A ternary rare earth composite fluorine selective nanofiltration membrane, its preparation method and application

By using a Zr-Ce-La ternary rare earth synergistic coordination system and a multi-layer gradient covalent integrated structure design of tannic acid-titanium chelate layer, the stability and antifouling problems of existing fluorine selective membranes in strong acid environments are solved, achieving high fluorine rejection rate and long-term antifouling nanofiltration membrane performance.

CN123102174APending Publication Date: 2026-11-17SHENZHEN SHANSHUI LE ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611610435.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing fluorine-selective membranes are difficult to adapt to the strongly acidic HF etching waste liquid in the cleaning process of photovoltaic silicon wafer manufacturing and the etching process of semiconductor wafers, resulting in membrane flux decay and fluorine rejection rate reduction. They are also susceptible to organic pollutants and are difficult to operate stably for a long time.

Method used

A modified ternary hybrid nanosphere is formed by hydrothermal reaction using a Zr-Ce-La ternary rare earth synergistic coordination system. Fluorine-containing alkylpiperazine comonomers are introduced during interfacial polymerization and combined with a tannic acid-titanium chelate layer to form a multi-layer gradient covalent integrated structure, achieving highly selective fluorine adsorption and anti-fouling performance.

Benefits of technology

It improves the membrane's fluoride rejection rate and resistance to interference from coexisting ions such as chloride and sulfate, reduces the impact of organic pollutants on the membrane, and ensures long-term stability and regenerability in strong acid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application relates to the field of special nanofiltration separation membrane materials for water treatment, specifically to a ternary rare-earth composite fluorine-selective nanofiltration membrane, its preparation method, and its application. The preparation method includes the following steps: base membrane activation, transition layer coating, preparation of modified ternary hybrid nanospheres, pre-loading, interfacial polymerization, and heat treatment. This application utilizes a multi-layered gradient covalent integrated structure design—"tannic acid-titanium chelate transition layer → modified ternary hybrid nanosphere functional layer → fluorinated polyamide separation layer"—with synergistic complementarity between layers, ultimately achieving a comprehensive performance breakthrough in high fluoride rejection rate, long-term resistance to lauryl alcohol pollution, resistance to strong hydrofluoric acid environments, and regeneration capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of special nanofiltration separation membrane materials for water treatment, specifically to a ternary rare earth composite fluorine selective nanofiltration membrane, its preparation method, and its application. Background Technology

[0002] The cleaning process in photovoltaic silicon wafer manufacturing and the etching process in semiconductor wafers involve the extensive use of hydrofluoric acid, NMP, and photoresist. Furthermore, cleaning agents commonly contain nonionic surfactants such as lauryl alcohol and lauryl alcohol polyoxyethylene ether, resulting in complex wastewater containing low pH (1-3), fluoride ions, organic surfactants, and photoresist. Existing fluoride-selective membranes often use a dopamine coating as an intermediate transition layer, combined with a physical blend of binary zirconium-cerium oxide powder into the polyamide layer. Dopamine is easily hydrolyzed and detached in strongly acidic HF etching wastewater with pH ≤ 3. Inorganic fillers only physically encapsulate the dopamine, leading to leaching and loss over long-term operation. The hydrophobic long chains of lauryl alcohol spread and adsorb on the membrane surface, simultaneously forming micelles that encapsulate zirconium-cerium adsorbed particles, obscuring fluoride coordination sites. This results in a flux decline of over 40% after 30 days of operation, and a precipitous drop in fluoride rejection rate. Summary of the Invention

[0003] To address the limitations of existing fluorine-selective membranes in handling wastewater generated during photovoltaic silicon wafer manufacturing processes and semiconductor wafer etching, this application provides a ternary rare-earth composite fluorine-selective nanofiltration membrane, its preparation method, and its applications.

[0004] In a first aspect, this application provides a method for preparing a ternary rare earth composite fluorine selective nanofiltration membrane, employing the following technical solution: A method for preparing a ternary rare earth composite fluorine selective nanofiltration membrane includes the following steps: Base membrane activation: The polyethersulfone ultrafiltration base membrane was activated by immersing it in sodium hydroxide solution, rinsing it, and then drying it to obtain the activated base membrane; Transition layer coating: Tannic acid and titanium tetrachloride are added to water and stirred to obtain a two-phase mixture; the activated base film is immersed in the two-phase mixture, then removed and allowed to stand to cure, and rinsed to obtain the initial coated activated base film; Preparation of modified ternary hybrid nanospheres: Zirconium oxychloride, cerium nitrate, and lanthanum nitrate were dissolved in water by stirring to obtain a three-phase mixture; then C3 sulfonate betaine was added to the three-phase mixture for hydrothermal reaction, cooled, filtered, washed, and then an aminosilane coupling agent was added and heated under reflux to obtain modified ternary hybrid nanospheres. Pre-loading: The modified ternary hybrid nanospheres are dispersed in water to form a dispersion, which is then loaded onto the initially coated activated base film using negative pressure filtration to obtain a pre-loaded activated base film; Interfacial polymerization: The preloaded activated base film is immersed in a piperazine aqueous solution, taken out, rinsed and dried, and then placed in an oil phase solution for reaction to obtain a polymerized activated base film; the oil phase solution is a solution of pyromellitic trimethylol chloride and fluorinated alkyl piperazine comonomer dissolved in n-hexane; Heat treatment: The polymerized activated base membrane is heated and then cooled and immersed in nitric acid solution. After rinsing, a ternary rare earth composite fluorine selective nanofiltration membrane is obtained.

[0005] By adopting the above technical solution, this application employs a Zr-Ce-La ternary rare earth synergistic coordination system. Zirconium oxychloride, cerium nitrate, and lanthanum nitrate are reacted hydrothermally to form ternary hybrid nanospheres. Zirconium, cerium, and lanthanum ions all possess strong coordination affinity for fluoride ions, enabling highly selective fluoride adsorption through MF chemical bonds. More importantly, the doping of lanthanum significantly enhances the system's resistance to interference from coexisting ions such as chloride and sulfate, improving the fluoride rejection rate of the finished membrane in the complex ionic environment of electronic wastewater.

[0006] This application achieves long-lasting antifouling against lauryl alcohol contamination through a dual antifouling mechanism of "internal barrier + surface oleophobicity". On the one hand, C3 short-chain betaine is grafted inside the nanospheres to block lauryl alcohol micelles from encapsulating fluoride adsorption sites from within the membrane, unlike traditional antifouling membranes that only modify the surface with hydrophilicity, thus reducing organic pollution at its source. On the other hand, fluorinated alkylpiperazine comonomers are introduced during the interfacial polymerization process to form fluorinated amphoteric blocks in situ with low doses in the polyamide layer, forming a low surface energy oleophobic barrier on the surface, repelling the spread and adsorption of long hydrophobic lauryl alcohol chains. The synergistic effect of these two mechanisms reduces membrane flux decay.

