Curved ceramic heating sheet and method for manufacturing the same
Patent Information
- Application Number
- CN202611062433.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-16
- Publication Date
- 2026-10-09
AI Technical Summary
[0009]本发明的目的在于克服现有技术的上述缺陷,提供一种曲面陶瓷发热片及其制备方法,解决曲面薄壁多层陶瓷发热片烧结变形坍塌、电阻精度低、良率差的问题,实现高精度、高良率、可批量的曲面发热片制备
首先,本发明通过固定生片原料配比锁定烧结收缩率,搭配收缩率自适应弧形定型工装的组合设计,从根源上解决了曲面薄壁生片高温烧结坍塌、曲率偏移的核心缺陷,产品成型良率提升至90%以上。本发明的生片配方将烧结收缩率稳定控制在10%~15%区间,工装弧形定型面可计算出补偿曲率,消除原料波动带来的尺寸偏差;低温阶段采用梯度减速升温方式,可分步匀速脱除生片内部粘结剂、溶剂等有机组分,避免快速升温导致的生片鼓泡、表层开裂,同时完成陶瓷基体的初步固化,固定生片基础姿态。进入中温塑性区间后,氧化铝陶瓷生片进入软化可塑状态,配套曲率经过收缩补偿的弧形夹具可对生片施加均匀约束压力,配合石墨纸柔性垫片分散成型应力,精准锁定目标曲面形态,杜绝烧结收缩过程中的翘曲、褶皱与边缘裂纹,无需后续二次整形工序。
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ceramic heating element preparation technology, specifically relating to a curved ceramic heating element and its preparation method. It is particularly suitable for curved irregular-shaped alumina ceramic heating elements with a curvature radius of 10~20mm and a thickness of 0.3~1.0mm, and can be widely used in small household appliance temperature control, precision heating, industrial constant temperature equipment and other fields. Background Technology
[0002] Ceramic heating elements, with their uniform heating, good chemical stability, and long service life, have become core components in the field of precision heating. Currently, the manufacturing technology for planar ceramic heating elements is relatively mature, generally employing an integrated constant-temperature sintering process: the multi-layered ceramic green sheets, after printing and lamination, are directly placed into a high-temperature furnace, completing the entire process of glue removal, curing, and densification in one go. This process is simple to operate and suitable for the mass production of regular flat products, but it cannot meet the manufacturing needs of curved, thin-walled multi-layer heating elements because the latter presents challenges such as deformation and grain control during the sintering process.
[0003] To address issues such as deformation and grain control during ceramic sintering, the industry has developed several improved segmented sintering schemes. For example, Chinese patent application CN115073145A discloses a method for preparing alumina bulletproof ceramics, employing a low-speed sintering process with ten consecutive heating steps. By suppressing grain growth through slow sintering at low temperatures, it can prepare curved bulletproof ceramic inserts, improving structural strength and dimensional stability. However, this scheme only addresses the densification control of a single alumina ceramic matrix and does not consider the differentiated thermal reaction characteristics of multilayer functional slurries, thus failing to solve the problem of heating layer resistance accuracy. Furthermore, thin-walled curved green sheets are still prone to collapse and curvature shift, making this scheme unsuitable for meeting the high-precision fabrication requirements of curved heating elements.
[0004] For example, Chinese patent application CN121517233A discloses a sintering process for a silicon nitride ceramic framework, employing a three-stage decreasing heating mode of preheating-surface diffusion-high-temperature densification, coupled with a gradient degreasing process, which can improve the dimensional accuracy of the porous framework. However, this scheme is designed for high-melting-point silicon nitride porous structures, and the material system is completely incompatible with alumina-based multilayer heating elements; moreover, the core objective is to control the density of the porous framework, which cannot be directly applied to the preparation of ceramic heating elements.
[0005] Existing technologies present difficulties in fabricating curved thin-walled multilayer heating elements, especially for curved thin-walled multilayer ceramic heating elements with a curvature radius of 10-20 mm and a thickness of 0.3-1.0 mm. These products are characterized by large curvature and low thickness, which exacerbates the problems encountered during the sintering of curved ceramics. These problems mainly include: First, curved thin-walled green sheets suffer from severe softening, collapse, and deformation at high temperatures. These products have large curvatures and extremely thin walls, and the green sheets contain a large amount of organic binder. When traditional processes rapidly heat to the high-temperature range, the green sheets soften quickly and are easily affected by gravity, airflow, and shrinkage stress, making them highly susceptible to defects such as surface collapse, curvature shift, and warping wrinkles. The thin-walled structure results in significant stress concentration and is also prone to causing edge micro-cracks and interlayer cracking, directly leading to product scrap.
[0006] Secondly, the asynchronous thermal reactions of the multi-layer functional pastes lead to uncontrolled resistance precision. Curved ceramic heating elements comprise multiple layers, including a ceramic substrate layer, a tungsten-containing heating paste layer, an electrode layer, and a protective glaze layer. The glass transition temperature and densification temperature of different pastes vary significantly. The traditional single-temperature process of printing first and then sintering as a whole cannot match the thermal reaction characteristics of each layer. In the low-temperature section, the paste is not fully cured; in the high-temperature section, the low-melting-point paste melts excessively; and the high-melting-point tungsten paste is prone to detachment due to thermal stress mismatch with the substrate. Ultimately, this results in large resistance deviations in the heating layer, a high risk of circuit breakage, and low temperature control precision, failing to meet the requirements of precision heating.
[0007] Third, the product yield is low, the process is cumbersome, and the batch stability is poor. Traditional processes result in curved surface products that deform excessively after a single sintering, with over 90% of defective products requiring manual reshaping and polishing. This not only increases the number of processes and costs but also easily causes substrate damage and interlayer delamination. Furthermore, the precision of manual shaping is inconsistent, resulting in large parameter dispersion in batch products and poor process reproducibility.
