Carbon nanotube-based wind-resistant and ice-resistant overhead high-voltage cable and preparation method thereof
By introducing a conductive and mechanically reinforcing network of carbon nanotubes into overhead high-voltage cables, combined with a high-performance insulation layer and core structure, the problem of cable damage under icing and strong winds has been solved, improving the structural stability and service life of the cables.
Patent Information
- Application Number
- CN202610501354.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-16
- Publication Date
- 2026-07-07
AI Technical Summary
Existing overhead high-voltage cables are unable to withstand both icing and strong wind damage simultaneously, resulting in poor structural stability and short service life.
The anti-icing and wind-resistant outer layer, which uses a continuous conductive network and a mechanically reinforced network formed by carbon nanotubes, is combined with a high-performance insulation layer and an inner core structure. The cable is made by setting a reinforcing core in the inner core and a wear-resistant coating on the outer layer. The manufacturing methods include stranding, extrusion molding and vacuum extrusion processes.
It significantly improves the tensile strength, flexural modulus, and fatigue resistance of cables, reduces wind resistance and wind load, achieves reliable anti-icing effect, extends cable service life, and meets the insulation requirements of high-voltage power transmission.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of power cable technology, specifically to a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes and its preparation method. Background Technology
[0002] As a core component of high-voltage transmission systems, overhead high-voltage cables are exposed to the natural environment for extended periods, and their operational stability directly determines the safety and reliability of high-voltage transmission lines. In actual service, overhead high-voltage cables often face two major threats: first, icing on the cable surface caused by low temperatures, high humidity, and freezing rain in winter. Icing significantly increases the cable's weight, leading to increased sag, tower tilting, conductor breakage, and even line paralysis. Second, fatigue damage caused by strong winds, typhoons, and wind-induced vibrations. Strong winds generate significant wind loads, causing increased cable swaying and swinging. Long-term wind vibration exacerbates internal structural wear and external cracking, reducing the cable's mechanical properties and service life. In severe cases, it can lead to cable breakage, affecting transmission safety.
[0003] In existing technologies, the design of overhead high-voltage cables often focuses on optimizing a single function, either by improving insulation performance or by addressing only the single requirement of anti-icing or wind resistance. This makes it difficult to simultaneously meet the dual performance requirements of wind resistance and anti-icing. For example, some anti-icing cables achieve de-icing by adding heating devices, but this results in high energy consumption, complex structure, and high maintenance costs, and does not consider wind resistance optimization, making them susceptible to damage in strong winds. Similarly, some wind-resistant cables achieve wind resistance by increasing the strength of the conductor core, but lack effective anti-icing measures, leaving the risk of icing in winter still present. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes and its preparation method, which solves the technical problems of existing overhead high-voltage cables being unable to simultaneously resist icing and strong wind damage, having poor structural stability, and having a short service life.
[0005] The technical solution of the present invention is: a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes, comprising a cable core and an insulation layer and an ice-resistant and wind-resistant outer layer sequentially sleeved on the outside of the cable core, with an outer diameter of 15~50mm; The cable core has a multi-strand stranded structure, consisting of 10 to 50 strands of copper alloy wire with a diameter of 0.5 to 2.0 mm, with a stranding pitch of 10 to 15 times the diameter of the cable core. The insulation layer has a thickness of 2-8 mm and comprises the following raw materials in parts by weight: 80-100 parts of EPDM rubber, 20-35 parts of fumed silica, 15-25 parts of aluminum hydroxide, 1.5-2.5 parts of dicumyl peroxide, 0.5-1.2 parts of triallyl isocyanurate, 1-2 parts of 2,8-di-tert-butyl-4-methylphenol, 0.3-0.8 parts of benzotriazole, and 2-5 parts of paraffin oil; The thickness of the anti-icing and wind-resistant outer layer is 0.8~3mm. The anti-icing and wind-resistant outer layer includes the following raw materials in parts by weight: 70~90 parts of polymer substrate, 1~10 parts of carbon nanotubes, 0.5~3 parts of anti-aging agent, 2~8 parts of toughening agent, 0.3~2 parts of dispersant, and 0.2~1.5 parts of UV protectant.
[0006] Furthermore, the preparation method of the insulating layer material is as follows: 1) Raw material pretreatment; EPDM rubber is plasticized on an open mill for 3-5 minutes at room temperature to obtain pretreated material; 2) Intensive blending; The pretreated material from step 1) is fed into a closed rubber mixing mill and plasticized for 2-3 minutes at a temperature of 60-70℃ and a speed of 30-40 r / min. Then, fumed silica and aluminum hydroxide are added sequentially, and the mixing temperature is controlled at 80-100℃ and the speed at 35-45 r / min for 4-6 minutes. Then, 2,8-di-tert-butyl-4-methylphenol, phenyltriazole and paraffin oil are added sequentially to the reaction system, and the temperature is maintained at 90-110℃ for 3-5 minutes. Then, the temperature of the mixing mill is increased to 100-115℃ and compacted at a speed of 30-40 r / min for 2-3 minutes. When the temperature of the reaction system drops to 90-115℃, the mixing is completed and the rubber is discharged to obtain the mixed material. 3) Vulcanization crosslinking; When the internal mixer in step 2) cools down to 50~70℃, add dicumyl peroxide and triallyl isocyanurate to the internal mixer and continue mixing for 2~3 minutes to obtain the crosslinked material; 4) Output the film; Place the crosslinking material from step 3) into a two-roll mill, control the sheet thickness from the two-roll mill to 2-3 mm, and obtain an insulating layer sheet. After the insulating layer sheet cools naturally to room temperature, let it stand for 8-12 hours to obtain the insulating layer material. Description: This invention fully softens EPDM rubber through a two-step plasticizing process, adds fillers and additives in stages to ensure uniform dispersion, and adds a crosslinking system at low temperature to achieve controlled crosslinking. After sheeting, a static treatment is performed to release internal stress. This method is mild, energy-efficient, and suitable for industrial mass production, producing insulating layer materials with good consistency and excellent insulation performance.