[0007] This application uses a tannic acid-titanium (TA-Ti) chelate layer to replace the dopamine coating frequently used in the prior art. Tannic acid molecules contain a large number of catechol groups, which can form a stable five-membered ring chelate structure with titanium ions. This structure is stable in the strong acid hydrofluoric acid etching waste liquid for a long time without delamination or hydrolysis, thus ensuring the long-term operational stability of the finished film in the hydrofluoric acid environment.

[0008] In this application, the inorganic nanofiller is chemically anchored within the membrane via an aminosilane coupling agent, forming a stable covalent cross-linked network. This eliminates the problem of free powder dissolution and ensures the integrity of the membrane structure during multiple regeneration processes. Combined with a two-step regeneration process—isopropanol-alkali organic stripping and dilute nitric acid activation—specifically designed for lauryl alcohol-based organic fouling, it can thoroughly remove segmented micelles from the membrane pores. The number of regeneration cycles is more than three times that of the traditional single acid washing process, significantly reducing the frequency of maintenance and cleaning.

[0009] In summary, this application achieves a breakthrough in comprehensive performance by using a multi-layered gradient covalent integrated structure design consisting of a tannic acid-titanium chelate transition layer, a modified ternary hybrid nanosphere functional layer, and a fluorinated polyamide separation layer. The layers complement each other, resulting in high fluoride rejection rate, long-lasting resistance to lauryl alcohol pollution, resistance to strong hydrofluoric acid environments, and regeneration capability.

[0010] Preferably, the molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture is 1:1-1.2.

[0011] By employing the above technical solution, tannic acid molecules contain a large number of catechol groups, each of which can form a stable five-membered ring chelate structure with titanium ions through coordination bonds. When the molar ratio of tannic acid to titanium tetrachloride is close to 1:1, the number of catechol groups available for coordination in the tannic acid molecule is optimally matched with the number of coordination sites for titanium ions, forming a three-dimensional network structure with tannic acid as the crosslinking node and titanium ions as the coordination center. This structure forms a uniform, continuous, and dense transition layer on the membrane surface. When the proportion of titanium ions is too low, there is an excess of tannic acid, and some catechol groups cannot participate in coordination crosslinking, resulting in a loose transition layer network structure with increased defects. In a hydrofluoric acid environment, this can easily lead to coating peeling due to acid hydrolysis. When the proportion of titanium ions is too high, the excess titanium ions cannot be effectively chelated and anchored by tannic acid, and are easily detached as free titanium dioxide particles during subsequent water washing. This not only leads to an uneven transition layer structure but also forms defect sites within the membrane, affecting retention performance.

[0012] This application controls the molar ratio of tannic acid to titanium tetrachloride within the range of 1:1-1.2. Under the condition of a slight excess of titanium ions, it can ensure that the catechol groups of tannic acid molecules are fully coordinated, and the transition layer network structure reaches the highest crosslinking density, giving the transition layer optimal chemical stability and structural integrity. This transition layer provides high-density anchoring sites for the subsequent loading of ternary hybrid nanospheres, improving the loading stability of nanospheres in the membrane. On the other hand, the TA-Ti chelate layer itself has excellent hydrophilicity and acid hydrolysis resistance. Even after long-term immersion in hydrofluoric acid environment, there are no problems of delamination, swelling or hydrolysis, ensuring the long-term operational stability of the finished membrane in a strong acid environment.

[0013] Preferably, the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture is 100:3.9-4.1:1.4-1.7.

[0014] By employing the above technical solutions, zirconium ions are the most important coordination adsorption sites for fluoride ions, possessing high charge density and strong affinity for fluoride ions, making them the main body for fluoride adsorption in the nanospheres. The introduction of cerium ions has two effects: firstly, cerium ions have variable valence characteristics, which can introduce oxygen vacancies and defect sites into the nanospheres, increasing the number of active adsorption sites for fluoride ions; secondly, the introduction of Ce can regulate the crystal structure and surface charge properties of the nanospheres, optimizing the adsorption kinetics of fluoride ions. Lanthanum ion doping is one of the key innovations of this application. Lanthanum ions have a large ionic radius and a unique electronic configuration. Its doping can change the electron cloud distribution of Zr-O and Ce-O bonds in the nanospheres, forming a steric hindrance effect around the fluoride adsorption sites. This effect has a strong repulsive effect on monovalent and divalent anions such as chloride and sulfate ions, thereby significantly improving the selectivity of the nanospheres for fluoride ions and enhancing the system's resistance to interference from coexisting ions such as chloride and sulfate ions.

[0015] When the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate is strictly controlled within the range of 100:3.9-4.1:1.4-1.7, lanthanum ions enter the Zr-Ce lattice in an appropriate proportion, producing superior lattice distortion and electronic modulation effects. This maximizes fluorine selectivity without significantly affecting the bulk fluorine adsorption capacity of the nanospheres. If the lanthanum ion doping level is too low, the resistance to ion interference is insufficient, and the fluorine rejection rate decreases significantly in the complex coexisting ion environment of electronic wastewater. If the lanthanum ion doping level is too high, the excess lanthanum ions will destroy the bulk lattice structure of the nanospheres, leading to a reduction in the number of zirconium ion active adsorption sites and a decrease in fluorine adsorption capacity.

[0016] Preferably, the C3 sulfonate betaine includes at least one of thiobetaine 12 and tetradecyl sulfonate betaine.

[0017] By employing the above technical solutions, thiobetaine 12 and tetradecylsulfobetaine both belong to the sulfobetaine class of zwitterionic surfactants. Their molecular structures contain quaternary ammonium cations and sulfonate anions, exhibiting overall electroneutrality but strong hydration capacity. When grafted onto the surface of ternary hybrid nanospheres via a hydrothermal reaction, the zwitterionic groups can form a robust hydration layer on the nanosphere surface through electrostatic interactions and hydrogen bonding. This hydration layer possesses the following key functions: First, the formation of the hydration layer endows the nanosphere surface with excellent hydrophilicity, effectively repelling the approach and adsorption of hydrophobic organic molecules such as lauryl alcohol. More importantly, since C3 sulfonate betaine is grafted onto the interior and surface of the nanospheres through a hydrothermal reaction during nanosphere preparation, this "internal grafting" method gives the nanospheres antifouling capabilities throughout their entire three-dimensional structure. Unlike traditional methods that only modify the outer layer of the nanospheres with hydrophilicity, this approach fundamentally blocks the fluorine adsorption sites encapsulated by lauryl alcohol micelles.