[0008] In summary, the industry currently lacks solutions to address the issues of deformation and low product yield in curved thin-walled structures, making the production of curved multilayer ceramic heating elements extremely challenging. Summary of the Invention
[0009] The purpose of this invention is to overcome the above-mentioned defects of the prior art and provide a curved ceramic heating element and its preparation method, which solves the problems of sintering deformation and collapse, low resistance accuracy and poor yield of curved thin-walled multilayer ceramic heating elements, and realizes the preparation of curved heating elements with high precision, high yield and mass production capability.
[0010] The development of this invention began with targeted improvements to address the defects of existing monolithic sintering processes. The inventors initially proposed the core concept of segmented sintering, dividing the preparation process into three independent phase reaction stages based on the inherent nature of the sintering process of ceramic green sheets: organic component removal, plastic deformation bonding, and high-temperature densification fusion. This results in the thermal reaction peaks of the multilayer functional slurry being distributed across different temperature ranges. By breaking down the single high-temperature sintering process into multiple independently temperature-controlled process units, the material reaction characteristics of each stage can be matched, theoretically solving the problems of binder removal defects and low resistivity accuracy simultaneously.
[0011] However, after initial testing, the inventors discovered new technical challenges: using only segmented temperature control, thin-walled curved green sheets with a curvature radius of 10-20 mm and a thickness of 0.3-1.0 mm still experience defects such as surface collapse, curvature deviation, and edge cracks during the mid-temperature softening stage due to the combined effects of their own gravity and sintering shrinkage stress. This cannot be solved by simply optimizing the segmented temperature control parameters; instead, external force is needed to provide appropriate support to prevent deformation of the product during sintering. Furthermore, improper matching of heating rates at different stages further amplifies the stress concentration effect, preventing the full realization of the precision advantages of segmented temperature control. This indicates that a suitable temperature range and a suitable heating rate are as important as external support. Simultaneously, inconsistent raw material ratios in the green sheets lead to fluctuations in sintering shrinkage, directly affecting the curvature compensation accuracy of the shaping tooling and amplifying dimensional deviations. Since the heating circuitry in the printed sintering process is prone to deformation and detachment with the shrinkage of the substrate, large dimensional deviations in the product can make it difficult to guarantee resistance consistency.
[0012] To address the aforementioned multiple challenges, the inventors simultaneously iterated and optimized the process from three dimensions: formulation, tooling, and process. At the formulation level, they fixed the raw material composition and ratio range of the alumina green sheets, and fixed the sintering shrinkage rate range, providing a standardized basis for tooling curvature compensation. At the tooling level, they developed a high-temperature shaping fixture with adaptive shrinkage rate. This fixture locks the green sheet shape through a pre-set arc-shaped shaping surface with shrinkage compensation, and, combined with flexible graphite paper to disperse contact stress, buffers the adverse effects of shrinkage rate fluctuations between different batches of products, playing a crucial role in solving the deformation problem during curved surface heating. At the process level, they first completed low-temperature... Pre-firing and initial substrate shaping are followed by demolding, printing of tungsten-containing heating circuitry and functional layers, and then tooling. This process involves sequentially performing medium-temperature shaping and high-temperature densification sintering. This avoids the impact of volatile organic compounds from the substrate on circuit adhesion and uses segmented temperature control to match the thermal reaction characteristics of each layer of paste. The low-temperature segment employs a gradient-deceleration heating process to ensure uniform discharge of organic components without bubbling; the medium-temperature segment uses slow heating and long-term holding to fully release internal stress and achieve initial bonding and morphological locking between the circuitry and the substrate; the high-temperature segment appropriately increases the heating rate and shortens the high-temperature dwell time to prevent abnormal grain growth that could affect resistance accuracy. After repeated testing, a complete preparation scheme was finally formed, combining a fixed formula, shaping tooling, and segmented temperature control. The resulting curved ceramic heating element exhibits high molding yield, high resistance accuracy, and high long-term reliability, eliminating the need for subsequent secondary shaping and enabling stable mass production.
[0013] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a curved ceramic heating element, wherein the curved ceramic heating element has a radius of curvature of 10-20 mm and a thickness of 0.3-1.0 mm, and the preparation method includes the following steps: S1. Preparation of green sheets: Ceramic green sheets are made from the following raw materials in parts by weight: 100 parts of α-alumina ceramic powder, 3-6 parts of binder, 30-45 parts of solvent, 2-4 parts of plasticizer, and 0.5-1.5 parts of dispersant; the above raw materials are mixed evenly to form a ceramic slurry, which is then cast into green sheets. S2. Tooling Assembly: The tooling includes an alumina ceramic arc-shaped clamp and a graphite paper flexible gasket. The radius of curvature of the arc-shaped shaping surface of the clamp is equal to the radius of curvature of the target finished ceramic product × (1 - ceramic sintering shrinkage rate). The ceramic sintering shrinkage rate corresponds to the shrinkage that occurs during the sintering of the green sheet made from the ceramic slurry. The graphite paper flexible gasket is placed between the arc-shaped surface of the clamp and the green sheet. The tooling adopts an upper and lower mold clamping structure to hold the green sheet located in the center. S3. Atmosphere replacement: Place the entire fixture into the sintering furnace, continuously introduce nitrogen to replace the air in the furnace, and start the sintering program after the oxygen content in the furnace is detected to be ≤50ppm. S4. Low-temperature preheating section: The temperature is raised to 580~780℃ using a gradient heating mode and held for 50~70 minutes to complete the substrate removal and initial curing and shaping. S5. Demolding and Printing: After the low-temperature pre-firing is completed, the furnace is cooled to room temperature. The pre-firing substrate is demolded and removed. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are printed in sequence. After drying, the substrate is reinstalled into the tooling. S6. Medium-high temperature segmented sintering, including: Medium-temperature setting stage: The temperature is increased to 980~1120℃ at a heating rate of 0.9~1.6℃ / min and held for 70~130min to complete the interlayer bonding between the heating layer and the substrate; High-temperature fusion section: The temperature is increased to 1480~1580℃ at a heating rate of 4.5~7.5℃ / min and held for 100~140min to achieve dense fusion of the structure; S7. Cool and demold to obtain the target product.
