Fluororubber composition and fluororubber molded product

The fluororubber composition with vinylidene fluoride, propylene hexafluoride, and silica with a silane coating addresses heat resistance and contamination issues, providing cost-effective high-performance sealing materials for semiconductor devices.

JP2024143288APending Publication Date: 2024-10-11MITSUBISHI CABLE INDUSTRIES LTD

Patent Information

Application Number
JP2023055883
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional fluororubber sealing materials used in semiconductor devices face issues with heat resistance and contamination due to carbon black, and high-cost alternatives like FFKM are expensive and difficult to implement.

Method used

A fluororubber composition comprising vinylidene fluoride, propylene hexafluoride, spherical silica with a silane coupling agent coating, and magnesium oxide or hydrotalcite, which improves heat resistance and reduces contamination risk at lower costs.

Benefits of technology

The composition achieves high heat resistance with a compression set rate of less than 40% at 250°C for 70 hours, reducing production costs and minimizing contamination concerns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143288000001_ABST
    Figure 2024143288000001_ABST
Patent Text Reader

Abstract

To provide a fluororubber composition which has high heat resistance and can be produced at low cost and a fluororubber molded product using the same.SOLUTION: There is provided a fluororubber composition which comprises vinylidene fluoride and propylene hexafluoride, which are binary fluororubber raw materials, a spherical silica composition, at least one of magnesium oxide or hydrotalcite and calcium hydroxide, wherein the silica composition comprises spherical silica and a coating layer containing a silane coupling agent covering the surface of the spherical silica and the silica composition is contained in the range of 1 pt.mass or more and 80 pts.mass or less based on 100 pts.mass of the binary fluororubber raw materials.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluororubber composition and a fluororubber molded product. [Background technology]

[0002] In recent years, as various electronic devices have become more highly integrated and perform better, the manufacturing environment for the components has become hotter. For example, in semiconductor devices used to manufacture integrated circuits, sealing materials are required to have high heat resistance as well as chemical resistance and plasma resistance.

[0003] Fluororubber (FKM) has been used as a sealing material for such semiconductor devices (see, for example, Patent Document 1). Fluororubber is roughly divided into binary fluororubber, which is a copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP), and ternary fluororubber, which is a copolymer of VDF, HFP, and tetrafluoroethylene (TFE). Of these, binary fluororubber is particularly excellent in heat resistance and has been used as a sealing material for semiconductor devices.

[0004] However, in recent years, the operating environments of semiconductor devices have become increasingly hotter and cleaner, raising concerns that conventional sealing materials using binary fluororubber may not have sufficient heat resistance, and because they generally contain carbon black, there is a problem of contamination.

[0005] When FKM is used as a sealing material for semiconductor devices, there is a concern that fluororubber containing carbon black will be black or a similar dark color and will be recognized as contamination. Therefore, a sealing material that uses tetrafluoroethylene perfluoromethyl vinyl ether copolymer (FFKM) is also known as a fluororubber that has a near-white color that is less likely to be recognized as contamination and has high heat resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2007-154043 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the sealing material disclosed in Patent Document 1 has a problem in that heat resistance is reduced because a fluororesin is further added to the fluororubber to enhance low odor retention.On the other hand, FFKM, which is said to have higher heat resistance than FKM, is very expensive (for example, about 50 times the price of FKM), and when the sealing material is applied to semiconductor devices that use many places, the manufacturing cost of the device increases significantly.

[0008] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a fluororubber composition which has high heat resistance and can be produced at low cost, and a fluororubber molded product using the same. [Means for solving the problem]

[0009] In order to solve the above problems, the fluororubber composition and fluororubber molded product according to one embodiment of the present invention propose the following measures. (1) A fluororubber composition according to a first aspect of the present invention is a fluororubber composition containing vinylidene fluoride and hexafluoropropylene as binary fluororubber raw materials, a spherical silica composition, at least one of magnesium oxide and hydrotalcite, and calcium hydroxide, wherein the silica composition is composed of spherical silica and a coating layer containing a silane coupling agent that covers the surface of the spherical silica, and the silica composition is contained in an amount of 1 part by mass or more and 80 parts by mass or less per 100 parts by mass of the binary fluororubber raw material.

[0010] (2) A second aspect of the present invention is characterized in that, in the fluororubber composition of the first aspect, the silane coupling agent is an alkyl-based silane coupling agent or a fluorine-based silane coupling agent.