[0018] Second, the hydrophobic alkyl chain lengths of thiobetaine 12 (C12 carbon chain) and tetradecyl sulfobetaine (C14 carbon chain) are moderate. On the one hand, they can assist the directional arrangement of zwitterionic groups on the surface of nanospheres through hydrophobic interactions, thereby enhancing the stability of the hydration layer. On the other hand, their carbon chain lengths will not cause excessive spatial obstruction of the fluorine adsorption sites of the nanospheres, ensuring that the fluorine adsorption function of the nanospheres is not affected.

[0019] Third, the strong hydration ability of zwitterionic groups gives the nanospheres good dispersion stability in water, allowing them to be uniformly dispersed in water during the pre-loading step. The uniform loading of nanospheres on the initial coated activated base film is achieved by negative pressure filtration, avoiding membrane defects and performance inhomogeneity caused by nanosphere aggregation.

[0020] Preferably, the C3 sulfonate betaine is a biphasic sulfonate betaine composed of thiobetaine 12 and tetradecyl sulfonate betaine; the mass ratio of thiobetaine 12 to tetradecyl sulfonate betaine in the biphasic sulfonate betaine is 1:0.8-1.

[0021] By employing the above technical solution, although thiobetaine 12 (C12 chain) and tetradecyl sulfobetaine (C14 chain) both belong to the sulfobetaine class of zwitterionic surfactants, their adsorption behavior, arrangement, and spatial configuration on the nanosphere surface are complementary due to the difference in the length of their hydrophobic alkyl chains. The shorter C12 chain has less steric hindrance, allowing it to more easily enter the microporous structure and defect sites on the nanosphere surface, achieving more comprehensive surface coverage. The longer C14 chain has stronger hydrophobic interactions, resulting in more robust adsorption on the nanosphere surface and a more stable hydrophilic layer. When used in combination, the C12 chain sulfobetaine molecules preferentially fill the fine pores and defect sites on the nanosphere surface, achieving full coverage, while the C14 chain sulfobetaine molecules provide stronger anchoring force and a more stable hydrophilic layer structure. Together, they achieve the dual effect of "full coverage + strong anchoring."

[0022] When the mass ratio of thiobetaine 12 to tetradecyl sulfobetaine is strictly controlled within the range of 1:0.8-1, the adsorption density of the two molecules on the surface of the nanospheres reaches the optimal ratio, and the resulting mixed hydrophilic layer possesses high coverage, high stability, and suitable hydrophilic properties. If the proportion of tetradecyl sulfobetaine is too low, the strong anchoring effect brought by the C14 chain is insufficient, and the long-term stability of the hydrophilic layer decreases; if the proportion of tetradecyl sulfobetaine is too high, the excessive long-chain alkyl group of the C14 chain may cause excessive spatial shielding of the fluorine adsorption sites on the surface of the nanospheres, affecting the fluorine adsorption capacity and adsorption kinetics of the nanospheres. At the same time, the difference in carbon chain length between the two molecules can also form micro-nano-scale surface roughness on the surface of the nanospheres, further enhancing the hydrophilicity and antifouling properties of the membrane surface. Therefore, the biphasic sulfobetaine compound system of this application produces a significant synergistic effect under optimized ratio, making the antifouling performance, dispersion stability, and fluorine adsorption performance of the nanospheres superior to the modification effect of any single component.

[0023] Preferably, the fluoroalkyl piperazine includes at least one of 1-(2-fluoroethyl)piperazine, 1-(3,3,3-trifluoropropyl)piperazine, and 1-(4,4,4-trifluorobutyl)piperazine.

[0024] By employing the above technical solution, in the interfacial polymerization reaction, piperazine (PIP) as an aqueous monomer undergoes a Schotten-Baumann polycondensation reaction with trimesoyl chloride (TMC) in the oil phase to form a cross-linked polyamide separation layer. The fluorinated alkyl piperazine introduced in this application also contains active secondary amine groups, enabling it to undergo the same polycondensation reaction with the acyl chloride groups of TMC. Therefore, it can be covalently embedded in situ into the polyamide molecular chain to form a "fluorinated amphoteric block" structure. This structure has the following key advantages: First, the fluorinated alkyl side chains have extremely low surface energy. During interfacial polymerization and heat treatment, these fluorinated side chains tend to accumulate and align on the membrane surface, forming an oleophobic barrier with a thickness only on the nanometer scale on the polyamide separation layer surface. This oleophobic barrier effectively repels the spread and adsorption of the hydrophobic long chains (C12 alkyl chains) of lauryl alcohol molecules on the membrane surface, making it difficult for lauryl alcohol molecules to adhere stably to the membrane surface, thereby significantly reducing the probability of organic pollution.

[0025] Second, the carbon chain length (C2~C4) of the fluorinated alkyl piperazine is a key parameter determined through optimization and screening in this application. When the carbon chain length is C2~C4, the fluorinated alkyl side chains possess moderate steric hindrance and molecular mobility: the C2 chain is the shortest, with the least steric hindrance, having the least impact on the interfacial polymerization rate and the degree of polyamide crosslinking, and can maintain the dense structure of the separation layer to the greatest extent; the C3 chain (such as trifluoropropyl) introduces three fluorine atoms, resulting in a higher fluorine content and a more significant oleophobic effect; the C4 chain provides the longest oleophobic barrier. Monomers of all three chain lengths can achieve surface oleophobic modification without significantly affecting the separation accuracy of the polyamide layer.

[0026] Preferably, the fluorinated alkyl piperazine is a biphase fluorinated alkyl piperazine consisting of a mixture of 1-(2-fluoroethyl) piperazine and 1-(3,3,3-trifluoropropyl) piperazine; the mass ratio of 1-(2-fluoroethyl) piperazine to 1-(3,3,3-trifluoropropyl) piperazine in the biphase fluorinated alkyl piperazine is 10:1.5-3.

[0027] By employing the above technical solutions, 1-(2-fluoroethyl)piperazine (C2 monomer) and 1-(3,3,3-trifluoropropyl)piperazine (C3 monomer) are complementary in molecular structure and reaction characteristics. The C2 monomer has the shortest fluorinated alkyl chain (containing only 2 carbon atoms and 1 fluorine atom), minimal steric hindrance, and the highest reactivity between its secondary amine group and the acyl chloride group of TMC. It can rapidly participate in the interfacial polymerization reaction and has minimal impact on the crosslinking degree and density of the polyamide network structure, making it a key component for ensuring high retention accuracy of the separation layer. The C3 monomer contains 3 carbon atoms and 3 fluorine atoms, with a higher fluorine content and lower surface energy, resulting in a more significant oleophobic effect. However, its longer carbon chain and relatively larger steric hindrance mean that its use alone in large quantities can adversely affect the interfacial polymerization reaction rate and the density of the separation layer.

