive chemical products, which can be pre-mixed uniformly under normal temperature and pressure. Moreover, the mass of the high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur is 0.1% to 0.3% of the mass of the base asphalt, and the cost is relatively low.

[0027] 3. The high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur in this embodiment can form a stable three-dimensional network crosslinking structure in SBS / rubber powder modified asphalt, thereby improving the segregation stability of SBS / rubber powder modified asphalt and enhancing its road performance such as rutting resistance and fatigue resistance.

[0028] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the molar ratio of sodium dimethyl dithiocarbamate to 2-mercaptobenzothiazole is (3~5):1, and the mixture is obtained after homogenization at room temperature and pressure. Everything else is the same as in Specific Implementation Method One.

[0029] Specific Implementation Method 3: This implementation method utilizes a highly efficient asphalt vulcanization crosslinking agent to replace elemental sulfur to prepare crosslinked modified asphalt, and is carried out according to the following steps:

[0030] The base asphalt is heated and melted, and then SBS or rubber powder is added. It is first dispersed and mixed by high-speed shearing, and then swelled and developed under low-speed stirring. 5 to 15 minutes before the end of the swelling and development process, a high-efficiency asphalt vulcanization crosslinking agent to replace elemental sulfur is added, and low-speed stirring continues until the swelling and development process is completed, thus completing the preparation of crosslinked modified asphalt.

[0031] Specific Implementation Method Four: This implementation method differs from Specific Implementation Method Three in that the base asphalt is heated and melted at a temperature of 160℃~180℃, and then SBS or rubber powder is added to the molten base asphalt at a temperature of 160℃~180℃. Everything else is the same as in Specific Implementation Method Three.

[0032] Specific Implementation Method Five: This implementation method differs from Specific Implementation Method Three or Four in that: the softening point of the base asphalt is 40℃~60℃; the base asphalt is one or more of straight-run petroleum asphalt, solvent-degraded petroleum asphalt, and blended petroleum asphalt. Everything else is the same as in Specific Implementation Method Three or Four.

[0033] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods Three to Five in that: the mass of SBS accounts for 3% to 6% of the mass of the base asphalt; and the mass of the rubber powder accounts for 3% to 6% of the mass of the base asphalt. Everything else is the same as in Specific Implementation Methods Three to Five.

[0034] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods Three to Six in that the mass of the high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur accounts for 0.1% to 0.3% of the mass of the base asphalt. Everything else is the same as in Specific Implementation Methods Three to Six.

[0035] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Methods Three to Seven in that the high-speed shear dispersion mixing is carried out at a temperature of 160℃~180℃ and a rotation speed of 4000r / min~6000r / min, with a high-speed shear dispersion mixing time of 30min~45min. Everything else is the same as in Specific Implementation Methods Three to Seven.

[0036] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Methods Three to Eight in that the temperature for low-speed stirring and swelling development is 165℃~175℃, and the rotation speed is 1000r / min~1500r / min. Everything else is the same as in Specific Implementation Methods Three to Eight.

[0037] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Methods Three to Nine in that the total time for the swelling and development process is 120-150 minutes. Everything else is the same as Specific Implementation Methods Three to Nine.

[0038] The beneficial effects of the present invention are verified using the following embodiments:

[0039] Example 1:

[0040] A highly efficient asphalt vulcanization crosslinking agent (PVAC) that can replace elemental sulfur is composed of sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole, specifically obtained by uniform mixing at room temperature and pressure.

[0041] The molar ratio of sodium dimethyl dithiocarbamate to 2-mercaptobenzothiazole is 3.5:1.

[0042] The method for preparing crosslinked modified asphalt using the above-mentioned high-efficiency asphalt vulcanization crosslinking agent that replaces elemental sulfur is carried out according to the following steps:

[0043] Weigh out 100 parts by weight of base asphalt, 4 parts by weight of SBS, and 0.2 parts by weight of a high-efficiency asphalt vulcanizing crosslinking agent that replaces elemental sulfur. Melt the 100 parts of base asphalt at 170°C. Then, at 170°C, add 4 parts by weight of SBS to the molten base asphalt. First, shear and disperse the mixture at 170°C and 5000 r / min for 30 min. Then, swell and develop the mixture at 170°C and 1000 r / min for 115 min. Add 0.2 parts by weight of the high-efficiency asphalt vulcanizing crosslinking agent that replaces elemental sulfur, and continue stirring at low speed for 5 min at 170°C and 1000 r / min to obtain sample S3. This completes the method for preparing crosslinked modified asphalt using a high-efficiency asphalt vulcanizing crosslinking agent that replaces elemental sulfur.