[0007] Furthermore, the polymer substrate is one of high-density polyethylene, polypropylene, fluoropolymer or silicone rubber; Carbon nanotubes are one of the single-walled and multi-walled carbon nanotubes. The diameter of carbon nanotubes is 30~50nm and the length is 15~45μm. Carbon nanotubes are uniformly dispersed in a polymer matrix to form a continuous conductive network and a mechanically reinforcing network. The anti-aging agent is one of hindered phenolic anti-aging agents, phosphite anti-aging agents, or amine anti-aging agents; the anti-aging agent can slow down the aging rate of the anti-icing and wind-resistant outer layer in harsh outdoor environments; The toughening agent is one of ethylene-vinyl acetate copolymer, polybutadiene rubber, or styrene-butadiene rubber; the toughening agent can improve the toughness and impact resistance of the anti-icing and wind-resistant outer layer and prevent the outer layer from cracking due to strong wind vibration. The dispersant is one of stearic acid, zinc stearate, or silane coupling agent; the dispersant can promote the uniform dispersion of carbon nanotubes in the polymer matrix and prevent carbon nanotubes from agglomerating. The UV stabilizer is one of the benzotriazole or benzophenone UV stabilizers; the UV stabilizer can resist ultraviolet radiation, prevent the outer material from aging and cracking, and further improve the weather resistance of the cable.
[0008] Furthermore, a reinforcing core is provided in the center of the cable core. The reinforcing core is one of aramid fiber core, glass fiber core or carbon fiber core, and the diameter of the reinforcing core is 1~3mm. Note: By adding a reinforcing core to the inner core of the cable, the tensile strength and wind vibration resistance of the inner core can be improved, preventing the cable from tensile breaking due to strong winds.
[0009] Furthermore, the anti-icing and wind-resistant outer layer is provided with a wear-resistant coating with a thickness of 0.05~0.1mm, and the wear-resistant coating is made of polytetrafluoroethylene or polyurethane material; Note: By applying a wear-resistant coating, the wear of particles carried by strong winds on the anti-icing and wind-resistant outer layer can be reduced without affecting the anti-icing and wind-resistant performance of the outer layer.
[0010] This invention also provides a method for preparing a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes, comprising the following steps: S1. Prepare the cable core; 10 to 50 strands of copper alloy wire are stranded using a stranding machine at a stranding speed of 50 to 150 r / min. After stranding, the inner core of the cable is annealed at a temperature of 200 to 300℃ for 30 to 60 minutes. S2. Prepare and coat the insulating layer; The insulation layer is added to the extruder and heated to a molten state. The melting temperature is controlled at 150~220℃. Then, the cable core from step S1 is fed into the extruder. An insulation layer is wrapped around the outside of the cable core by extrusion molding. The extrusion speed is controlled at 5~20m / min. After the wrapping is completed, a cooling water tank is used for cooling and shaping. The cooling temperature is 20~50℃ and the cooling time is 10~30min to obtain the insulated wire core. S3. Preparation of anti-icing and wind-resistant composite materials; Weigh out the polymer matrix, carbon nanotubes, anti-aging agent, toughening agent, dispersant, and UV stabilizer separately. First, add the polymer matrix to a high-speed mixer and heat it to 120-200℃ to melt it. Then add the dispersant and stir for 5-10 minutes. Next, add the carbon nanotubes and stir at high speed for 10-20 minutes, controlling the stirring speed at 1000-2000 r / min. Finally, add the anti-aging agent, toughening agent, and UV stabilizer, and melt-blend at 120-200℃ for 10-30 minutes to obtain the anti-icing and wind-resistant composite material. S4. Covered with an anti-icing and wind-resistant outer layer; The anti-icing and wind-resistant composite material from step S3 is added to an extruder and heated to 130~210℃. Then, polyurethane adhesive is coated on the surface of the insulated core from step S2, and the insulated core is fed into the extruder. An anti-icing and wind-resistant outer layer is coated on the outside of the insulation layer by extrusion coating. The extrusion speed is controlled at 5~20m / min and the coating thickness is 0.8~3mm. After coating, it is sent to a cooling water tank for cooling and shaping. The cooling temperature is 20~50℃ and the cooling time is 15~40min to obtain the finished cable.
[0011] Furthermore, in step S1, the annealing process is performed under inert gas protection, with nitrogen as the inert gas and a flow rate of 0.5~2m³. 3 / h; Note: By using inert gas to protect the cable core during the annealing process, oxidation of the metal conductor can be prevented, ensuring the electrical conductivity and mechanical properties of the cable core.
[0012] Furthermore, in step S3, before the carbon nanotubes are added to the high-speed mixer, the carbon nanotubes are surface modified using a silane coupling agent, with the modification temperature controlled at 80~120℃ and the modification time at 30~60min. Note: By modifying carbon nanotubes, the hydroxyl content on the surface of carbon nanotubes can be improved, thereby enhancing the compatibility between carbon nanotubes and polymer substrates and preventing agglomeration.