[0011] (3) A fluororubber molded article according to the third aspect of the present invention is characterized in that it is obtained by molding a fluororubber obtained by copolymerizing vinylidene fluoride and propylene hexafluoride of the fluororubber composition according to the first or second aspect.

[0012] (4) A fourth aspect of the present invention is characterized in that in the fluororubber molded article of the third aspect, the fluororubber has a compression set rate of less than 40% at 250° C. for 70 hours. Effect of the Invention

[0013] According to the present invention, it is possible to provide a fluororubber composition which has high heat resistance and can be produced at low cost, and a fluororubber molded product and a sealing material using the same. [Brief description of the drawings]

[0014] [Figure 1] 1 is a graph showing the compression set of fluororubber depending on the type of silane coupling agent. [Diagram 2] 1 is a graph showing the tensile strength of fluororubber depending on the type of silane coupling agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] A fluororubber composition according to an embodiment of the present invention and a fluororubber molded product using the same will be described below. Note that the following embodiment is specifically described to better understand the gist of the invention, and does not limit the present invention unless otherwise specified.

[0016] (Fluororubber composition) The fluororubber composition of the present embodiment is a raw material for producing fluororubber, and contains vinylidene fluoride and hexafluoropropylene which are binary fluororubber raw materials, a spherical silica composition, at least one of magnesium oxide and hydrotalcite, and calcium hydroxide, and the silica composition is composed of spherical silica and a coating layer containing a silane coupling agent that covers the surface of the spherical silica, and the silica composition is contained in an amount of 1 part by mass or more and 80 parts by mass or less per 100 parts by mass of the binary fluororubber raw material.

[0017] The vinylidene fluoride (C 2 H 2 F 2 :VDF) and hexafluoropropylene (C 3 F 6 By copolymerizing two types of monomers, vinylidene fluoride-hexafluoropropylene (HFP), through a crosslinking reaction, it is possible to obtain fluororubber containing vinylidene fluoride-hexafluoropropylene copolymer (hereinafter simply referred to as binary FKM). Such fluororubber has excellent heat resistance, oil resistance, and chemical resistance because it has strong C-F bonds (fluorine bonds) in the copolymer composition.

[0018] Binary FKMs produce grades with different properties depending on the combined ratio of monomers. The composition ratio (molar ratio) of vinylidene fluoride and propylene hexafluoride contained in the fluororubber composition of this embodiment may be in the range of 1:1 to 1:6, for example.

[0019] The vulcanization method when copolymerizing vinylidene fluoride and propylene hexafluoride may be either polyol vulcanization or polyamine vulcanization. Polyol vulcanization and polyamine vulcanization are carried out by forming double bonds from molecular chains of binary FKM by dehydrofluorination (hydrogen fluoride) reaction using amines or onium salts (ammonium salts, phosphonium salts, etc.) as catalysts, and then adding diamines or bisphenol compounds to the double bonds to perform vulcanization. In either vulcanization method, it is necessary to add a metal oxide as an acid acceptor to neutralize the generated hydrofluoric acid.

[0020] As a vulcanizing agent for polyamine vulcanization, hexamethylenediamine carbamate, a salt of hexamethylenediamine and cinnamaldehyde, cyclohexyldiamine carbamate, etc. can be used. In addition, since the vulcanizing agent does not have a catalytic action, an onium salt and calcium hydroxide as a cocatalyst are used.

[0021] In the fluororubber composition of this embodiment, calcium hydroxide (Ca(OH) 2 Calcium hydroxide may be mixed in an amount of, for example, 3 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the binary FKM raw material.

[0022] The acid acceptor for neutralizing the hydrofluoric acid used in the polyamine vulcanization and polyol vulcanization may be any acid acceptor that reacts with hydrofluoric acid to produce a fluorine compound. Magnesium oxide (MgO) or hydrotalcite (MgO) is suitable for use in the production of a fluorine compound that can maintain a good compression set rate. 6 Al 2 CO 3 (OH) 16 4(H 2 O))Use.

[0023] The fluororubber composition of the present embodiment contains at least one or both of magnesium oxide and hydrotalcite, which may be blended in a ratio of 1 part by mass to 8 parts by mass per 100 parts by mass of the binary FKM raw material.

