A spatially selectively modified porous carbon, its preparation method, and silicon-carbon anode materials
Patent Information
- Application Number
- CN202610654803.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-13
- Publication Date
- 2026-08-04
AI Technical Summary
[0007]为克服现有气相沉积硅碳负极材料中硅-碳界面结合弱、SEI膜不稳定等问题,本发明通过在硅沉积之前,对多孔碳进行分子级、空间可控的功能化修饰,预先构筑一种能够增强硅-碳界面结合并诱导形成稳定SEI的友好界面层
[0031] (1) Spatial selective modification of interface function: By utilizing the molecular size effect of lithium dyes and combining the gradient pore structure of porous carbon, the functional phase containing Li, S and N elements was precisely positioned and modified on the inner surface of the pores with larger diameters on the outer layer of porous carbon, while avoiding the blockage of the internal micropore mass transfer channels.
Smart Images

Figure CN122501848A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery anode material technology, specifically relating to a spatially selectively modified porous carbon, its preparation method, and a silicon-carbon anode. Background Technology
[0002] With the rapid development of high-energy-density lithium-ion batteries in new energy vehicles and energy storage, traditional graphite anode materials are gradually approaching their theoretical capacity limit (372 mAh / g), making it difficult to meet the urgent energy density requirements of next-generation battery systems. Silicon-based anode materials, with their theoretical specific capacity of approximately 4200 mAh / g, are considered one of the most promising next-generation anode materials. However, the huge volume change (up to 300%) that accompanies the lithium insertion / extraction process in silicon can cause severe structural pulverization, electrode failure, and interface instability, severely restricting their practical application.
[0003] To mitigate the volume expansion effect of silicon anodes, constructing silicon-carbon composite materials has become one of the most mainstream and effective technological approaches. Porous carbon, due to its excellent conductivity, designable pore structure, and buffering capacity against silicon volume expansion, is widely used as a silicon carrier material. Among numerous silicon-carbon composite methods, chemical vapor deposition (CVD), with its controllability over the size, distribution, and interface structure of the silicon phase, is widely recognized as one of the most promising industrial routes for preparing high-performance silicon-carbon anode materials. This process introduces gaseous silanes into the pores of porous carbon, causing them to undergo thermal decomposition at a specific temperature, thereby depositing silicon in situ as nanoparticles or amorphous particles on the inner walls and surface of the porous carbon pores. Compared to traditional silicon-carbon composite materials that are mechanically mixed or liquid-phase coated, CVD silicon-carbon composite anode materials have advantages in reversible specific capacity and initial coulombic efficiency. However, the performance limits and long-term cycling stability of CVD silicon-carbon composite anode materials are still largely limited by the selected porous carbon framework structure and surface chemical properties. Current vapor deposition technology for silicon-carbon still faces the following key technological bottlenecks:
[0004] (1) The silicon-carbon interface bonding mechanism remains fragile: Although silicon and carbon formed by vapor deposition have a closer contact than in a physically mixed system, their interface bonding is still mainly based on physical adsorption and local weak chemical interaction. During long-term repeated lithium insertion / extraction, the stress generated by volume changes can easily lead to local debonding or deterioration of electrical contacts, which in turn causes capacity decay.
[0005] (2) The problem of unstable electrode / electrolyte interface (SEI) has not been fundamentally solved: After silicon loading, the macropores and main channels of the porous carbon outer layer are still directly exposed to the electrolyte. During the first cycle, the silicon and the highly active carbon surface induce electrolyte decomposition, forming an unstable SEI film. This SEI film continuously breaks down and reconstructs with the change in silicon volume during subsequent cycles, continuously consuming active lithium and electrolyte, becoming the main reason for the shortened cycle life and increased interfacial impedance.
[0006] Therefore, simply relying on the optimization of deposition process parameters is no longer sufficient to overcome the performance bottleneck of gas-phase silicon-carbon anodes. It is urgent to systematically regulate the interfacial chemical state of porous carbon from the material design source. Summary of the Invention
[0007] To overcome the problems of weak silicon-carbon interface bonding and unstable SEI film in existing vapor-deposited silicon-carbon anode materials, this invention pre-constructs a friendly interface layer that enhances silicon-carbon interface bonding and induces the formation of a stable SEI by performing molecular-level, spatially controllable functionalization modification on porous carbon before silicon deposition. Specifically, by introducing lithium-based dyes, a nitrogen / sulfur / lithium co-modified functional interface layer is constructed in situ on the inner surface of the larger pores on the outer layer of the porous carbon, thereby achieving active control over the key interface of the silicon-carbon anode and significantly improving its cycle stability and interface reliability.
[0008] To achieve the above objectives, the present invention adopts the following technical solution:
[0009] A method for preparing spatially selectively modified porous carbon includes the following steps:
[0010] (S1) Dissolve sulfonate aromatic azo dyes in a mixed solvent of water and polar aprotic organic solvent to form solution A. Add a soluble lithium source to solution A under an inert atmosphere. After dissolution, heat the solution to carry out an ion exchange reaction. After the reaction is completed, the solution is purified to obtain lithium dyes.