[0028] When used in a mass ratio of 10:1.5-3, the C2 monomer acts as the main component, ensuring the normal progress of the interfacial polymerization reaction and the highly cross-linked and dense structure of the separation layer. The C3 monomer, as a functional regulating component, is embedded in the surface of the separation layer in a low-dose manner, providing stronger oleophobic properties. During the interfacial polymerization process, the two form a synergistic structure of "dense main body + oleophobic function": the C2 monomer ensures the high retention accuracy of fluoride ions in the separation layer, while the high fluoride content side chains of the C3 monomer form a more stable oleophobic barrier on the membrane surface. Together, they achieve the dual goals of "high retention + strong antifouling".

[0029] When the proportion of C3 monomer is too low, the fluorine content on the membrane surface is insufficient, the oleophobic barrier is not dense enough, and the improvement in anti-laurhein pollution performance is limited. When the proportion of C3 monomer is too high, the long chain structure of the excessive C3 monomer will interfere with the normal progress of the interfacial polymerization reaction, resulting in a decrease in the degree of crosslinking of the separation layer, an increase in defects, damage to density, and a significant reduction in fluorine rejection rate.

[0030] Secondly, this application provides a ternary rare earth composite fluorine selective nanofiltration membrane, which adopts the following technical solution: A ternary rare earth composite fluorine selective nanofiltration membrane is prepared using the above-mentioned preparation method for ternary rare earth composite fluorine selective nanofiltration membrane.

[0031] Thirdly, this application provides a method for regenerating a ternary rare-earth composite fluorine selective nanofiltration membrane, employing the following technical solution: A method for regenerating a ternary rare-earth composite fluorine selective nanofiltration membrane includes the following steps: Organic fouling removal: Prepare a flushing solution and circulate it to flush the contaminated ternary rare earth composite fluorine selective nanofiltration membrane to obtain a pre-treated nanofiltration membrane; the raw materials of the flushing solution include isopropanol and sodium carbonate solution; Fluorine site activation: The pre-treated nanofiltration membrane is immersed in nitric acid solution and rinsed with pure water until neutral to obtain a regenerated ternary rare earth composite fluorine selective nanofiltration membrane.

[0032] By adopting the above technical solution, this application uses isopropanol and sodium carbonate buffered alkaline solution to prepare the rinsing solution, which is then circulated and rinsed at room temperature. The mechanism of action is as follows: Lauryl alcohol molecules have an amphiphilic structure with a C12 hydrophobic long chain and a hydrophilic head group, readily aggregating and firmly adsorbing in micelle form on the membrane surface and within the membrane pores. Isopropanol, as an organic solvent with both hydrophilic and hydrophobic properties, can insert into the hydrophobic core of the lauryl alcohol micelles, disrupting the hydrophobic interactions and intermolecular van der Waals forces, causing the micelles to dissociate into individual lauryl alcohol molecules. Simultaneously, isopropanol can reduce the surface tension of the rinsing solution, enhancing its penetration and wetting ability into the narrow spaces within the membrane pores, ensuring that the cleaning solution can reach deep into the membrane pores.

[0033] Sodium carbonate buffer solution provides a mild alkaline environment that promotes the deprotonation of the carboxyl (or sulfate) groups of lauryl alcohol molecules, increasing the water solubility of lauryl alcohol molecules and causing them to desorb from the membrane surface and pores and disperse into the rinsing solution. Simultaneously, this alkaline condition does not damage the membrane material itself, avoiding the hydrolysis of the polyamide layer caused by strong alkaline cleaning.

[0034] After prolonged operation, the coordination sites of zirconium, cerium, and lanthanum ions in the ternary hybrid nanospheres become saturated with fluoride ions (forming MF bonds), losing their ability to further adsorb fluoride ions. Upon immersion in dilute nitric acid, hydrogen ions compete with the coordinated fluoride ions for metal active sites. Through protonation, the MF bonds break, and fluoride ions desorb from the nanosphere surface into the solution in the form of HF or F⁻. The metal active sites are then re-exposed in the form of hydroxyl coordination (M-OH), completing the regeneration of the active sites.

[0035] Compared to traditional single-step acid washing processes, the core advantage of this application lies in its thorough removal of organic contaminants such as lauryl alcohol (organic fouling removal) before fluorine site activation. This avoids interference from organic contaminants during acid washing with the regeneration effect of fluorine sites. If only acid washing is performed, lauryl alcohol micelles within the membrane pores will cover fluorine adsorption sites, hindering the contact between hydrogen ions and metal active sites, resulting in incomplete fluorine site activation and low performance recovery rate after regeneration. Therefore, this application's two-step regeneration strategy of "organic removal followed by site activation" achieves efficient and thorough recovery of membrane performance by precisely removing different types of contaminants step by step.

[0036] Fourthly, this application provides an application of a ternary rare earth composite fluorine selective nanofiltration membrane, employing the following technical solution: Applications of a ternary rare earth composite fluorine selective nanofiltration membrane include its use in the resource recovery treatment of photovoltaic texturing and cleaning wastewater and semiconductor wafer hydrofluoric acid etching and cleaning wastewater.

[0037] By employing the aforementioned technical solution, the texturing process of photovoltaic cells extensively uses a mixed solution of hydrofluoric acid and nitric acid for silicon wafer surface texturing treatment. This results in wastewater with high fluoride ion concentrations, along with a large amount of coexisting anions such as nitrate, chloride, and sulfate ions, as well as residual organic pollutants from texturing additives. The nanofiltration membrane of this application exhibits good fluoride ion rejection, and lanthanum ion doping endows it with excellent resistance to interference from coexisting ions. It maintains high fluoride selectivity even in complex ionic environments, and the effluent fluoride concentration meets wastewater discharge standards and reuse requirements. Furthermore, the membrane's excellent resistance to lauryl alcohol fouling and its regenerable characteristics allow for longer continuous operation cycles and lower maintenance costs in wastewater containing organic matter from texturing additives.

[0038] The wastewater generated during the hydrofluoric acid etching and cleaning of wafers in semiconductor manufacturing processes has extremely high fluoride ion concentrations and is highly acidic. This application uses a tannic acid-titanium chelate transition layer to replace the traditional dopamine coating, achieving long-term stability in the highly acidic hydrofluoric acid environment without delamination or hydrolysis issues. This fundamentally solves the problem of conventional nanofiltration membranes' inability to operate stably for extended periods in highly acidic, fluoride-containing wastewater. The treated effluent allows for the recovery and reuse of fluoride resources, and the treated water quality can be reused in the cleaning process, realizing the resource utilization of wastewater and meeting the requirements of clean production and circular economy development in the electronics industry.