[0014] Furthermore, the binder is polyvinyl butyral, the solvent is a mixture of anhydrous ethanol and xylene, the plasticizer is dibutyl phthalate (DBP), and the dispersant is trioleic acid glyceride; the sintering shrinkage rate of the ceramic is 10%~15%.
[0015] Furthermore, the gradient heating mode of the low-temperature preheating section is specifically as follows: the heating rate from room temperature to 500℃ is 2.2~2.8℃ / min, and the heating rate from 500℃ to the target holding temperature is 1.6~2.2℃ / min.
[0016] Furthermore, the holding time for the low-temperature preheating section is 60-70 minutes, the holding time for the medium-temperature setting section is 90-100 minutes, and the holding time for the high-temperature fusion section is 120-130 minutes.
[0017] Furthermore, the thickness of the graphite paper flexible gasket is 0.1~0.3mm, and the graphite paper flexible gasket is respectively disposed on the upper and lower surfaces of the green sheet.
[0018] Furthermore, the printing in S5 adopts screen printing, and after printing, it is dried at 75~85℃ for 25~35 minutes.
[0019] Furthermore, the S7 employs a gradient cooling method, including a cooling rate of 3~5℃ / min at the end of the high-temperature section to 1200℃, and natural cooling with the furnace below 1200℃.
[0020] The present invention also protects the curved ceramic heating element prepared by the method described above.
[0021] Furthermore, the molding yield of the heating element exceeds 90%, and the resistance deviation of more than 90% of the products is ≤±2%.
[0022] Furthermore, after 500 cycles of heating and cooling at 20℃~150℃, the resistance drift rate of the heating element is ≤3%.
[0023] Beneficial effects Firstly, this invention addresses the core defects of high-temperature sintering collapse and curvature deviation in curved thin-walled green sheets by fixing the raw material ratio and combining it with an adaptive arc-shaped shaping fixture. This fundamentally improves the product forming yield to over 90%. The green sheet formulation of this invention stably controls the sintering shrinkage rate within the range of 10% to 15%. The arc-shaped shaping surface of the fixture can calculate and compensate for curvature, eliminating dimensional deviations caused by raw material fluctuations. In the low-temperature stage, a gradient deceleration heating method is used to remove organic components such as binders and solvents from the green sheet in a step-by-step and uniform manner, avoiding bubbling and surface cracking caused by rapid heating. Simultaneously, it completes the initial curing of the ceramic matrix and fixes the basic posture of the green sheet. After entering the medium-temperature plastic range, the alumina ceramic green sheet enters a softened and plastic state. The matching arc-shaped fixture with shrinkage compensation can apply uniform constraint pressure to the green sheet. With the help of the graphite paper flexible gasket to disperse the forming stress, the target curved surface shape is accurately locked, eliminating warping, wrinkles and edge cracks during the sintering shrinkage process, and eliminating the need for subsequent secondary shaping processes.
[0024] Secondly, this invention employs a process of "low-temperature substrate shaping - circuit printing - medium-high temperature sintering," combined with sintering at differentiated temperature ranges. This comprehensively considers the thermal reaction characteristics of multi-layer functional pastes, significantly improving the product's resistance accuracy and electrical consistency. In this invention, the low-temperature pre-firing stage first completes the full removal of the organic carrier from the substrate and the initial solidification of the ceramic phase. After pre-firing, there are no volatile residues in the substrate. At this stage, printing the tungsten-containing heating paste, electrodes, and protective glaze avoids circuit bubbling and misalignment caused by the adhesive removal process. The medium-temperature shaping stage matches the glass phase softening temperature, achieving initial bonding between the tungsten paste layer and the ceramic substrate, fixing the heating circuit shape. The high-temperature fusion stage matches the densification temperature of the alumina substrate and the tungsten metal paste, allowing each layer of material to complete the reaction and sintering within the optimal temperature range. This avoids the problems of excessive melting and volatilization of low-melting-point pastes and insufficient densification of high-melting-point pastes, ultimately controlling the resistance deviation of the heating layer within ±2%, meeting the temperature control requirements for precision heating.
[0025] Furthermore, this invention employs a differentiated heating rate control logic of "deceleration at medium and low temperatures and acceleration at high temperatures," ensuring both product performance and production efficiency. Specifically, the slow heating at medium and low temperatures fully releases internal stress and ensures the quality of binder removal and shaping; while the increased heating rate at high temperatures during densification allows for rapid passage through the sensitive temperature range for abnormal grain growth, suppressing excessive growth of ceramic grains and the metallic phase. This ensures both matrix density and bonding strength, while avoiding the decline in mechanical properties caused by coarse grains. Simultaneously, it effectively shortens the high-temperature sintering cycle, reducing production energy consumption and time costs.
[0026] Furthermore, this invention significantly improves the long-term reliability of the product through the synergistic effect of a fully inert, low-oxygen atmosphere and a segmented sintering process. Full-process nitrogen protection controls the oxygen content in the furnace to below 50 ppm, preventing the oxidation and failure of tungsten, silver, and other metal heating pastes at high temperatures, thus ensuring the long-term stability of the heating layer's resistance. Combined with a segmented stress-relieving sintering process, the product has no residual internal stress, stable dimensions, and significantly improved thermal shock resistance. After 500 cycles of thermal cycling from -20℃ to 150℃, the resistance drift can be controlled within 3%, with no cracking or failure, significantly extending the service life.
[0027] In summary, this invention breaks through the limitations of traditional ceramic sintering processes and solves multiple technical problems such as curved surface structure forming, multi-layer slurry matching, and balancing production efficiency and reliability. Compared with existing technologies, it has made significant and substantial progress and has high industrial application value. Detailed Implementation
[0028] The present invention will be further described in detail below with reference to specific embodiments. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or the product instructions; where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be obtained commercially. In the following embodiments, unless otherwise specified, "%" refers to weight percentage.
