Coil component

By employing a specific ratio of ferrite and glass layers in the common-mode noise filter, the problems of low strength and poor sinterability of the dielectric glass layer are solved, thereby improving the strength and high-frequency characteristics of the preform.

CN121693787APending Publication Date: 2026-03-17MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480053171.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-08-17
Filing Date
2024-06-06
Publication Date
2026-03-17

AI Technical Summary

Technical Problem

The outermost dielectric glass layer of existing common-mode noise filters has low strength and is prone to cracking due to substrate flexural stress. It also has poor sinterability, and the Si content easily corrodes the magnetic body, affecting the sinterability of the blank.

Method used

A structure consisting of a first ferrite layer, a second ferrite layer, a glass layer, a third ferrite layer, and a fourth ferrite layer stacked in sequence is adopted. The ratio of Zn and Ni in the ferrite layers is controlled. By reducing the Zn content in the second and third ferrite layers, the Si content in the glass layer is suppressed, thereby improving sinterability and green body strength.

Benefits of technology

This approach achieves both sinterability maintenance and improved strength of the blank, while also enhancing the high-frequency characteristics of the coil components and preventing the reduction in sinterability caused by the chemical reaction between the glass layer and the ferrite layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121693787A_ABST
    Figure CN121693787A_ABST
Patent Text Reader

Abstract

A coil component (1) is provided with: a green body (10) comprising a laminate in which a first ferrite layer (17a), a second ferrite layer (16a), a glass layer (15), a third ferrite layer (16b), and a fourth ferrite layer (17b) are laminated in this order; a coil (30) provided inside the glass layer (15); and an external electrode (20) provided on the outer surface of the element (10) and electrically connected to the coil (30), the ferrite materials constituting the first ferrite layer (17a), the second ferrite layer (16a), the third ferrite layer (16b), and the fourth ferrite layer (17b) containing X (X > = 0) mol% of Zn and Y (Y > = 0) mol% of Ni in terms of Zn and Ni in terms of ZnO and NiO, respectively, when Fe, Zn, Cu, and Ni are converted into Fe2O3, ZnO, CuO, and NiO, respectively, and the total content of Fe2O3, ZnO, CuO, and NiO is 100 mol%. X + Y > 0, X / (X + Y) of the ferrite material constituting the second ferrite layer (16a) and the third ferrite layer (16b) is 0 to 0.73 inclusive, and X / (X + Y) of the ferrite material constituting the first ferrite layer (17a) and the fourth ferrite layer (17b) is more than 0.73 and 1.0 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to coil components. Background Technology

[0002] Patent Document 1 discloses a common-mode noise filter comprising: a first non-magnetic body portion, a first magnetic body portion formed on the lower surface of the first non-magnetic body portion, a second magnetic body portion formed on the upper surface of the first non-magnetic body portion, a first coil and a second coil embedded in the first non-magnetic body portion and made of Ag, and a second non-magnetic body portion formed on at least one of the lower surface of the first magnetic body portion and the upper surface of the second magnetic body portion and located on the outermost side, wherein the first non-magnetic body portion and the second non-magnetic body portion are made of filler and glass, and the filler content of the second non-magnetic body portion is less than the filler content of the first non-magnetic body portion.

[0003] Patent Document 1: Japanese Patent No. 6569078

[0004] In the common-mode noise filter described in Patent Document 1, the outermost second non-magnetic body is a dielectric glass layer, which has low strength and is prone to cracking in the blank due to substrate flexural stress. In addition, when firing the unfired blank, the Si component contained in the central first non-magnetic body may erode into the first and second magnetic body parts, which may reduce the sinterability of the blank. Summary of the Invention

[0005] The present invention was made to solve the above-mentioned problems, and its purpose is to provide a coil component that maintains both sinterability and high strength of the blank.

[0006] The coil component of the present invention comprises: a blank, including a laminate formed by stacking a first ferrite layer, a second ferrite layer, a glass layer, a third ferrite layer, and a fourth ferrite layer in the order of the first ferrite layer, the second ferrite layer, the glass layer, the third ferrite layer, and the fourth ferrite layer; a coil disposed inside the glass layer; and an external electrode disposed on the outer surface of the blank and electrically connected to the coil, wherein Fe, Zn, Cu, and Ni are respectively converted to Fe2O3, ZnO, CuO, and NiO, and the total content of Fe2O3, ZnO, CuO, and NiO is set to 100%. When the content is mol%, the ferrite materials constituting the first ferrite layer, the second ferrite layer, the third ferrite layer, and the fourth ferrite layer respectively convert Zn and Ni to ZnO and NiO respectively, and contain X (X≥0) mol% Zn and Y (Y≥0) mol% Ni, and X + Y > 0. The X / (X + Y) of the ferrite material constituting the second ferrite layer and the third ferrite layer is 0 or more and 0.73 or less, and the X / (X + Y) of the ferrite material constituting the first ferrite layer and the fourth ferrite layer exceeds 0.73 and is 1.0 or less.

[0007] According to the present invention, it is possible to provide a coil component that maintains both sinterability and high strength of the blank. Attached Figure Description

[0008] Figure 1 This is a perspective view schematically illustrating an example of a coil component of the present invention.

[0009] Figure 2 It is a schematic representation Figure 1 A cross-sectional view of an example of a coil component along line segment A1-A1.

[0010] Figure 3 It means to Figure 1 An exploded perspective view of an example of the disassembled state of the coil component shown (wherein, apart from the external electrodes).

[0011] Figure 4 It is a graph showing the cutoff frequencies of the samples of each embodiment and each comparative example obtained through simulation. Detailed Implementation

[0012] The coil component of the present invention will now be described. Furthermore, the present invention is not limited to the following structure, and appropriate modifications may be made without departing from the spirit of the invention. Additionally, a structure formed by combining multiple preferred structures described below is also part of the present invention.

[0013] The following example, as a coil component of the present invention, shows a common-mode choke coil. The coil component of the present invention can also be applied to coil components other than common-mode choke coils.

[0014] The accompanying drawings are schematic diagrams, and their dimensions, aspect ratios, and scales may sometimes differ from the actual product. In the drawings, identical or equivalent parts use the same reference numerals. Furthermore, in each drawing, the same reference numerals are used for the same elements, and redundant descriptions are omitted.

[0015] In this specification, terms indicating relationships between elements (e.g., "parallel", "orthogonal", etc.) and terms indicating the shape of elements do not necessarily mean a strict form as they are literally, but also imply a range of substantially equivalents, such as a range that includes a difference of about a few percent.

[0016] In the coil component of the present invention, the blank includes a laminate formed by stacking a first ferrite layer, a second ferrite layer, a glass layer, a third ferrite layer and a fourth ferrite layer in the order of the first ferrite layer, the second ferrite layer, the glass layer, the third ferrite layer and the fourth ferrite layer.

[0017] Figure 1 This is a perspective view schematically illustrating an example of a coil component of the present invention. Figure 2 It is a schematic representation Figure 1 A cross-sectional view of an example of a coil component along line segment A1-A1. Figure 3 It means to Figure 1 An exploded perspective view of an example of the disassembled state of the coil component shown (wherein, apart from the external electrodes).

[0018] Figure 1 The coil component 1 shown is a so-called common-mode choke coil, which includes a blank 10 and a coil 30 disposed inside the blank 10 (see reference). Figure 2 as well as Figure 3 ), and an external electrode 20 disposed on the outer surface of the blank 10 and electrically connected to the coil 30.