[0013] Furthermore, in step S4, when the anti-icing and wind-resistant outer layer is coated, a vacuum extrusion process is used to control the vacuum degree to -0.08~-0.05MPa; Note: By using vacuum extrusion technology, air bubbles can be avoided inside the anti-icing and wind-resistant outer layer, ensuring a dense outer layer structure, which is beneficial to improving its mechanical properties and anti-icing performance.
[0014] Furthermore, it also includes step S5, S5. Inspection and winding; The finished cable from step S4 is inspected for appearance, dimensions, electrical performance, mechanical performance, anti-icing performance, and wind resistance. After passing the inspection, it is wound up using a winding machine, and the winding speed is controlled at 5~15m / min. Note: Performance testing of finished cables helps improve their reliability during use, while rewinding facilitates transportation and transfer.
[0015] Compared with the prior art, the beneficial effects of the present invention are reflected in the following aspects: First, this invention incorporates carbon nanotubes into the anti-icing and wind-resistant outer layer, forming a continuous conductive network and a mechanically reinforcing network within the outer layer. The conductive network enables low-power, uniform heating and actively inhibits ice adhesion and growth, ensuring reliable anti-icing performance. The mechanically reinforcing network, combined with a smooth surface design, significantly improves the cable's tensile strength, flexural modulus, and fatigue resistance, reducing wind resistance and wind load, and effectively resisting damage from strong winds and wind-induced vibrations. Secondly, the finished cable of the present invention adopts a coaxial and tightly bonded structure of inner core, insulation layer and anti-icing and wind-resistant outer layer, and the insulation layer is made of high-performance insulation material with excellent electrical insulation performance, which can meet the insulation requirements of high voltage power transmission and avoid insulation breakdown accidents. Third, by adding anti-aging agents and UV inhibitors to the anti-icing and wind-resistant outer layer, the present invention utilizes the excellent weather resistance of carbon nanotubes, which can slow down the aging rate of the cable in harsh outdoor environments. By setting a wear-resistant coating on the surface of the anti-icing and wind-resistant outer layer, the wear of the anti-icing and wind-resistant outer layer by strong wind-carried particles can be reduced, further extending the service life of the cable. Detailed Implementation
[0016] Example 1: A wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes, comprising a cable core and an insulation layer and an ice-resistant and wind-resistant outer layer sequentially sleeved on the outside of the cable core, with an outer diameter of 15mm. The cable core has a multi-strand stranded structure, consisting of 10 strands of copper alloy wire with a diameter of 0.5mm, with a stranding pitch of 10 times the diameter of the cable core. The insulation layer has a thickness of 2mm and comprises the following raw materials in parts by weight: 80 parts of EPDM rubber, 20 parts of fumed silica, 15 parts of aluminum hydroxide, 1.5 parts of dicumyl peroxide, 0.5 parts of triallyl isocyanurate, 1 part of 2,8-di-tert-butyl-4-methylphenol, 0.3 parts of benzotriazole, and 2 parts of paraffin oil. The preparation method of the insulating layer material is as follows: 1) Raw material pretreatment; EPDM rubber was plasticized on an open mill for 3 minutes at room temperature to obtain a pretreated material; 2) Intensive blending; The pretreated material from step 1) is put into a closed rubber mixing mill and plasticized for 2 minutes at a temperature of 60℃ and a speed of 30 r / min. Then, fumed silica and aluminum hydroxide are added sequentially, and the mixing temperature is controlled at 80℃ and the speed at 35 r / min for 4 minutes. Then, 2,8-di-tert-butyl-4-methylphenol, phenyltriazole and paraffin oil are added sequentially to the reaction system, and the temperature is maintained at 90℃ for 3 minutes. Then, the temperature of the mixing mill is increased to 100℃ and compacted and mixed for 2 minutes at a speed of 30 r / min. When the temperature of the reaction system drops to 90℃, the mixing is completed and the rubber is discharged to obtain the mixed material. 3) Vulcanization crosslinking; When the internal mixer in step 2) cools down to 50°C, add dicumyl peroxide and triallyl isocyanurate to the internal mixer and continue mixing for 2 minutes to obtain the crosslinked material; 4) Output the film; Place the crosslinking material from step 3) into a two-roll mill, control the sheet thickness of the two-roll mill to 2mm, and obtain an insulating layer sheet. After the insulating layer sheet cools naturally to room temperature, let it stand for 8 hours to obtain the insulating layer material. The thickness of the anti-icing and wind-resistant outer layer is 0.8mm. The anti-icing and wind-resistant outer layer includes the following raw materials in parts by weight: 70 parts of polymer substrate, 1 part of carbon nanotube, 0.5 parts of anti-aging agent, 2 parts of toughening agent, 0.3 parts of dispersant, and 0.2 parts of UV protectant.
[0017] The polymer substrate is high-density polyethylene, the carbon nanotubes are single-walled carbon nanotubes with a diameter of 30 nm and a length of 15 μm; the anti-aging agent is antioxidant 1010; the toughening agent is ethylene-vinyl acetate copolymer; the dispersant is stearic acid; and the UV stabilizer is UV-326.