[0029] All test samples in the embodiments and comparative examples of this invention are uniformly multi-layer curved ceramic heating elements. The finished product structure consists of an alumina ceramic substrate layer, a tungsten-containing heating paste layer, a silver electrode layer, and an insulating protective glaze layer. The ceramic raw sheet is made from the following raw materials in parts by weight: 100 parts of α-alumina ceramic powder, 3-6 parts of binder, 30-45 parts of solvent, 2-4 parts of plasticizer, and 0.5-1.5 parts of dispersant. The binder is polyvinyl butyral, and the solvent is a mixture of anhydrous ethanol and xylene. According to the test, the above formula, using the segmented heating process of this invention, corresponds to a ceramic sintering shrinkage rate of 10%-15%. In specific embodiments, the shrinkage rate varies within the above range depending on the slight adjustment of the formula.
[0030] The following methods were used for product testing: Curvature dimensional deviation test: The curvature radius of the finished product is measured using a coordinate measuring machine, and the average dimensional deviation is statistically analyzed.
[0031] Molding yield test: 10 samples are randomly selected. The samples are qualified if there is no collapse, deformation, warping, edge cracks, or delamination between layers, and the absolute value of the curvature radius deviation is ≤0.3mm. The yield rate is then calculated.
[0032] Resistance accuracy test: A high-precision multimeter is used to test the resistance value at room temperature. The absolute value of the resistance deviation is ≤2% to be considered qualified. The pass rate is calculated.
[0033] Thermal cycling reliability test: Perform 500 cycles of thermal cycling from -20℃ to 150℃. Calculate the resistance drift rate based on the change in resistance value before and after the test: the absolute value of the change in resistance value / the original resistance value.
[0034] Example 1 The target product in this embodiment is a curved ceramic heating element with a curvature radius of 15mm and a thickness of 0.6mm. The preparation steps are as follows: S1. Preparation of green sheets: Weigh the raw materials according to the following proportions by weight: 100 parts of α-alumina ceramic powder, 4.5 parts of polyvinyl butyral (PVB) binder, 25 parts of anhydrous ethanol, 12 parts of xylene, 3 parts of dibutyl phthalate (DBP) plasticizer, and 1 part of trioleic acid glyceride dispersant. Mix the above raw materials and place them in a ball mill jar. Use zirconia balls as the grinding medium and ball mill for 24 hours to obtain a uniform and stable ceramic slurry. After vacuum degassing, prepare 0.6 mm thick ceramic substrates through a casting machine. Cut the substrates into curved green sheets of the target size and remove edge burrs. The ceramic sintering shrinkage rate corresponding to this formula is 12%.
[0035] S2. Tooling Assembly: Select an alumina ceramic arc-shaped fixture. Based on a sintering shrinkage rate of 12%, calculate the radius of curvature of the arc-shaped shaping surface of the fixture as 15mm × (1-12%) = 13.2mm. Place the fixture on the arc-shaped surface of the lower mold, and then lay a 0.2mm thick graphite paper flexible gasket on the fixture. Dry it at high temperature to remove impurities and ensure that the gasket is free of bubbles and wrinkles. Place the curved green sheet precisely against the gasket, close the upper mold, and apply uniform micro-pressure through the fixing buckle to confirm that the green sheet is free of displacement and wrinkles.
[0036] S3. Atmosphere Replacement: Place the entire fixture into the high-temperature atmosphere sintering furnace, continuously introduce high-purity nitrogen to replace the air in the furnace, and start the sintering process after detecting that the oxygen content in the furnace is ≤50ppm.
[0037] S4. Low-temperature preheating section: Gradient heating mode is used to complete the glue removal and preliminary curing: the heating rate from room temperature to 500℃ is 2.5℃ / min, the heating rate from 500℃ to 700℃ is 2℃ / min, and the temperature is held at 700℃ for 60 minutes to complete the gradient glue removal and preliminary curing and shaping of the green sheet.
[0038] S5. Demolding and Printing: After low-temperature pre-firing, the substrate is cooled to room temperature in the furnace. The tooling is removed and the substrate is demolded. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are sequentially printed on the surface of the pre-fired ceramic substrate by screen printing. After printing, the substrate is placed in an 80℃ oven to dry for 30 minutes to remove the solvent components in the paste. After drying, the printed side is facing up, and the graphite paper gasket is reattached and installed into the arc-shaped fixture in the same way as before. The mold is closed and the buckle is fixed to ensure there is no offset.
[0039] S6. Medium and high temperature segmented sintering: (1) Medium temperature shaping section: High-purity nitrogen gas is introduced again to replace the air in the furnace. After the oxygen content is ≤50ppm, the temperature is raised to 1050℃ at a rate of 1.2℃ / min and held for 90min. The target curvature is locked by tooling to fully release the structural stress and complete the initial interlayer bonding between the heating layer and the substrate. (2) High temperature fusion section: The temperature is raised to 1530℃ at a rate of 6℃ / min and held for 120min to achieve dense fusion of the multilayer structure.
[0040] S7. Cooling and Demolding: After sintering, the temperature is gradually reduced from 1530℃ to 1200℃ at a rate of 4℃ / min. The temperature is then allowed to cool naturally to room temperature below 1200℃. The tooling is then removed and the finished product is obtained.
[0041] In this embodiment, gradient heating and glue removal can prevent the raw film from bubbling and collapsing, pre-setting before printing can ensure the stability of the circuit shape, medium-temperature slow heat preservation can fully release stress and ensure the setting accuracy, and high-temperature medium-speed heating can balance densification and production efficiency.