[0039] The nanofiltration membrane of this application can be regenerated and recycled multiple times, significantly reducing the replacement frequency and operating costs of membrane modules. Combined with the two-step regeneration process of isopropanol-alkali organic stripping and dilute nitric acid activation, the total regeneration time per cycle is short, operation is simple, and online cleaning can be achieved, further reducing maintenance difficulty and costs. Therefore, the nanofiltration membrane of this application has broad application prospects and significant economic and environmental benefits in the resource-based treatment of fluoride-containing wastewater from the photovoltaic and semiconductor industries.

[0040] In summary, this application has the following beneficial effects: This application utilizes a multi-layered gradient covalent integrated structure design consisting of a "tannic acid-titanium chelate transition layer → modified ternary hybrid nanosphere functional layer → fluorinated polyamide separation layer." The layers complement each other, ultimately achieving a comprehensive performance breakthrough with high fluoride rejection rate, long-lasting resistance to lauryl alcohol pollution, resistance to strong hydrofluoric acid environments, and regeneration capability. Detailed Implementation

[0041] The raw materials in this application include the following: Thiobetaine 12: The commercially available product with CAS number 14933-08-5 is used; Tetradecyl sulfobetaine: Use the commercially available product with CAS number 14933-09-6; 1-(2-Fluoroethyl)piperazine: Use the commercially available product with CAS number 541505-04-8; 1-(3,3,3-trifluoropropyl)piperazine: The commercially available product with CAS number 399580-61-1 is used; 1-(4,4,4-trifluorobutyl)piperazine: The commercially available product with CAS number 939983-60-5 is used; The present application will be further described in detail below with reference to embodiments and comparative examples.

[0042] Example 1: A method for preparing a ternary rare earth composite fluorine selective nanofiltration membrane, comprising the following steps: Base membrane activation: Immerse the polyethersulfone ultrafiltration base membrane in a sodium hydroxide solution (sodium hydroxide mass fraction 3wt%, or 2-4wt%) for 50 min (40-60 min is acceptable), rinse with pure water and dry to obtain the activated base membrane; Transition layer coating: Tannic acid and titanium tetrachloride were added to water and stirred to obtain a two-phase mixture; the activated base film was immersed in the two-phase mixture, then removed and allowed to stand for 40 min (30-50 min is acceptable), and rinsed with pure water to obtain the initial coated activated base film; the molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture was 1:1.1; the total molar concentration of the solute in the two-phase mixture was 2.5 mmol / L; Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture; then 1.6 g of thiobetaine 12 was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is also acceptable) for 10 h (8-12 h is also acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres; the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. Preloading: 0.5g of modified ternary hybrid nanospheres were dispersed in 1L of water to prepare a dispersion, which was then loaded onto the pre-coated activated base film using negative pressure filtration to obtain a pre-loaded activated base film; Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction of 1 wt%) for 2 min, removed, rinsed with deionized water and dried, and then placed in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film; the oil phase solution was a solution of trimesoyl chloride (mass fraction of 1 wt%) and 1-(2-fluoroethyl)piperazine (mass fraction of 1 wt%, or within 0.8-1.2 wt%) dissolved in n-hexane; Heat treatment: The polymerized activated base membrane is heated at 70℃ (60-80℃ is acceptable) for 15 min (10-20 min is acceptable), cooled and then immersed in nitric acid solution (nitric acid mass fraction of 0.8wt%, 0.5-1wt% is acceptable), and rinsed to obtain ternary rare earth composite fluorine selective nanofiltration membrane.

[0043] Examples 2-5 Example 2 is based on the preparation method of Example 1, but with adjustments: Transition layer coating: Tannic acid and titanium tetrachloride are added to water and stirred to obtain a two-phase mixture; the activated base film is immersed in the two-phase mixture, then removed and allowed to stand for 40 min (30-50 min is acceptable), and rinsed with pure water to obtain the initial coated activated base film; the molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture is 1:0.9; the total molar concentration of solute in the two-phase mixture is 2.5 mmol / L.

[0044] Example 3 is based on the preparation method of Example 1, but with adjustments: Transition layer coating: Tannic acid and titanium tetrachloride are added to water and stirred to obtain a two-phase mixture; the activated base film is immersed in the two-phase mixture, then removed and allowed to stand for 40 min (30-50 min is acceptable), and rinsed with pure water to obtain the initial coated activated base film; the molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture is 1:1; the total molar concentration of solute in the two-phase mixture is 2.5 mmol / L.

[0045] Example 4 is based on the preparation method of Example 1, but with adjustments: Transition layer coating: Tannic acid and titanium tetrachloride are added to water and stirred to obtain a two-phase mixture; the activated base film is immersed in the two-phase mixture, then removed and allowed to stand for 40 min (30-50 min is acceptable), and rinsed with pure water to obtain the initial coated activated base film; the molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture is 1:1.2; the total molar concentration of solute in the two-phase mixture is 2.5 mmol / L.

[0046] Example 5 is based on the preparation method of Example 1, but with adjustments: Transition layer coating: Tannic acid and titanium tetrachloride are added to water and stirred to obtain a two-phase mixture; the activated base film is immersed in the two-phase mixture, then removed and allowed to stand for 40 min (30-50 min is acceptable), and rinsed with pure water to obtain the initial coated activated base film; the molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture is 1:1.3; the total molar concentration of solute in the two-phase mixture is 2.5 mmol / L.

[0047] Comparative Examples 1-2 Comparative Example 1 modifies the preparation method based on the preparation method of Example 1: Preloading: 0.5g of modified ternary hybrid nanospheres were dispersed in 1L of water to prepare a dispersion, which was then loaded onto the activated base membrane using negative pressure filtration to obtain a preloaded activated base membrane.

[0048] Comparative Example 2 adjusts the preparation method based on the preparation method of Example 1: Interfacial polymerization: The initially coated activated base film is immersed in a piperazine aqueous solution (piperazine mass fraction of 1 wt%) for 2 min, removed, rinsed with deionized water and dried, and then placed in an oil phase solution to react for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film; the oil phase solution is a solution of pyromellitic trimethylol chloride (mass fraction of 1 wt%) and 1-(2-fluoroethyl)piperazine (mass fraction of 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane.

[0049] Performance testing The ternary rare earth composite fluorine selective nanofiltration membranes of Examples 1-5 and Comparative Examples 1-2 were subjected to the following performance tests, and the test results are shown in Table 1.