[0018] Example 2: This example describes the preparation method of the wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes according to Example 1, including the following steps: S1. Prepare the cable core; Ten strands of copper alloy wire were stranded using a stranding machine at a speed of 50 r / min. After stranding, the inner core of the cable was annealed at a controlled temperature of 200℃ for 30 min. The annealing process was performed under inert gas protection, using nitrogen gas at a flow rate of 0.5 m³ / min. 3 / h; S2. Prepare and coat the insulating layer; The insulation layer is added to the extruder and heated to a molten state. The melting temperature is controlled at 150°C. Then, the cable core from step S1 is fed into the extruder. An insulation layer is wrapped around the outside of the cable core by extrusion molding. The extrusion speed is controlled at 5m / min. After the wrapping is completed, a cooling water tank is used for cooling and shaping. The cooling temperature is 20°C and the cooling time is 10min to obtain the insulated wire core. S3. Preparation of anti-icing and wind-resistant composite materials; Surface modification of carbon nanotubes was performed using a silane coupling agent, with the modification temperature controlled at 80℃ and the modification time at 30 min. Then, polymer substrate, modified carbon nanotubes, anti-aging agent, toughening agent, dispersant, and UV stabilizer were weighed separately. The polymer substrate was first added to a high-speed mixer and heated to 120℃ to melt it. Then, the dispersant was added and stirred for 5 min. Next, the carbon nanotubes were added and stirred at high speed for 10 min at a controlled speed of 1000 r / min. Finally, the anti-aging agent, toughening agent, and UV stabilizer were added, and the mixture was melt-blended at 120℃ for 10 min to obtain an anti-icing and wind-resistant composite material. S4. Covered with an anti-icing and wind-resistant outer layer; The anti-icing and wind-resistant composite material from step S3 is added to an extruder and heated to 130°C. Then, polyurethane adhesive is coated on the surface of the insulated core from step S2, and the insulated core is fed into the extruder. Vacuum extrusion is used, and the vacuum degree is controlled at -0.08MPa. An anti-icing and wind-resistant outer layer is coated on the outside of the insulation layer by extrusion coating, with the extrusion speed controlled at 5m / min and the coating thickness at 0.8mm. After coating, the cable is sent to a cooling water tank for cooling and shaping at 20°C for 15min to obtain the finished cable.
[0019] Example 3: A wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes, comprising a cable core and an insulation layer and an ice-resistant and wind-resistant outer layer sequentially sleeved on the outside of the cable core, with an outer diameter of 30mm. The cable core has a multi-strand stranded structure, consisting of 35 strands of copper alloy wire with a diameter of 1.2mm, with a stranding pitch 12 times the diameter of the cable core; a reinforcing core with an aramid fiber core and a diameter of 1mm is set in the center of the cable core. The insulation layer has a thickness of 5 mm and comprises the following raw materials in parts by weight: 90 parts of EPDM rubber, 30 parts of fumed silica, 22 parts of aluminum hydroxide, 2 parts of dicumyl peroxide, 0.8 parts of triallyl isocyanurate, 1.5 parts of 2,8-di-tert-butyl-4-methylphenol, 0.6 parts of benzotriazole, and 4 parts of paraffin oil. The preparation method of the insulating layer material is as follows: 1) Raw material pretreatment; EPDM rubber was plasticized on an open mill for 4 minutes at room temperature to obtain a pretreated material; 2) Intensive blending; The pretreated material from step 1) was put into a closed rubber mixing mill and plasticized for 2.4 min at a temperature of 66℃ and a speed of 35 r / min. Then, fumed silica and aluminum hydroxide were added in sequence, and the mixing temperature was controlled at 92℃ and the speed at 40 r / min for 5 min. Then, 2,8-di-tert-butyl-4-methylphenol, phenyltriazole and paraffin oil were added to the reaction system in sequence, and the temperature was maintained at 105℃ for 4 min. Then, the temperature of the mixing mill was increased to 110℃ and compacted for 2.4 min at a speed of 35 r / min. When the temperature of the reaction system dropped to 100℃, the mixing was completed and the rubber was discharged to obtain the mixed material. 3) Vulcanization crosslinking; When the internal mixer in step 2) cools down to 60°C, dicumyl peroxide and triallyl isocyanurate are added to the internal mixer, and the mixture is continued to be mixed for 2.5 minutes to obtain the crosslinked material. 4) Output the film; Place the crosslinking material from step 3) into a two-roll mill, control the sheet thickness from the two-roll mill to 2.5 mm, and obtain an insulating layer sheet. After the insulating layer sheet cools naturally to room temperature, let it stand for 10 hours to obtain the insulating layer material. The anti-icing and wind-resistant outer layer has a thickness of 2.1 mm and comprises the following raw materials in parts by weight: 80 parts of polymer substrate, 7 parts of carbon nanotubes, 2 parts of anti-aging agent, 6 parts of toughening agent, 1.8 parts of dispersant, and 0.8 parts of UV stabilizer. The surface of the anti-icing and wind-resistant outer layer is provided with a wear-resistant coating with a thickness of 0.05 mm, which is made of polytetrafluoroethylene. The polymer substrate is polypropylene; the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 4 nm and a length of 35 μm; the anti-aging agent is trioctyl phosphite; the toughening agent is polybutadiene rubber; the dispersant is zinc stearate; and the UV stabilizer is UV-214.