[0042] Example 2 The target product in this embodiment is a curved ceramic heating element with a radius of curvature of 12mm and a thickness of 0.4mm. The preparation steps are as follows: S1. Preparation of green sheets: Weigh the raw materials according to the following proportions by weight: 100 parts of α-alumina ceramic powder, 3.5 parts of polyvinyl butyral (PVB) binder, 22 parts of anhydrous ethanol, 10 parts of xylene, 2.5 parts of dibutyl phthalate (DBP) plasticizer, and 0.8 parts of trioleic acid glyceride dispersant. Mix the above raw materials and place them in a ball mill jar. Use zirconia balls as the grinding medium and ball mill for 26 hours to obtain a uniform and stable ceramic slurry. After vacuum degassing, prepare 0.4 mm thick ceramic substrates through a casting machine. Cut the substrates into curved green sheets of the target size and remove edge burrs. The ceramic sintering shrinkage rate corresponding to this formula is 11%.
[0043] S2. Tooling Assembly: Alumina ceramic arc-shaped fixtures are selected. Based on the sintering shrinkage rate of 11%, the radius of curvature of the arc-shaped shaping surface of the fixture is calculated to be 12mm × (1-11%) = 10.68mm. A 0.15mm thick graphite paper flexible gasket is laid on the arc-shaped surface of the lower mold using a vacuum bonding process to completely eliminate air bubbles and ensure uniform pressure distribution. The curved green sheet is precisely placed in accordance with the gasket. After the mold is closed, uniform micro-pressure is applied through the fixing buckle to confirm that the green sheet has no displacement or wrinkles.
[0044] S3. Atmosphere Replacement: Place the entire fixture into the high-temperature atmosphere sintering furnace, continuously introduce high-purity nitrogen to replace the air in the furnace, and start the sintering process after detecting that the oxygen content in the furnace is ≤40ppm.
[0045] S4. Low-temperature preheating section: Gradient heating mode is used to complete the glue removal and preliminary curing: the heating rate from room temperature to 500℃ is 2.2℃ / min, the heating rate from 500℃ to 680℃ is 1.8℃ / min, and the temperature is held at 680℃ for 70 minutes. The low-speed gradient fully removes the glue to avoid deformation caused by organic residue in the later stage.
[0046] S5. Demolding and Printing: After low-temperature pre-firing, the substrate is cooled to room temperature in the furnace. The tooling is removed and the substrate is demolded. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are sequentially printed on the surface of the pre-fired ceramic substrate by screen printing. After printing, the substrate is placed in a 75°C oven to dry for 35 minutes to remove the solvent components in the paste. After drying, the printed side is facing up, and the graphite paper gasket is accurately re-attached and installed into the arc-shaped fixture. The mold is closed and the buckle is fixed to ensure there is no offset.
[0047] S6. Medium-high temperature segmented sintering: (1) Medium temperature shaping section: High-purity nitrogen gas is introduced again to replace the air in the furnace. After the oxygen content is ≤40ppm, the temperature is raised to 1020℃ at a rate of 0.9℃ / min and held for 120min. The ultra-long slow holding fully releases the internal stress of the thin-walled structure and accurately locks the curvature size of the curved surface and the shape of the heating circuit.
[0048] (2) High temperature fusion section: The temperature is increased to 1500℃ at a rate of 5℃ / min and held for 140min. The low temperature and long time densification matches the thermal reaction characteristics of fine tungsten paste to maximize the improvement of resistance accuracy.
[0049] S7. Cooling and Demolding: After sintering, the temperature is gradually reduced from 1500℃ to 1200℃ at a rate of 3℃ / min. The temperature is then allowed to cool naturally to room temperature below 1200℃. The tooling is then removed and the finished product is obtained.
[0050] This embodiment further improves dimensional accuracy and resistance consistency by using a lower heating rate, a longer holding time, and more uniform tooling pressure, thus meeting the needs of high-precision customized products.
[0051] Example 3 The target product in this embodiment is a curved ceramic heating element with a curvature radius of 18mm and a thickness of 0.8mm. The preparation steps are as follows: S1. Preparation of green sheets: Weigh the raw materials according to the following proportions by weight: 100 parts of α-alumina ceramic powder, 5.5 parts of polyvinyl butyral (PVB) binder, 28 parts of anhydrous ethanol, 14 parts of xylene, 3.5 parts of dibutyl phthalate (DBP) plasticizer, and 1.2 parts of trioleic acid glyceride dispersant. Mix the above raw materials and place them in a ball mill jar. Use zirconia balls as the grinding medium and ball mill for 22 hours to obtain a uniform and stable ceramic slurry. After vacuum degassing, prepare 0.8 mm thick ceramic substrates through a casting machine. Cut the substrates into curved green sheets of the target size and remove edge burrs. The ceramic sintering shrinkage rate corresponding to this formula is 14%.
[0052] S2. Tooling Assembly: Alumina ceramic arc-shaped fixture is selected. Based on the sintering shrinkage rate of 14%, the radius of curvature of the arc-shaped shaping surface of the fixture is calculated to be 18mm×(1-14%)=15.48mm. A 0.25mm thick graphite paper flexible pad is laid flat on the arc-shaped surface of the lower mold and dried at high temperature to remove impurities. The curved green sheet is precisely placed in accordance with the pad. After the mold is closed, uniform micro pressure is applied through the fixing buckle to confirm that the green sheet has no displacement or wrinkles.
[0053] S3. Atmosphere Replacement: Place the entire fixture into a high-temperature atmosphere sintering furnace and continuously circulate high-purity nitrogen to ensure uniform temperature and atmosphere inside the furnace. After the oxygen content inside the furnace is detected to be ≤50ppm, start the sintering process.
[0054] S4. Low-temperature preheating section: The gradient heating mode is used to complete the glue removal and preliminary curing: the heating rate from room temperature to 500℃ is 2.8℃ / min, the heating rate from 500℃ to 720℃ is 2.2℃ / min, and the temperature is held at 720℃ for 50 minutes to quickly complete the glue removal and curing, shortening the early process cycle.
[0055] S5. Demolding and Printing: After low-temperature pre-firing, the substrate is cooled to room temperature in the furnace. The tooling is removed and the substrate is demolded. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are sequentially printed on the surface of the pre-fired ceramic substrate by screen printing. After printing, the substrate is placed in an 85℃ oven to dry for 25 minutes to remove the solvent components in the paste. After drying, the printed side is facing up, and the graphite paper gasket is accurately re-attached and installed into the arc-shaped fixture. The mold is closed and the buckle is fixed to ensure there is no offset.