[0011] (S2) The lithium dye is dissolved in a mixed solvent of water and a polar aprotic organic solvent to form solution B. The porous carbon is placed in solution B for impregnation treatment to obtain composite porous carbon. By controlling the impregnation conditions, the loading of lithium dye is 2~4wt%.
[0012] (S3) The composite porous carbon was heat-treated under an inert atmosphere to obtain spatially selectively modified porous carbon.
[0013] Further, in step (S1), the sulfonate aromatic azo dye is selected from at least one of methyl orange, Congo red, orange yellow I, and chrome black T; preferably methyl orange or orange yellow I; more preferably methyl orange. The sulfonate aromatic azo dye of the present invention is anionic dye. Because it contains aromatic and azo groups, its molecular size is relatively large, generally 1~3 nm.
[0014] Further, in step (S1), the soluble lithium source is selected from at least one of lithium chloride (LiCl), lithium hydroxide (LiOH), and lithium hydroxide hydrate.
[0015] Further, in step (S1), the Na in the sulfonate aromatic azo dye... + With Li in the lithium source + The molar ratio is 1:1.5~3, preferably 1:1.5~2. Excess lithium source is used to ensure the Na content in sulfonate aromatic azo dyes. + With Li + The exchange reaction is complete, and the optimal range balances reaction efficiency and economy.
[0016] Further, in steps (S1) and (S2), the volume ratio of water to polar aprotic solvent in the mixed solvent is 7:3 to 8:2, and the polar aprotic solvent is selected from at least one of acetonitrile, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO); the concentration of solution A is 0.2 to 0.8 wt%; the inert atmosphere is nitrogen and / or argon; the temperature is raised to 70 to 80°C, and the ion exchange reaction time is 4 to 8 hours. During the ion exchange reaction in step (S1), the soluble lithium source dissociates into lithium ions (Li) in the mixed solvent of water and polar aprotic solvent. + ), Li + Due to its small ionic radius and strong nucleophilicity, it readily exchanges with exchangeable metal ions (such as Na+) in sulfonate aromatic azo dye molecules. + An ion exchange reaction occurs, i.e., Li + The Na group on the sulfonate group in the substituted dye molecule + This process generates lithium dyes (such as lithium methyl orange and lithium Congo red), while also producing byproducts (such as NaOH or NaCl).
[0017] The purification process in step (S1) varies depending on the lithium source: When the lithium source is lithium chloride (LiCl), a polar aprotic solvent is added to the reaction solution to make the volume fraction of the polar aprotic solvent in the mixed solvent ≥ 85%. At this time, the byproduct NaCl precipitate is precipitated, and the lithium dye is retained in the liquid phase. After removing the precipitate by filtration, the filtrate is concentrated by vacuum distillation and freeze-dried to obtain lithium dye powder. When the lithium source is lithium hydroxide (LiOH) or lithium hydroxide hydrate, CO2 gas is first introduced into the reaction solution until the pH of the system is 10~11, so that the byproduct NaOH is converted into Na2CO3. Then, a polar aprotic solvent is added to make the volume fraction of the polar aprotic solvent in the mixed solvent ≥ 85%. At this time, Na2CO3 precipitate is precipitated, and the lithium dye is retained in the liquid phase. After removing the precipitate by filtration, the filtrate is concentrated by vacuum distillation and freeze-dried to obtain lithium dye powder.
[0018] The dye is methyl orange (C 14 H 14 Taking N3NaO3S and lithium sources lithium hydroxide monohydrate (LiOH·H2O) and lithium chloride (LiCl) as examples, the chemical formulas of the ion exchange reactions are as follows:
[0019] C 14 H 14 N3NaO3S + LiOH·H2O C 14 H 14 N3LiO3S + NaOH + H2O
[0020] C 14 H 14 N3NaO3S + LiCl C 14 H 14 N3LiO3S + NaCl
[0021] Further, in step (S2), the BET specific surface area of the porous carbon is 1500~2500 m². 2 The porous carbon has an average pore size of 1.4–2.5 nm, and based on the gas adsorption BET method, it comprises 60–90% micropores and 10–30% mesopores. It should be noted that this porous carbon inevitably contains a very small amount of macropores, but because the content is extremely low and exceeds the effective testing range of the BET method, it is not included in the above percentages. Porous carbon can be prepared in-house or commercially available.
[0022] Preferably, in step (S2), the loading of the lithium dye is 2~3 wt%. The loading of the lithium dye needs to be controlled within the above range. If the loading of the lithium dye is too high, it will block the channels; if the loading of the lithium dye is too low, a continuous and effective functional interface cannot be formed.
[0023] Further, in step (S2), the concentration of solution B is 0.2~0.8wt%; the impregnation conditions are: porous carbon is impregnated in solution B at a solid-liquid ratio of 1g:5~20mL, the temperature is 40~60℃, the impregnation time is 2~4h, and after impregnation treatment, it is dried at 80~100℃ for 6~12h to obtain composite porous carbon.
[0024] The sulfonate-based aromatic azo dyes of this invention have relatively large molecular sizes due to the presence of aromatic and azo groups. The lithium-ion dyes obtained after lithium-ion exchange reactions also have relatively large molecular sizes (generally 1-3 nm). Therefore, during the impregnation process, due to the size sieving effect, the lithium-ion dyes preferentially enter and adsorb onto the inner surface of the larger pores in the outer layer of porous carbon (mainly mesopores and a very small number of macropores), making it difficult for them to enter the smaller microporous regions.