[0020] Example 4: This example describes the preparation method of the wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes according to Example 3, including the following steps: S1. Prepare the cable core; Thirty-five strands of copper alloy wire were stranded using a stranding machine, with an aramid fiber core added to the copper alloy wire. The stranding speed was 100 r / min. After stranding, the cable core was annealed at a controlled temperature of 240℃ for 48 min. The annealing process was performed under inert gas protection, with nitrogen gas used as the inert gas and a flow rate of 1.2 m³ / min. 3 / h; S2. Prepare and coat the insulating layer; The insulation layer is added to the extruder and heated to a molten state. The melting temperature is controlled at 190°C. Then, the cable core from step S1 is fed into the extruder. An insulation layer is wrapped around the outside of the cable core by extrusion molding. The extrusion speed is controlled at 15m / min. After the wrapping is completed, a cooling water tank is used for cooling and shaping. The cooling temperature is 36°C and the cooling time is 22min to obtain the insulated wire core. S3. Preparation of anti-icing and wind-resistant composite materials; Surface modification of carbon nanotubes was performed using a silane coupling agent, with the modification temperature controlled at 105℃ and the modification time at 50 min. Then, polymer substrate, modified carbon nanotubes, anti-aging agent, toughening agent, dispersant, and UV stabilizer were weighed separately. The polymer substrate was first added to a high-speed mixer and heated to 165℃ to melt it. Then, the dispersant was added and stirred for 7 min. Next, the carbon nanotubes were added and stirred at high speed for 16 min at a controlled speed of 1500 r / min. Finally, the anti-aging agent, toughening agent, and UV stabilizer were added, and the mixture was melt-blended at 180℃ for 25 min to obtain an anti-icing and wind-resistant composite material. S4. Covered with an anti-icing and wind-resistant outer layer; The anti-icing and wind-resistant composite material from step S3 is added to an extruder and heated to 175°C. Then, polyurethane adhesive is coated on the surface of the insulated core from step S2, and the insulated core is fed into the extruder. Vacuum extrusion is used, and the vacuum degree is controlled at -0.06MPa. An anti-icing and wind-resistant outer layer is coated on the outside of the insulation layer by extrusion coating, with the extrusion speed controlled at 13m / min and the coating thickness at 2mm. After coating, the cable is sent to a cooling water tank for cooling and shaping at 35°C for 30min to obtain the finished cable. Finally, a wear-resistant coating is applied to the surface of the finished cable. S5. Inspection and winding; The finished cable from step S4 is inspected for appearance, dimensions, electrical performance, mechanical performance, anti-icing performance, and wind resistance. After passing the inspection, it is wound up using a winding machine, with the winding speed controlled at 5m / min.
[0021] Example 5: A wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes, comprising a cable core and an insulation layer and an ice-resistant and wind-resistant outer layer sequentially sleeved on the outside of the cable core, with an outer diameter of 50mm. The cable core has a multi-strand stranded structure, consisting of 50 strands of copper alloy wire with a diameter of 2.0mm, with a stranding pitch 15 times the diameter of the cable core; a reinforcing core with a diameter of 3mm is set in the center of the cable core. The insulation layer has a thickness of 8mm and comprises the following raw materials in parts by weight: 100 parts EPDM rubber, 35 parts fumed silica, 25 parts aluminum hydroxide, 2.5 parts dicumyl peroxide, 1.2 parts triallyl isocyanurate, 2 parts 2,8-di-tert-butyl-4-methylphenol, 0.8 parts benzotriazole, and 5 parts paraffin oil. The preparation method of the insulating layer material is as follows: 1) Raw material pretreatment; EPDM rubber was plasticized on an open mill for 5 minutes at room temperature to obtain a pretreated material; 2) Intensive blending; The pretreated material from step 1) is put into a closed rubber mixing mill and plasticized for 3 minutes at a temperature of 70℃ and a speed of 40 r / min. Then, fumed silica and aluminum hydroxide are added sequentially, and the mixing temperature is controlled at 100℃ and the speed at 45 r / min for 6 minutes. Then, 2,8-di-tert-butyl-4-methylphenol, phenyltriazole and paraffin oil are added sequentially to the reaction system, and the temperature is maintained at 110℃ for 5 minutes. Then, the temperature of the mixing mill is increased to 115℃, and the mixture is compacted and mixed for 3 minutes at a speed of 40 r / min. When the temperature of the reaction system drops to 115℃, the mixing is completed and the rubber is discharged to obtain the mixed material. 3) Vulcanization crosslinking; When the internal mixer in step 2) cools down to 70°C, add dicumyl peroxide and triallyl isocyanurate to the internal mixer and continue mixing for 3 minutes to obtain the crosslinked material; 4) Output the film; Place the crosslinking material from step 3) into a two-roll mill, control the sheet thickness of the two-roll mill to 3mm, and obtain the insulating layer sheet. After the insulating layer sheet cools naturally to room temperature, let it stand for 12 hours to obtain the insulating layer material. The anti-icing and wind-resistant outer layer is 3mm thick and comprises the following raw materials in parts by weight: 90 parts polymer substrate, 10 parts carbon nanotubes, 3 parts anti-aging agent, 8 parts toughening agent, 2 parts dispersant, and 1.5 parts UV stabilizer. The surface of the anti-icing and wind-resistant outer layer is provided with a wear-resistant coating, which is 0.1mm thick and made of polyurethane material. The polymer substrate is high-density silicone rubber; the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 50 nm and a length of 45 μm; the anti-aging agent is antioxidant 4020; the toughening agent is styrene-butadiene rubber; the dispersant is a silane coupling agent; and the UV stabilizer is UV-9.