[0056] S6. Medium-high temperature segmented sintering: (1) Medium temperature setting section: Recirculate high-purity nitrogen gas, and start heating after the oxygen content is ≤50ppm. Heat up to 1080℃ at a rate of 1.5℃ / min, and hold for 70min to quickly complete the morphological setting and interlayer bonding, thereby improving production efficiency.
[0057] (2) High temperature fusion section: The temperature is raised to 1560℃ at a rate of 7℃ / min and held for 100min. The high temperature and rapid dense fusion ensures performance while significantly shortening the sintering cycle.
[0058] S7. Cooling and Demolding: After sintering, the temperature is gradually reduced from 1560℃ to 1200℃ at a rate of 5℃ / min. The temperature is then allowed to cool naturally to room temperature below 1200℃. The tooling is then removed and the finished product is obtained.
[0059] This embodiment significantly shortens the sintering cycle while ensuring yield and accuracy by optimizing the heating rate and holding time, thus meeting the needs of large-scale industrial production.
[0060] Example 4 The target product in this embodiment is a curved ceramic heating element with a curvature radius of 15mm and a thickness of 0.6mm. The specific preparation steps are as follows: S1. Preparation of green sheets: Weigh the raw materials according to the following proportions by weight: 100 parts of α-alumina ceramic powder, 3 parts of polyvinyl butyral (PVB) binder, 20 parts of anhydrous ethanol, 10 parts of xylene, 2 parts of dibutyl phthalate (DBP) plasticizer, and 0.5 parts of trioleic acid glyceride dispersant. Mix the above raw materials and place them in a ball mill jar. Use zirconia balls as the grinding medium and ball mill for 24 hours to obtain a uniform and stable ceramic slurry. After vacuum degassing, prepare 0.6 mm thick ceramic substrates through a casting machine. Cut the substrates into curved green sheets of the target size and remove edge burrs. The ceramic sintering shrinkage rate corresponding to this formula is 10%.
[0061] S2. Tooling Assembly: Select an alumina ceramic arc-shaped fixture. Based on a sintering shrinkage rate of 10%, calculate the radius of curvature of the arc-shaped shaping surface of the fixture as 15mm × (1-10%) = 13.5mm. Lay a 0.2mm thick graphite paper flexible pad on the arc-shaped surface of the lower mold and dry it at high temperature to remove impurities. Place the curved green sheet precisely against the pad. After closing the mold, apply uniform micro-pressure through the fixing buckle to confirm that the green sheet has no displacement or wrinkles.
[0062] S3. Atmosphere Replacement: Place the entire fixture into the high-temperature atmosphere sintering furnace, continuously introduce high-purity nitrogen to replace the air in the furnace, and start the sintering process after detecting that the oxygen content in the furnace is ≤50ppm.
[0063] S4. Low-temperature preheating section: Gradient heating mode is used to complete the glue removal and preliminary curing: heating rate from room temperature to 500℃ is 2.2℃ / min, heating rate from 500℃ to 580℃ is 1.6℃ / min, and holding at 580℃ for 50min.
[0064] S5. Demolding and Printing: After low-temperature pre-firing, the substrate is cooled to room temperature in the furnace. The tooling is removed and the substrate is demolded. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are sequentially printed on the surface of the pre-fired ceramic substrate by screen printing. After printing, the substrate is placed in an 80℃ oven to dry for 30 minutes to remove the solvent components in the paste. After drying, the printed side is facing up, and the graphite paper gasket is accurately re-attached and installed into the arc-shaped fixture. The mold is closed and the buckle is fixed to ensure there is no offset.
[0065] S6. Medium-high temperature segmented sintering: (1) Medium temperature setting section: High-purity nitrogen gas is introduced again to replace the air in the furnace. After the oxygen content is ≤50ppm, the temperature is raised to 980℃ at a rate of 0.9℃ / min and held for 70min.
[0066] (2) High temperature fusion section: Heat to 1480℃ at a rate of 4.5℃ / min and hold for 100min.
[0067] S7. Cooling and Demolding: After sintering, the temperature is gradually reduced from 1480℃ to 1200℃ at a rate of 3℃ / min. The temperature is then allowed to cool naturally to room temperature below 1200℃. The tooling is then removed and the finished product is obtained.
[0068] Example 5 The target product in this embodiment is a curved ceramic heating element with a curvature radius of 15mm and a thickness of 0.6mm. The specific preparation steps are as follows: S1. Preparation of green sheets: Weigh the raw materials according to the following proportions by weight: 100 parts of α-alumina ceramic powder, 6 parts of polyvinyl butyral (PVB) binder, 30 parts of anhydrous ethanol, 15 parts of xylene, 4 parts of dibutyl phthalate (DBP) plasticizer, and 1.5 parts of trioleic acid glyceride dispersant. Mix the above raw materials and place them in a ball mill jar. Use zirconia balls as the grinding medium and ball mill for 24 hours to obtain a uniform and stable ceramic slurry. After vacuum degassing, prepare 0.6 mm thick ceramic substrates through a casting machine. Cut the substrates into curved green sheets of the target size and remove edge burrs. The ceramic sintering shrinkage rate corresponding to this formula is 15%.
[0069] S2. Tooling Assembly: Alumina ceramic arc-shaped fixture is selected. Based on the sintering shrinkage rate of 15%, the radius of curvature of the arc-shaped shaping surface of the fixture is calculated to be 15mm×(1-15%)=12.75mm. A 0.2mm thick graphite paper flexible pad is laid flat on the arc-shaped surface of the lower mold and dried at high temperature to remove impurities. The curved green sheet is precisely placed in accordance with the pad. After the mold is closed, uniform micro pressure is applied through the fixing buckle to confirm that the green sheet has no displacement or wrinkles.