[0025] Further, in step (S3), the inert atmosphere is nitrogen and / or argon; the heat treatment conditions are: 700~850℃ for 1~3 hours. During the heat treatment, the lithium dye undergoes thermal decomposition and in-situ carbonization within the macropores and main channels of the porous carbon outer layer where it is adsorbed, forming a uniform interface layer containing S, N, and Li at the adsorption site, i.e., a functional interface layer is obtained on the inner wall of the macropores and main channels of the porous carbon outer layer. This functional interface layer is only distributed on the inner wall of the macropores and main channels of the porous carbon outer layer, without blocking the microporous structure inside the porous carbon, thereby ensuring efficient mass transfer channels inside the material. It can be directly used as a carrier material in chemical vapor deposition processes for the subsequent preparation of silicon-carbon composite anode materials.
[0026] Secondly, the present invention also provides a spatially selectively modified porous carbon, which is prepared by the above-described preparation method.
[0027] Thirdly, the present invention also provides a silicon-carbon anode material, which is prepared by sequentially vapor-depositing silicon and carbon coating of the aforementioned spatially selectively modified porous carbon.
[0028] The processes of vapor-phase silicon deposition and carbon coating are well-known in the art and are not particularly limited. For example, the conditions for vapor-phase silicon deposition are as follows: spatially selectively modified porous carbon is chemically vapor-deposited at 450–550 °C for 3–5 h under an inert atmosphere using an organosilicon source gas. The ratio of spatially selectively modified porous carbon to organosilicon source gas is 1 kg: 500–1000 L. The organosilicon source gas is selected from at least one of silane, dichlorosilane, trichlorosilane, silicon tetrachloride, silicon tetrafluoride, and disilane. The conditions for carbon coating are as follows: porous carbon after silicon deposition is reacted with a gaseous carbon source at 500–700 °C for 1–3 h under an inert atmosphere. The ratio of porous carbon after silicon deposition to gaseous carbon source is 1 kg: 200–500 L. The gaseous carbon source is selected from at least one of C1–4 alkanes, C2–4 alkenes, and C2–4 alkynes.
[0029] Furthermore, the silicon content in the silicon-carbon anode material is 48-55 wt%, and the carbon coating layer accounts for 1.0-3.0 wt% of the silicon-carbon anode material.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) Spatial selective modification of interface function: By utilizing the molecular size effect of lithium dyes and combining the gradient pore structure of porous carbon, the functional phase containing Li, S and N elements was precisely positioned and modified on the inner surface of the pores with larger diameters on the outer layer of porous carbon, while avoiding the blockage of the internal micropore mass transfer channels.
[0032] (2) Enhance the bonding strength of silicon-carbon interface: The functional interface layer formed by pyrolysis with Li, S and N co-modification can form a stronger interface bond with silicon in the subsequent vapor deposition process (such as S-Si bond or Li-Si interaction), effectively suppressing interface debonding and electrical contact deterioration caused by volume expansion.
[0033] (3) Inducing the formation of a stable SEI film and improving cycle stability: The uniformly distributed Li, S and N elements in the functional interface layer can be used as pre-set interface regulation components to guide the formation of a thin and dense, structurally stable SEI film, reduce electrolyte decomposition and active lithium consumption, reduce interface impedance, and thus improve the battery's first coulombic efficiency and long-term cycle stability. Attached Figure Description
[0034] Figure 1 The images show the SEM image and S element mapping of the spatially selectively modified porous carbon obtained in Example 1. Figure 1 (a) is a SEM image. Figure 1 (b) is the S-element mapping graph.
[0035] Figure 2 The nitrogen adsorption-desorption curves are shown for the spatially selectively modified porous carbon prepared in Example 1 and the raw porous carbon. Detailed Implementation
[0036] The present invention will be further described below with reference to specific embodiments, but the present invention is not limited to the following embodiments.
[0037] Unless otherwise specified, the experimental methods described in the following examples are conventional methods; unless otherwise specified, the reagents and materials are commercially available.
[0038] The porous carbon is a resin-based porous carbon prepared by physical activation method. Its specific surface area is 2170.2 m² / g, the average pore size is 1.74 nm, the micropore ratio is 83.6%, and the mesopore ratio is 16.4%.
[0039] Example 1
[0040] (S1) Add 20g of methyl orange to a mixed solvent of 5 L of water and acetonitrile (the volume ratio of water to acetonitrile is 7:3), stir and heat to 45°C until the methyl orange is completely dissolved to obtain a homogeneous methyl orange solution; then add 3.84g of LiOH·H2O (i.e., Na+ from methyl orange) to the solution. + Li with LiOH·H2O + With a molar ratio of 1:1.5, the system was heated to 75°C and refluxed for 6 hours under a nitrogen atmosphere to complete the Na content in methyl orange. + With Li + The reaction involves an ion exchange reaction. After the reaction is complete, dry CO2 gas is slowly introduced into the reaction solution, and the reaction is stirred until the pH of the system reaches 10.5, completely converting the byproduct NaOH into Na2CO3. Acetonitrile is then added to make the volume fraction of acetonitrile in the mixed solvent 85% (approximately 20 L). The mixture is stirred for 15 min, at which point Na2CO3 precipitates out, while lithium-ionized methyl orange remains in the liquid phase. The mixture is then filtered under a vacuum of -0.095 MPa to remove the precipitated Na2CO3. Finally, the filtrate is concentrated by vacuum distillation to remove the solvent, and then freeze-dried (-40 °C, 0.01 MPa) to obtain lithium-ionized methyl orange.