[0044] The base asphalt is 90# base asphalt with a softening point of 45.2℃.

[0045] The total time for the swelling and development phase is 120 minutes.

[0046] Example 2: This example differs from Example 1 in that, under conditions of 170℃ and 1000 r / min, the mixture was allowed to swell and develop for 110 min. Then, 0.2 parts of a high-efficiency asphalt vulcanizing crosslinking agent to replace elemental sulfur were added, and the mixture was stirred at low speed for another 10 min at 170℃ and 1000 r / min to obtain sample S4. Everything else was the same as in Example 1.

[0047] Example 3: This example differs from Example 1 in that, under conditions of 170℃ and 1000 r / min, the mixture was allowed to swell and develop for 105 min. Then, 0.2 parts of a high-efficiency asphalt vulcanizing crosslinking agent to replace elemental sulfur were added, and the mixture was stirred at low speed for another 15 min at 170℃ and 1000 r / min to obtain sample S5. Everything else was the same as in Example 1.

[0048] Comparative Experiment 1: This comparative experiment differs from Example 1 in that the addition of the high-efficiency asphalt vulcanizing crosslinking agent to replace elemental sulfur is omitted; firstly, the mixture is subjected to high-speed shear dispersion and mixing for 30 minutes at a temperature of 170℃ and a rotation speed of 5000 r / min, and then swells and develops for 120 minutes at a temperature of 170℃ and a rotation speed of 1000 r / min to obtain sample S1. Everything else is the same as in Example 1.

[0049] Comparative Experiment 2: This comparative experiment differs from Example 1 in that, under conditions of 170℃ and 1000 r / min, the swelling and development process lasted for 117 min. Then, 0.2 parts of a high-efficiency asphalt vulcanization crosslinking agent to replace elemental sulfur were added, and the mixture was stirred at low speed for another 3 min at 170℃ and 1000 r / min to obtain sample S2. All other procedures were the same as in Example 1.

[0050] Comparative Experiment 3: This comparative experiment differs from Example 1 in that: first, high-speed shear dispersion mixing was performed for 30 minutes at a temperature of 170℃ and a rotation speed of 5000 r / min; then, swelling and development were carried out for 105 minutes at a temperature of 170℃ and a rotation speed of 1000 r / min; 0.5 parts of sulfur (analytical grade) were added; and low-speed stirring was continued for 15 minutes at a temperature of 170℃ and a rotation speed of 1000 r / min to obtain sample D1. All other procedures were the same as in Example 1.

[0051] Comparative Experiment 4: This comparative experiment differs from Example 1 in that: first, high-speed shear dispersion mixing was performed for 30 minutes at a temperature of 170℃ and a rotation speed of 5000 r / min; then, swelling and development were carried out for 60 minutes at a temperature of 170℃ and a rotation speed of 1000 r / min; 0.5 parts of sulfur (analytical grade) were added; and low-speed stirring was continued for 60 minutes at a temperature of 170℃ and a rotation speed of 1000 r / min to obtain sample D2. All other procedures were the same as in Example 1.

[0052] Comparative Experiment 5: This comparative experiment differs from Example 1 in that: first, the mixture was subjected to high-speed shear dispersion for 30 minutes at a temperature of 170℃ and a rotation speed of 5000 r / min; then, 0.2 parts of stabilizer DS-03 (from Shandong Dashan Road and Bridge Engineering Co., Ltd.) were added; and finally, the mixture was allowed to swell and develop for 120 minutes at a temperature of 170℃ and a rotation speed of 1000 r / min to obtain sample D3. All other procedures were the same as in Example 1.

[0053] Different SBS modified asphalt final samples were prepared according to the above examples and comparative experimental methods. Their penetration, softening point, and 48h segregation softening point difference were tested. The results are shown in Table 2.

[0054] Table 2 Measured technical parameters of the examples and comparative experiments

[0055]

[0056] Figure 1 This is a comparison chart showing the measured penetration, softening point, and 48-hour segregation softening point difference parameters of the final samples of different SBS modified asphalt from the examples and comparative experiments.

