PTC (Positive Temperature Coefficient) ceramic material with uniform fine grain structure as well as preparation method and application of PTC ceramic material

By employing a sintering method with segmented temperature control and differentiated heating rates, combined with a specific raw material formulation, the problem of uneven grain growth in traditional PTC ceramic materials has been solved. This has resulted in the preparation of uniform fine-grained PTC ceramic materials with low resistivity and excellent resistance to energy shocks, thereby improving their reliability and lifespan in high-end applications.

CN121673043APending Publication Date: 2026-03-17MEISHAN QINCHUAN SMART SENSOR CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202512000228.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-29
Publication Date
2026-03-17

AI Technical Summary

Technical Problem

The sintering process of traditional PTC ceramic materials is difficult to achieve a uniform fine-grained structure, resulting in high resistivity and poor resistance to energy shocks, which limits its development in high-end application fields.

Method used

By employing a sintering method with segmented temperature control and differentiated heating rates, and by continuously providing stable kinetic energy to ensure uniform grain growth, combined with specific raw material formulations and process improvements, PTC ceramic materials with uniform microcrystalline grain size were prepared.

Benefits of technology

The PTC ceramic material achieves low resistivity and uniform fine-grained structure, improves the voltage withstand capability per unit thickness and the resistance to high-energy impact, avoids problems such as delamination failure, edge arcing and breakdown, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121673043A_ABST
    Figure CN121673043A_ABST
Patent Text Reader

Abstract

The invention discloses a PTC (Positive Temperature Coefficient) ceramic material with a uniform fine grain structure as well as a preparation method and application thereof, and belongs to the technical field of PTC ceramic materials. According to the invention, growth kinetic energy of crystal grains is accurately supplied, so that the growth continuity is guaranteed; the growth consistency is improved by regulating and controlling the synchronous growth of crystal grains in the whole region; by controlling the sintering temperature and the sintering time, abnormal growth of crystal grains is inhibited, and finally, the PTC ceramic material forms a fine grain structure with uniform microcosmic grain size and regular grain boundary distribution, so that the basic requirement of the PTC ceramic material on low resistivity can be met, the unit thickness voltage resistance and high energy impact resistance of the material can be remarkably improved, and the service life of the PTC ceramic material is prolonged. And the problems of layering failure, edge sparking flashover, breakdown and the like which are easy to occur in the traditional material are effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of PTC ceramic materials, and particularly relates to a PTC ceramic material with a uniform fine-grain structure and a preparation method and application thereof. BACKGROUND

[0002] PTC (Positive Temperature Coefficient) ceramic materials are widely used in the fields of overcurrent protection, surge current suppression, self-limiting heating and temperature sensing due to their unique resistance-temperature characteristics. The current technology of PTC ceramic materials is mature, and the switching temperature range thereof can reach-20℃ to +320℃, and the resistance value range thereof covers 0.1Ω to 100KΩ. In order to achieve excellent electrical properties and reliability, the PTC ceramic material needs to have a low resistivity and a uniform microstructure, and the micro-grain size is one of the key factors affecting the performance of the material. Studies have shown that the micro-grain size of the PTC ceramic material usually needs to be controlled to be 5μm or more. If the grain size is too small (such as less than 5μm), the resistivity of the material will increase significantly, and even it is difficult to achieve semi-conductivity, so that the basic requirements of the PTC effect cannot be met.

[0003] In the preparation process of the PTC ceramic material, sintering is the core process that determines the final microstructure and performance of the PTC ceramic material. The traditional process of the PTC ceramic material usually includes the following steps: twice wet ball milling, pre-sintering to synthesize the main crystal phase, drying after twice ball milling, adding a binder to granulation, molding and sintering, etc. The process (such as shown in FIG. 1) has significant defects (the use of a fixed maximum temperature and holding time is easy to cause the grain size distribution to widen and the microstructure to be non-uniform), which makes it difficult to obtain a uniform fine-grain structure, and also magnifies the asynchronization of the grain growth in different regions, thereby causing abnormal growth. Figure 1

[0004] Therefore, the traditional sintering method cannot effectively control the uniformity of the grain growth, and it is difficult to prepare a high-performance PTC ceramic material with low resistivity and a uniform fine-grain structure, which limits the further development of the PTC ceramic material in high-end application fields. SUMMARY

[0005] The purpose of the present application is to provide a PTC ceramic material with a uniform fine-grain structure and a preparation method and application thereof, which can effectively inhibit the abnormal growth of grains and realize the uniformity of the microstructure, thereby improving the comprehensive performance of the PTC ceramic material.

[0006] To achieve the above purpose, the present application provides a preparation method of a PTC ceramic material with a uniform fine-grain structure, which comprises the following steps: After the raw materials are weighed according to a predetermined proportion and mixed uniformly, drying is performed to obtain a mixture; ​The mixture is pre-sintered, then secondarily ball-milled and dried to obtain the pretreated raw material; The pretreated raw material is molded and sintered to obtain the PTC ceramic material. The sintering process includes the following stages: a temperature rising stage, a glass phase melting stage, a highest temperature sintering stage, and a cooling stage. The sintering process is carried out in a neutral atmosphere. The highest temperature sintering stage is sintered by continuously increasing the temperature to provide stable kinetic energy for grain growth. The micro-grain size of the PTC ceramic material is 1.8 μm to 2.2 μm.

[0007] Further, the temperature rising stage includes: increasing the temperature to 580 °C to 620 °C at a rate of 290 °C / h to 310 °C / h, and maintaining the temperature for 25 min to 35 min.

[0008] Further, the glass phase melting stage includes: increasing the temperature to 1150 °C to 1300 °C at a rate of 270 °C / h to 290 °C / h to accelerate the melting to form a glass phase.

[0009] Further, the highest temperature sintering stage includes: continuously increasing the temperature to 1300 °C to 1325 °C within 10 min to 30 min to perform a first sintering process; continuously increasing the temperature to 1325 °C to 1340 °C within 30 min to 90 min to perform a second sintering process.

[0010] Further, the cooling stage includes: a first cooling stage of decreasing the temperature to 800 °C at a rate of 100 °C / h to 240 °C / h, and a second cooling stage of naturally cooling or air cooling to room temperature by using residual heat.

[0011] Further, the raw material includes a ceramic phase material, a semi-conducting agent, a glass phase material, and a manganese nitrate solution. The formula of the ceramic phase material is (Ba 1-x-y-z Sr x Pb y Ca z )TiO3. The value range of x is 0.01 to 0.045, the value range of y is 0.06 to 0.10, and the value range of z is 0.12 to 0.22. The molar ratio of the semi-conducting agent to titanium dioxide in the ceramic phase material is 0.15% to 0.25%. The addition amount of the glass phase material is 0.8 wt% to 1.3 wt% of the ceramic phase material. The concentration of the manganese nitrate solution is 0.4 mol / L to 0.6 mol / L. The ratio of the manganese nitrate solution to the ceramic phase material is (0.25 mL to 0.6 mL):100 g.

[0012] Further, the pre-sintering process comprises the following steps: heating to 1100-1200°C at a rate of 4-5°C / min in an air atmosphere, holding for 120-160 min; cooling to 800°C at a rate of 3-4°C / min, and naturally cooling to room temperature.

[0013] Further, in the drying granulation process, the drying temperature is 140-160°C, and the drying time is 1.5-2.5 h; the granulation method comprises: adding 12-18 mL of PVA solution with a concentration of 10-20 wt% to 100 g of dry powder, mixing uniformly, and then sieving and drying at a temperature of 110-130°C for 25-35 min.

[0014] The application also provides a PTC ceramic material prepared by the above preparation method.