[0041] (S2) Dissolve 20g of lithium methyl orange in a mixed solvent of 5 L water and acetonitrile (the volume ratio of water to acetonitrile is 7:3) to form a solution. Add 600g of porous carbon to the solution and impregnate the solution by stirring at 200 rpm at 50°C for 2 h. After impregnation, separate the solid and liquid components. Dry the solid at 80°C for 12 h to obtain composite porous carbon with a lithium methyl orange loading of 2.0 wt% (determined by the weight gain method).
[0042] (S3) The composite porous carbon was placed in a heat treatment furnace and heated to 800℃ at a heating rate of 5℃ / min under an argon atmosphere. It was then held at this temperature for 2 hours and allowed to cool naturally to room temperature after the holding period to obtain the space-selectively modified porous carbon.
[0043] Example 2
[0044] The rest is the same as in Example 1, except that in step (S1), equimolar amounts of Orange I (based on sodium element) are used instead of methyl orange, specifically:
[0045] (S1) Add 20g of Orange Yellow I to a mixed solvent of 5 L of water and acetonitrile (the volume ratio of water to acetonitrile is 7:3), stir and heat to 45℃ to completely dissolve Orange Yellow I, obtaining a homogeneous Orange Yellow I solution; then add 3.59g of LiOH·H2O (i.e., Na+ in Orange Yellow I) to the solution. +Li with LiOH·H2O + With a molar ratio of 1:1.5, the system was heated to 75°C and refluxed for 6 hours under a nitrogen atmosphere to complete the Na content in Orange-Yellow I. + With Li + The ion exchange reaction was carried out; after the reaction was completed, dry CO2 gas was slowly introduced into the reaction solution and the reaction was stirred until the pH of the system was 10.5, completely converting the byproduct NaOH into Na2CO3; then acetonitrile was added to make the volume fraction of acetonitrile in the mixed solvent 85%, and the mixture was stirred for 15 min. At this time, Na2CO3 precipitated out, while lithium orange I remained in the liquid phase; then the mixture was filtered under a vacuum of -0.095 MPa to remove the precipitated Na2CO3. Finally, the filtrate was concentrated by vacuum distillation to remove the solvent, and then freeze-dried (-40℃, 0.01 MPa) to obtain lithium orange I;
[0046] (S2) Dissolve 20g of lithium orange I in a mixed solvent of 5 L water and acetonitrile (the volume ratio of water to acetonitrile is 7:3) to form a solution. Add 600g of porous carbon to the solution and impregnate the solution by stirring at 200 rpm at 50°C for 2 h. After impregnation, separate the solid and liquid components. Dry the solid at 80°C for 12 h to obtain composite porous carbon with a lithium orange I loading of 2.1 wt% (determined by the weight gain method).
[0047] (S3) Same as Example 1.
[0048] Example 3
[0049] The rest is the same as in Example 1, except that in step (S1), Congo red is used in equimolar amounts (based on sodium element) instead of methyl orange, specifically:
[0050] (S1) Add 20g of Congo red to a mixed solvent of 5L water and acetonitrile (the volume ratio of water to acetonitrile is 7:3), stir and heat to 45℃ to completely dissolve the Congo red, obtaining a homogeneous Congo red solution; then add 3.62g of LiOH·H2O (i.e., Na+ in Congo red) to the solution. + Li with LiOH·H2O + With a molar ratio of 1:1.5, the system was heated to 75°C and refluxed for 6 hours under a nitrogen atmosphere to complete the Na content in Congo red. + With Li +The reaction involved an ion exchange reaction. After the reaction was complete, dry CO2 gas was slowly introduced into the reaction solution, and the reaction was stirred until the pH of the system reached 10.5, completely converting the byproduct NaOH into Na2CO3. Acetonitrile was then added to make the volume fraction of acetonitrile in the mixed solvent 85%, and the mixture was stirred for 15 min. At this point, Na2CO3 precipitated out, while lithium Congo red remained in the liquid phase. The mixture was then filtered under a vacuum of -0.095 MPa to remove the precipitated Na2CO3. Finally, the filtrate was concentrated by vacuum distillation to remove the solvent, and then freeze-dried (-40℃, 0.01 MPa) to obtain lithium Congo red.
[0051] (S2) 20g of lithium Congo red was dissolved in a mixed solvent of 5L water and acetonitrile (the volume ratio of water to acetonitrile was 7:3) to form a solution. 600g of porous carbon was added to the solution and the mixture was stirred at 200rpm at 50℃ for 2h for impregnation treatment. After impregnation, the solid and liquid were separated. The solid was dried at 80℃ for 12h to obtain composite porous carbon with a lithium Congo red loading of 2.2wt% (determined by the weight gain method).