[0019] In this instruction manual, such as Figure 1 As shown, the length, height, and width directions are defined by L, T, and W, respectively. Here, the length direction L, height direction T, and width direction W are orthogonal to each other.

[0020] The blank 10 is, for example, a cuboid or a substantially cuboid shape, having a first end face 11a and a second end face 11b opposite each other in the length direction L, a first main face 12a and a second main face 12b opposite each other in the height direction T, and a first side face 13a and a second side face 13b opposite each other in the width direction W.

[0021] When the coil component 1 is mounted on the substrate, the first main surface 12a of the blank 10 becomes the mounting surface.

[0022] The blank 10 may also have rounded corners and edges. The corners of the blank 10 are the parts where three faces of the blank 10 intersect. The edges of the blank 10 are the parts where two faces of the blank 10 intersect.

[0023] The blank 10 comprises a laminated body formed by stacking a first ferrite layer 17a, a second ferrite layer 16a, a glass layer 15, a third ferrite layer 16b, and a fourth ferrite layer 17b in the order of the first ferrite layer 17a, the second ferrite layer 16a, the glass layer 15, the third ferrite layer 16b, and the fourth ferrite layer 17b. Figure 1 , Figure 2 as well as Figure 3 In the example shown, the first ferrite layer 17a, the second ferrite layer 16a, the glass layer 15, the third ferrite layer 16b, and the fourth ferrite layer 17b are stacked in the height direction T.

[0024] In other words, the preform 10 includes a glass layer 15, a second ferrite layer 16a and a third ferrite layer 16b sandwiching the glass layer 15 in the stacking direction (here, the height direction T), and a first ferrite layer 17a and a fourth ferrite layer 17b sandwiching the second ferrite layer 16a and the third ferrite layer 16b in the stacking direction (here, the height direction T). Specifically, in the stacking direction (here, the height direction T), the second ferrite layer 16a is disposed on one main surface of the glass layer 15, and the third ferrite layer 16b is disposed on the other main surface of the glass layer 15. Furthermore, in the stacking direction (here, the height direction T), the first ferrite layer 17a is disposed on one main surface of the second ferrite layer 16a (the main surface opposite to the glass layer 15), and the fourth ferrite layer 17b is disposed on the other main surface of the third ferrite layer 16b (the main surface opposite to the glass layer 15).

[0025] Thus, the outermost first ferrite layer 17a and fourth ferrite layer 17b are ferrite layers, not glass layers, so the blank 10 has strong resistance to substrate flexural stress.

[0026] When Fe, Zn, Cu, and Ni are converted to Fe2O3, ZnO, CuO, and NiO respectively, and the total content of Fe2O3, ZnO, CuO, and NiO is set to 100 mol%, the ferrite materials constituting the first ferrite layer 17a, the second ferrite layer 16a, the third ferrite layer 16b, and the fourth ferrite layer 17b each have Zn and Ni converted to ZnO and NiO respectively, and contain X (X≥0, i.e., X is 0). The ferrite material comprising the second ferrite layer 16a and the third ferrite layer 16b contains 0 or more and less than 100 mol% Zn and Y (Y≥0, i.e., Y is a real number greater than or equal to 0 and less than 100) mol% Ni, and X+Y>0, and the X / (X+Y) of the ferrite material comprising the first ferrite layer 17a and the fourth ferrite layer 17b is greater than 0.73 and less than 1.0.

[0027] In the following, when Fe, Zn, Cu, and Ni are converted to Fe2O3, ZnO, CuO, and NiO respectively, and the total content of Fe2O3, ZnO, CuO, and NiO is set to 100 mol%, and the content of Zn and Ni in the ferrite material constituting a certain ferrite layer is set to X mol% and Y mol% respectively when converted to ZnO and NiO (X and Y are real numbers greater than 0 and less than 100), the ratio calculated according to the formula X / (X+Y) will be expressed as Zn / (Zn+Ni) of the ferrite layer (ferrite material).

[0028] When firing the unfired blank 10, there is a risk that the Si component contained in the glass layer 15 may erode into the second ferrite layer 16a and the third ferrite layer 16b. Furthermore, generally speaking, if the proportion of Zn in the ferrite layer increases, the erosion of Si from the glass layer into the ferrite layer becomes more prolonged. This is believed to be because the Si component in the glass layer readily substitutes for the Zn component in the ferrite layer.

[0029] In contrast, in coil component 1, by reducing the ZnO content of the second ferrite layer 16a and the third ferrite layer 16b, specifically by making the Zn / (Zn+Ni) values ​​of the second ferrite layer 16a and the third ferrite layer 16b below 0.73, the erosion of Si from the glass layer 15 into the second ferrite layer 16a and the third ferrite layer 16b can be suppressed. That is, the reduction in sinterability caused by the chemical reaction between the second ferrite layer 16a and the third ferrite layer 16b and the glass layer 15 can be suppressed.

[0030] On the other hand, if the Zn / (Zn+Ni) ratio of the second ferrite layer 16a and the third ferrite layer 16b exceeds 0.73, there is a risk that the compatibility between the second ferrite layer 16a and the third ferrite layer 16b and the glass will deteriorate. As a result, the Si composition in the glass layer 15 is more likely to erode into the second ferrite layer 16a and the third ferrite layer 16b.

[0031] Furthermore, the Zn / (Zn+Ni) ratio of the first ferrite layer 17a and the fourth ferrite layer 17b exceeds 0.73, but the second ferrite layer 16a and the third ferrite layer 16b are sandwiched between the first ferrite layer 17a and the fourth ferrite layer 17b and the glass layer 15, respectively. Therefore, there is no particular problem with the sinterability of the first ferrite layer 17a and the fourth ferrite layer 17b.

[0032] Based on the above, in coil component 1, it is possible to maintain sinterability while improving the strength of the blank 10.

[0033] Furthermore, by providing a first ferrite layer 17a and a fourth ferrite layer 17b in addition to the second ferrite layer 16a and the third ferrite layer 16b, the high-frequency characteristics of the coil component 1 can be improved compared to the case where the first ferrite layer 17a and the fourth ferrite layer 17b are not provided.

[0034] The Zn / (Zn+Ni) ratio of the second ferrite layer 16a and the third ferrite layer 16b is preferably 0.02 or more and 0.73 or less, more preferably 0.36 or more and 0.72 or less.

[0035] The Zn / (Zn+Ni) ratio of the second ferrite layer 16a and the Zn / (Zn+Ni) ratio of the third ferrite layer 16b are preferably the same, but they can also be different from each other.

[0036] The Zn / (Zn+Ni) ratio of the first ferrite layer 17a and the fourth ferrite layer 17b is not particularly limited as long as it exceeds 0.73 and is less than 1.0, but it is preferably more than 0.95 and less than 1.0.

[0037] The Zn / (Zn+Ni) ratio of the first ferrite layer 17a and the Zn / (Zn+Ni) ratio of the fourth ferrite layer 17b are preferably the same, but they can also be different from each other.

[0038] like Figure 2 As shown, the glass layer 15 has, for example, a multilayer structure consisting of multiple insulating layers stacked in the stacking direction (here, the height direction T).

[0039] Here, the glass layer 15 is formed by sequentially stacking insulating layers 15a, 15b, 15c, 15d, and 15e in the stacking direction (here, the height direction T). More specifically, in the glass layer 15, insulating layers 15a, 15b, 15c, 15d, and 15e are sequentially stacked from the first main surface 12a side of the blank 10 toward the second main surface 12b side.