[0015] The application also provides a use of the PTC ceramic material in the preparation of an electrode material, wherein the preparation of the electrode material comprises the following steps: sputtering a nickel layer on the surface of the PTC ceramic material by a magnetron sputtering process as a bottom electrode; printing silver paste on the surface of the PTC ceramic material by a printing sintering process as a surface electrode.

[0016] In summary, the application has the following advantages: In view of the defects of the traditional PTC ceramic sintering process, such as insufficient grain growth energy, asynchronous regional growth, and abnormal growth, the application improves the sintering process, provides multiple safeguards such as continuous energy supply, synchronous growth in all regions, and inhibition of abnormal growth, and finally enables the PTC ceramic material to form a fine-grained structure with uniform micro-grain size and regular grain boundary distribution (for example, the application can stably achieve a uniform grain size of about 2 μm). This fine-grained structure not only meets the basic requirement of low resistivity for PTC ceramic materials, but also significantly improves the voltage resistance per unit thickness and the high-energy impact resistance of the material, effectively avoiding problems such as delamination failure, edge sparking, and breakdown that are prone to occur in traditional materials, and provides key process support for the preparation of high-performance PTC ceramic materials. BRIEF DESCRIPTION OF DRAWINGS

[0017] Figure 1 a schematic diagram of the temperature curve of the traditional sintering method; Figure 2 a schematic diagram of the temperature curve of the sintering process according to the application; Figure 3 a photo of the ceramic sheet obtained by the traditional sintering method under an optical microscope at 400 times magnification; Figure 4A photograph of the ceramic piece prepared for Example 1 of this application, magnified 400 times under an optical microscope. Detailed Implementation

[0018] The principles and features of this application are described below with reference to embodiments. The examples are for illustrative purposes only and are not intended to limit the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0019] PTC (Positive Temperature Coefficient) ceramic materials are widely used in overcurrent protection, surge current suppression, self-limiting heating, and temperature sensing due to their unique resistance-temperature characteristics. Currently, mature PTC ceramic materials have switching temperatures ranging from -20℃ to 320℃ and resistance values ​​from 0.1Ω to 100KΩ. To achieve excellent electrical performance and reliability, PTC ceramic materials need to possess low resistivity and a uniform microstructure. Among these, the grain size is one of the key factors affecting material performance. Research shows that the grain size of PTC ceramic materials typically needs to be controlled at 5μm or larger. If the grain size is too small (e.g., less than 5μm), the resistivity of the material will increase significantly, making it difficult to achieve semiconductivity and thus failing to meet the basic requirements of the PTC effect.

[0020] In the preparation process of PTC ceramic materials, sintering is the core process that determines its final microstructure and properties. The traditional process for PTC ceramic materials typically includes steps such as secondary wet ball milling, pre-sintering to synthesize the main crystalline phase, drying after secondary ball milling, adding binder for granulation, molding, and sintering. Among these, the sintering process generally employs a staged heating method, such as... Figure 1 As shown: First, the temperature is raised to around 600℃ at a certain heating rate and held for a period of time to fully remove volatile substances such as binders and moisture from the green body (i.e., the debinding process). Then, the temperature is raised to the highest sintering temperature (usually above 1300℃) and held at this temperature for 1 to 2.5 hours to complete the grain growth, ceramic densification, and semiconductorization processes. Finally, sintering is completed by controlling the cooling rate. During the sintering process, as the temperature rises, the glassy phase material in the green body gradually melts and disperses uniformly, which plays a role in lowering the sintering temperature, absorbing harmful impurities, and promoting semiconductorization. After entering the high-temperature stage, grain growth proceeds rapidly, and small grains gradually disappear and aggregate into micro-grains of the target size (the initial powder micro-size is about 0.6μm, with high activity and a fast initial grain growth rate).

[0021] However, the traditional sintering method has significant defects, mainly manifested in the difficulty in obtaining a uniform fine crystal structure, and the specific reasons are as follows: (1) Non-uniform sintering kinetic energy and abnormal grain growth. During the holding period at the highest sintering temperature, the sintering kinetic energy of different regions of the porcelain body shows a non-uniform decay trend over time. Part of the region has a higher sintering kinetic energy, and the grain growth continues; while another part of the region has a lower sintering kinetic energy, and the grain growth slows down or stops. This difference between regions leads to inconsistent grain growth rates, which easily causes abnormal grain growth (i.e., part of the grain size significantly exceeds the average level), destroying the uniformity of the microstructure. (2) Inherent contradiction between temperature and time parameters. The grain growth process needs to rely on both temperature and time: higher temperature can provide more sintering kinetic energy, promoting grain growth, but excessively high temperature will significantly increase the risk of abnormal grain growth; prolonging the high-temperature holding time can compensate for the lack of temperature, but it will exacerbate the difference in sintering kinetic energy between different regions of the porcelain body, leading to excessive grain growth in some regions and insufficient growth in some regions. The traditional process mode of fixed highest temperature and fixed holding time is difficult to balance this contradiction, and is easy to cause the widening of the grain size distribution and the non-uniformity of the microstructure. (3) Regional temperature difference and activity decay. In the early stage of sintering, the powder activity is high (the initial powder size is about 0.6 μm), and the grain growth rate is fast; but as the holding time is prolonged, the overall activity of the material decreases, and there is a temperature gradient between the center and the surface of the porcelain body due to the difference in heat transfer, further amplifying the asynchronization of grain growth in different regions and exacerbating the problem of abnormal growth.

[0022] The non-uniformity of the above microstructure directly leads to the deterioration of the performance of the PTC ceramic material, and the macroscopic manifestations are: the breakdown voltage is reduced (the unit thickness voltage resistance is decreased), the porcelain body is easily layered under high energy impact, breakdown and edge sparking, etc., which seriously affects the reliability and service life of the product. Therefore, due to the inability to effectively control the uniformity of grain growth, the traditional sintering method is difficult to prepare high-performance PTC ceramic materials with low resistivity and uniform fine crystal structure, which limits its further development in high-end application fields. Based on this, the present application provides a PTC ceramic material with a uniform fine crystal structure and its preparation method and application. Through the improvement of raw materials, formula and process, a PTC ceramic material with low resistivity and uniform fine crystal structure (microscopic grain size controlled at about 2 μm) can be obtained, thereby improving the energy impact resistance of the material.

[0023] In a first aspect, the present application provides a preparation method of a PTC ceramic material with a uniform fine crystal structure, comprising the following steps: S1, the raw materials are weighed according to the predetermined proportion, mixed uniformly and dried to obtain a mixture.

[0024] In the specific embodiment, the raw materials include ceramic phase materials, semi-conducting agents, glass phase materials and manganese nitrate solution, wherein the formula of the ceramic phase materials is (Ba 1-x-y-zSr x Pb y Ca z )TiO3, x is in the range of 0.01-0.045, y is in the range of 0.06-0.10, and z is in the range of 0.12-0.22; the molar ratio of the semi-conducting agent to titanium dioxide in the ceramic phase material is 0.15%-0.25%; the addition amount of the glass phase material is 0.8wt%-1.3wt% of the ceramic phase material; the concentration of the manganese nitrate solution is 0.4mol / L-0.6mol / L, and the ratio of the manganese nitrate solution to the ceramic phase material is (0.25mL-0.6mL):100g. Preferably, the raw materials are weighed according to the preset ratio, that is, the high-purity materials used are determined according to the target product, the accurate mass of each raw material required is calculated according to the stoichiometric ratio, and then the raw materials are accurately weighed.

