Method for preventing corrosion of metal member
By adding phosphorus and zinc compounds to cooling water and polyamines to steam, along with scale inhibitors, the method addresses corrosion issues in metal parts exposed to alternating steam and cooling water, ensuring effective corrosion protection and heat transfer.
Patent Information
- Application Number
- JP2023091035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-12
- Estimated Expiration
- 2043-06-01
AI Technical Summary
Conventional corrosion prevention methods fail to adequately protect metal parts that alternately contact steam and cooling water, leading to corrosion product accumulation and reduced heat transfer efficiency, necessitating frequent cleaning.
A method involving the addition of phosphorus compounds and/or zinc compounds to cooling water, and an anticorrosive film-forming substance, such as polyamines, to both the cooling water and steam, along with a scale inhibitor like (meth)acrylic acid polymers, to form a protective film on metal surfaces.
This approach effectively prevents corrosion and maintains heat transfer efficiency by forming a durable film on metal surfaces exposed to alternating steam and cooling water, reducing maintenance needs.
Smart Images

Figure 2024172953000001 
Figure 2024172953000002 
Figure 2024172953000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preventing corrosion of metal members, and more particularly to a method for preventing corrosion of metal members of a reactor, a molding machine, or the like that are alternately in contact with steam and cooling water. [Background technology]
[0002] In order to inhibit corrosion of carbon steel heat exchangers and piping in an open circulating cooling water system, phosphorus compounds such as orthophosphates, hexametaphosphates, hydroxyethylidenephosphonates, and phosphonobutanetricarboxylates, zinc salts, dichromates, and the like are sometimes added to the cooling water alone or in combination (Patent Document 1).
[0003] When the above-mentioned corrosion inhibitor is added to the cooling water to prevent corrosion of metal components such as a reactor vessel that is alternately in contact with steam and cooling water, the cooling water is diluted with the steam, reducing the concentration of the corrosion inhibitor, and therefore metal corrosion cannot be sufficiently suppressed.
[0004] Patent Document 1 discloses a method for inhibiting metal corrosion in an aqueous system by adding low concentrations of phosphate and zinc salt (each 1 mg / L or less) and an M alkalinity component to the aqueous system to achieve a Langelier index of 1.2 or more at 30°C. However, in a reaction vessel in which steam and cooling water are in contact alternately, the cooling water is diluted by the steam, so that the concentration of the M alkalinity component is low, making it difficult to provide sufficient corrosion protection. Furthermore, when the reaction vessel is heated by steam, the reaction vessel becomes so hot that it exceeds the specification temperature of the cooling water system corrosion inhibitor, making it impossible to provide sufficient corrosion protection.
[0005] One method for inhibiting corrosion of carbon steel is to use a long-chain aliphatic amine, which is a film-forming substance (Patent Document 2). The mechanism of corrosion prevention using a long-chain aliphatic amine is that the long-chain aliphatic amine adsorbs onto the surface of the metal via the amino group to form a dense film of a monomolecular or polymolecular layer, thereby preventing contact between the metal and water and inhibiting corrosion of the metal.
[0006] In the corrosion prevention method using a long-chain aliphatic amine, if the long-chain aliphatic amine is not continuously added to the aqueous system, the adsorbed coating will peel off. Therefore, even if the corrosion prevention method using a long-chain aliphatic amine is applied to the corrosion prevention of metal members that are in contact with cooling water and steam alternately, a sufficient corrosion prevention effect cannot be obtained. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2009-299161 A [Patent Document 2] JP 2011-033301 A Summary of the Invention [Problem to be solved by the invention]
[0008] Conventional methods for preventing corrosion of metal members cannot sufficiently suppress corrosion of metal members that are in contact with steam and cooling water alternately, so that corrosion products accumulate on the metal surface over long periods of use, inhibiting heat transfer, resulting in reduced production and longer reaction times. Periodic cleaning is also required.
[0009] An object of the present invention is to provide a method for preventing corrosion of metal members, which can sufficiently prevent corrosion of metal members that are alternately in contact with steam and cooling water. [Means for solving the problem]
[0010] The corrosion protection method for metal components of the present invention is a method for protecting metal components that are alternately in contact with cooling water and steam, and is characterized by adding a phosphorus compound and / or a zinc compound to the cooling water and adding a corrosion-resistant film-forming substance to the steam.
[0011] In one aspect of the present invention, the metal member is a steel reaction kettle or molding machine.
[0012] In one embodiment of the invention, the phosphorus compound is at least one of hexametaphosphoric acid, tripolyphosphoric acid, orthophosphoric acid, phosphonobutanetricarboxylic acid, hydroxyethylidene diphosphonic acid (HEDP), and aminotrimethylphosphonic acid.