[0040] The insulating layers 15a, 15b, 15c, 15d, and 15e are preferably made of the same material as each other, but they may also be different from each other or partially different.

[0041] In addition, Figure 2 For ease of explanation, the boundaries between the insulating layers constituting the glass layer 15 are shown, but in reality these boundaries are not clearly visible.

[0042] Preferably, the glass layer 15 is composed of a glass-ceramic material comprising glass material and filler. In this case, the glass material comprising the glass layer 15 preferably contains at least an alkali metal (preferably K), B, and Si. Furthermore, the filler comprising the glass layer 15 preferably contains at least one selected from the group consisting of quartz (SiO2), alumina (Al2O3), and forsterite (2MgO·SiO2). In particular, the filler comprising the glass layer 15 preferably contains quartz, alumina, and forsterite.

[0043] When the glass-ceramic material comprises glass material and quartz, alumina and forsterite as fillers, the glass-ceramic material preferably comprises 70% to 80% by weight of glass material containing at least alkali metal (preferably K), B and Si, 2% to 4% by weight of alumina, 12% to 14% by weight of quartz and 5% to 15% by weight of forsterite.

[0044] The preferred glass-ceramic material, when the total weight is set to 100 wt%, contains 9 wt% to 13 wt% B when B is converted to B2O3, 2 wt% to 4 wt% Al when Al is converted to Al2O3, 75 wt% to 85 wt% Si when SiO2 is converted to SiO2, 0.5 wt% to 2 wt% K when K2O is converted to K, and 3 wt% to 10 wt% Mg when MgO is converted to MgO.

[0045] The thickness (dimension T in the height direction) of the glass layer 15 is, for example, 20 μm or more and 300 μm or less, preferably 30 μm or more and 200 μm or less. Furthermore, in this disclosure, when the thickness of the glass layer 15 is not constant, measurements are taken randomly at 15, and the average value is set as "the thickness of the glass layer 15".

[0046] like Figure 2 As shown, the second ferrite layer 16a and the third ferrite layer 16b each have, for example, a multilayer structure formed by stacking multiple insulating layers in the stacking direction (here, the height direction T), as described later.

[0047] Here, the second ferrite layer 16a is formed by stacking insulating layers 16aa and 16ab in the stacking direction (here, the height direction T). More specifically, in the second ferrite layer 16aa and 16ab are stacked sequentially from the glass layer 15 side.

[0048] In addition, Figure 2 For ease of explanation, the boundaries between the insulating layers constituting the second ferrite layer 16a are shown, but in reality these boundaries are not clearly visible.

[0049] The third ferrite layer 16b is formed by stacking insulating layers 16ba and 16bb in the stacking direction (here, the height direction T). More specifically, in the third ferrite layer 16b, insulating layers 16ba and 16bb are stacked sequentially from the glass layer 15 side.

[0050] In addition, Figure 2 For ease of explanation, the boundaries between the insulating layers constituting the third ferrite layer 16b are shown, but in reality these boundaries are not clearly visible.

[0051] The ferrite materials constituting the second ferrite layer 16a and the third ferrite layer 16b can be the same or different. Preferably, the second ferrite layer 16a and the third ferrite layer 16b are composed of the same ferrite material.

[0052] The ferrite material constituting the second ferrite layer 16a and the third ferrite layer 16b (hereinafter referred to as Zn-free ferrite material) contains, for example, Fe, Zn, Cu, and Ni as main components. In addition to the above-mentioned main components, the Zn-free ferrite material may also contain auxiliary components such as Mn, Co, Sn, Bi, and Si. Furthermore, the Zn-free ferrite material may contain unavoidable impurities.

[0053] The preferred Zn-free ferrite materials are those in which Fe is converted to Fe2O3 and contains 40 mol% to 56 mol% of Fe, Zn is converted to ZnO and contains 1 mol% to 35 mol% of Zn, Cu is converted to CuO and contains 6 mol% to 14 mol% of Cu, and Ni is converted to NiO and contains 8 mol% to 40 mol% of Ni.

[0054] Zn-free ferrite materials can also be magnetic ferrite materials. The permeability of magnetic ferrite materials at 1MHz can also be above 30.

[0055] The thickness (dimension T in the height direction) of the second ferrite layer 16a and the third ferrite layer 16b is preferably 3.3 μm or more, and more preferably 5.0 μm or more. By setting the thickness of the second ferrite layer 16a and the third ferrite layer 16b to 3.3 μm or more, it is possible to suppress the Si component in the glass layer 15 from eroding into the second ferrite layer 16a and the third ferrite layer 16b and reaching the first ferrite layer 17a and the fourth ferrite layer 17b.

[0056] The thickness of the second ferrite layer 16a and the third ferrite layer 16b is preferably 110 μm or less, and more preferably 30 μm or less. By setting the thickness of the second ferrite layer 16a and the third ferrite layer 16b to 110 μm or less, the high-frequency characteristics of the coil component 1 are improved. More specifically, the cutoff frequency (the frequency at which the signal transmission characteristic Sdd21 becomes -3dB) can be 6 GHz or more.

[0057] Furthermore, the thickness of the second ferrite layer 16a can be the same as or different from the thickness of the third ferrite layer 16b. In this disclosure, when the thickness of the second ferrite layer 16a is not constant, measurements are taken randomly at 15 locations, and the average value is defined as the "thickness of the second ferrite layer 16a". Similarly, when the thickness of the third ferrite layer 16b is not constant, measurements are taken randomly at 15 locations, and the average value is defined as the "thickness of the third ferrite layer 16b".

[0058] The first ferrite layer 17a and the fourth ferrite layer 17b each have, for example, a multilayer structure formed by stacking multiple insulating layers in the stacking direction (here, the height direction T), as described later.

[0059] Here, the first ferrite layer 17a is formed by stacking insulating layers 17aa, 17ab, and 17ac in the stacking direction (here, the height direction T). More specifically, in the first ferrite layer 17a, insulating layers 17aa, 17ab, and 17ac are stacked sequentially from the glass layer 15 side.

[0060] In addition, Figure 2 For ease of explanation, the boundaries between the insulating layers constituting the first ferrite layer 17a are shown, but in reality these boundaries are not clearly visible.

[0061] The fourth ferrite layer 17b is formed by stacking insulating layers 17ba, 17bb, and 17bc in the stacking direction (here, the height direction T). More specifically, in the fourth ferrite layer 17b, insulating layers 17ba, 17bb, and 17bc are stacked sequentially from the glass layer 15 side.

[0062] In addition, Figure 2 For ease of explanation, the boundaries between the insulating layers constituting the fourth ferrite layer 17b are shown, but in reality these boundaries are not clearly visible.

[0063] The ferrite materials constituting the first ferrite layer 17a and the fourth ferrite layer 17b can be the same or different. Preferably, the first ferrite layer 17a and the fourth ferrite layer 17b are composed of the same ferrite material.

[0064] The ferrite material constituting the first ferrite layer 17a and the fourth ferrite layer 17b (hereinafter referred to as Zn-rich ferrite material) contains, for example, Fe, Zn, Cu, and Ni as main components. However, it may also not contain Ni. In addition to the aforementioned main components, the Zn-rich ferrite material may also contain auxiliary components such as Mn, Co, Sn, B, and Si. Furthermore, the Zn-rich ferrite material may unavoidably contain impurities.

[0065] The preferred Zn-rich ferrite materials are respectively converted to Fe2O3 containing 40 mol% to 56 mol% of Fe, converted to ZnO containing 36 mol% to 55 mol% of Zn, converted to CuO containing 6 mol% to 14 mol% of Cu, and converted to NiO containing 0 mol% to 8 mol% of Ni.