[0025] The application adopts a strontium-lead-calcium co-formulation system as the main component system, and strontium (Sr), lead (Pb), and calcium (Ca) elements as the basis combined with titanium (Ti) elements to form the main crystal phase skeleton. Through the synergistic effect of the three elements, a stable crystal structure basis is provided for the material, and at the same time, by adjusting the ratio of the three, the lattice parameters of the main crystal phase are preliminarily controlled, leaving adjustment space for subsequent semi-conducting and performance optimization. Transition metal oxides such as Nb2O5, Y2O3, La2O3, and Sm2O3 are used, which can be used alone or in various combinations, as key semi-conducting additives. The core function is to control the lattice defects and carrier concentration by ion doping into the main crystal lattice, and to promote the material to realize semi-conducting. Appropriate addition of SiO2, Al2O3, Li2CO3, and BN, etc. Such substances can melt to form a glass phase during sintering, playing a dual function of sintering and impurity control. A small amount of manganese ions (Mn 2+ ) is added, and by precisely controlling the amount of manganese ions, the positive temperature coefficient effect of the material is optimized, and the temperature sensitivity and electrical performance stability of the material are further improved.

[0026] In the specific implementation, the semi-conducting agent includes at least one of Nb2O5 (di-niobium pentoxide), Y2O3 (yttrium oxide), La2O3 (lanthanum oxide), and Sm2O3 (samarium oxide), and the glass phase material includes at least one of TiO2 (titanium dioxide), SiO2 (silicon dioxide), Al2O3 (aluminum oxide), Li2CO3 (lithium carbonate), and BN (boron nitride). Among them, the transition metal oxides selected by the application have excellent semi-conducting effect. The +3 valence ions such as Y 3+ , La 3+ , and Sm 3+ in such oxides replace the A-site ions (Ba 2+ , Sr 2+ , Pb2+ and Ca 2+ ) or Nb 5+ 5+ valence ions to replace the titanium ions in the B site of the perovskite structure (main crystal phase), effectively increasing the carrier concentration in the crystal lattice, and promoting the transition of the material from an insulating state to a semi-conducting state. At the same time, the combination of multiple transition metal oxides can reduce the lattice distortion or doping saturation problems that may occur with single impurity doping through ion synergistic doping, ensuring uniform distribution of carrier concentration and avoiding resistance fluctuations caused by local carrier concentration that is too high or too low, and ensuring the stability and consistency of the semi-conducting properties of the material. Among them, the glass phase forming substances play a key auxiliary role in the sintering process: first, the melting temperature of such substances is lower than the sintering temperature of the main crystal phase, which can melt and form a flowable glass phase in the high-temperature sintering stage, filling the interstitial space between the main crystal phase particles, reducing the sintering activation energy of the main crystal phase, achieving low-temperature sintering effect, which can not only reduce the excessive promotion of grain growth caused by high-temperature sintering, but also improve the density of the ceramic body; secondly, the glass phase has strong impurity adsorption capacity, which can wrap and fix the harmful impurities (such as alkali metal ions, heavy metal impurities) in the material at the grain boundary, avoiding the influence of impurities on the semi-conducting effect by entering the main crystal phase, and the purified grain boundary can form a more stable barrier structure to ensure the full play of the PTC effect. In addition, the addition of boron nitride can further optimize the dispersibility of the glass phase, avoiding uneven grain boundary performance caused by local aggregation of the glass phase.

[0027] In the specific implementation, the raw materials of the ceramic phase material can be selected as follows: barium carbonate, strontium carbonate, calcium carbonate, lead oxide, and titanium dioxide. The manganese ions in this application are added in the form of manganese nitrate solution, and the addition of a small amount of manganese ions is the key to optimizing the PTC effect of the material. As an acceptor impurity, manganese ions can selectively adsorb at the grain boundary of the main crystal phase, form charge compensation with the donor ions (such as Nb 5+ ) at the grain boundary, regulate the height of the grain boundary barrier, and thus significantly improve the positive temperature coefficient effect (i.e. the characteristic of rapid increase of resistivity with temperature rise) of the material; at the same time, manganese ions can also inhibit the migration of defects at the grain boundary, reduce the degradation of the grain boundary structure under high-temperature working environment, improve the electrical performance stability of the material in long-term temperature cycling, reduce the risk of product failure caused by PTC effect decay, and further ensure the application reliability of the material.

[0028] In the specific implementation, the method for mixing the raw materials includes: mixing the raw materials with pure water and ball milling medium (preferably agate ball) in a mass ratio of 1:1.3:3, and then ball milling on a planetary ball mill at a speed of 420 Hz for 4 hours.

[0029] In the specific implementation, the drying temperature is 140°C-160°C, and the drying time is 1.5h-2.5h.

[0030] S2, after the pre-sintering treatment of the mixture, the second ball milling and drying granulation, the pretreated raw material is obtained.

[0031] In the embodiment, the pre-sintering treatment comprises the following steps: heating to 1100℃-1200℃ at a rate of 4℃ / min-5℃ / min in air atmosphere, holding for 120min-160min; cooling to 800℃ at a rate of 3℃ / min-4℃ / min, and naturally cooling to room temperature.

[0032] In the embodiment, the second ball milling method comprises: mixing the material obtained by the pre-sintering treatment with pure water and ball milling medium (preferably agate ball) according to the mass ratio of 1:0.8:3, then wet ball milling, the ball milling time is 4h, and the ball milling speed is 420Hz.

[0033] In the embodiment, the drying comprises: the drying temperature is 140℃-160℃, and the drying time is 1.5h-2.5h.

[0034] In the embodiment, the granulation method comprises: adding 12mL-18mL PVA solution with a concentration of 10wt%-20wt% to 100g dry powder, mixing uniformly, and then sieving and drying treatment at a temperature of 110℃-130℃ for 25min-35min. Preferably, the polymerization degree of the PVA material is 500.

[0035] S3, the pretreated raw material is subjected to forming treatment and sintering treatment to obtain the PTC ceramic material. The sintering refers to the process that the green body of the PTC ceramic powder is subjected to high temperature, the particles in the green body are bonded and the substance is transferred, the pores are removed, the volume is shrunk, the strength is improved, and the green body gradually becomes a dense body with certain geometric shape and solid sintered body, that is, the process of semi-conducting of the PTC functional material.

[0036] In the embodiment, the forming treatment comprises: placing the pretreated raw material after the granulation in a single punch press to obtain a green body with a size of φ(18mm-20mm, diameter)×(2mm-3mm, thickness) and a weight of 2.93g-2.97g.

[0037] In the embodiment, the sintering process includes the following stages: a temperature rising stage, a glass phase melting stage, a maximum temperature sintering stage, and a cooling stage. The sintering process is in a neutral atmosphere (i.e. natural environment), and the maximum temperature sintering stage is sintered by continuous heating. The sintering atmosphere affects the performance of the PTC ceramic by affecting the chemical reaction and microstructure of the material. The PTC ceramic functional material needs to avoid the interference of oxidation or reduction reaction on the semiconductor characteristics, so the neutral atmosphere sintering is preferred in the application. For large sintering equipment such as a tunnel furnace, the atmosphere control strategy is further optimized in the application, and the imported end exhaust + tail end air supply mode is adopted. On the one hand, the exhaust removes the gas volatilized by the blank in the temperature rising stage, avoiding the influence of gas residue on sintering. On the other hand, the fresh air with appropriate oxygen content is sent into the furnace by air supply, so as to optimize the electrical properties of the material. In addition, the heat discharged at the tail end of the furnace can be transported to the front end by the tail end air supply, realizing heat recycling and saving energy.