[0052] (S3) Same as Example 1.
[0053] Example 4
[0054] The rest is the same as in Example 1, except that in step (S1), methyl orange is replaced with equimolar amounts of Chrome Black T (based on sodium element). Specifically:
[0055] (S1) Add 20g of Chrome Black T to a mixed solvent of 5 L of water and acetonitrile (the volume ratio of water to acetonitrile is 7:3), stir and heat to 45℃ to completely dissolve Chrome Black T, obtaining a homogeneous Chrome Black T solution; then add 2.73g of LiOH·H2O (i.e., Na+ in Chrome Black T) to the solution. + Li with LiOH·H2O + With a molar ratio of 1:1.5, the system was heated to 75°C and refluxed for 6 hours under a nitrogen atmosphere to complete the Na content in chrome black T. + With Li + The ion exchange reaction was carried out; after the reaction was completed, dry CO2 gas was slowly introduced into the reaction solution and the reaction was stirred until the pH of the system was 10.5, and the byproduct NaOH was completely converted into Na2CO3; then acetonitrile was added to make the volume fraction of acetonitrile in the mixed solvent 85%, and the mixture was stirred for 15 min. At this time, Na2CO3 precipitated out, while Eriochrome Black T remained in the liquid phase; then the mixture was filtered under a vacuum of -0.095 MPa to remove the precipitated Na2CO3. Finally, the filtrate was concentrated by vacuum distillation to remove the solvent, and then freeze-dried (-40℃, 0.01 MPa) to obtain lithium-ionized Eriochrome Black T;
[0056] (S2) Dissolve 20g of lithium chromium black T in a mixed solvent of 5L water and acetonitrile (the volume ratio of water to acetonitrile is 7:3) to form a solution. Add 600g of porous carbon to the solution and impregnate the solution by stirring at 200rpm at 50℃ for 2h. After impregnation, separate the solid and liquid components. Dry the solid at 80℃ for 12h to obtain composite porous carbon with a lithium chromium black T loading of 2.1wt% (determined by the weight gain method).
[0057] (S3) Same as Example 1.
[0058] Example 5
[0059] The rest is the same as in Example 1, except that: in step (S1), lithium chloride (LiCl) is used instead of lithium hydroxide monohydrate (LiOH·H2O); and a mixed solvent of water and DMF (volume ratio of water to DMF is 8:2) is used instead of a mixed solvent of water and acetonitrile (volume ratio of water to acetonitrile is 7:3); specifically:
[0060] (S1) Add 20g of methyl orange to a mixed solvent of 5 L of water and DMF (water to DMF volume ratio of 8:2), stir and heat to 45℃ to completely dissolve the methyl orange, obtaining a homogeneous methyl orange solution; then add 3.88g of LiCl (i.e., Na from methyl orange) to the solution. + Li with LiCl + With a molar ratio of 1:1.5, the system was heated to 70°C and refluxed for 5 h under a nitrogen atmosphere to complete the Na+ extraction from methyl orange. + With Li + The ion exchange reaction was carried out; after the reaction was completed, DMF was added to make the volume fraction of DMF in the mixed solvent 85%, and the mixture was stirred for 15 min. At this time, NaCl precipitated out, while lithium methyl orange remained in the liquid phase; then the mixture was filtered under vacuum of -0.095 MPa to remove the precipitated NaCl. Finally, the filtrate was concentrated by vacuum distillation to remove the solvent, and then freeze-dried (-40℃, 0.01 MPa) to obtain lithium methyl orange.
[0061] (S2) 20g of lithium methyl orange was dissolved in a mixed solvent of 5 L water and DMF (the volume ratio of water to DMF was 8:2) to form a solution. 600g of porous carbon was added to the solution and impregnated by stirring at 200 rpm at 50°C for 2 h. After impregnation, the solid and liquid were separated and the solid was dried at 80°C for 12 h to obtain composite porous carbon with a lithium methyl orange loading of 2.3 wt% (determined by the weight gain method).
[0062] (S3) Same as Example 1.
[0063] Example 6
[0064] The rest is the same as in Example 1, except that the impregnation conditions in step (S2) are different, specifically:
[0065] (S1) Same as Example 1;
[0066] (S2) 25g of lithium methyl orange was dissolved in a mixed solvent of 5.5 L of water and acetonitrile (the volume ratio of water to acetonitrile was 7:3) to form a solution. 600g of porous carbon was added to the solution and impregnated by stirring at 200 rpm at 50°C for 3 h. After impregnation, the solid and liquid were separated. The solid was dried at 80°C for 12 h to obtain composite porous carbon with a lithium methyl orange loading of 3.0 wt% (determined by the weight gain method).
[0067] (S3) Same as Example 1.
[0068] Example 7
[0069] The rest is the same as in Example 1, except that the impregnation conditions in step (S2) are different, specifically:
[0070] (S1) Same as Example 1;
[0071] (S2) 32g of lithium methyl orange was dissolved in a mixed solvent of 6L water and acetonitrile (the volume ratio of water to acetonitrile was 7:3) to form a solution. 600g of porous carbon was added to the solution and the mixture was stirred at 200rpm at 55℃ for 4h for impregnation treatment. After impregnation, the solid and liquid were separated. The solid was dried at 80℃ for 12h to obtain composite porous carbon with a lithium methyl orange loading of 4.1wt% (determined by the weight gain method).