[0066] Zn-rich ferrite materials can also be non-magnetic ferrite materials. The permeability of non-magnetic ferrite materials at 1 MHz can also be below 3.

[0067] The thickness (dimension T in the height direction) of each of the first ferrite layer 17a and the fourth ferrite layer 17b is, for example, 80 μm or more and 190 μm or less, preferably 160 μm or more and 185 μm or less.

[0068] The thickness of the first ferrite layer 17a can be the same as or different from the thickness of the fourth ferrite layer 17b. Furthermore, in this disclosure, when the thickness of the first ferrite layer 17a is not constant, measurements are randomly taken at 15 locations, and the average value is defined as the "thickness of the first ferrite layer 17a". Similarly, when the thickness of the fourth ferrite layer 17b is not constant, measurements are randomly taken at 15 locations, and the average value is defined as the "thickness of the fourth ferrite layer 17b".

[0069] The glass layer and each ferrite layer are distinguished as follows: First, the coil component is sealed with resin as needed. Then, the coil component is ground in a first direction (e.g., length direction) orthogonal to the stacking direction (e.g., height direction) to expose a cross-section along a second direction (e.g., width direction) orthogonal to both the stacking direction and the first direction, approximately at the center of the first direction. Next, for regions in the exposed cross-section of the blank where different layers can be inferred to exist (e.g., regions where different layers can be inferred to exist based on differences in hue, etc.), the composition (the content ratio of the detected elements) is determined using scanning transmission electron microscopy-energy dispersive X-ray analysis (STEM-EDX). Then, based on the obtained composition, it is determined whether the constituent material of each layer is a glass-ceramic material or a ferrite material, thereby distinguishing the glass layer and the ferrite layer. Furthermore, each ferrite layer is distinguished based on the obtained composition.

[0070] Coil 30 may include, for example, two coils, specifically, a primary coil 30a and a secondary coil 30b. The number of coils 30 is not limited to two; it may be one or more.

[0071] exist Figure 2 In this structure, the primary coil 30a and the secondary coil 30b are disposed inside the glass layer 15. The primary coil 30a and the secondary coil 30b are insulated from each other.

[0072] The primary coil 30a and the secondary coil 30b are arranged sequentially in the stacking direction (here, the height direction T) of the blank 10 to form a common mode choke coil.

[0073] The coil 30, including the primary coil 30a and the secondary coil 30b, is made of a conductive material such as Ag or Cu. The conductive material constituting the coil 30 is preferably Ag. Thus, it is preferable that the coil 30 contains at least Ag.

[0074] like Figure 3 As shown, the primary coil 30a and the secondary coil 30b have a spiral pattern wound in the same direction when viewed from the stacking direction (here, the height direction T). The coil 30, including the primary coil 30a and the secondary coil 30b, is electrically connected to any one of the external electrodes 20.

[0075] Specifically, the primary coil 30a includes: a coil conductor 31 wound in a spiral shape; a lead-out conductor 71a connected to one end of the spiral outer periphery of the coil conductor 31; a through-hole conductor 61 connected to the other end of the center side of the coil conductor 31; and a lead-out conductor 71b connected to the through-hole conductor 61. Furthermore, one end of the spiral outer periphery of the coil conductor 31 is connected to one end of the lead-out conductor 71a, and the other end of the lead-out conductor 71a is led out to the outer surface of the blank 10. The other end of the spiral center side of the coil conductor 31 is connected to one end of the lead-out conductor 71b via the through-hole conductor 61 disposed inside the glass layer 15, and the other end of the lead-out conductor 71b is led out to the outer surface of the blank 10.

[0076] Similarly, the secondary coil 30b includes: a coil conductor 32 wound in a spiral shape, a lead-out conductor 72a connected to one end of the spiral outer periphery of the coil conductor 32, a through-hole conductor 62 connected to the other end of the center side of the coil conductor 32, and a lead-out conductor 72b connected to the through-hole conductor 62. Furthermore, one end of the spiral outer periphery of the coil conductor 32 is connected to one end of the lead-out conductor 72a, and the other end of the lead-out conductor 72a is led out to the outer surface of the blank 10. The other end of the spiral center side of the coil conductor 32 is connected to one end of the lead-out conductor 72b via the through-hole conductor 62 disposed inside the glass layer 15, and the other end of the lead-out conductor 72b is led out to the outer surface of the blank 10.

[0077] The greater the distance from the primary coil 30a to the second ferrite layer 16a, the better the high-frequency characteristics of the coil component 1. Specifically, as... Figure 2 As shown, the distance D1 in the stacking direction (here, the height direction T) between the primary coil 30a (lead conductor 71b) and the second ferrite layer 16a is preferably 5 μm or more, more preferably 10 μm or more. The upper limit of the distance D1 can be appropriately set, but it is preferably 40 μm or less, more preferably 25 μm or less.

[0078] Similarly, the greater the distance from the secondary coil 30b to the third ferrite layer 16b, the better the high-frequency characteristics of the coil component 1. Specifically, as... Figure 2 As shown, the distance D2 in the stacking direction (here, the height direction T) between the secondary coil 30b (lead conductor 72b) and the third ferrite layer 16b is preferably 5 μm or more, more preferably 10 μm or more. The upper limit of the distance D2 can be appropriately set, but it is preferably 40 μm or less, more preferably 25 μm or less.

[0079] The external electrodes 20 include, for example, a first external electrode 21, a second external electrode 22, a third external electrode 23, and a fourth external electrode 24. The number of the external electrodes 20 is not limited to four (i.e., two pairs), and varies according to the number of the coils 30. Therefore, the number of the external electrodes 20 can be two (i.e., one pair), or three or more, for example, six (i.e., three pairs) or more.

[0080] The external electrodes 20 are electrically connected to the coils 30. In Figure 2 and Figure 3 the primary coil 30a is led out to the outer surface of the green body 10 at one end and connected to the first external electrode 21, and is led out to the outer surface of the green body 10 at the other end and connected to the second external electrode 22. Similarly, the secondary coil 30b is led out to the outer surface of the green body 10 at one end and connected to the third external electrode 23, and is led out to the outer surface of the green body 10 at the other end and connected to the fourth external electrode 24.

[0081] The external electrodes 20 exist on the outer surface of the green body 10 over the first ferrite layer 17a, the second ferrite layer 16a, the glass layer 15, the third ferrite layer 16b, and the fourth ferrite layer 17b, respectively. In Figure 1 the first external electrode 21 and the third external electrode 23 are provided on the first side surface 13a of the green body 10, and the second external electrode 22 and the fourth external electrode 24 are provided on the second side surface 13b of the green body 10. The first external electrode 21, the second external electrode 22, the third external electrode 23, and the fourth external electrode 24 may also extend in a U-shape (C-shape) to the first main surface 12a and the second main surface 12b of the green body 10 as shown in Figure 1 .

[0082] As shown in Figure 1 , a plurality of external electrodes 20 may exist adjacent to each other on one outer surface of the green body 10. In the example shown in Figure 1 , the first external electrode 21 and the third external electrode 23 exist adjacent to each other on the first side surface 13a of the green body 10, and the second external electrode 2, and the fourth external electrode 24 exist adjacent to each other on the second side surface 13b of the green body 10.

[0083] The external electrodes 20 include, for example, a base electrode and a plating electrode provided on the base electrode. The plating electrode may be one layer or two or more layers. Preferably, the external electrodes 20 contain at least Ag.