[0038] In the embodiment, the temperature rising stage includes: rising to 580-620°C at a rate of 290-310°C / h, and keeping for 25-35 min. In the application, the temperature rising rate can consider the sintering efficiency and the integrity of the blank. In the conventional case, the temperature rising rate is preferably 300°C / h, and the temperature rising rate is adjusted dynamically according to the size of the blank. The larger the size of the blank, the lower the temperature rising rate should be, so as to ensure that the internal gas is fully discharged. When the size of the blank is small, the temperature rising rate can be appropriately accelerated, so as to improve the production efficiency under the premise of ensuring the quality. 580-620°C is a degassing stage, and the core target is to completely remove the binder in the blank, so as to avoid the carbonization of the binder at high temperature and cause adverse effects on sintering. The PVA is fully burned, decomposed and completely volatilized in the constant temperature environment of about 600°C, so as to clear the impurities and obstacles for subsequent high temperature sintering, and ensure the structural stability of the blank at high temperature.

[0039] In the specific embodiment, the glass phase melting section includes: heating at a rate of 270℃ / h~290℃ / h to 1150℃~1300℃ to accelerate melting to form a glass phase. Among them, the glass phase melting section is the key melting interval of the glass phase forming substance in the PTC ceramic formula, and the core role of this stage is to realize low-temperature sintering through the formation of a glass phase and to create conditions for subsequent uniform grain growth. As the sintering temperature rises, the atomic diffusion rate increases, the ceramic particles change from point contact to surface contact, the voids gradually shrink and form closed isolated pores, and small particles begin to disappear and move with the grain boundaries and gradually grow. At the same time, the glass phase formers such as silicon dioxide, aluminum oxide, lithium carbonate and boron nitride added in the formula will melt to form a flowable glass phase in this temperature interval. The core function of the glass phase in this application mainly reflects two aspects: one is to fill the gap between particles, reduce the sintering activation energy of the main crystal phase, realize low-temperature sintering, and avoid excessive promotion of grain growth at high temperature; the second is to adsorb harmful impurities in the material, and provide a clean environment for the semi-conducting of the material. In order to ensure the rapid and uniform melting of the glass phase, which wraps the small particles that have not grown, this application adopts a rapid heating strategy, and the heating rate in the 600℃~(1150℃~1300℃) interval is controlled to be 270℃ / h~290℃ / h. By rapidly crossing the glass phase melting interval, the local glass phase aggregation is reduced, the uniform distribution of the glass phase in the body is ensured, and the foundation for subsequent uniform grain growth is laid.

[0040] In the specific embodiment, the highest temperature sintering section includes: continuously heating to 1300℃~1325℃ within 10min~30min to perform first sintering treatment; continuously heating to 1325℃~1340℃ within 30min~90min to perform second sintering treatment. Among them, the highest sintering temperature of 1300℃~1340℃ is divided into two sections for temperature control, and stable kinetic energy is provided for grain growth by continuously increasing the temperature. The first stage (1300℃~1325℃): the holding time is set to 10min~30min, which mainly provides initial kinetic energy for grain growth, promotes the grain into the early stage of rapid growth, and ensures that the grains in each region start growing synchronously; the second stage (1325℃~1340℃): the holding time is set to 30min~90min, which is the key period of grain growth, and the influence on the material resistivity is significantly greater than the first stage. By adjusting the holding time of this stage, the material resistivity can be precisely controlled. Through the treatment of the two stages, this application can ensure that the temperature continuously and slowly rises in the high temperature interval, and continuously provides kinetic energy for the grain growth of each region (including the center and the surface) of the body, avoids regional growth differences, and finally realizes uniform grain growth and overall uniformity of the ceramic body.

[0041] In the embodiment, the cooling section comprises: a first cooling section for cooling to 800 DEG C at a rate of 100 DEG C / h-240 DEG C / h, and a second cooling section for using waste heat for natural cooling or air cooling. In the application, the cooling rate is controlled at 100 DEG C / h-240 DEG C / h, which can be dynamically adjusted according to the target normal temperature resistance value, for example, when the normal temperature resistance value needs to be increased, the cooling rate is reduced; when the normal temperature resistance value needs to be reduced, the cooling rate is appropriately increased. At the same time, the lower limit of the cooling temperature is set to 800 DEG C, and the temperature above 800 DEG C is cooled by controlled cooling, and the temperature below 800 DEG C can be naturally cooled or accelerated by blowing controlled air into the furnace through the furnace tail, which guarantees the performance while taking into account the cooling efficiency.

[0042] In a second aspect, based on the overall inventive concept, the application also provides a PTC ceramic material obtained by the above preparation method, wherein the microcrystalline grain size of the PTC ceramic material is 1.8-2.2 microns.

[0043] The PTC ceramic material obtained by the traditional sintering method has a micro size of about 5 mu m. It can be seen from the micro size that the significant increase in the number of crystal grains directly leads to the exponential increase in the number of grain boundaries. The number and distribution of the grain boundaries, as key structural units of the PTC ceramic material, have a decisive influence on the electrical properties, mechanical stability and failure resistance of the material, and lay a microstructure foundation for subsequent performance optimization. For example (1), in the application process of the PTC ceramic material, the voltage will be distributed among the crystal grains in the thickness direction after the voltage is applied, and the voltage of a single crystal grain directly affects the voltage effect (such as parameters of a sudden input current, maximum input power and the like) of the material. The voltage effect is a core inducement of problems such as delamination failure, edge sparking arc and breakdown of the material, so the smaller the maximum input power is, the lower the failure possibility is. The single crystal grain voltage of the fine crystal material of 1.8 mu m to 2.2 mu m of the application is only 40% of that of the traditional material. According to the electrical properties of the PTC ceramic material, the lower the single crystal grain voltage is, the smaller the resistance value of the crystal grain caused by the voltage is, and then the maximum input power of the material is significantly reduced, which fundamentally reduces the failure risk of delamination, sparking, breakdown and the like caused by high power impact. For example (2), the optimization of the voltage effect also has a positive influence on the working balance temperature of the PTC ceramic material. Under the action of high voltage, the voltage effect of the traditional coarse crystal material is more significant due to the higher single crystal grain voltage, which is manifested as a greater resistance value reduction range, greater energy consumption in the material and higher working balance temperature. The voltage effect of the fine crystal material of about 2 mu m of the application is weakened due to the low single crystal grain voltage, which reduces the energy consumption and makes the working balance temperature of the material under high voltage conditions present a low level stable trend. From the material aging mechanism, the working balance temperature is a key factor affecting the aging performance. The lower the balance temperature is, the slower the thermal degradation speed of the microstructure in the material is, and the smaller the attenuation range of the core performances such as grain boundary stability and resistivity consistency is, thereby greatly prolonging the service life of the material and improving the long-term working reliability. For example (3), from the material aging mechanism, the working balance temperature is a key factor affecting the aging performance. The lower the balance temperature is, the slower the thermal degradation speed of the microstructure in the material is, and the smaller the attenuation range of the core performances such as grain boundary stability and resistivity consistency is, thereby greatly prolonging the service life of the material and improving the long-term working reliability. For example (4), when the PTC ceramic material is subjected to energy impact, micro defects (such as micro cracks) will be generated in the material. The expansion speed and path of the defects directly determine the energy impact resistance of the material. Research shows that the minimum size of the defects of the PTC ceramic material is equivalent to the micro grain size, so the reduction of the grain size can optimize the energy impact resistance from two dimensions. The minimum size of the defects of the fine crystal material of about 2 mu m of the application is much smaller than that of the traditional coarse crystal material of about 5 mu m, and the expansion size of the defects caused by energy impact is limited in a smaller range, which avoids the macro failure caused by the rapid expansion of the defects.At the same time, since the number of 2pm grains is about 15 times of the number of 5pm grains, the defects need to cross more grain boundaries in the expansion process, and the path is significantly lengthened. Assuming that the defect expansion scale caused by each energy impact is in the order of a single grain size, the grain boundary resistance that needs to be overcome in the defect expansion in the fine-grained material is greater, and the expansion speed is slower, thereby greatly improving the energy impact resistance of the material.