[0050] 1. Fluorine rejection rate The fluoride rejection rate of the ternary rare earth composite fluorine selective nanofiltration membrane was determined according to GB / T 34242-2017. The fluoride-containing wastewater used in the test was hydrofluoric acid etching and cleaning wastewater from semiconductor wafers, with pH=2.2, fluoride ion concentration of 38 mg / L, lauryl alcohol polyoxyethylene ether concentration of 220 mg / L, and containing NMP and photoresist impurities.

[0051] 2. Flux stability Under simulated operating conditions, the pure water flux A of the ternary rare earth composite fluorine selective nanofiltration membrane was recorded on day 1. After 90 days of continuous operation, the pure water flux B of the ternary rare earth composite fluorine selective nanofiltration membrane was recorded. Flux decay rate = [(AB) / A] × 100%.

[0052] Table 1 Performance test results of Examples 1-5 and Comparative Examples 1-2

[0053] Referring to Table 1, comparing Examples 1-5 and Comparative Examples 1-2, it can be seen that the ternary rare earth composite fluorine-selective nanofiltration membrane prepared using the above preparation method exhibits high fluorine rejection rate and resistance to the strong acid environment of hydrofluoric acid. The main reason is that this application employs a Zr-Ce-La ternary rare earth synergistic coordination system. Zirconium oxychloride, cerium nitrate, and lanthanum nitrate form ternary hybrid nanospheres through a hydrothermal reaction. Zirconium, cerium, and lanthanum ions all possess strong coordination affinity for fluoride ions, enabling highly selective fluorine adsorption through MF chemical bonds. More importantly, the doping of lanthanum significantly enhances the system's resistance to interference from coexisting ions such as chloride and sulfate, improving the fluorine rejection rate of the finished membrane in the complex ionic environment of electronic wastewater. This application uses a tannic acid-titanium (TA-Ti) chelating layer to replace the dopamine coating frequently used in existing technologies. Tannic acid molecules contain a large number of catechol groups, which can form a stable five-membered ring chelate structure with titanium ions. This structure is stable in the strong acid hydrofluoric acid etching waste liquid for a long time without delamination or hydrolysis, thus ensuring the long-term operational stability of the finished film in the hydrofluoric acid environment.

[0054] Examples 6-9 Example 6 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: In the step of preparing modified ternary hybrid nanospheres, the total molar concentration of solute in the three-phase mixture was 52.75 mmol, and the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate was 100:3.5:2.

[0055] Example 7 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: In the step of preparing modified ternary hybrid nanospheres, the total molar concentration of solute in the three-phase mixture was 52.75 mmol, and the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate was 100:3.9:1.7.

[0056] Example 8 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: In the step of preparing modified ternary hybrid nanospheres, the total molar concentration of solute in the three-phase mixture was 52.75 mmol, and the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate was 100:4.1:1.4.

[0057] Example 9 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: In the step of preparing modified ternary hybrid nanospheres, the total molar concentration of solute in the three-phase mixture was 52.75 mmol, and the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate was 100:4.5:1.

[0058] The ternary rare earth composite fluorine selective nanofiltration membranes of Examples 6-9 were subjected to the above performance tests, and the test results are shown in Table 2.

[0059] Table 2 Performance test results for Examples 1 and 6-9

[0060] Referring to Table 2, comparing Examples 1 and 6-9, it can be seen that when the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture is 100:3.9-4.1:1.4-1.7, the prepared ternary rare earth composite fluorine selective nanofiltration membrane has a better effect.

[0061] Examples 10-15 Example 10 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture; then 1.6 g tetradecyl sulfobetaine was added to the three-phase mixture and hydrothermally reacted at 170 °C (160-180 °C is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g KH-550 was added and heated under reflux at 80 °C for 3 h to obtain modified ternary hybrid nanospheres; the molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5.

[0062] Example 11 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture. Then, 1.6 g of biphase sulfonate betaine was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and the mixture was heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres. The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. The biphase sulfonate betaine was composed of a mixture of thiobetaine 12 and tetradecyl sulfonate betaine, with a mass ratio of 1:0.6.

[0063] Example 12 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture. Then, 1.6 g of biphase sulfonate betaine was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and the mixture was heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres. The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. The biphase sulfonate betaine was composed of a mixture of thiobetaine 12 and tetradecyl sulfonate betaine, with a mass ratio of 1:0.8.

[0064] Example 13 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture. Then, 1.6 g of biphase sulfonate betaine was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and the mixture was heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres. The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. The biphase sulfonate betaine was composed of a mixture of thiobetaine 12 and tetradecyl sulfonate betaine, with a mass ratio of 1:0.9.

[0065] Example 14 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture. Then, 1.6 g of biphase sulfonate betaine was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and the mixture was heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres. The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. The biphase sulfonate betaine was composed of a mixture of thiobetaine 12 and tetradecyl sulfonate betaine, with a mass ratio of 1:1.

[0066] Example 15 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture. Then, 1.6 g of biphase sulfonate betaine was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and the mixture was heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres. The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. The biphase sulfonate betaine was composed of a mixture of thiobetaine 12 and tetradecyl sulfonate betaine, with a mass ratio of 1:1.2.

[0067] The ternary rare earth composite fluorine selective nanofiltration membranes of Examples 10-15 were subjected to the above performance tests, and the test results are shown in Table 3.

[0068] Table 3 Performance test results for Examples 1 and 10-15

[0069] Referring to Table 3, a comparison of Examples 1 and 10-15 shows that when preparing modified ternary hybrid nanospheres, adding C3 sulfonate betaine alone is more effective than adding thiobetaine 12. Adding biphasic sulfonate betaine, with the mass ratio of thiobetaine 12 to tetradecyl sulfonate betaine limited to 1:0.8-1, yields even better results.

[0070] Examples 16-20 Example 16 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film is immersed in a piperazine aqueous solution (piperazine mass fraction of 1 wt%) for 2 min, taken out, rinsed with deionized water and dried, and then placed in an oil phase solution to react for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film; the oil phase solution is a solution of pyromellitic trimethylol chloride (mass fraction of 1 wt%) and 1-(3,3,3-trifluoropropyl)piperazine (mass fraction of 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane.

[0071] Example 17 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film is immersed in a piperazine aqueous solution (piperazine mass fraction of 1 wt%) for 2 min, removed, rinsed with deionized water and dried, and then placed in an oil phase solution to react for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film; the oil phase solution is a solution of pyromellitic trimethylol chloride (mass fraction of 1 wt%) and 1-(4,4,4-trifluorobutyl)piperazine (mass fraction of 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane.