[0084] When the external electrode 20 includes a base electrode and a plating electrode, the base electrode is preferably a base electrode containing Ag or Cu, more preferably a base electrode containing Ag. The plating electrode is preferably either or both of a Ni-plated electrode and a Sn-plated electrode, more preferably both. In particular, the external electrode 20 preferably includes an Ag-containing base electrode, a Ni-plated electrode disposed on the base electrode, and a Sn-plated electrode further disposed on the Ni-plated electrode.

[0085] For example, coil component 1 can be manufactured using the following method.

[0086] <Processes for manufacturing glass-ceramic materials>

[0087] For example, K2O, B2O3, SiO2, and Al2O3 are weighed to achieve a specified ratio and mixed in a platinum crucible.

[0088] Next, the resulting mixture is melted by heat treatment. The heat treatment temperature is, for example, set to above 1500°C and below 1600°C.

[0089] Then, the resulting melt is rapidly cooled to produce glass material.

[0090] The glass material preferably contains at least K, B and Si, more preferably K is converted to K2O and contains 0.5% to 5% K, B is converted to B2O3 and contains 10% to 25% B, Si is converted to SiO2 and contains 70% to 85% Si, and Al is converted to Al2O3 and contains 0% to 5% Al.

[0091] Next, glass powder is prepared by crushing the glass material. Regarding the median particle size D of the glass powder... 50 For example, the particle size is set to be 1 μm or larger and 3 μm or smaller. Additionally, quartz powder, alumina powder, and forsterite powder are prepared as fillers, for example. Regarding the median particle size D of the quartz powder, alumina powder, and forsterite powder... 50 For example, it can be set to be 0.5 μm or larger and 2.0 μm or smaller. Here, the median particle size D of glass powder, quartz powder, alumina powder, and forsterite powder is... 50 It is the particle size when the cumulative probability of the volume reference becomes 50%.

[0092] Then, glass-ceramic materials (non-magnetic materials) are made by adding quartz powder, alumina powder, and forsterite powder as fillers to glass powder.

[0093] The preferred glass-ceramic material contains 70% to 80% glass powder, 2% to 4% alumina powder, 12% to 14% quartz powder, and 5% to 15% forsterite powder.

[0094] In addition, the preferred glass-ceramic material, when the total weight is set to 100 wt%, contains 9 wt% to 13 wt% B when B is converted to B2O3, 2 wt% to 4 wt% Al when Al is converted to Al2O3, 75 wt% to 85 wt% Si when SiO2 is converted to SiO2, 0.5 wt% to 2 wt% K when K2O is converted to K, and 3 wt% to 10 wt% Mg when MgO is converted to MgO.

[0095] <Processes for making glass-ceramic sheets>

[0096] Glass-ceramic slurry is prepared by mixing the obtained glass-ceramic material, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol or toluene, and plasticizers with PSZ media in a ball mill.

[0097] Next, after forming the glass-ceramic slurry into a sheet of a specified thickness using methods such as a scraper, it is punched into a specified shape to produce a glass-ceramic sheet. The thickness of the glass-ceramic sheet is, for example, set to be 20 μm or more and 30 μm or less. The shape of the glass-ceramic sheet is, for example, set to a rectangular shape.

[0098] <Process for producing Zn-free ferrite materials>

[0099] For example, Fe2O3, ZnO, CuO, and NiO are weighed to achieve a specified ratio. At this time, additives (auxiliary components) such as Mn3O4, Co3O4, SnO2, Bi2O3, and SiO2 may also be added. Additionally, unavoidable impurities may be present.

[0100] Next, after mixing these weighed materials, pure water, dispersant, etc., with the PSZ media in a ball mill, they are pulverized.

[0101] Then, after drying the resulting pulverized material, it is calcined. The calcination temperature is set, for example, above 700°C and below 800°C. The calcination time is set, for example, above 2 hours and below 3 hours.

[0102] In this way, powdered Zn-free ferrite materials can be produced.

[0103] The Zn / (Zn+Ni) ratio of the Zn-free ferrite material is 0 or higher and 0.73 or lower. Preferably, the Zn-free ferrite material contains 40 mol% to 56 mol% Fe when converted to Fe₂O₃, 1 mol% to 35 mol% Zn when converted to ZnO, 6 mol% to 14 mol% Cu when converted to CuO, and 8 mol% to 40 mol% Ni when converted to NiO.

[0104] <Process for manufacturing Zn-free ferrite sheets>

[0105] A Zn-free ferrite slurry is prepared by mixing the obtained powdered Zn-free ferrite material, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol or toluene, and PSZ media together in a ball mill and then pulverizing the mixture.

[0106] Next, after forming the Zn-free ferrite slurry into sheets of a specified thickness using methods such as the scraper method, it is punched into a specified shape to produce Zn-free ferrite sheets. For example, the shape of the Zn-free ferrite sheets can be rectangular.

[0107] <Process for producing Zn-rich ferrite materials>

[0108] For example, Fe2O3, ZnO, CuO, and NiO are weighed to achieve a specified ratio. At this time, additives (auxiliary components) such as Mn3O4, Co3O4, SnO2, Bi2O3, and SiO2 may also be added. Additionally, unavoidable impurities may be present.

[0109] Next, after mixing these weighed materials, pure water, dispersant, etc., with the PSZ media in a ball mill, they are pulverized.

[0110] Then, after drying the resulting pulverized material, it is calcined. The calcination temperature is set, for example, above 700°C and below 800°C. The calcination time is set, for example, above 2 hours and below 3 hours.

[0111] In this way, powdered Zn-rich ferrite materials can be produced.

[0112] The Zn / (Zn+Ni) ratio of the Zn-rich ferrite material is greater than 0.73 and less than 1.0. Preferably, the Zn-rich ferrite material contains 40 mol% to 56 mol% Fe when converted to Fe₂O₃, 36 mol% to 55 mol% Zn when converted to ZnO, 6 mol% to 14 mol% Cu when converted to CuO, and 0 mol% to 8 mol% Ni when converted to NiO.

[0113] <Process for producing Zn-rich ferrite sheets>

[0114] Zn-rich ferrite slurry is prepared by mixing the obtained powdered Zn-rich ferrite material, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol or toluene, and PSZ media together in a ball mill and then pulverizing them.

[0115] Next, after forming the Zn-rich ferrite slurry into sheets of a specified thickness using methods such as the scraper method, it is punched into a specified shape to produce Zn-rich ferrite sheets. For example, the shape of the Zn-rich ferrite sheets can be rectangular.

[0116] <Process for forming conductor patterns>

[0117] By using methods such as screen printing to coat conductive pastes such as Ag paste onto specified glass-ceramic sheets, a structure equivalent to... Figure 3 The coil conductors of the coil conductors 31 and 32 shown are represented by conductor patterns equivalent to... Figure 3 The conductor patterns of the via conductors 61 and 62 shown are equivalent to... Figure 3 The conductor patterns for lead-out conductors 71a, 71b, 72a, and 72b are shown. When forming the conductor patterns for through-hole conductors, through-holes are pre-formed by laser irradiation at designated locations on a glass-ceramic sheet, and then filled with conductive paste.