[0044] In a third aspect, based on the overall inventive concept, the application further provides an application of the PTC ceramic material in the preparation of an electrode material, wherein the preparation of the electrode material comprises the following steps: S101, sputtering a nickel layer on the surface of the PTC ceramic material by a magnetron sputtering process as a bottom electrode.

[0045] In the embodiment, the PTC ceramic material needs to be cleaned and dried before being prepared into an electrode material, wherein the cleaning is performed by an ultrasonic cleaning device at a frequency of 20 kHz for 12-20 minutes; the drying temperature is 175-185℃, and the drying time is 3.5-4.5 hours.

[0046] In the embodiment, the target material current of the magnetron sputtering process is 23-27 A, the vacuum degree is 5x10 -3 Pa, and the thickness of the nickel layer is greater than or equal to 0.3pm.

[0047] S102, printing silver paste on the surface of the PTC ceramic material by a printing and sintering process as a surface electrode.

[0048] In the embodiment, the silver paste is PTC special silver paste with a solid content of 80%, the screen mesh number of the printing and sintering process is 180 meshes, the sintering temperature is 550-580℃, the holding time is 15-25 minutes, and the thickness of the silver paste is preferably 3.5-6.5pm.

[0049] In the application, the bottom nickel electrode and the surface silver electrode are combined to form a composite electrode structure. The existence of the nickel layer can improve the adhesion between the electrode and the ceramic substrate, buffer thermal stress, and prevent the diffusion of the surface silver into the ceramic interior (to avoid affecting the PTC effect). The surface silver electrode can ensure efficient current conduction due to its high conductivity. The combination of the two solves the problems of insufficient conductivity of a single nickel electrode, the inability of a single silver electrode to achieve ohmic contact with the ceramic body, and poor electrode reliability. Through pretreatment processes and precise parameter control, the performance of the electrode (conductivity, adhesion, stability) is optimized in all directions, and the reliability and consistency of the PTC ceramic electrode product in the long-term use process are finally ensured.

[0050] In summary, the application has at least the following beneficial effects: (1) The application breaks through the limitation of fixed temperature in the high temperature stage of traditional sintering process, scientifically divides the high temperature sintering temperature region of PTC ceramic material sintering, and matches the different heating speed according to the grain growth demand of different temperature sections. Through slow and orderly sintering temperature promotion mode, the sintering kinetic energy is continuously and stably supplied for the grain growth process. Compared with the problem that the kinetic energy gradually decreases with the holding time in the high temperature stage of traditional process, the sintering method of the application can avoid the grain growth stagnation caused by the interruption or shortage of kinetic energy supply, and ensure that the grains can obtain sufficient energy support in the whole high temperature sintering stage, laying a foundation for subsequent uniform growth.

[0051] (2) Based on the synergistic effect of segmented temperature control and different heating speed, the application can effectively solve the problem of uneven sintering kinetic energy in different regions of the ceramic body in the traditional process. By accurately controlling the heating rhythm of each temperature section, the temperature field distribution of each region (including the central region and the surface region) in the ceramic body can be made more uniform, so that the grains in different regions can obtain similar growth environment and kinetic energy conditions in the same sintering stage, and the grain growth process in the whole region of the ceramic body can be carried out synchronously. Thus, the unbalanced state of the traditional process that the grain growth in some regions tends to slow down or stops, while the grain growth in some regions is still rapid is completely changed, the spatial consistency of grain growth is greatly improved, and the problem of microstructure unevenness caused by regional growth difference is reduced from the root.

[0052] (3) The application realizes double precise control of key parameters of the sintering process by segmenting the temperature and synergistically controlling the different heating speed: on the one hand, through the temperature segmentation design, the highest temperature threshold of each stage can be reasonably controlled according to the rate characteristics of grain growth in different temperature intervals, so as to avoid the excessive growth of grains caused by the continuous action of single high temperature; on the other hand, combined with the optimization of the heating speed of each temperature section, the actual effective holding time at different temperatures can be indirectly limited to prevent the imbalance of grain size caused by too long holding time in a certain temperature interval. The above double control mechanism can effectively inhibit the core conditions of abnormal grain growth, and eliminate the phenomenon of uneven grain size distribution and abnormal coarse grains caused by unreasonable temperature or time parameter setting in the traditional process.

[0053] The above technical solutions of the application will be described in detail in combination with specific embodiments.

[0054] The raw materials and equipment involved in the following embodiments include: Barium carbonate (BaCO3), with a purity of 99.5%, produced by Sichuan Mianyang Yuanda New Material Co., Ltd.

[0055] Strontium carbonate (SrCO3), with a purity of 99.5%, produced by Chongqing Dazu Hongdie Strontium Industry Co., Ltd.

[0056] Calcium carbonate (CaCO3), purity 99.3%, manufacturer Shandong Dongying New Century Optoelectronic Material Co., Ltd.

[0057] Lead oxide (PbO), purity 99.5%, manufacturer Guangdong Jinyusha Chemical Co., Ltd.

[0058] Titanium dioxide (TiO2), purity 99.9%, manufacturer Hubei Tianchi Electronic Material Co., Ltd.

[0059] Lanthanum trioxide (La2O3), 3N standard, manufacturer Jiangxi Zhongli Tantalum-Niobium Co., Ltd.

[0060] Samarium oxide (Sm2O3), 3N standard, manufacturer Jiangxi Zhongli Tantalum-Niobium Co., Ltd.

[0061] Niobium pentoxide (Nb2O5), 4N standard, manufacturer Jiangxi Zhongli Tantalum-Niobium Co., Ltd.

[0062] Silicon dioxide (SiO2), AR standard, manufacturer Xilong Science Co., Ltd.

[0063] Aluminum trioxide (Al2O3), AR standard, manufacturer Sinoreagent Co., Ltd.

[0064] Lithium carbonate (Li2CO3), AR standard, manufacturer Sinoreagent Co., Ltd.

[0065] Boron nitride (BN), purity 99.9%, manufacturer Hebei Keze Metal Material Co., Ltd.

[0066] Manganese nitrate (Mn(NO3)2), AR standard, manufacturer Chongqing Chuandong Chemical Co., Ltd.

[0067] Electric heating air drying oven TDB-216SCBF, Chengdu Xingtianyu Experimental Instrument Co., Ltd.

[0068] Resistance meter DMM6500, KEITHEY.

[0069] High-temperature box-type resistance furnace ZZ-6-14, Chengdu Langchen Electronics Co., Ltd.

[0070] Laser particle size analyzer JL-1155, Chengdu Jingxin Powder Testing Equipment Co., Ltd.

[0071] Powder tablet press SFJ-160KN, Jiangsu Wujing Chaoyu Press.

[0072] Electronic balance (620g / 0.01g), Sartorius Industrial Technology Co., Ltd.

[0073] Planetary ball mill YXQM-4L, Changsha Miqil Instrument and Equipment Co., Ltd.

[0074] Optical microscope HJ1, Nanjing Nanpai Technology Co., Ltd.

[0075] Example 1 The present example provides a PTC ceramic material with a uniform fine-grained structure, which is prepared by the following method: (1) Weighing raw materials Including 107.64 g of barium carbonate, 0.55 g of strontium carbonate, 14.32 g of calcium carbonate, 17.17 g of lead oxide, 61.68 g of titanium dioxide, 0.24 g of yttrium oxide, 0.22 g of niobium pentoxide, 0.82 g of silicon dioxide, 0.12 g of lithium carbonate, 0.25 g of boron nitride, and 0.85 mL of manganese nitrate solution (0.5 mol / L).