[0072] Example 18 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, removed, rinsed with deionized water, dried, and then placed in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic trimethylol chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine, with a mass ratio of 10:2.5.

[0073] Example 19 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, rinsed with deionized water and dried, and then reacted in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic tricarboxylic acid chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(4,4,4-trifluorobutyl)piperazine, with a mass ratio of 10:2.5.

[0074] Example 20 adjusts the preparation method based on the preparation method of Example 1 as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, removed, rinsed with deionized water, dried, and then placed in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic trimethylol chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(3,3,3-trifluoropropyl)piperazine and 1-(4,4,4-trifluorobutyl)piperazine, with a mass ratio of 2.5:2.5.

[0075] The ternary rare earth composite fluorine selective nanofiltration membranes of Examples 16-20 were subjected to the above performance tests, and the test results are shown in Table 4.

[0076] Table 4 Performance test results for Examples 1 and 16-20

[0077] Referring to Table 4, a comparison of Examples 1 and 16-20 shows that, during interfacial polymerization, when adding fluorinated alkyl piperazine alone, the addition of 1-(2-fluoroethyl)piperazine is more effective. When fluorinated alkyl piperazines are combined in pairs, the combination of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine is more effective.

[0078] Examples 21-25 Example 21 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, rinsed with deionized water and dried, and then reacted in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic tricarboxylic acid chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine, with a mass ratio of 10:1.

[0079] Example 22 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, rinsed with deionized water and dried, and then reacted in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic tricarboxylic acid chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine, with a mass ratio of 10:1.5.

[0080] Example 23 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, removed, rinsed with deionized water, dried, and then placed in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic tricarboxylic acid chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine, with a mass ratio of 10:3.

[0081] Example 24 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, rinsed with deionized water and dried, and then reacted in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic tricarboxylic acid chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine, with a mass ratio of 10:3.5.

[0082] Example 25 is based on the preparation method of Example 1, but the preparation method is adjusted as follows: Preparation of modified ternary hybrid nanospheres: 50 mmol zirconium oxychloride, 2 mmol cerium nitrate, and 0.75 mmol lanthanum nitrate were dissolved in 200 mL of water by stirring to obtain a three-phase mixture. Then, 1.6 g of biphase sulfonate betaine was added to the three-phase mixture and hydrothermally reacted at 170℃ (160-180℃ is acceptable) for 10 h (8-12 h is acceptable). After cooling, filtration, and washing, 1 g of KH-550 was added and the mixture was heated under reflux at 80℃ for 3 h to obtain modified ternary hybrid nanospheres. The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture was 100:4:1.5. The biphase sulfonate betaine was composed of a mixture of thiobetaine 12 and tetradecyl sulfonate betaine, with a mass ratio of 1:0.9.

[0083] Interfacial polymerization: The pre-loaded activated base film was immersed in a piperazine aqueous solution (piperazine mass fraction 1 wt%) for 2 min, removed, rinsed with deionized water, dried, and then placed in an oil phase solution for 30 s (20-40 s is acceptable) to obtain a polymerized activated base film. The oil phase solution was a solution of pyromellitic trimethylol chloride (mass fraction 1 wt%) and biphase fluorinated alkyl piperazine (mass fraction 1 wt%, 0.8-1.2 wt% is acceptable) dissolved in n-hexane. The biphase fluorinated alkyl piperazine was composed of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine, with a mass ratio of 10:2.5.

[0084] The ternary rare earth composite fluorine selective nanofiltration membranes of Examples 21-25 were subjected to the above performance tests, and the test results are shown in Table 5.

[0085] Table 5 Performance test results for Examples 1 and 21-25

[0086] Referring to Table 5, a comparison of Examples 1 and 21-25 shows that when adding biphase fluorinated alkyl piperazine, the mass ratio of 1-(2-fluoroethyl)piperazine to 1-(3,3,3-trifluoropropyl)piperazine is 10:1.5-3, resulting in better performance. Furthermore, biphase sulfonate betaine was used in the preparation of modified ternary hybrid nanospheres, and biphase fluorinated alkyl piperazine was used in interfacial polymerization, yielding even better results.

[0087] Examples 26-29 Example 26: A regeneration method for the ternary rare earth composite fluorine selective nanofiltration membrane of Example 1, comprising the following steps: Organic fouling removal: Prepare a flushing solution and circulate it to flush the contaminated ternary rare earth composite fluorine selective nanofiltration membrane for 45 min (30-60 min is acceptable) to obtain a pre-treated nanofiltration membrane; the flushing solution is isopropanol added to a sodium carbonate solution with a pH of 9.5 (pH 9-10 is acceptable), and the volume fraction of isopropanol is 8% (6-9% is acceptable). Fluorine site activation: The pre-treated nanofiltration membrane is immersed in a nitric acid solution (nitric acid mass fraction of 0.8wt%, or 0.5-1wt%) for 25 min (or 20-30 min), and then rinsed with pure water until neutral to obtain a regenerated ternary rare earth composite fluorine selective nanofiltration membrane.

[0088] Example 27: A method for regenerating the ternary rare earth composite fluorine selective nanofiltration membrane of Example 13, comprising the following steps: Organic fouling removal: Prepare a flushing solution and circulate it to flush the contaminated ternary rare earth composite fluorine selective nanofiltration membrane for 45 min (30-60 min is acceptable) to obtain a pre-treated nanofiltration membrane; the flushing solution is isopropanol added to a sodium carbonate solution with a pH of 9.5 (pH 9-10 is acceptable), and the volume fraction of isopropanol is 8% (6-9% is acceptable). Fluorine site activation: The pre-treated nanofiltration membrane is immersed in a nitric acid solution (nitric acid mass fraction of 0.8wt%, or 0.5-1wt%) for 25 min (or 20-30 min), and then rinsed with pure water until neutral to obtain a regenerated ternary rare earth composite fluorine selective nanofiltration membrane.

[0089] Example 28: A method for regenerating the ternary rare earth composite fluorine selective nanofiltration membrane of Example 18, comprising the following steps: Organic fouling removal: Prepare a flushing solution and circulate it to flush the contaminated ternary rare earth composite fluorine selective nanofiltration membrane for 45 min (30-60 min is acceptable) to obtain a pre-treated nanofiltration membrane; the flushing solution is isopropanol added to a sodium carbonate solution with a pH of 9.5 (pH 9-10 is acceptable), and the volume fraction of isopropanol is 8% (6-9% is acceptable). Fluorine site activation: The pre-treated nanofiltration membrane is immersed in a nitric acid solution (nitric acid mass fraction of 0.8wt%, or 0.5-1wt%) for 25 min (or 20-30 min), and then rinsed with pure water until neutral to obtain a regenerated ternary rare earth composite fluorine selective nanofiltration membrane.