[0022] Example 6: This example describes the preparation method of the wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes according to Example 5, including the following steps: S1. Prepare the cable core; Fifty strands of copper alloy wire were stranded using a stranding machine, with a glass fiber core added to the copper alloy wire. The stranding speed was 150 r / min. After stranding, the cable core was annealed at a controlled temperature of 300℃ for 60 min. The annealing process employed inert gas protection, with nitrogen gas at a flow rate of 2 m³ / min. 3 / h; S2. Prepare and coat the insulating layer; The insulation layer is added to the extruder and heated to a molten state. The melting temperature is controlled at 220°C. Then, the cable core from step S1 is fed into the extruder and an insulation layer is wrapped around the outside of the cable core by extrusion molding. The extrusion speed is controlled at 20m / min. After the wrapping is completed, a cooling water tank is used for cooling and shaping. The cooling temperature is 50°C and the cooling time is 30min to obtain the insulated wire core. S3. Preparation of anti-icing and wind-resistant composite materials; Surface modification of carbon nanotubes was performed using a silane coupling agent, with the modification temperature controlled at 120℃ and the modification time at 60 min. Polymer substrate, modified carbon nanotubes, anti-aging agent, toughening agent, dispersant, and UV stabilizer were weighed separately. First, the polymer substrate was added to a high-speed mixer and heated to 200℃ to melt it. Then, the dispersant was added and stirred for 10 min. Next, the carbon nanotubes were added and stirred at high speed for 20 min at a controlled speed of 2000 r / min. Finally, the anti-aging agent, toughening agent, and UV stabilizer were added, and the mixture was melt-blended at 200℃ for 30 min to obtain an anti-icing and wind-resistant composite material. S4. Covered with an anti-icing and wind-resistant outer layer; The anti-icing and wind-resistant composite material from step S3 is added to an extruder and heated to 210°C. Then, polyurethane adhesive is coated onto the surface of the insulated core from step S2, and the insulated core is fed into the extruder. Vacuum extrusion is used, and the vacuum degree is controlled at -0.05MPa. An anti-icing and wind-resistant outer layer is coated onto the outside of the insulation layer by extrusion coating, with the extrusion speed controlled at 20m / min and the coating thickness at 3mm. After coating, the cable is placed in a cooling water bath for cooling and shaping at 50°C for 40min to obtain the finished cable. Finally, an abrasion-resistant coating with a thickness of 0.1mm is coated onto the surface of the finished cable. The abrasion-resistant coating is made of polyurethane material. S5. Inspection and winding; The finished cable from step S4 is inspected for appearance, dimensions, electrical performance, mechanical performance, anti-icing performance, and wind resistance. After passing the inspection, it is wound up using a winding machine, with the winding speed controlled at 5~15m / min.
[0023] The performance of the finished cables prepared in Examples 2, 4, and 6 were tested respectively, and the results are shown in Table 1.
[0024] Table 1: Performance of the finished cables prepared in Examples 2, 4, and 6
[0025] The data in Table 1 shows that: As the number of conductor strands, diameter, stranding speed, and annealing temperature / time all gradually increase, the tensile strength of the core increases from 200MPa to 400MPa; while the insulation layer thickness increases from 2mm to 8mm, and the insulation layer breakdown field strength increases from 20kV / mm to 32kV / mm. The insulation performance is significantly optimized with the increase of voltage level, effectively resisting leakage current and insulation breakdown risk under high voltage; the thickness of the anti-icing and wind-resistant outer layer increases from 0.8mm to 3.0mm, and the wind resistance coefficient decreases from 0.35 to 0.2; the wind and ice resistance performance gradually increases with the increase of voltage level, adapting to harsher outdoor environments; moreover, the performance of Example 6 is superior to that of Example 2 and Example 4, and Example 6 is the best example.
[0026] Comparative Experiment 1: Investigating the effect of carbon nanotube addition amount on the performance of finished cable Comparative Example 1-1: In this example, the cable preparation method is the same as in Example 2, except that the amount of carbon nanotubes added is 0.5 parts; Comparative Examples 1-2: In this example, the cable preparation method is the same as in Example 2, except that the amount of carbon nanotubes added is 2 parts; Comparative Examples 1-3: In this example, the cable preparation method is the same as in Example 2, except that the amount of carbon nanotubes added is 5 parts; Comparative Examples 1-4: In this example, the cable preparation method is consistent with that in Example 2, except that the amount of carbon nanotubes added is 6 parts. Comparative Examples 1-5: In this example, the cable preparation method is the same as in Example 2, except that the amount of carbon nanotubes added is 11 parts; The performance of the finished cables prepared by Comparative Examples 1-1, 1-2, 1-3, 1-4, and 1-5 was tested respectively, and the test results are shown in Table 2.
[0027] Table 2: Performance of finished cables prepared in Comparative Examples 1-1, 1-2, 1-3, 1-4, and 1-5
[0028] The data in Table 2 shows that: 1. The amount of carbon nanotubes added is positively correlated with the anti-icing effect. When the amount added is higher than 1 part, a continuous conductive network can be formed, achieving effective active anti-icing. When the amount added is 0.5 parts, the carbon nanotubes are unevenly dispersed and cannot form a continuous conductive network, so the anti-icing effect is ineffective. When the amount added exceeds 5 parts, the improvement in the anti-icing effect slows down because the conductive network is close to saturation. 2. The amount of carbon nanotubes added is positively correlated with the tensile strength of the anti-icing and wind-resistant outer layer. As the amount added increases, the mechanical reinforcement network becomes denser, and the wind resistance and wind vibration resistance are improved. However, when the amount added is higher than 11 parts, the increase in tensile strength is minimal, and the carbon nanotubes are prone to agglomeration, which increases the difficulty of preparation. 3. Excessive addition of carbon nanotubes will reduce the insulation performance of the cable and significantly decrease the breakdown field strength. Because carbon nanotubes are conductive fillers, excessive addition can easily form conductive channels, affecting the reliability of insulation. It is evident that the optimal range for carbon nanotube addition is 4 to 7 parts, which ensures excellent anti-icing, wind resistance, and mechanical properties while maintaining good insulation performance, thus balancing effectiveness and reliability.