[0076] (2) First ball milling After mixing the weighed raw materials, mix with pure water and agate balls in a mass ratio of 1:1.3:3 and wet ball mill at a speed of 420 Hz for 4 h. After ball milling, transfer to a clean enamel plate and place in an electric heating air drying oven at a temperature of 150°C for drying for 2 hours to obtain a mixture.

[0077] (3) Pre-sintering Put the mixture into a corundum mullite crucible, cover it, and pre-sinter it in an air atmosphere. As shown in Table 1, the pre-sintering process includes: the first segment is uniformly heated from room temperature to 1150°C, and the heating time is 270 min; then keep the temperature at 1150°C for 150 min; then reduce the temperature from 1150°C to 800°C in 90 min; finally, reduce to room temperature in 60 min, to obtain a pre-sintered material. Figure 1 (4) Second ball milling and drying granulation

[0078] Mix the pre-sintered material with pure water and agate balls in a mass ratio of 1:0.8:3, then ball mill on a planetary ball mill at a speed of 420 Hz for 4 h. After ball milling, transfer the slurry to a clean enamel plate and place it in an electric heating air drying oven to obtain a dry powder, the drying temperature is 150°C, and the time is 2h. According to the weight of 15 mL PVA solution (concentration of 17wt%, PVA polymerization degree of 500) per 100 g of dry powder, mix uniformly in a mortar, then pass through a 40 mesh sieve, and then dry at 120°C for 0.5h to obtain a pretreated raw material.

[0079] (5) Forming

[0080] ​The pretreated raw material is placed in a single punch press to be pressed into a green body with a diameter of 18.68 mm, a thickness of 2.98 mm, and a weight of 2.97 g.

[0081] (6) Sintering The green body is placed on a V-shaped groove, the V-shaped groove is placed in a high-alumina sagger and covered, the high-alumina sagger is placed on the base of a cover furnace, the base is sent into the cover by an automatic lifting device, the two are sealed in a close manner, and air convection between the sealed area and the outside is prevented. The sintering process of all examples and comparative examples in the present application is carried out in a V-shaped groove + high-alumina sagger + cover furnace. The size of the high-alumina sagger is 170 mm x 170 mm x 45 mm in length, width and height, respectively, the wall thickness of the sagger is 10 mm, and the sagger mouth has four air-permeable notches with a width of 30 mm and a depth of 5 mm. The V-shaped groove has a length of 53 mm, a width of 18 mm, and a thickness of 3 mm, and is made of yttrium-stabilized zirconia material and sintered at a temperature of 1600°C or above. The inner wall of the cover furnace is made of lightweight high-alumina fiber, which has the characteristics of light weight, temperature resistance, and excellent heat preservation performance. The cover furnace is divided into a cover and a product-bearing base, and the cover is fixed.

[0082] During the sintering process, a neutral atmosphere is introduced, as shown in the sintering curve, which includes: Figure 2 heating at a rate of 300°C / h to 600°C, holding for 30 min to remove glue; controlling the heating rate to be 280°C / h to continuously heat to 1300°C to promote the formation of a glass phase; continuously heating to 1325°C for 30 min and to 1335°C for 45 min to continuously provide kinetic energy for sintering and ensure uniform growth of the grains in each region; After the heating is completed, cooling at a rate of 130°C / h to 800°C, and then naturally cooling to room temperature to obtain a PTC ceramic material (raw sheet). The photograph under an optical microscope at 400 times magnification is shown in Figure 4 .

[0083] The present embodiment also provides a preparation method of a PTC ceramic material electrode, which comprises: The obtained PTC ceramic material is ultrasonically cleaned in pure water for 15 min at an ultrasonic frequency of 20 kHz, divided into four cleaning tanks, cleaned with running water, and then dried at a temperature of 180°C for 4 h.

[0084] A nickel layer with a thickness of 0.35 μm is sputtered on the surface of the cleaned PTC ceramic material by a magnetron sputtering process as an ohmic electrode. The target current of the magnetron sputtering process is 25 A, and the vacuum degree is 5 x 10 -3 Pa.​

[0085] After sputtering of the nickel electrode is completed, the PTC ceramic material electrode surface is printed with PTC special silver paste (solid content of 80%) by a printing and sintering process, and the printing thickness is 3.5 μm, serving as a surface silver electrode. In the printing and sintering process, the silk screen mesh number is 180 meshes, the sintering temperature is 560 ℃, and the holding time is 20 min.

[0086] Example 2 The present embodiment provides a PTC ceramic material with a uniform fine-grained structure, which is prepared by the following method: (1) Weighing raw materials Including 107.64 g of barium carbonate, 0.55 g of strontium carbonate, 14.32 g of calcium carbonate, 17.17 g of lead oxide, 61.68 g of titanium dioxide, 0.24 g of yttrium oxide, 0.22 g of niobium pentoxide, 0.82 g of silicon dioxide, 0.12 g of lithium carbonate, 0.25 g of boron nitride, and 0.85 mL of manganese nitrate solution (0.5 mol / L).

[0087] (2) First ball milling After the weighed raw materials are mixed, they are mixed with pure water and agate balls at a mass ratio of 1:1.3:3 and wet ball milled at a speed of 420 Hz for 4 h. After ball milling, the slurry is transferred to a clean enamel tray and dried in an electric heating air drying oven at a temperature of 150 ℃ for 2 hours to obtain a mixed material.

[0088] (3) Pre-sintering The mixed material is placed in a corundum mullite crucible, covered, and pre-sintered in an air atmosphere. The pre-sintering process includes: uniformly heating from room temperature to 1150 ℃ for 270 min; then holding at 1150 ℃ for 150 min; then reducing the temperature from 1150 ℃ to 800 ℃ in 90 min; and finally reducing to room temperature in 60 min, to obtain a pre-sintered material.

[0089] (4) Second ball milling and drying granulation The pre-sintered material is mixed with pure water and agate balls at a mass ratio of 1:0.8:3, and then ball milled on a planetary ball mill at a speed of 420 Hz for 4 h. After ball milling, the slurry is transferred to a clean enamel tray and dried in an electric heating air drying oven to obtain a dry powder. The drying temperature is 150 ℃, and the time is 2 h.

[0090] According to the weight of 15 mL of PVA solution (concentration of 13 wt%, degree of polymerization of 500) per 100 g of dry powder, mix uniformly in a mortar, then pass through a 40 mesh sieve, and then dry at 120 ℃ for 0.5 h to obtain a pretreated raw material.

[0091] (5) Forming The pretreated raw material was placed in a single punch press to be pressed into a green body with a diameter of 18 mm, a thickness of 2.95 mm, and a weight of 2.95 g.

[0092] (6) Sintering The sintering process was carried out in a neutral atmosphere, and the sintering curve included: The temperature was raised to 600℃ at a rate of 290℃ / h, and the glue was removed for 30 min; The temperature was continuously raised to 1280℃ at a rate of 280℃ / h to promote the formation of a glass phase; The temperature was continuously raised to 1325℃ for 30 min, and then continuously raised to 1340℃ for 45 min to provide kinetic energy for sintering and ensure uniform growth of the grains in each region; After the temperature raising was completed, the temperature was cooled to 800℃ at a rate of 130℃ / h, and then naturally cooled to room temperature to obtain a PTC ceramic material (raw sheet).

[0093] The embodiment also provides a preparation method of a PTC ceramic material electrode, which comprises: The obtained PTC ceramic material is ultrasonically cleaned in pure water for 15 min at an ultrasonic frequency of 20 kHz, is divided into four cleaning tanks, is cleaned by flowing water, and is cleaned on the surface, and then is dried at a temperature of 180℃ for 4 h.