[0072] (S3) Same as Example 1.
[0073] Comparative Example 1
[0074] The rest is the same as in Example 1, except that step (S1) is omitted, that is, methyl orange is used directly for impregnation without lithium treatment. Specifically:
[0075] (S1) Omitted;
[0076] (S2) Dissolve 20g of methyl orange in a mixed solvent of 5L water and acetonitrile (the volume ratio of water to acetonitrile is 7:3) to form a solution. Add 600g of porous carbon to the solution and impregnate the solution by stirring at 200rpm at 50℃ for 2h. After impregnation, separate the solid and liquid components. Dry the solid at 80℃ for 12h to obtain composite porous carbon with a methyl orange loading of 2.1wt% (determined by the weight gain method).
[0077] (S3) Same as Example 1.
[0078] Comparative Example 2
[0079] The rest is the same as in Example 1, except that in step (S1), Alizarin Red S (sodium salt of 1,2-dihydroxy-9,10-dioxo-anthracene-3-sulfonate, i.e., anthraquinone sulfonate dye, non-azo dye) is used in place of methyl orange in equimolar amounts (based on sodium element). Specifically:
[0080] (S1) Add 20g of Alizarin Red S to a mixed solvent of 5L water and acetonitrile (the volume ratio of water to acetonitrile is 7:3), stir and heat to 45℃ to completely dissolve Alizarin Red S, obtaining a homogeneous Alizarin Red S solution; then add 3.68g of LiOH·H2O (i.e., Na+ in Alizarin Red S) to the solution. + Li with LiOH·H2O + With a molar ratio of 1:1.5, the system was heated to 75°C and refluxed for 6 hours under a nitrogen atmosphere to complete the Na content in Alizarin Red S. + With Li + The reaction involved an ion exchange reaction. After the reaction was complete, dry CO2 gas was slowly introduced into the reaction solution, and the reaction was stirred until the pH of the system reached 10.5, completely converting the byproduct NaOH into Na2CO3. Acetonitrile was then added to make the volume fraction of acetonitrile in the mixed solvent 85%, and the mixture was stirred for 15 min. At this point, Na2CO3 precipitated out, while Alizarin Red S remained in the liquid phase. The mixture was then filtered under a vacuum of -0.095 MPa to remove the precipitated Na2CO3. Finally, the filtrate was concentrated by vacuum distillation to remove the solvent, and then freeze-dried (-40℃, 0.01 MPa) to obtain lithium Alizarin Red S.
[0081] (S2) 20g of lithium alizarin red S was dissolved in a mixed solvent of 5 L of water and acetonitrile (the volume ratio of water to acetonitrile was 7:3) to form a solution. 600g of porous carbon was added to the solution and impregnated by stirring at 200 rpm at 60°C for 2 h. After impregnation, the solid and liquid were separated. The solid was dried at 80°C for 12 h to obtain composite porous carbon with a lithium alizarin red S loading of 2.2 wt% (determined by the weight gain method).
[0082] (S3) Same as Example 1.
[0083] Comparative Example 3
[0084] The rest is the same as in Example 1, except that the impregnation conditions in step (S2) are different, and the loading of lithium dye is too high, specifically:
[0085] (S1) Same as Example 1;
[0086] (S2) 40g of lithium methyl orange was dissolved in a mixed solvent of 6.5L water and acetonitrile (the volume ratio of water to acetonitrile was 7:3) to form a solution. 600g of porous carbon was added to the solution and the mixture was stirred at 200rpm at 55℃ for 4h for impregnation treatment. After impregnation, the solid and liquid were separated. The solid was dried at 80℃ for 12h to obtain composite porous carbon with a lithium methyl orange loading of 5.3wt% (determined by the weight gain method).
[0087] (S3) Same as Example 1.
[0088] Comparative Example 4
[0089] The rest is the same as in Example 1, except that the impregnation conditions in step (S2) are different, and the loading of lithium dye is too low, specifically:
[0090] (S1) Same as Example 1;
[0091] (S2) 20g of lithium methyl orange was dissolved in a mixed solvent of 5L water and acetonitrile (the volume ratio of water to acetonitrile was 7:3) to form a solution. 600g of porous carbon was added to the solution and impregnated by stirring at 200rpm for 1h at 50℃. After impregnation, the solid and liquid were separated and the solid was dried at 80℃ for 12h to obtain composite porous carbon with a lithium methyl orange loading of 1.1wt% (determined by the weight gain method).
[0092] (S3) Same as Example 1.