[0029] Comparative Experiment 2: Investigating the Influence of Carbon Nanotube State on the Performance of Finished Cables Comparative Example 2-1: In this example, the cable preparation method is the same as in Example 2, except that the carbon nanotubes are not modified; Comparative Example 2-2: In this example, the cable preparation method is the same as in Example 2, except that the carbon nanotubes are modified with a silane coupling agent; Comparative Examples 2-3: In this example, the cable preparation method is the same as in Example 2, except that the carbon nanotubes are modified with a titanate coupling agent; The performance of the finished cables prepared by Comparative Examples 2-1, 2-2, and 2-3 was tested respectively, and the test results are shown in Table 3.
[0030] Table 3: Performance of finished cables prepared in Comparative Examples 2-1, 2-2, and 2-3
[0031] The data in Table 3 shows that: 1. After surface modification, carbon nanotubes exhibit significantly improved compatibility with polymer substrates, resulting in uniform dispersion without agglomeration. Unmodified carbon nanotubes have low hydroxyl content, poor compatibility, and are prone to agglomeration, which disrupts the continuity of the conductive network and the mechanical reinforcement network. 2. Modified carbon nanotubes form a more continuous conductive network, have lower volume resistivity, more uniform heating, and stable anti-icing effect; unmodified carbon nanotubes, due to aggregation, have a discontinuous conductive network, uneven heating, and localized icing. 3. The modified carbon nanotubes bond more tightly with the substrate, resulting in a more significant mechanical reinforcement effect and a significantly higher tensile strength than the unmodified group. The unmodified group suffers from decreased outer layer mechanical properties due to agglomeration, and is prone to cracking under long-term wind vibration. The modification effects of silane coupling agents and titanate coupling agents are similar, both effectively improving dispersibility and overall performance, and can be flexibly selected according to actual production costs. It is evident that surface modification of carbon nanotubes ensures their uniform dispersion in polymer substrates, thereby achieving a synergistic improvement in anti-icing, mechanical, and wind-vibration resistance properties. Unmodified carbon nanotubes cannot meet the requirements for cable use.
[0032] Comparative Experiment 3: Investigating the Influence of Anti-icing and Wind-resistant Outer Layer Thickness on the Performance of Finished Cables Comparative Example 3-1: In this example, the cable preparation method is the same as in Example 2, except that the thickness of the anti-icing and wind-resistant outer layer is 0.5 mm; Comparative Example 3-2: In this example, the cable preparation method is the same as in Example 2, except that the thickness of the anti-icing and wind-resistant outer layer is 1.5 mm; Comparative Example 3-3: In this example, the cable preparation method is the same as in Example 2, except that the thickness of the anti-icing and wind-resistant outer layer is 2 mm; Comparative Examples 3-4: In this example, the cable preparation method is the same as in Example 2, except that the thickness of the anti-icing and wind-resistant outer layer is 2.5 mm; Comparative Examples 3-5: In this example, the cable preparation method is the same as in Example 2, except that the thickness of the anti-icing and wind-resistant outer layer is 3.5 mm; The performance of the finished cables prepared by Comparative Examples 3-1, 3-2, 3-3, 3-4, and 3-5 was tested respectively, and the test results are shown in Table 4.
[0033] Table 4: Performance of finished cables prepared in Comparative Examples 3-1, 3-2, 3-3, 3-4, and 3-5
[0034] The data in Table 4 shows that: 1. When the thickness of the anti-icing and wind-resistant outer layer exceeds 0.8mm, the heat generation is uniform and the anti-icing effect is stable; when the thickness is 0.5mm, the outer layer is too thin, the carbon nanotubes are unevenly distributed, the heat generation is uneven, and although it can prevent icing, the stability is poor; when the thickness exceeds 2.0mm, the heating rate decreases slightly because the heat conduction efficiency is reduced due to the increased outer layer thickness, but it does not affect the anti-icing effect. 2. The thickness of the anti-icing and wind-resistant outer layer is positively correlated with the drag coefficient. As the thickness increases, the wind resistance increases and the wind load increases slightly. When the thickness of the anti-icing and wind-resistant outer layer exceeds 0.8mm, it can meet the wind resistance requirements at a wind speed of 40m / s. When the thickness is 0.5mm, the mechanical strength of the outer layer is insufficient and it is easily damaged by wind vibration. 3. The thickness of the anti-icing and wind-resistant outer layer is positively correlated with its wear resistance; the greater the thickness, the stronger the wear resistance. However, when the thickness exceeds 3.5mm, it will significantly increase the overall weight of the cable and increase the load-bearing pressure on the tower. It is evident that the optimal range for the thickness of the anti-icing and wind-resistant outer layer is 1.8~2.2mm, which ensures uniform anti-icing, excellent wind and abrasion resistance, while also controlling the cable weight, thus balancing practicality and economy.
Claims
1. A wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes, characterized in that, It includes the cable core and an insulation layer and an anti-icing and wind-resistant outer layer sequentially sleeved on the outside of the cable core; The inner core of the cable has a multi-strand stranded structure, consisting of 10 to 50 strands of copper alloy wires with a diameter of 0.5 to 2.0 mm, with a stranding pitch of 10 to 15 times the diameter of the inner core of the cable. The insulating layer comprises the following raw materials in parts by weight: 80-100 parts of ethylene propylene diene monomer (EPDM) rubber, 20-35 parts of fumed silica, 15-25 parts of aluminum hydroxide, 1.5-2.5 parts of dicumyl peroxide, 0.5-1.2 parts of triallyl isocyanurate, 1-2 parts of 2,8-di-tert-butyl-4-methylphenol, 0.3-0.8 parts of benzotriazole, and 2-5 parts of paraffin oil; The anti-icing and wind-resistant outer layer comprises the following raw materials in parts by weight: 70-90 parts of polymer substrate, 1-10 parts of carbon nanotubes, 0.5-3 parts of anti-aging agent, 2-8 parts of toughening agent, 0.3-2 parts of dispersant, and 0.2-1.5 parts of UV protectant.