[0094] A nickel layer with a thickness of 0.4 μm is sputtered on the surface of the cleaned PTC ceramic material by a magnetron sputtering process to serve as an ohmic electrode. In the magnetron sputtering process, the target current is 25 A, and the vacuum degree is 5×10 -3 Pa.

[0095] After the nickel electrode sputtering is completed, a PTC special silver paste (solid content of 80%) is printed on the electrode surface of the PTC ceramic material by a printing sintering process to serve as a surface silver electrode. The printing sintering process has a screen mesh of 180 meshes, a sintering temperature of 560℃, and a holding time of 20 min.

[0096] Example 3 The embodiment provides a PTC ceramic material with a uniform fine-grained structure, which is prepared by the following method: (1) Weighing raw materials The raw materials include 107.64 g of barium carbonate, 0.55 g of strontium carbonate, 14.32 g of calcium carbonate, 17.17 g of lead oxide, 61.68 g of titanium dioxide, 0.24 g of yttrium trioxide, 0.22 g of niobium pentoxide, 0.82 g of silicon dioxide, 0.12 g of lithium carbonate, 0.25 g of boron nitride, and 0.85 mL of manganese nitrate solution (0.5 mol / L).

[0097] (2) First ball milling After the weighed raw materials were mixed, they were mixed with pure water and agate balls at a mass ratio of 1:1.3:3 and wet ball milled at a speed of 420 Hz for 4 h. After the ball milling was completed, the slurry was transferred to a clean enamel plate and placed in an electric heating air drying oven to dry at a temperature of 150°C for 2 h to obtain a mixture.

[0098] (3) Pre-sintering The mixture was placed in a corundum mullite crucible, covered, and pre-sintered in an air atmosphere. The pre-sintering process included: uniformly increasing the temperature from room temperature to 1150°C for 270 min; then maintaining the temperature at 1150°C for 150 min; then reducing the temperature from 1150°C to 800°C in 90 min; and finally reducing the temperature to room temperature in 60 min to obtain a pre-sintered material.

[0099] (4) Second ball milling and drying and granulation The pre-sintered material was mixed with pure water and agate balls at a mass ratio of 1:0.8:3, and then ball milled on a planetary ball mill at a speed of 420 Hz for 4 h. After the ball milling was completed, the slurry was transferred to a clean enamel plate and placed in an electric heating air drying oven to obtain a dry powder. The drying temperature was 150°C, and the time was 2 h.

[0100] According to the weight of 100 g of dry powder, 15 mL of PVA solution (concentration of 13 wt%, degree of polymerization of 500) was added. After mixing uniformly in a mortar, it was sieved through a 40 mesh sieve, and then dried at 120°C for 0.5 h to obtain a pretreated raw material.

[0101] (5) Forming The pretreated raw material was placed in a single punch press to form a green body with a diameter of 18.68 mm, a thickness of 2.98 mm, and a weight of 2.97 g.

[0102] (6) Sintering The sintering process was carried out in a neutral atmosphere, and the sintering curve included: Increasing the temperature to 600°C at a rate of 305°C / h for 30 min to remove the glue; Controlling the heating rate to 280°C / h to continuously increase the temperature to 1305°C to promote the formation of a glass phase; Continuously increasing the temperature to 1325°C for 30 min, and then to 1335°C for 45 min to continuously provide kinetic energy for sintering and ensure uniform growth of the grains in each region; After the temperature was increased, the temperature was cooled to 800°C at a rate of 130°C / h, and then naturally cooled to room temperature to obtain a PTC ceramic material (raw sheet).

[0103] The embodiment also provides a preparation method of the PTC ceramic material electrode, comprising the following steps: The obtained PTC ceramic material is ultrasonically cleaned in pure water for 15 min at an ultrasonic frequency of 20 kHz, is divided into four cleaning tanks, is cleaned by flowing water, and is then dried at a temperature of 180 DEG C for 4 h.

[0104] A nickel layer with a thickness of 0.5 mu m is sputtered on the surface of the cleaned PTC ceramic material by a magnetron sputtering process, as an ohmic electrode. -3 Pa.

[0105] After the sputtering of the nickel electrode is completed, PTC special silver paste (solid content of 80%) is printed on the electrode surface of the PTC ceramic material by a printing and sintering process, as a surface silver electrode, and the printing thickness is 6.5 mu m.

[0106] Comparative Example 1 The comparative example provides a preparation method of a PTC ceramic material, which is different from the embodiment 1 in that: Figure 3 a traditional sintering curve is used in the sintering process, the temperature is increased to 1330 DEG C and kept for 75 min, then the temperature is decreased to 800 DEG C at a rate of 120 DEG C / h, and then the temperature is naturally cooled to room temperature to obtain a blank sheet.

[0107] The remaining steps are the same.

[0108] Comparative Example 2 The comparative example provides a preparation method of a PTC ceramic material, which is different from the embodiment 1 in that: (1) the dosages of raw materials are adjusted and selected: the dosage of strontium carbonate is 1.54 g, the dosage of calcium carbonate is 14.21 g, the dosage of lead oxide is 15.58 g, the dosage of niobium pentoxide is 0.25 g, the dosage of silicon dioxide is 0.95 g, the dosage of lithium carbonate is 0.08 g, and the dosage of manganese nitrate is 0.6 mL; no yttrium trioxide and boron nitride is added, and 0.12 g of lanthanum trioxide and 0.3 g of aluminum trioxide are additionally added.

[0109] (2) a traditional sintering curve is used in the sintering process, the temperature is increased to 1330 DEG C and kept for 95 min, then the temperature is decreased to 800 DEG C at a rate of 135 DEG C / h, and then the temperature is naturally cooled to room temperature to obtain a blank sheet.

[0110] The remaining steps are the same.

[0111] Comparative Example 3 This comparative example provides a method for preparing PTC ceramic materials, which differs from Example 1 in that: (1) Adjustment of raw material dosage and selection: The dosage of barium carbonate is 108.88g, strontium carbonate is 0.56g, lead oxide is 15.67g, niobium pentoxide is 0.32g, silicon dioxide is 0.88g, lithium carbonate is 0.07g, boron nitride is 0.35g, and manganese nitrate is 0.6mL. Yttrium oxide and lanthanum oxide are not added, and 0.35g of aluminum oxide is added in addition.

[0112] (2) The sintering process adopts the traditional sintering curve, heating to 1330℃ and holding for 120 min, then cooling to 800℃ at a rate of 110℃ / h, and then naturally cooling to room temperature to obtain raw sheet.

[0113] The remaining steps are the same.

[0114] The raw materials and amounts used in Example 1 and Comparative Examples 1-3 are shown in Table 1, and the performance parameters of the obtained PTC ceramic materials and electrode materials are shown in Table 2.

[0115] Table 1. Reference Table of Raw Materials and Usage

[0116] Table 2 Performance Parameters

[0117] Table 2 lists the performance and parameter testing methods as follows: (1) The diameter and thickness of the product are measured by micrometer.

[0118] (2) Resistance value at room temperature: Place the product in an environment of 25℃±2℃ for more than 4 hours and then test the resistance value with a resistance meter.

[0119] (3) Switching temperature: A resistance-temperature characteristic testing device is used to automatically test the resistance value corresponding to the temperature range of 25℃ to 250℃. Every 4℃ is a temperature test point. After the temperature is constant, the corresponding resistance value is tested and recorded. After the test is completed, the resistance-temperature characteristic curve is simulated by an algorithm, and the switching temperature value is calculated.