[0118] <Process of making layered blocks>

[0119] For example, individual glass-ceramic sheets with conductor patterns are arranged according to... Figure 3 The order shown is... Figure 3 The insulating layers 15a, 15b, 15c, and 15d shown are stacked in sequence along the stacking direction (here, the height direction T). Then, as... Figure 3 As shown, on a principal plane along the stacking direction (here, the height direction) of the obtained laminate, i.e. Figure 3 The insulating layer 15e shown is a glass-ceramic sheet without a conductor pattern, which is stacked at that location. Furthermore, although in Figure 3 Not shown, but glass-ceramic sheets without conductor patterns can also be stacked on another main surface in the stacking direction (here, the height direction T) of the resulting laminate. There is no particular limitation on the number of glass-ceramic sheets without conductor patterns.

[0120] Next, a predetermined number of Zn-free ferrite sheets without conductive patterns are stacked on the principal surfaces of both sides of the obtained glass-ceramic sheet laminate in the lamination direction (here, the height direction T). More specifically, in Figure 3 The insulating layers 16aa and 16ab shown are stacked with Zn-free ferrite sheets, and... Figure 3 The positions of insulating layers 16ba and 16bb shown are stacked with Zn-free ferrite sheets.

[0121] Next, relative to the two stacked portions of the resulting Zn-free ferrite sheet, a predetermined number of Zn-rich ferrite sheets without conductor patterns are stacked in the stacking direction (here, the height direction). More specifically, in Figure 3 The positions of insulating layers 17aa, 17ab, and 17ac shown are stacked with Zn-rich ferrite sheets, and... Figure 3 The positions of insulating layers 17ba, 17bb, and 17bc shown are stacked with Zn-rich ferrite sheets.

[0122] Then, for example, the laminates of glass-ceramic sheets, Zn-free ferrite sheets, and Zn-rich ferrite sheets are pressed together by hot isostatic pressing (WIP) or similar processes at a temperature of 80°C and a pressure of 100 MPa or higher and 160 MPa or lower to produce a laminated block.

[0123] <Processes for making the blank and coil>

[0124] First, the stacked blocks are cut into specified sizes using a cutting machine or similar equipment, thereby creating individual chips.

[0125] Next, individual chips are fired. The firing temperature is set, for example, above 860°C and below 920°C. The firing time is set, for example, above 1 hour and below 2 hours.

[0126] By firing individualized chips, glass-ceramic sheets, Zn-free ferrite sheets, and Zn-rich ferrite sheets become insulating layers, respectively. As a result, the stacked portion of the glass-ceramic sheets becomes a glass layer. Furthermore, the two stacked portions of the Zn-free ferrite sheets become a second ferrite layer and a third ferrite layer, respectively. Additionally, the two stacked portions of the Zn-rich ferrite sheets become a first ferrite layer and a fourth ferrite layer, respectively. Moreover, the conductor patterns for the coil conductor, the lead conductor, and the via conductor become the coil conductor, the lead conductor, and the via conductor, respectively, and a coil is formed by electrically connecting them. Furthermore, in this disclosure, the coil conductor, the lead conductor, and the via conductor are all included within the coil.

[0127] Thus, for example, a blank 10 is made comprising a laminate consisting of a first ferrite layer 17a, a second ferrite layer 16a, a glass layer 15, a third ferrite layer 16b, and a fourth ferrite layer 17b stacked in the order of the first ferrite layer 17a, the second ferrite layer 16a, the glass layer 15, the third ferrite layer 16b, and the fourth ferrite layer 17b, and a coil 30 comprising a primary coil 30a and a secondary coil 30b disposed inside the glass layer 15.

[0128] For example, the blank 10 can be rolled by placing the blank 10 together with the medium into a rotary tumbling mill, thereby rounding the corners and edges.

[0129] <Process for forming external electrodes>

[0130] For example, at least four locations, including two on the first side 13a of the blank body 10 and two on the second side 13b of the blank body 10, are coated with a conductive paste containing Ag and glass frit.

[0131] Next, the resulting coatings are baked at approximately 800°C to form a base electrode on the outer surface of the preform 10.

[0132] Then, by means of electroplating, plating electrodes, such as Ni-plated electrodes and Sn-plated electrodes, are sequentially formed on the surface of each base electrode.

[0133] Thus, an external electrode 20, including a base electrode and a plated electrode, is formed on the outer surface of the blank 10.

[0134] Based on the above, manufacture coil component 1.

[0135] The following information is disclosed in this specification.

[0136] <1> A coil component, comprising:

[0137] The blank includes a laminate formed by stacking a first ferrite layer, a second ferrite layer, a glass layer, a third ferrite layer and a fourth ferrite layer in the order of the first ferrite layer, the second ferrite layer, the glass layer, the third ferrite layer and the fourth ferrite layer.

[0138] A coil is disposed inside the aforementioned glass layer; and

[0139] External electrodes are disposed on the outer surface of the blank and electrically connected to the coil.

[0140] When Fe, Zn, Cu, and Ni are converted to Fe₂O₃, ZnO, CuO, and NiO respectively, and the total content of Fe₂O₃, ZnO, CuO, and NiO is set to 100 mol%, the ferrite materials constituting the first ferrite layer, the second ferrite layer, the third ferrite layer, and the fourth ferrite layer each have Zn and Ni converted to ZnO and NiO respectively, containing X mol% Zn and Y mol% Ni, where X ≥ 0, Y ≥ 0, and X + Y > 0.

[0141] The X / (X+Y) ratio of the ferrite material constituting the second and third ferrite layers is 0 or more and 0.73 or less.

[0142] The X / (X+Y) ratio of the ferrite material constituting the first ferrite layer and the fourth ferrite layer exceeds 0.73 and is less than 1.0.

[0143] <2> According to the coil component described in <1>, wherein,

[0144] The thickness of the second ferrite layer and the third ferrite layer is 3.3 μm or more.

[0145] <3> According to the coil components described in <1> or <2>, wherein,

[0146] The thickness of the second ferrite layer and the third ferrite layer is 110 μm or less.

[0147] <4> The coil component described in any one of <1> to <3>, wherein,

[0148] The glass layer described above contains at least one filler selected from the group consisting of quartz, alumina and forsterite.

[0149] <5> The coil component described in any one of <1> to <4>, wherein,

[0150] The aforementioned coil components are a common-mode choke coil consisting of a first coil and a second coil disposed inside the aforementioned glass layer.

[0151] <6> The coil component described in any one of <1> to <5>, wherein,

[0152] The first ferrite layer and the fourth ferrite layer respectively convert Fe to Fe2O3 and contain 40 mol% to 56 mol% Fe, convert Zn to ZnO and contain 36 mol% to 55 mol% Zn, convert Cu to CuO and contain 6 mol% to 14 mol% Cu, and convert Ni to NiO and contain 0 mol% to 8 mol% Ni.

[0153] <7> The coil component described in any one of <1> to <6>, wherein,

[0154] The second ferrite layer and the third ferrite layer respectively convert Fe to Fe2O3 and contain 40 mol% to 56 mol% Fe, convert Zn to ZnO and contain 1 mol% to 35 mol% Zn, convert Cu to CuO and contain 6 mol% to 14 mol% Cu, and convert Ni to NiO and contain 8 mol% to 40 mol% Ni.

[0155] <8> The coil component described in any one of <1> to <7>, wherein,

[0156] The permeability of the first ferrite layer and the fourth ferrite layer at 1MHz is 3 or less.

[0157] <9> The coil component described in any one of <1> to <8>, wherein,

[0158] The permeability of the second ferrite layer and the third ferrite layer at 1 MHz is 30 or higher.

[0159] Example

[0160] The following describes embodiments of the coil component of the present invention in more detail. However, the present invention is not limited to these embodiments.