[0090] Example 29: A method for regenerating the ternary rare earth composite fluorine selective nanofiltration membrane of Example 25, comprising the following steps: Organic fouling removal: Prepare a flushing solution and circulate it to flush the contaminated ternary rare earth composite fluorine selective nanofiltration membrane for 45 min (30-60 min is acceptable) to obtain a pre-treated nanofiltration membrane; the flushing solution is isopropanol added to a sodium carbonate solution with a pH of 9.5 (pH 9-10 is acceptable), and the volume fraction of isopropanol is 8% (6-9% is acceptable). Fluorine site activation: The pre-treated nanofiltration membrane is immersed in a nitric acid solution (nitric acid mass fraction of 0.8wt%, or 0.5-1wt%) for 25 min (or 20-30 min), and then rinsed with pure water until neutral to obtain a regenerated ternary rare earth composite fluorine selective nanofiltration membrane.

[0091] The regenerated ternary rare earth composite fluorine selective nanofiltration membranes of Examples 26-29 were subjected to the following performance tests, and the test results are shown in Table 6.

[0092] 3. Fluorine Retention Rate The fluoride rejection rate of the regenerated ternary rare earth composite fluorine selective nanofiltration membrane after 18 regenerations was determined according to GB / T 34242-2017. The fluoride-containing wastewater used in the test was hydrofluoric acid etching and cleaning wastewater from semiconductor wafers, with pH=2.2, fluoride ion concentration of 38 mg / L, lauryl alcohol polyoxyethylene ether concentration of 220 mg / L, and containing NMP and photoresist impurities.

[0093] 4. Flux stability Under simulated operating conditions, the pure water flux C of the ternary rare earth composite fluorine selective nanofiltration membrane was recorded on the first day of the first regeneration. After 18 regenerations, the pure water flux D of the regenerated ternary rare earth composite fluorine selective nanofiltration membrane was recorded. Flux recovery rate = (D / C) × 100%.

[0094] Table 6 Performance Test Tables for Examples 26-29

[0095] Referring to Table 6, and comparing Examples 26-29, it can be seen that the ternary rare earth composite fluorine selective nanofiltration membrane prepared in this application can resist lauryl alcohol pollution for a long time and can be regenerated multiple times.

[0096] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A method for preparing a ternary rare-earth composite fluorine selective nanofiltration membrane, characterized in that, Includes the following steps: Base membrane activation: The polyethersulfone ultrafiltration base membrane was activated by immersing it in sodium hydroxide solution, rinsing it, and then drying it to obtain the activated base membrane; Transition layer coating: Tannic acid and titanium tetrachloride are added to water and stirred to obtain a two-phase mixture; the activated base film is immersed in the two-phase mixture, then removed and allowed to stand to cure, and rinsed to obtain the initial coated activated base film; Preparation of modified ternary hybrid nanospheres: Zirconium oxychloride, cerium nitrate, and lanthanum nitrate were dissolved in water by stirring to obtain a three-phase mixture; then C3 sulfonate betaine was added to the three-phase mixture for hydrothermal reaction, cooled, filtered, washed, and then an aminosilane coupling agent was added and heated under reflux to obtain modified ternary hybrid nanospheres. Pre-loading: The modified ternary hybrid nanospheres are dispersed in water to form a dispersion, which is then loaded onto the initially coated activated base film using negative pressure filtration to obtain a pre-loaded activated base film; Interfacial polymerization: The preloaded activated base film is immersed in a piperazine aqueous solution, taken out, rinsed and dried, and then placed in an oil phase solution for reaction to obtain a polymerized activated base film; the oil phase solution is a solution of pyromellitic trimethylol chloride and fluorinated alkyl piperazine comonomer dissolved in n-hexane; Heat treatment: The polymerized activated base membrane is heated, cooled, and then immersed in nitric acid solution. After rinsing, a ternary rare earth composite fluorine selective nanofiltration membrane is obtained.

2. The method for preparing the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 1, characterized in that: The molar ratio of tannic acid to titanium tetrachloride in the two-phase mixture is 1:1-1.

2.

3. The method for preparing the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 1, characterized in that: The molar ratio of zirconium oxychloride, cerium nitrate, and lanthanum nitrate in the three-phase mixture is 100:3.9-4.1:1.4-1.

7.

4. The method for preparing the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 1, characterized in that: The C3 sulfonate betaine includes at least one of thiobetaine 12 and tetradecyl sulfonate betaine.

5. The method for preparing the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 4, characterized in that: The C3 sulfonate betaine is a biphasic sulfonate betaine composed of thiobetaine 12 and tetradecyl sulfobetaine; the mass ratio of thiobetaine 12 to tetradecyl sulfobetaine in the biphasic sulfonate betaine is 1:0.8-1.

6. The method for preparing the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 1, characterized in that: The fluorinated alkyl piperazine includes at least one of 1-(2-fluoroethyl)piperazine, 1-(3,3,3-trifluoropropyl)piperazine, and 1-(4,4,4-trifluorobutyl)piperazine.

7. The method for preparing the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 6, characterized in that: The fluorinated alkyl piperazine is a biphase fluorinated alkyl piperazine consisting of a mixture of 1-(2-fluoroethyl)piperazine and 1-(3,3,3-trifluoropropyl)piperazine; the mass ratio of 1-(2-fluoroethyl)piperazine to 1-(3,3,3-trifluoropropyl)piperazine in the biphase fluorinated alkyl piperazine is 10:1.5-3.

8. A ternary rare earth composite fluorine selective nanofiltration membrane, characterized in that: The ternary rare earth composite fluorine selective nanofiltration membrane is prepared by any one of claims 1-7.

9. A method for regenerating the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 8, characterized in that, Includes the following steps: Organic fouling removal: Prepare a flushing solution and circulate it to flush the contaminated ternary rare earth composite fluorine selective nanofiltration membrane to obtain a pre-treated nanofiltration membrane; the raw materials of the flushing solution include isopropanol and sodium carbonate solution; Fluorine site activation: The pre-treated nanofiltration membrane is immersed in nitric acid solution and rinsed with pure water until neutral to obtain a regenerated ternary rare earth composite fluorine selective nanofiltration membrane.

10. An application of the ternary rare earth composite fluorine selective nanofiltration membrane according to claim 8, characterized in that: This includes applications in the resource recovery treatment of photovoltaic texturing and cleaning wastewater and semiconductor wafer hydrofluoric acid etching and cleaning wastewater.