[0120] (4) Breakdown voltage: In a normal temperature environment, use a 50Hz AC power supply, start applying voltage from 0V, apply voltage slowly, the voltage step gradient is 3V for voltages below 10V, the voltage step gradient is 30V for voltages from 10V to 100V, and the voltage step gradient is 50V for voltages above 100V. Apply voltage until the product is damaged, and the maximum test voltage shall not exceed 1200V.

[0121] (5) Dynamic withstand voltage test: In an environment of 25℃±5℃, a 20KVA transformer is used as the voltage source. The PTC thermistor is connected in series with a fixed resistor with a resistance of 25 ohms (power 50W). The initial voltage is 350V, and each voltage value is applied for 5 seconds. Observe whether there is any flashing phenomenon at the moment of power-on. Then disconnect and observe whether the appearance of the PTC thermistor is damaged after cooling for 10 minutes. Test and record the room temperature resistance value of the PTC thermistor. The voltage increase gradient is 20V each time. The method of each step is the same until a product fails. The dynamic withstand voltage value is the test voltage of the failed product minus 20V.

[0122] Depend on Figure 1 and Figure 2 It can be seen that the main difference between the sintering method of this application and the traditional sintering method lies in the high-temperature sintering stage. In traditional sintering methods, the maximum temperature is a fixed value. As the holding time increases, the sintering kinetic energy continuously decreases, leading to uneven grain growth in different regions. This results in uneven grain size and even abnormal grain growth, ultimately degrading the product's performance. In contrast, the high-temperature sintering stage of this application employs a continuous heating method, continuously enhancing the sintering kinetic energy of the material.

[0123] As shown in Table 1, the PTC chip material for motor starting prepared from the PTC ceramic material obtained by the preparation method of Example 1 of this application has a diameter of 15.6 mm, a thickness of 2.5 mm, a switching temperature of 135 °C, and a resistance of 13.5 Ω. Under the same specifications, the withstand voltage of the PTC chip material of Example 1 is 900VAC~950VAC, while the withstand voltage of the PTC chip material obtained by the conventional sintering method is 700VAC~810VAC.

[0124] The PTC chip materials in Table 1 were subjected to a maximum surge current withstand test. The method was as follows: 10 samples were grouped together, and in a room temperature environment, a series resistor of 25Ω was applied. The initial voltage was 350VAC. After energizing for 5 seconds, the samples were cooled for 10 minutes, and the resistance value was measured and the appearance was observed. Then, the voltage was applied again for cyclic testing, with each voltage increase being 20VAC, until a sample failed. The results were as follows: Using the traditional sintering method, the product began to fail at 390VAC (where VAC is the unit of AC voltage, representing the effective value of AC current, V represents volts (a unit of voltage), and AC specifically refers to alternating current). The product sintered in Example 1 of this application did not fail until 470VAC.

[0125] The PTC chip materials in Table 1 were subjected to aging performance tests. The method was as follows: a switching test was conducted at 350VAC with a maximum current not exceeding 8A. After 1000 hours of testing, the resistance change rate of the product in Example 1 of this application (switching temperature of 135℃) was generally in the range of 0% to 5%.

[0126] While specific embodiments of this application have been described in detail, this should not be construed as limiting the scope of protection of this application. Various modifications and variations that can be made by those skilled in the art without inventive effort within the scope described in the claims still fall within the scope of protection of this application.

Claims

1. A method for producing a PTC ceramic material having a uniform fine crystal structure, characterized by, The method comprises the following steps: The raw materials are weighed according to a preset proportion, mixed uniformly, and dried to obtain a mixture; The mixture is pre-sintered, secondarily ball milled, and dried and granulated to obtain pre-processed raw materials; The pre-processed raw materials are subjected to forming treatment and sintering treatment to obtain the PTC ceramic material; The sintering treatment comprises the following stages: a temperature rising stage, a glass phase melting stage, a highest temperature sintering stage, and a cooling stage; the sintering treatment is carried out in a neutral atmosphere; the highest temperature sintering stage is sintered by continuously increasing the temperature to provide stable kinetic energy for grain growth; The microcrystalline grain size of the PTC ceramic material is 1.8 μm to 2.2 μm.

2. The production method according to claim 1, characterized by, The temperature rising stage comprises the following steps: the temperature is increased to 580 °C to 620 °C at a rate of 290 °C / h to 310 °C / h, and the temperature is maintained for 25 min to 35 min.

3. The preparation method according to claim 1, characterized in that, The glass phase melting stage comprises the following steps: the temperature is increased to 1150 °C to 1300 °C at a rate of 270 °C / h to 290 °C / h to accelerate the melting to form a glass phase.

4. The method of claim 1, wherein, The highest temperature sintering stage comprises the following steps: The temperature is continuously increased to 1300 °C to 1325 °C for 10 min to 30 min to perform first sintering treatment; The temperature is continuously increased to 1325 °C to 1340 °C for 30 min to 90 min to perform second sintering treatment.

5. The preparation method according to claim 1, characterized in that, The cooling stage comprises the following steps: the temperature is decreased to 800 °C at a rate of 100 °C / h to 240 °C / h in a first cooling stage, and the temperature is decreased to room temperature by natural cooling or air cooling in a second cooling stage.

6. The method of claim 1, wherein, The raw materials comprise a ceramic phase material, a semi-conducting agent, a glass phase material, and a manganese nitrate solution, wherein The ceramic phase material is formulated as (Ba 1-x-y-z Sr x Pb y Ca z )TiO3, x is in the range of 0.01-0.045, y is in the range of 0.06-0.10, and z is in the range of 0.12-0.

22. The molar ratio of the semi-conducting agent to titanium dioxide in the ceramic phase material is 0.15% to 0.25%; The addition amount of the glass phase material is 0.8 wt% to 1.3 wt% of the ceramic phase material; The concentration of the manganese nitrate solution is 0.4 mol / L to 0.6 mol / L, and the ratio of the manganese nitrate solution to the ceramic phase material is (0.25 mL to 0.6 mL): 100 g.

7. The preparation method according to claim 1, characterized in that, The pre-sintering treatment comprises the following steps: The temperature is increased to 1100 °C to 1200 °C at a rate of 4 °C / min to 5 °C / min in an air atmosphere, and the temperature is maintained for 120 min to 160 min; The temperature is decreased to 800 °C at a rate of 3 °C / min to 4 °C / min, and the temperature is naturally cooled to room temperature.

8. The method of claim 1, wherein, In the drying and granulating process, the drying temperature is 140 °C to 160 °C, and the drying time is 1.5 h to 2.5 h; The granulating method comprises the following steps: 12 mL to 18 mL of PVA solution with a concentration of 10 wt% to 20 wt% is added to 100 g of dry powder, the mixture is uniformly mixed, sieved, and dried at a temperature of 110 °C to 130 °C for 25 min to 35 min.

9. A PTC ceramic material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of a PTC ceramic material according to claim 9 for the production of an electrode material, characterized in that The method for preparing an electrode material comprises the following steps: A nickel layer is sputtered on the surface of the PTC ceramic material by a magnetron sputtering process to serve as a bottom electrode; Silver paste is printed on the surface of the PTC ceramic material by a printing and sintering process to serve as a surface electrode.

Citation Information

Patent Citations

  • Doped and modified barium strontium calcium titanate heat-release pyroelectric ceramic material and preparation method thereof

    CN102060527A

  • Preparation method of laminated barium titanate PTC (positive temperature coefficient) ceramic

    CN102503408A

  • Barium titanate-based leadless piezoelectric ceramic and preparation method thereof

    CN104016674A

  • Preparation method of substrate-type PTC superfine ceramic for adjusting barium titanate with Y / Mn substance ratio

    CN104725037A

  • Process of forming a ceramic body

    US2696651A