[0161] [Example 1]

[0162] Glass powder, alumina powder, quartz powder, and forsterite powder are weighed in a specified ratio, and glass ceramic sheets are produced by the methods described in the above-mentioned "Process for Making Glass-Ceramic Materials" and "Process for Making Glass-Ceramic Sheets".

[0163] Fe₂O₃ powder, NiO powder, ZnO powder, and CuO powder are weighed in a specified ratio, and Zn-free ferrite sheets are produced using the methods described in the above-mentioned "Process for Producing Zn-Free Ferrite Material" and "Process for Producing Zn-Free Ferrite Sheets". The Zn / (Zn+Ni) ratio of the produced Zn-free ferrite material is 0 or more and 0.73 or less.

[0164] Fe₂O₃ powder, NiO powder, ZnO powder, and CuO powder are weighed in a specified ratio, and Zn-rich ferrite sheets are prepared using the methods described in the above-mentioned "Process for Preparing Zn-Rich Ferrite Material" and "Process for Preparing Zn-Rich Ferrite Sheets". The Zn / (Zn+Ni) ratio of the prepared Zn-rich ferrite material is greater than 0.73 and less than 1.0.

[0165] After printing the conductor pattern on the specified glass-ceramic sheet using the method described in the above-mentioned "Process for Forming Conductor Patterns", ... Figure 3 The sequence shown involves stacking glass-ceramic sheets, with Zn-free ferrite sheets stacked above and below, and Zn-rich ferrite sheets stacked above and below. A blank (chip) comprising the fired stack is produced according to the steps described in the <Process for Manufacturing a Stacked Block> and <Process for Manufacturing a Blank and Coil>. Specifically, a blank is produced comprising a stack of a first ferrite layer, a second ferrite layer, a glass layer, a third ferrite layer, and a fourth ferrite layer stacked in the order of the first ferrite layer, the second ferrite layer, the glass layer, the third ferrite layer, and the fourth ferrite layer.

[0166] In this embodiment, the thickness of the glass layer is set to 100 μm, the thickness of the second ferrite layer and the third ferrite layer is set to 5 μm, and the thickness of the first ferrite layer and the fourth ferrite layer is set to 185 μm.

[0167] In addition, the fired blank is placed in a rotary tumbling mill along with the medium to tumble the blank, thereby rounding the corners and edges.

[0168] The external electrode is formed relative to the fired blank according to the steps described in the <Forming External Electrode Process> above.

[0169] Based on the above, a coil component was fabricated as a sample for Example 1.

[0170] [Example 2]

[0171] Except that the thickness of the second and third ferrite layers was set to 10 μm and the thickness of the first and fourth ferrite layers was set to 180 μm, the coil component of the sample used in Example 2 was fabricated using the same method as in Example 1.

[0172] [Example 3]

[0173] Except that the thickness of the second and third ferrite layers was set to 20 μm and the thickness of the first and fourth ferrite layers was set to 170 μm, the coil component of the sample used in Example 3 was fabricated using the same method as in Example 1.

[0174] [Example 4]

[0175] Except that the thickness of the second and third ferrite layers was set to 30 μm and the thickness of the first and fourth ferrite layers was set to 160 μm, the coil component of the sample used in Example 4 was fabricated using the same method as in Example 1.

[0176] [Example 5]

[0177] Except that the thickness of the second and third ferrite layers was set to 50 μm and the thickness of the first and fourth ferrite layers was set to 140 μm, the coil component of the sample used in Example 5 was fabricated using the same method as in Example 1.

[0178] [Example 6]

[0179] Except that the thickness of the second and third ferrite layers was set to 70 μm and the thickness of the first and fourth ferrite layers was set to 120 μm, the coil component of the sample used in Example 6 was fabricated using the same method as in Example 1.

[0180] [Example 7]

[0181] Except that the thickness of the second and third ferrite layers was set to 90 μm and the thickness of the first and fourth ferrite layers was set to 100 μm, the coil component of the sample used in Example 7 was fabricated using the same method as in Example 1.

[0182] [Example 8]

[0183] Except that the thickness of the second and third ferrite layers was set to 110 μm and the thickness of the first and fourth ferrite layers was set to 80 μm, the coil component of the sample used in Example 8 was fabricated using the same method as in Example 1.

[0184] [Comparative Example 1]

[0185] Except for omitting the second and third ferrite layers, and stacking a first ferrite layer and a fourth ferrite layer with a thickness of 190 μm on the top and bottom of the glass layer, the coil component of the sample used as Comparative Example 1 was fabricated using the same method as in Example 1.

[0186] [Comparative Example 2]

[0187] Except for omitting the first and fourth ferrite layers, and stacking a second and third ferrite layer with a thickness of 190 μm on top and bottom of the glass layer, the coil component of the sample used as Comparative Example 2 was fabricated using the same method as in Example 1.

[0188] [Reference Example]

[0189] Except for the ferrite layers made of ferrite materials with different Zn / (Zn+Ni) values ​​due to varying ratios of Fe2O3, ZnO, CuO and NiO, which are respectively stacked on top and below the glass layer, coil components of samples serving as multiple reference examples were fabricated using the same method as in Example 1.

[0190] In the samples of each embodiment, comparative example, and reference example, the dimensions of the coil component were: length direction L = 1.25 mm, width direction W = 1.0 mm, and height direction T = 0.50 mm.

[0191] [Evaluation 1]

[0192] For each reference example specimen, the specimen was placed vertically so that its length direction L was perpendicular, and the circumference of the specimen was fixed with resin. Then, a grinder was used to grind the specimen along its length direction L until the depth of approximately the center of the length direction L was exposed.

[0193] In the cross-section obtained by grinding (WT cross-section), Si mapping was performed near the interface between the glass layer and the ferrite layer using electric field emission wavelength dispersive X-ray diffraction (FE-WDX). FE-WDX was performed using a JXA-8530F X-ray diffraction instrument manufactured by JEOL Ltd. The analytical conditions are shown below.

[0194] Accelerating voltage: 15.0kV

[0195] Irradiation current: 5×10 -8 A

[0196] Number of Pixels: 256×256

[0197] Pixel size: 0.4 (1000x)

[0198] Dwell Time (time to acquire a pixel): 40ms

[0199] Analysis depth: 1μm~2μm

[0200] As a result, in the reference example sample with Zn / (Zn+Ni) = 1.0, i.e., in the sample where the ferrite layer does not contain Ni and the Zn content is relatively high, the Si component in the glass layer erodes into the ferrite layer, and the erosion length is 4 μm.

[0201] Furthermore, for the reference example sample with Zn / (Zn+Ni) = 0.73, i.e., the sample containing Ni in the ferrite layer and with a relatively low Zn content, the Si component in the glass layer also erodes into the ferrite layer, but the erosion length becomes shorter to 3.3 μm. That is, if Zn / (Zn+Ni) is below 0.73, the erosion of the Si component in the glass layer into the ferrite layer can be suppressed compared to the case where Zn / (Zn+Ni) = 1.0.

[0202] Furthermore, in the reference example where Zn / (Zn+Ni) = 0.73, the ferrite material used converts Fe to Fe2O3 and contains 48.5 mol% Fe, converts Zn to ZnO and contains 31.75 mol% Zn, converts Cu to CuO and contains 8.0 mol% Cu, and converts Ni to NiO and contains 11.8 mol% Ni.

[0203] [Evaluation 2]

[0204] For the specimens of each embodiment and each comparative example, they were placed vertically so that the length direction L of the specimen was perpendicular, and the circumference of the specimen was fixed with resin. Then, a grinding machine was used to grind the specimen along the length direction L until the depth of the approximately central part of the length direction L was exposed.