[0024] The spherical silica composition is a filler that is dispersed in the binary FKM after copolymerization, and is composed of spherical silica and a coating layer that covers the surface of the spherical silica. The spherical silica composition may be contained in an amount of 1 part by mass or more and 80 parts by mass or less, preferably 1 part by mass or more and 50 parts by mass or less, per 100 parts by mass of the binary fluororubber raw material consisting of vinylidene fluoride and propylene hexafluoride.

[0025] The spherical silica constituting the silica composition is, for example, silica (SiO 2 The average particle size of the spherical silica may be, for example, in the range of 1 μm or more and 30 μm or less. Such spherical silica can be obtained, for example, by melting pulverized raw silica stone in a high-temperature flame and spheroidizing it by surface tension. Specific examples of spherical silica include EXELICA (Tokuyama Corporation), ADMAFINE (Admatechs Corporation), Denka spherical silica filler (Denka Co., Ltd.), and SUNSPHARE (AGC Si-Tech Co., Ltd.).

[0026] The coating layer covering the surface of the spherical silica is composed of a silane coupling agent. The silane coupling agent used in the coating layer is preferably an alkyl-based silane coupling agent or a fluorine-based silane coupling agent.

[0027] Specific examples of alkyl-based silane coupling agents include trimethoxy-normal-octylsilane, triethoxy-normal-octylsilane, decyltriethoxysilane, dodecyltrimethoxysilane, decyltrimethoxysilane, hexadecyltrimethoxysilane, octadecyltrimethoxysilane, and octadecyltriethoxysilane.

[0028] Specific examples of fluorine-based silane coupling agents include trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, trimethoxy(3,3,3-trifluoropropyl)silane, trimethoxy(1H,1H,2H,2H-nonafluorohexyl)silane, trimethoxy(1H,1H,2H,2H-perfluoro-normal-octyl)silane, triethoxy(1H,1H,2H,2H-perfluoro-normal-octyl)silane, and trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane.

[0029] Specific examples of alkyl-based silane coupling agents include trimethoxy-normal-octylsilane, triethoxy-normal-octylsilane, decyltriethoxysilane, dodecyltrimethoxysilane, and decyltrimethoxysilane. A specific example of a fluorine-based silane coupling agent is trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane.

[0030] The coverage of the coating layer with respect to the surface of the spherical silica may be, for example, 80% or more, and preferably 90% or more.

[0031] By dispersing the silica composition of this composition in a binary FKM in which vinylidene fluoride and propylene hexafluoride are copolymerized, the heat resistance is significantly improved and the compression set rate, which is an index of heat resistance, can be improved compared to a binary FKM that does not contain the silica composition. In addition, the mold releasability may also be improved.

[0032] (Fluororubber moldings) The fluororubber molded product of this embodiment is obtained by crosslinking (vulcanizing) a copolymer of vinylidene fluoride and propylene hexafluoride, which is a binary fluororubber raw material contained in the above-mentioned fluororubber composition, and molding it into a desired shape.

[0033] Specifically, a filler, a vulcanizing agent, etc. are added to the fluororubber composition, and the mixture is kneaded using a roll, kneader, etc. The kneaded rubber is then cut into a sheet shape, etc., to perform preforming. After being charged into a mold that resembles the shape of the mold, a crosslinking reaction occurs between vinylidene fluoride and hexafluoropropylene by applying pressure and heat, and a fluororubber molded product in the shape of the mold is formed. The molded product is then heat-treated to become the final molded product.

[0034] According to the fluororubber molded product of this embodiment, by dispersing a spherical silica composition in the binary FKM formed by a crosslinking reaction, it is possible to produce a fluororubber molded product at low cost that has significantly improved heat resistance, compared to a fluororubber molded product that does not contain a filler or the like in the binary FKM. For example, the compression set rate, which is an index of the heat resistance of the fluororubber molded product of this embodiment, is less than 40% under conditions of 250° C. for 70 hours, and thus the product has excellent heat resistance.

[0035] (Sealing material) The sealing material of this embodiment is obtained by crosslinking (vulcanizing) a copolymer of vinylidene fluoride and propylene hexafluoride, which is a binary fluororubber raw material contained in the above-mentioned fluororubber composition, and molding it to fit the shape of the location where the sealing material is to be installed. For example, specific examples of the sealing material include O-rings and packings installed at pipe joints in semiconductor devices, etc.