2. The wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 1, characterized in that, The method for preparing the insulating layer material is as follows: 1) Raw material pretreatment; The EPDM rubber was plasticized on an open mill for 3-5 minutes at room temperature to obtain a pretreated material; 2) Intensive blending; The pretreated material described in step 1) is fed into a closed rubber mixing mill and plasticized for 2-3 minutes at a temperature of 60-70℃ and a speed of 30-40 r / min. Then, fumed silica and aluminum hydroxide are added sequentially, and the mixing temperature is controlled at 80-100℃ and the speed at 35-45 r / min for 4-6 minutes. Then, 2,8-di-tert-butyl-4-methylphenol, phenyltriazole and paraffin oil are added sequentially to the reaction system, and the temperature is maintained at 90-110℃. The mixing continues for 3-5 minutes. Then, the temperature of the mixing mill is increased to 100-115℃, and the mixture is compacted and mixed for 2-3 minutes at a speed of 30-40 r / min. When the temperature of the reaction system drops to 90-115℃, the mixing is completed and the rubber is discharged to obtain the mixed material. 3) Vulcanization crosslinking; When the internal mixer described in step 2) cools down to 50~70℃, dicumyl peroxide and triallyl isocyanurate are added to the internal mixer, and the mixture is continued to be mixed for 2~3 minutes to obtain the crosslinked material; 4) Output the film; Place the crosslinking material described in step 3) into a two-roll mill, control the sheet thickness of the two-roll mill to 2-3 mm, and obtain an insulating layer sheet. After the insulating layer sheet cools naturally to room temperature, let it stand for 8-12 hours to obtain the insulating layer material.
3. The wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 1, characterized in that, The polymer substrate is one of high-density polyethylene, polypropylene, fluoropolymer or silicone rubber; The carbon nanotubes are either single-walled carbon nanotubes or multi-walled carbon nanotubes, with a diameter of 30-50 nm and a length of 15-45 μm. The anti-aging agent is one of hindered phenolic anti-aging agents, phosphite anti-aging agents, or amine anti-aging agents; The toughening agent is one of ethylene-vinyl acetate copolymer, polybutadiene rubber, or styrene-butadiene rubber; The dispersant is one of stearic acid, zinc stearate, or silane coupling agent; The UV-blocking agent is one of the benzotriazole or benzophenone UV-blocking agents.
4. The wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 1, characterized in that, The cable has a reinforcing core at its center, which is one of aramid fiber, glass fiber, or carbon fiber, and has a diameter of 1-3 mm.
5. The wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 1, characterized in that, The anti-icing and wind-resistant outer layer is provided with a wear-resistant coating, the thickness of which is 0.05~0.1mm, and the wear-resistant coating is made of polytetrafluoroethylene or polyurethane material.
6. A method for preparing a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. Prepare the cable core; 10 to 50 strands of copper alloy wire are stranded using a stranding machine at a stranding speed of 50 to 150 r / min. After stranding, the inner core of the cable is annealed at a temperature of 200 to 300℃ for 30 to 60 minutes. S2. Prepare and coat the insulating layer; The insulation layer is added to the extruder and heated to a molten state. The melting temperature is controlled at 150~220℃. Then, the cable core described in step S1 is fed into the extruder. An insulation layer is wrapped around the outside of the cable core by extrusion molding. The extrusion speed is controlled at 5~20m / min. After the wrapping is completed, a cooling water tank is used for cooling and shaping. The cooling temperature is 20~50℃ and the cooling time is 10~30min to obtain the insulated wire core. S3. Preparation of anti-icing and wind-resistant composite materials; Weigh out the polymer matrix, carbon nanotubes, anti-aging agent, toughening agent, dispersant, and UV stabilizer separately. First, add the polymer matrix to a high-speed mixer and heat it to 120-200℃ to melt it. Then add the dispersant and stir for 5-10 minutes. Next, add the carbon nanotubes and stir at high speed for 10-20 minutes, controlling the stirring speed at 1000-2000 r / min. Finally, add the anti-aging agent, toughening agent, and UV stabilizer, and melt-blend at 120-200℃ for 10-30 minutes to obtain the anti-icing and wind-resistant composite material. S4. Covered with an anti-icing and wind-resistant outer layer; The anti-icing and wind-resistant composite material described in step S3 is added to an extruder and heated to 130~210℃. Then, polyurethane adhesive is coated on the surface of the insulated core described in step S2, and the insulated core is fed into the extruder. An anti-icing and wind-resistant outer layer is coated on the outside of the insulation layer by extrusion coating. The extrusion speed is controlled at 5~20m / min and the coating thickness is 0.8~3mm. After coating, it is sent to a cooling water tank for cooling and shaping. The cooling temperature is 20~50℃ and the cooling time is 15~40min to obtain the finished cable.
7. The method for preparing a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 6, characterized in that, In step S1, the annealing process is performed under inert gas protection, wherein the inert gas is nitrogen, and the inert gas flow rate is 0.5~2m³. 3 / h.
8. The method for preparing a wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 6, characterized in that, In step S3, before the carbon nanotubes are added to the high-speed mixer, the carbon nanotubes are surface modified using a silane coupling agent, with the modification temperature controlled at 80~120℃ and the modification time at 30~60min.
9. A wind-resistant and ice-resistant overhead high-voltage cable based on carbon nanotubes as described in claim 6, characterized in that, A reinforcing core is provided at the center of the inner core of the cable.