[0205] In the cross-section obtained by grinding (WT cross-section), the area near the interface between the glass layer and the ferrite layer was processed by focused ion beam (FIB) and observed by scanning ion microscopy (SIM) at 20kx magnification, and SIM images were captured. The obtained images were observed to confirm whether there was erosion at the interface between the glass layer and the ferrite layer; specifically, to confirm whether the Si component in the glass layer was eroding into the ferrite layer. The results are shown in Table 1 below.

[0206] [Evaluation 3]

[0207] For the samples of each embodiment and each comparative example, S-parameter simulations were performed to calculate the cutoff frequency (the frequency at which the signal transmission characteristic Sdd21 becomes -3dB). Table 1 below and... Figure 4 The results are shown.

[0208] Figure 4 It is a graph showing the cutoff frequencies of the samples of each embodiment and each comparative example obtained through simulation.

[0209] In addition, Figure 4The cutoff frequencies obtained according to the following models are also shown: The model is the same as in Example 1, except that the thicknesses of the second and third ferrite layers are each set to 25 μm, and the thicknesses of the first and fourth ferrite layers are each set to 165 μm; the model is the same as in Example 1, except that the thicknesses of the second and third ferrite layers are each set to 40 μm, and the thicknesses of the first and fourth ferrite layers are each set to 150 μm; the model is the same as in Example 1, except that the thicknesses of the second and third ferrite layers are each set to 60 μm, and the thicknesses of the first and fourth ferrite layers are each set to 130 μm; the model is the same as in Example 1, except that the thicknesses of the second and third ferrite layers are each set to 80 μm, and the thicknesses of the first and fourth ferrite layers are each set to 110 μm. The same model as Example 1; except that the thickness of the second and third ferrite layers is set to 100 μm and the thickness of the first and fourth ferrite layers is set to 90 μm; the same model as Example 1 except that the thickness of the second and third ferrite layers is set to 120 μm and the thickness of the first and fourth ferrite layers is set to 70 μm; the same model as Example 1 except that the thickness of the second and third ferrite layers is set to 150 μm and the thickness of the first and fourth ferrite layers is set to 40 μm; and the same model as Example 1 except that the thickness of the second and third ferrite layers is set to 170 μm and the thickness of the first and fourth ferrite layers is set to 20 μm.

[0210] Furthermore, the calculated cutoff frequency was evaluated using the following criteria. The results are shown in Table 1 below.

[0211] ○ (Good): Cutoff frequency above 6GHz

[0212] × (Poor): Cutoff frequency less than 6GHz

[0213] [Table 1]

[0214]

[0215] As shown in Table 1 above, in the samples of each embodiment and Comparative Example 2 in which the glass layer is sandwiched by a second ferrite layer and a third ferrite layer made of Zn-free ferrite material, no erosion of the Si component in the glass layer into the second ferrite layer and the third ferrite layer was confirmed.

[0216] Additionally, as shown in Table 1 above and Figure 4As shown, if the thickness of the second ferrite layer and the third ferrite layer is less than 110 μm, the cutoff frequency becomes above 6 GHz, resulting in good high-frequency characteristics (the higher the Sdd21, the better).

[0217] Furthermore, in the sample of Comparative Example 1, the cutoff frequency was 10.0 GHz. This is because the upper limit of the cutoff frequency in the simulation is 10.0 GHz, and it is assumed that the actual cutoff frequency of the sample of Comparative Example 1 exceeds 10.0 GHz.

[0218] Explanation of reference numerals in the attached drawings: 1…coil component; 10…blank; 11a…first end face of the blank; 11b…second end face of the blank; 12a…first main face of the blank; 12b…second main face of the blank; 13a…first side face of the blank; 13b…second side face of the blank; 15…glass layer; 15a, 15b, 15c, 15d, 15e, 16aa, 16ab, 16ba, 16bb, 17aa, 17ab, 17ac, 17ba, 17bb, 17bc…insulating layer; 16a… Second ferrite layer; 16b…Third ferrite layer; 17a…First ferrite layer; 17b…Fourth ferrite layer; 20…External electrode; 21…First external electrode; 22…Second external electrode; 23…Third external electrode; 24…Fourth external electrode; 30…Coil; 30a…Primary coil; 30b…Secondary coil; 31, 32…Coil conductors; 61, 62…Through hole conductors; 71a, 71b, 72a, 72b…Lead conductors; L…Length direction; T…Height direction; W…Width direction.

Claims

1. A coil component, wherein, Possessing: a green body including a laminate of a first ferrite layer, a second ferrite layer, a glass layer, a third ferrite layer, and a fourth ferrite layer, which are stacked in the order of the first ferrite layer, the second ferrite layer, the glass layer, the third ferrite layer, and the fourth ferrite layer; a coil provided inside the glass layer; and an external electrode provided on an outer surface of the green body and electrically connected to the coil, when Fe, Zn, Cu, and Ni are converted into Fe2O3, ZnO, CuO, and NiO, respectively, and the total content of Fe2O3, ZnO, CuO, and NiO is set to 100 mol%, the ferrite material constituting the first ferrite layer, the second ferrite layer, the third ferrite layer, and the fourth ferrite layer each contains X mol% of Zn and Y mol% of Ni, with Zn and Ni being converted into ZnO and NiO, respectively, and X ≥ 0, Y ≥ 0, and X + Y > 0, X / (X + Y) of the ferrite material constituting the second ferrite layer and the third ferrite layer is 0 or more and 0.73 or less, X / (X + Y) of the ferrite material constituting the first ferrite layer and the fourth ferrite layer exceeds 0.73 and is 1.0 or less.

2. The coil component according to claim 1, wherein the thickness of each of the second ferrite layer and the third ferrite layer is 3.3 μm or more.

3. The coil component according to claim 1 or 2, wherein the thickness of each of the second ferrite layer and the third ferrite layer is 110 μm or less.

4. The coil component according to any one of claims 1 to 3, wherein the glass layer contains at least one filler selected from the group consisting of quartz, alumina, and forsterite.

5. The coil component according to any one of claims 1 to 4, wherein the coil component is a common mode choke coil in which a first coil and a second coil are provided inside the glass layer as the coil.

6. The coil component according to any one of claims 1 to 5, wherein each of the first ferrite layer and the fourth ferrite layer contains 40 mol% or more and 56 mol% or less of Fe, 36 mol% or more and 55 mol% or less of Zn, 6 mol% or more and 14 mol% or less of Cu, and 0 mol% or more and 8 mol% or less of Ni, with Fe, Zn, Cu, and Ni being converted into Fe2O3, ZnO, CuO, and NiO, respectively.

7. The coil component according to any one of claims 1 to 6, wherein each of the second ferrite layer and the third ferrite layer contains 40 mol% or more and 56 mol% or less of Fe, 1 mol% or more and 35 mol% or less of Zn, 6 mol% or more and 14 mol% or less of Cu, and 8 mol% or more and 40 mol% or less of Ni, with Fe, Zn, Cu, and Ni being converted into Fe2O3, ZnO, CuO, and NiO, respectively.

8. The coil member according to any one of claims 1 to 7, wherein the permeability at 1 MHz of the first ferrite layer and the fourth ferrite layer is 3 or less.

9. The coil member according to any one of claims 1 to 8, wherein the permeability at 1 MHz of the second ferrite layer and the third ferrite layer is 30 or more.