[0036] For example, the sealing material of the present embodiment is significantly cheaper than high-cost sealing materials such as conventional FFKM, and therefore can reduce the cost of equipment such as semiconductor devices. In addition, the sealing material of this embodiment uses a binary FKM in which a silica composition is dispersed, in which highly white spherical silica is covered with a coating layer made of a silane coupling agent. Therefore, compared to conventional sealing materials in which carbon black is dispersed as a filler, the sealing material is not black, and there is little concern that it will be recognized as a contamination even when used as a sealing material for semiconductor devices. For example, the sealing material of this embodiment can realize a non-black sealing material, as compared with conventional black sealing materials in which carbon black is dispersed.

[0037] Although the embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope of the invention and its equivalents as described in the claims, as well as in the scope and spirit of the invention. EXAMPLES

[0038] The effect of the present invention was verified. (Verification example 1) (Example 1 of the present invention) First, a silica composition was formed. 50 g of spherical silica (FB-3SDC (particle size 3 μm): manufactured by Denka Co., Ltd.) and 0.25 g of decyltrimethoxysilane as a silane coupling agent were weighed and mixed for 5 minutes using a mixer (Thinky Mixer: manufactured by Thinky Co., Ltd.). This mixture was left at room temperature (25° C.) for 1 hour, and then heat-treated at 150° C. for 3 hours using a thermostatic bath. After this, it was washed with acetone to obtain a silica composition in which the surface of the spherical silica was covered with a silane coupling agent (coating layer).

[0039] Next, 100 parts by mass of a mixture of vinylidene fluoride and propylene hexafluoride was mixed with 3.0 parts by mass of magnesium oxide, 6.0 parts by mass of calcium hydroxide, and 5 parts by mass of the above-mentioned silica composition using a 6-inch roll to obtain a fluororubber composition. Then, this fluororubber composition was vulcanized to crosslink the polymer, thereby obtaining the fluororubber (sample) of Example 1 of the present invention.

[0040] (Example 2 of the present invention) This was the same as Inventive Example 1, except that the amount of the silica composition contained in the fluororubber composition was changed to 20 parts by mass.

[0041] (Example 3 of the present invention) This was the same as Inventive Example 1, except that the amount of the silica composition contained in the fluororubber composition was changed to 80 parts by mass.

[0042] Comparative Example 1 A fluororubber composition was obtained by mixing 100 parts by mass of a mixture of vinylidene fluoride and propylene hexafluoride with 3.0 parts by mass of magnesium oxide and 6.0 parts by mass of calcium hydroxide (no filler was included). Then, this fluororubber composition was subjected to a vulcanization treatment to copolymerize vinylidene fluoride and propylene hexafluoride, thereby obtaining the fluororubber (sample) of Comparative Example 1.

[0043] Comparative Example 2 This was the same as Inventive Example 1, except that the amount of the silica composition contained in the fluororubber composition was 100 parts by mass.

[0044] Comparative Example 3 A fluororubber composition was obtained by mixing 100 parts by mass of a mixture of vinylidene fluoride and propylene hexafluoride with 3.0 parts by mass of magnesium oxide, 6.0 parts by mass of calcium hydroxide, and 20 parts by mass of spherical silica (the spherical silica had no coating layer of a silane coupling agent). Then, this fluororubber composition was subjected to a vulcanization treatment to copolymerize vinylidene fluoride and propylene hexafluoride, thereby obtaining the fluororubber (sample) of Comparative Example 3.

[0045] The following tests were carried out using the above-mentioned samples of Inventive Examples 1 to 3 and Comparative Examples 1 to 3. (Hardness measurement) In accordance with JIS K6253:1997, the hardness (instantaneous value) of each sample formed by stacking three 2 mm rubber sheets was measured using a type A durometer.

[0046] (tensile strength, elongation, 100% tensile stress) The tensile strength, elongation, and 100% tensile stress were tested according to JIS K6251. JIS No. 3 dumbbell shapes were punched out from the molded sheets, and the tensile strength (MPa), maximum elongation (%) relative to the length before the test, and 100% tensile stress of each sample were measured using a tensile tester. The tensile strength is calculated by dividing the stress at the time of specimen breakage by the initial cross-sectional area of ​​the specimen, and the 100% tensile stress is calculated by dividing the stress when the specimen is elongated by 100% by the initial cross-sectional area of ​​the specimen.