[0093] Application examples
[0094] The modified porous carbon prepared in the examples and comparative examples was subjected to silicon and carbon vapor deposition to obtain silicon-carbon anode materials. Taking Example 1 as an example, the specific method is as follows: 1000g of the prepared space-selectively modified porous carbon was placed in a tube rotary furnace at a rotation speed of 50 r / min. Nitrogen gas was introduced at a flow rate of 10 L / min. Under nitrogen atmosphere, the temperature was raised to 500℃ at a heating rate of 5℃ / min. The nitrogen flow rate was maintained and silane (SiH4) gas was introduced at a flow rate of 2.5 L / min for chemical vapor deposition for 5h. Silane decomposed to form nano-silicon deposited in the pores of the porous carbon. After the deposition was completed, the silane gas was stopped, and nitrogen gas was continuously introduced at a flow rate of 5 L / min to remove excess silane gas. Then, acetylene gas was introduced at a flow rate of 1.5 L / min and the temperature was maintained at 550℃ for vapor deposition for 2.5h. After the acetylene gas decomposed, a carbon coating layer was formed, and the silicon-carbon anode material was obtained. The modified porous carbon obtained in other examples and comparative examples were used to replace the modified porous carbon in Example 1 to prepare corresponding silicon-carbon anode materials.
[0095] Testing and Analysis
[0096] 1) Performance testing of space-selectively modified porous carbon
[0097] Microstructure and elemental distribution characterization: The modified porous carbon prepared in Example 1 was characterized by scanning electron microscopy (SEM) combined with energy dispersive spectroscopy (EDS) for micromorphological morphology and elemental distribution analysis. The SEM images and S-element mapping diagrams are shown below. Figure 1 As shown.
[0098] Specific surface area and pore size distribution determination: According to GB / T 19587-2017 Gas Adsorption BET Method, a Tristar II 3020 fully automated specific surface area and pore size analyzer (Micromeritics Instrument Corporation, USA) was used to conduct low-temperature nitrogen adsorption experiments on the modified porous carbon prepared in the examples and comparative examples to determine their specific surface area, pore size distribution, and pore volume. The nitrogen adsorption-desorption comparison curves of the spatially selectively modified porous carbon prepared in Example 1 and the raw material porous carbon are shown below. Figure 2 As shown in Table 1, the specific data for each embodiment and comparative example are as follows.
[0099] Table 1. Pore size distribution, pore volume, and specific surface area of modified porous carbon
[0100]
[0101] As shown in Table 1, the porous carbon modified by the method of the present invention exhibits changes in pore size distribution, pore volume, and specific surface area. Compared to the raw porous carbon, the proportion of micropores in the examples and comparative examples generally increases, while the proportion of mesopores decreases accordingly. This indicates that dye molecules are mainly adsorbed within the mesopores of the porous carbon, especially dyes with smaller molecular sizes (such as those in Examples 1 and 2), which have a more significant impact on the mesopores. Simultaneously, the pore volume decreases after dye adsorption, and this decrease is related to the dye molecule size and adsorption amount. The larger decrease in pore volume in Example 1 may be due to the smaller molecular size of lithium-ion methyl orange compared to the lithium-ion dyes in the other examples, thus making it easier for the molecule to occupy the mesopore channels. Correspondingly, the specific surface area increases slightly with the change in the proportion of micropores.
[0102] A comparison of Examples 1, 6-7, and Comparative Examples 3-4 shows that the pore volume gradually decreases as the amount of lithium dye increases; however, the proportion of mesopores and the pore volume of Comparative Example 3 decrease too much, indicating that the excessive loading of lithium dye causes severe mesopore blockage, which will affect subsequent silicon deposition and hinder ion transport; the proportion of mesopores and the pore volume of Comparative Example 4 change little, possibly because the loading of lithium dye is too low, making it difficult to form an effective functional interface layer.
[0103] Although the changes in pore size distribution in Comparative Examples 1 and 2 were basically consistent with those in the Examples, their subsequent electrochemical performance was poor (see Table 2 for details). This shows that changes in pore structure alone are not the only factor in performance improvement; interfacial chemical composition (the synergistic effect of Li, N, and S) is also crucial.
[0104] 2) Performance testing of silicon-carbon anode materials
[0105] The silicon-carbon anode materials prepared in the above application examples and comparative application examples were used as anodes in lithium-ion batteries, assembled into lithium batteries, and their electrochemical performance was tested. Specifically, the silicon-carbon composite anode material was mixed with polyacrylic acid (PAA) and conductive carbon black (Super P) in a mass ratio of 8:1:1, ground into a slurry using deionized water as a solvent, and then uniformly coated onto copper foil, controlling the wet film thickness to be 200 μm. The material was then vacuum dried at 80°C for 12 hours, and the dried material was punched into 12 mm electrode sheets. In an argon glove box, a lithium metal sheet was used as the counter electrode, Celgard 2600 as the separator, and a 1 M LiPF6 solution was selected as the electrolyte. The solvent was prepared at a volume ratio of ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1, and 25% fluoroethylene carbonate (FEC) was added as an additive. Finally, a CR2032 button cell was assembled. Charge-discharge tests were conducted using the Landon CT2001A test system at a voltage range of 0.01~1.5 V and a current density of 100 mA / g. The test results are shown in Table 2.