[0070] S3. Atmosphere Replacement: Place the entire fixture into the high-temperature atmosphere sintering furnace, continuously introduce high-purity nitrogen to replace the air in the furnace, and start the sintering process after detecting that the oxygen content in the furnace is ≤50ppm.
[0071] S4. Low-temperature preheating section: Gradient heating mode is used to complete the glue removal and preliminary curing: heating rate from room temperature to 500℃ is 2.8℃ / min, heating rate from 500℃ to 780℃ is 2.2℃ / min, and holding at 780℃ for 70min.
[0072] S5. Demolding and Printing: After low-temperature pre-firing, the substrate is cooled to room temperature in the furnace. The tooling is removed and the substrate is demolded. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are sequentially printed on the surface of the pre-fired ceramic substrate by screen printing. After printing, the substrate is placed in an 80℃ oven to dry for 30 minutes to remove the solvent components in the paste. After drying, the printed side is facing up, and the graphite paper gasket is accurately re-attached and installed into the arc-shaped fixture. The mold is closed and the buckle is fixed to ensure there is no offset.
[0073] S6. Medium-high temperature segmented sintering: (1) Medium temperature setting section: High-purity nitrogen gas is introduced again to replace the air in the furnace. After the oxygen content is ≤50ppm, the temperature is raised to 1120℃ at a rate of 1.6℃ / min and held for 130min.
[0074] (2) High temperature fusion section: Heat to 1580℃ at a rate of 7.5℃ / min and hold for 140min.
[0075] S7. Cooling and Demolding: After sintering, the temperature is gradually reduced from 1580℃ to 1200℃ at a rate of 5℃ / min. The temperature is then allowed to cool naturally to room temperature below 1200℃. The tooling is then removed and the finished product is obtained.
[0076] Comparative Example 1 This comparative example omits the dedicated shaping tooling, but the remaining process parameters are the same as in Example 1. The specific preparation steps are as follows: S1. Preparation of raw sheet: Same as in Example 1, corresponding to a sintering shrinkage rate of 12%.
[0077] S2. Placement of raw sheets: Place the curved raw sheets directly on the firing plate (flat plate) of the sintering furnace, keeping a 2cm gap between the raw sheets, without clamps or graphite paper pads.
[0078] S3, Atmosphere replacement: Same as in Example 1.
[0079] S4, Low-temperature preheating section: The temperature, heating rate, and holding time parameters are the same as in Example 1.
[0080] S5. Circuit printing: After the low-temperature pre-firing is completed, the substrate is cooled to room temperature in the furnace. The substrate is then removed from the firing plate and printed sequentially with tungsten heating paste, silver electrode paste, and insulating protective glaze paste using the same process as in Example 1. After drying at 80°C for 30 minutes, the substrate is placed back flat on the firing plate.
[0081] S6, Medium-high temperature sintering: (1) Medium-temperature shaping section: The atmosphere parameters are the same as in Example 1, and the heating rate, holding temperature and time are the same as in Example 1. (2) High-temperature fusion section: The parameters are the same as in Example 1.
[0082] S7. Cooling and Removal: After sintering, the product is cooled to room temperature in the furnace and then removed directly.
[0083] Comparative Example 2 This comparative example omits the intermediate-temperature setting stage and retains only the low-temperature pre-firing and high-temperature fusion processes. All other parameters are consistent with Example 1. The specific preparation steps are as follows: S1. Preparation of raw sheet: Same as in Example 1, corresponding to a sintering shrinkage rate of 12%.
[0084] S2. Tooling assembly: Same as in Example 1.
[0085] S3, Atmosphere replacement: Same as in Example 1.
[0086] S4, Low-temperature preheating section: Parameters are the same as in Example 1.
[0087] S5. Demolding and printing: Same as in Example 1, after printing and drying, reinstall the tooling.
[0088] S6. High-temperature sintering: After the low-temperature holding period ends and the printing is re-mounted, the temperature is directly increased to 1530℃ at a rate of 6℃ / min and held for 120min. There is no intermediate-temperature setting stage.
[0089] S7. Cooling and demolding: Same as in Example 1.
[0090] Comparative Example 3 In this comparative example, the temperature of the temperature setting stage is 1200℃, and the remaining process parameters are completely consistent with those of Example 1. The specific preparation steps are as follows: S1. Preparation of raw sheet: Same as in Example 1, corresponding to a sintering shrinkage rate of 12%.
[0091] S2. Tooling assembly: Same as in Example 1.
[0092] S3, Atmosphere replacement: Same as in Example 1.
[0093] S4, Low-temperature preheating section: Parameters are the same as in Example 1.
[0094] S5. Demolding and printing: Same as in Example 1, after printing and drying, reinstall the tooling.
[0095] S6. Segmented sintering: (1) Medium temperature setting section: Heat to 1200℃ at a rate of 1.2℃ / min and hold for 90min.
[0096] (2) High-temperature fusion section: The parameters are the same as in Example 1.
[0097] S7. Cooling and demolding: Same as in Example 1.
[0098] Comparative Example 4 In this comparative example, the holding time for the medium-temperature setting stage is 30 minutes, and the remaining process parameters are completely consistent with those of Example 1. The specific preparation steps are as follows: S1. Preparation of raw sheet: Same as in Example 1, corresponding to a sintering shrinkage rate of 12%.
[0099] S2. Tooling assembly: Same as in Example 1.
[0100] S3, Atmosphere replacement: Same as in Example 1.
[0101] S4, Low-temperature preheating section: Parameters are the same as in Example 1.
[0102] S5. Demolding and printing: Same as in Example 1, after printing and drying, reinstall the tooling.
[0103] S6. Segmented sintering: (1) Medium temperature setting section: Heat to 1050℃ at a rate of 1.2℃ / min and hold for 30min.
[0104] (2) High-temperature fusion section: The parameters are the same as in Example 1.
[0105] S7. Cooling and demolding: Same as in Example 1.