[0047] (Compression set) The compression set was measured according to JIS K6262. The test was performed by compressing each sample by 25% at 250° C. and holding it for 72 hours, and measuring the percentage (%) of the compression set that was not restored to its thickness before the test started. The results of each test item as described above are summarized in Table 1.

[0048] [Table 1]

[0049] According to the results shown in Table 1, inventive examples 1 to 3, the compression set at 250°C, which is an index of heat resistance, was all less than 40%, confirming that they had superior heat resistance compared to comparative examples 1 to 3, all of which had a compression set exceeding 40%. It was also confirmed that inventive examples 1 to 3, the tensile strength, elongation, and 100% tensile stress were equal to or greater than comparative examples 1 and 3, which did not contain spherical silica covered with a silane coupling agent.

[0050] (Verification example 2) Next, when forming the silica composition, the fluororubber (sample) was formed using the fluororubber composition formed by changing the type of silane coupling agent, and the compression set and tensile strength were measured. The sample was prepared in the same manner as in Example 1 of the present invention in Example 1 of Verification Example 1, except that the type of silane coupling agent was changed. The types of silane coupling agents used are as follows: Decyltriethoxysilane (alkyl type) Vinyltrimethoxysilane (vinyl type) 3-Glycidoxypropyltrimethoxysilane (epoxy type) 3-Aminopropyltrimethoxysilane (amino type) Trimethoxy-normal-octylsilane (alkyl type) Triethoxy-normal-octylsilane (alkyl type) Decyltrimethoxysilane (alkyl type) Dodecyltrimethoxysilane (alkyl type)

[0051] The compression set (%) of the fluororubbers containing the silica compositions using these respective silane coupling agents at 250° C. for 72 hours is shown in FIG 2. The tensile strength (MPa) is also shown in FIG 3.

[0052] According to Figure 2, the compression set does not change significantly depending on the type of silane coupling agent, but silane coupling agents with ethoxy groups tend to have better compression set than silane coupling agents with methoxy groups. It was confirmed that when vinyl and epoxy silane coupling agents were used, a large amount of white foreign matter was generated in the obtained fluororubber.

[0053] It was also confirmed that the fluororubbers containing silica compositions using triethoxy-normal-octylsilane and decyltriethoxysilane as silane coupling agents had particularly excellent tensile strength. [Industrial Applicability]

[0054] The fluororubber composition and fluororubber molded product of the present invention can provide a fluororubber having high heat resistance at low cost by dispersing a silica composition in which spherical silane is covered with a coating layer made of a silane coupling agent in a binary FKM, and therefore have industrial applicability.

Claims

1. A fluororubber composition containing vinylidene fluoride and hexafluoropropylene as binary fluororubber raw materials, a spherical silica composition, at least one of magnesium oxide and hydrotalcite, and calcium hydroxide, The silica composition is composed of spherical silica and a coating layer containing a silane coupling agent that covers the surface of the spherical silica, The fluororubber composition is characterized in that the silica composition is contained in an amount of 1 part by mass or more and 80 parts by mass or less per 100 parts by mass of the binary fluororubber raw material.

2. 2. The fluororubber composition according to claim 1, wherein the silane coupling agent is an alkyl-based silane coupling agent or a fluorine-based silane coupling agent.

3. 3. A fluororubber molded article, obtained by molding a fluororubber obtained by copolymerizing vinylidene fluoride and hexafluoropropylene in the fluororubber composition according to claim 1 or 2.

4. 4. The fluororubber molded article according to claim 3, wherein the fluororubber has a compression set rate of less than 40% at 250° C. for 70 hours.

Citation Information

Patent Citations

  • Fluororubber composition, vulcanizable fluororubber composition, inner layer material for fuel hose, vulcanizable fluororubber laminate, rubber material for fuel and fuel hose

    JP2004131543A

  • Fluororubber composition and sealant comprising the composition

    JP2005306931A

  • Fluorine-containing elastomer composition and molded article comprising the same

    JP2006316112A

  • Rubber compound composition

    JP2007302812A

  • Fluororubber composition

    JP2010126721A

Cited By

  • Modified perfluoroether rubber as well as preparation method and application thereof

    CN120484412A

  • Active material-conductive agent composite, electrode for rechargeable battery including active material-conductive agent composite, rechargeable battery, and non-aqueous electrolyte rechargeable battery

    CN121601609A

  • Peroxide-crosslinked fluororubber composition, rubber molded article, and fluororubber cured product

    WO2026079069A1