[0106] Table 2 Performance Tests
[0107]
[0108] Table 2 shows that the carbon anode material prepared by the porous carbon modified by the method of the present invention is significantly better than the comparative examples in terms of initial coulombic efficiency (ICE) and cycle stability. The initial coulombic efficiency (1.5V) of the examples is above 94%, and the capacity retention rate after 100 cycles at 0.5C is above 90%, showing good cycle stability. In contrast, Comparative Example 1, due to the lack of pre-placed lithium source to compensate for the initial irreversible lithium consumption because the dye is not lithiated, shows a significant decrease in initial coulombic efficiency and capacity retention rate. The dye used in Comparative Example 2 is an anthraquinone sulfonate dye, a non-azo dye, i.e., it does not contain nitrogen, and its initial coulombic efficiency and capacity retention rate are also worse than the examples. Comparative Example 3 (with excessively high lithiated dye loading) has poor initial coulombic efficiency and capacity retention rate. Based on the data in Table 1, it can be inferred that the main reason is severe mesopore blockage, which hinders silicon deposition and ion transport. Comparative Example 4 (with insufficient lithium dye loading) showed better initial coulombic efficiency and capacity retention than Comparative Examples 1 and 2, but significantly lower than the Example. This may be due to the insufficient lithium dye loading causing discontinuity in the functional interface layer. Therefore, selecting appropriate lithium dyes and controlling their dosage is key to achieving synergistic optimization of pore structure and surface functionalization. This can effectively reduce irreversible lithium consumption in the first cycle while maintaining pore connectivity, thereby significantly improving the energy efficiency and cycle life of porous carbon anode materials.
Claims
1. A method for preparing spatially selectively modified porous carbon, characterized in that, Includes the following steps: (S1) Dissolve sulfonate aromatic azo dyes in a mixed solvent of water and polar aprotic organic solvent to form solution A. Add a soluble lithium source to solution A under an inert atmosphere. After dissolution, heat the solution to carry out an ion exchange reaction. After the reaction is completed, the solution is purified to obtain lithium dyes. (S2) Lithium-ionized dye is dissolved in a mixed solvent of water and a polar aprotic organic solvent to form solution B. Porous carbon is then impregnated in solution B to obtain composite porous carbon. By controlling the impregnation conditions, the loading of lithium-ionized dye is made to be 2-4 wt%. (S3) The composite porous carbon was heat-treated under an inert atmosphere to obtain spatially selectively modified porous carbon.
2. The preparation method according to claim 1, characterized in that, In step (S1), the sulfonate aromatic azo dye is selected from at least one of methyl orange, Congo red, orange yellow I, and chrome black T, preferably methyl orange or orange yellow I; the soluble lithium source is selected from at least one of lithium chloride (LiCl), lithium hydroxide (LiOH), and lithium hydroxide hydrate.
3. The preparation method according to claim 1, characterized in that, In step (S1), the Na in the sulfonate aromatic azo dye + With Li in the lithium source + The molar ratio is 1:1.5~3, preferably 1:1.5~2.
4. The preparation method according to claim 1, characterized in that, In steps (S1) and (S2), the volume ratio of water to polar aprotic solvent in the mixed solvent is 7:3 to 8:
2. The polar aprotic solvent is selected from at least one of acetonitrile, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO). The concentration of solution A is 0.2 to 0.8 wt%. The inert atmosphere is nitrogen and / or argon. The temperature is raised to 70 to 80°C, and the ion exchange reaction time is 4 to 8 hours.
5. The preparation method according to claim 1, characterized in that, The purification process in step (S1) varies depending on the lithium source: When the lithium source is lithium chloride (LiCl), a polar aprotic solvent is added to the reaction solution to make the volume fraction of the polar aprotic solvent in the mixed solvent ≥ 85%. At this time, the byproduct NaCl precipitate is precipitated, and the lithium dye is retained in the liquid phase. After removing the precipitate by filtration, the filtrate is concentrated by vacuum distillation and freeze-dried to obtain lithium dye powder. When the lithium source is lithium hydroxide (LiOH) or lithium hydroxide hydrate, CO2 gas is first introduced into the reaction solution until the pH of the system is 10~11, so that the byproduct NaOH is converted into Na2CO3. Then, a polar aprotic solvent is added to make the volume fraction of the polar aprotic solvent in the mixed solvent ≥ 85%. At this time, Na2CO3 precipitate is precipitated, and the lithium dye is retained in the liquid phase. After removing the precipitate by filtration, the filtrate is concentrated by vacuum distillation and freeze-dried to obtain lithium dye powder.
6. The preparation method according to claim 1, characterized in that, In step (S2), the BET specific surface area of the porous carbon is 1500~2500 m². 2 / g, with an average pore size of 1.4~2.5nm, based on the gas adsorption BET method, with micropores accounting for 60~90% and mesopores accounting for 10~30%.
7. The preparation method according to claim 1, characterized in that, In step (S2), the loading of the lithium dye is 2~3 wt%.
8. The preparation method according to claim 1, characterized in that, In step (S2), the concentration of solution B is 0.2~0.8wt%; the impregnation conditions are: porous carbon is impregnated in solution B at a solid-liquid ratio of 1g:5~20mL, at a temperature of 40~60℃, for 2~4h, and then dried at 80~100℃ for 6~12h to obtain composite porous carbon; and / or, In step (S3), the inert atmosphere is nitrogen and / or argon; the heat treatment conditions are: 700~850℃ for 1~3h.
9. A spatially selectively modified porous carbon, prepared by the preparation method according to any one of claims 1-8.
10. A silicon-carbon anode material, which is prepared by sequentially vapor-depositing silicon and carbon coating of porous carbon obtained by the preparation method according to any one of claims 1-8.