[0106] The intermediate temperature setting and heat preservation time in this comparative example is insufficient and is not within the scope of protection of the independent claims of this invention. It is used to verify the impact of intermediate temperature heat preservation time on the setting effect and product performance.
[0107] Performance test results The performance test results of the examples and comparative examples are shown in the table below: Table 1 Performance Test Results
[0108] Test results show that the molding yield, resistance accuracy, and dimensional accuracy of Examples 1-3 are all at a high level; the performance of Examples 4-5 is slightly lower than that of Examples 1-3, but still far superior to the comparative examples; among the four comparative examples, Comparative Example 1 has a low product molding yield due to the lack of tooling fixtures for shaping, and suffers from large curvature radius deviation and large resistance drift, requiring secondary shaping to remove surface deformation, warping, edge cracks, and other defects; Comparative Example 2 uses two-stage sintering, lacking a mid-temperature shaping stage for stress release, resulting in poor curvature shaping effect, large curvature radius variation, and decreased bonding strength between ceramic and circuit, manifested as a high thermal cycling resistance drift rate; the temperature of the mid-temperature shaping stage in Comparative Example 3 is too high, and the holding time of the mid-temperature shaping stage in Comparative Example 4 is too short, both failing to achieve satisfactory shaping effects, resulting in a decrease in molding yield, resistance accuracy, and dimensional accuracy. The above fully verifies the necessity and integrity of the various technical features of this invention. Only when the operating steps, positioning fixtures, and process parameters are all present can the significant technical effects be realized.
[0109] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0110] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0111] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A method for preparing a curved ceramic heating element, characterized in that, The curved ceramic heating element has a radius of curvature of 10-20 mm and a thickness of 0.3-1.0 mm. The preparation method includes the following steps: S1. Preparation of green sheets: Ceramic green sheets are made from the following raw materials in parts by weight: 100 parts of α-alumina ceramic powder, 3-6 parts of binder, 30-45 parts of solvent, 2-4 parts of plasticizer, and 0.5-1.5 parts of dispersant; the above raw materials are mixed evenly to form a ceramic slurry, which is then cast into green sheets. S2. Tooling Assembly: The tooling includes an alumina ceramic arc-shaped clamp and a graphite paper flexible gasket. The radius of curvature of the arc-shaped shaping surface of the clamp is equal to the radius of curvature of the target finished ceramic product × (1 - ceramic sintering shrinkage rate). The ceramic sintering shrinkage rate corresponds to the shrinkage that occurs during the sintering of the green sheet made from the ceramic slurry. The graphite paper flexible gasket is placed between the arc-shaped surface of the clamp and the green sheet. The tooling adopts an upper and lower mold clamping structure to hold the green sheet located in the center. S3. Atmosphere replacement: Place the entire fixture into the sintering furnace, continuously introduce nitrogen to replace the air in the furnace, and start the sintering program after the oxygen content in the furnace is detected to be ≤50ppm. S4. Low-temperature preheating section: The temperature is raised to 580~780℃ using a gradient heating mode and held for 50~70 minutes to complete the substrate removal and initial curing and shaping. S5. Demolding and Printing: After the low-temperature pre-firing is completed, the furnace is cooled to room temperature. The pre-firing substrate is demolded and removed. Tungsten heating paste, silver electrode paste, and insulating protective glaze paste are printed in sequence. After drying, the substrate is reinstalled into the tooling. S6. Medium-high temperature segmented sintering, including: Medium-temperature setting stage: The temperature is increased to 980~1120℃ at a heating rate of 0.9~1.6℃ / min and held for 70~130min to complete the interlayer bonding between the heating layer and the substrate; High-temperature fusion section: The temperature is increased to 1480~1580℃ at a heating rate of 4.5~7.5℃ / min and held for 100~140min to achieve dense fusion of the structure; S7. Cool and demold to obtain the target product.
2. The method for preparing the curved ceramic heating element according to claim 1, characterized in that, The binder is polyvinyl butyral, the solvent is a mixture of anhydrous ethanol and xylene, the plasticizer is dibutyl phthalate (DBP), and the dispersant is trioleic acid glyceride; the sintering shrinkage rate of the ceramic is 10%~15%.
3. The method for preparing the curved ceramic heating element according to claim 1, characterized in that, The gradient heating mode of the low-temperature preheating section is as follows: the heating rate from room temperature to 500℃ is 2.2~2.8℃ / min, and the heating rate from 500℃ to the target holding temperature is 1.6~2.2℃ / min.
4. The method for preparing the curved ceramic heating element according to claim 3, characterized in that, The holding time for the low-temperature preheating section is 60-70 minutes, the holding time for the medium-temperature setting section is 90-100 minutes, and the holding time for the high-temperature fusion section is 120-130 minutes.
5. The method for preparing the curved ceramic heating element according to any one of claims 1-4, characterized in that, The thickness of the graphite paper flexible gasket is 0.1~0.3mm, and the graphite paper flexible gasket is respectively disposed on the upper and lower surfaces of the green sheet.
6. The method for preparing the curved ceramic heating element according to any one of claims 1-4, characterized in that, The printing in S5 uses screen printing. After printing, it is dried at 75~85℃ for 25~35 minutes.
7. The method for preparing the curved ceramic heating element according to claim 1, characterized in that, The S7 uses a gradient cooling method, including a cooling rate of 3~5℃ / min at the end of the high-temperature section to 1200℃, and natural cooling with the furnace below 1200℃.
8. The curved ceramic heating element prepared by the method according to any one of claims 1-7.
9. The curved ceramic heating element according to claim 8, characterized in that, The molding yield of the heating element exceeds 90%, and the resistance deviation of more than 90% of the products is ≤±2%.
10. The curved ceramic heating element according to claim 8 or 9, characterized in that, After 500 cycles of hot and cold cycling at 20℃~150℃, the resistance drift of the heating element is ≤3%.
Citation Information
Patent Citations
Alumina bulletproof ceramic and preparation method thereof
CN115073145A
3D printing photocuring forming method of silicon nitride ceramic skeleton
CN121517233A