[0057] The combined results of the examples and comparative experiments show that the PVAC system achieves better overall performance with a significantly shorter reaction time, and its modification effect is significantly superior to that of the traditional elemental sulfur system and commercially available stabilizers. After 5 minutes of reaction in the example products, the changes in indicators such as penetration and softening point tended to converge, indicating that the main crosslinking modification process was essentially completed within a short time, forming a stable three-dimensional network structure. Therefore, further extending the reaction time has limited effect on performance improvement.

[0058] PVAC significantly increases the softening point of modified asphalt and reduces the segregation softening point difference within a short period of 5-15 minutes, demonstrating a clear advantage over the 60-minute and 120-minute processing times in the comparative experiments, resulting in a substantial improvement in reaction efficiency. Regarding storage stability, the segregation softening point difference of the example samples at 48 hours was significantly lower than that of the traditional elemental sulfur system, and it achieved better segregation suppression than the commercially available DS-03 stabilizer within a shorter reaction time. This indicates that PVAC can more efficiently promote the improvement of asphalt-SBS compatibility and construct a more uniform and stable three-dimensional cross-linked network.

[0059] From an economic and environmental perspective, PVAC exhibits significant modification effects even with a small addition (0.2 wt%), and raw material costs are controllable. Although a small amount of gas is generated during the reaction, the cumulative release of harmful substances is significantly reduced compared to the long-duration, high-temperature reaction required by traditional elemental sulfur systems due to the greatly shortened reaction time, thus demonstrating excellent environmental performance.

Claims

1. A high performance asphalt sulfur vulcanization crosslinker in place of elemental sulfur, characterized in that, The sodium dimethyl dithiocarbamate and 2-mercaptobenzothiazole are mixed.

2. The high efficient asphalt sulfur curing crosslinker for replacing elemental sulfur according to claim 1, characterized in that, The molar ratio of the sodium dimethyl dithiocarbamate to the 2-mercaptobenzothiazole is (3-5):1, and the mixture is uniformly mixed at normal temperature and pressure.

3. A process for the preparation of cross-linking modified bitumen using the high efficient bitumen sulfur vulcanizing cross-linking agent as claimed in claim 1, wherein, The following steps are performed: The base asphalt is heated and melted, and then the SBS or rubber powder is added, which is first dispersed and mixed by high-speed shearing, and then swells and develops under low-speed stirring, and the high-efficiency asphalt vulcanization crosslinking agent replacing elemental sulfur is added 5min-15min before the swelling and development process is completed, and the low-speed stirring is continued until the swelling and development process is completed, that is, the preparation of the crosslinked modified asphalt is completed.

4. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The base asphalt is heated and melted at a temperature of 160-180℃, and then the SBS or rubber powder is added in the melted base asphalt at a temperature of 160-180℃.

5. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur curing cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The softening point of the base asphalt is 40-60℃, and the base asphalt is one or more of straight-run petroleum asphalt, solvent-deasphalted petroleum asphalt and blended petroleum asphalt.

6. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur curing cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The mass of the SBS accounts for 3-6% of the mass of the base asphalt, and the mass of the rubber powder accounts for 3-6% of the mass of the base asphalt.

7. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur curing cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The mass of the high-efficiency asphalt vulcanization crosslinking agent replacing elemental sulfur accounts for 0.1-0.3% of the mass of the base asphalt.

8. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur curing cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The high-speed shearing dispersion mixing is specifically performed at a temperature of 160-180℃ and a rotation speed of 4000-6000r / min, and the high-speed shearing dispersion mixing time is 30-45min.

9. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur curing cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The low-speed stirring swelling development temperature is 165-175℃, and the rotation speed is 1000-1500r / min.

10. The process for preparing cross-linking modified bitumen using high efficient bitumen sulfur curing cross-linking agent with alternative elemental sulfur as claimed in claim 3, wherein, The total swelling and development processing time is 120-150min.

Citation Information

Patent Citations

  • SBS (styrene-butadiene-styrene block copolymer) asphalt stabilizer

    CN106751947A

  • SBS modified asphalt stabilizer, and preparation method and application thereof

    CN107556764A

  • SBS modified asphalt stabilizer, SBS modified asphalt and preparation process of SBS modified asphalt

    CN118185328A