[0013] In one embodiment of the invention, the corrosion protective film-forming material is an anodic inhibitor.
[0014] In one embodiment of the present invention, the corrosion-protective film-forming substance is a polyamine represented by the following formula:
[0015] R1-[NH-(CH2) m ] n -NH2…(1) (In the formula, R1 represents a saturated or unsaturated hydrocarbon group having 10 to 22 carbon atoms, m represents an integer of 1 to 8, and n represents an integer of 1 to 7. When n is 2 or more, a plurality of NH-(CH2) m may be the same or different.)
[0016] In one embodiment of the present invention, a (meth)acrylic acid-based polymer is further added to the cooling water as a scale inhibitor.
[0017] In one embodiment of the present invention, the ratio A / B of the amount A of the scale inhibitor to the amount B of the anticorrosive film-forming substance is set to 6 or less. Effect of the Invention
[0018] In the method for protecting metal members from corrosion of the present invention, a phosphorus compound and / or a zinc salt is added to the cooling water, and a substance for forming a corrosion-resistant film, such as a polyamine and / or a sarcosine, is added to the steam.
[0019] This provides an excellent anticorrosive effect even for metal members that are alternately in contact with steam and cooling water, such as a reactor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The corrosion protection method for metal components of the present invention is a method for protecting metal components that are alternately in contact with cooling water and steam, in which a phosphorus compound and / or a zinc compound is added to the cooling water, and a corrosion-protective film-forming substance is added to the steam.
[0021] The metal member is preferably a steel member that alternately comes into contact with steam and cooling water, and examples of such members include a reaction vessel and a heating / cooling type molding machine. The metal member may be a carbon steel member, a stainless steel member, etc. The temperature of the steam is preferably about 150 to 200°C, and the temperature of the cooling water is preferably about 10 to 40°C.
[0022] The phosphorus compound to be added to the cooling water is preferably phosphoric acid or a phosphate, and specific examples thereof include inorganic phosphoric acid (orthophosphoric acid, polymeric phosphoric acid) and its salts, organic phosphoric acid and its salts or its esters, and various phosphonic acids, which can be used alone or in combination of two or more. As the salt, sodium salts, potassium salts, etc. are preferred.
[0023] Suitable phosphoric acids and phosphates include hexametaphosphoric acid, tripolyphosphoric acid, orthophosphoric acid, phosphonobutanetricarboxylic acid (PBTC), hydroxyethylidene diphosphonic acid (HEDP), aminotrimethylphosphonic acid, and salts thereof.
[0024] The amount of the phosphorus compound added is preferably about 2.0 to 12.0 mg / L, particularly about 5.0 to 7.0 mg / L in terms of PO4.
[0025] The zinc salt to be added to the cooling water is preferably zinc chloride, zinc sulfate, zinc nitrate, zinc acetate, zinc malate, zinc citrate, etc., and these can be used alone or in combination of two or more. The amount of zinc salt to be added is preferably about 0.5 to 5.0 mg / L, particularly preferably about 1.0 to 3.0 mg / L.
[0026] The anticorrosive film-forming material is preferably added directly to the steam, but may also be added to boiler water or the like.
[0027] As the anticorrosive film forming substance, an anodic inhibitor is preferred, specifically, a polyamine or a sarcosine, particularly a polyamine.
[0028] A preferred polyamine is represented by the following general formula (1):
[0029] R1-[NH-(CH2) m ] n -NH2…(1) (In the formula, R1 represents a saturated or unsaturated hydrocarbon group having 10 to 22 carbon atoms, m represents an integer of 1 to 8, and n represents an integer of 1 to 7. When n is 2 or more, a plurality of NH-(CH2) m may be the same or different.)
[0030] The saturated or unsaturated hydrocarbon group for R1 may be linear, branched, or cyclic, and examples thereof include alkyl groups, alkenyl groups, alkadienyl groups, and alkynyl groups. Preferred are linear alkyl groups and linear alkenyl groups, and the number of carbon atoms for R1 is preferably 15 to 22.
[0031] m is an integer of 1 to 8, and from the viewpoint of corrosion inhibition, is preferably an integer of 2 to 6. (CH2) m Examples of the group include a methylene group, an ethylene group (dimethylene group), a propylene group (trimethylene group) or a butylene group (tetramethylene group), with a propylene group being preferred.
[0032] Moreover, n is preferably an integer of 1 to 3 from the viewpoint of corrosion inhibition.
[0033] Specific examples of such polyamines include dodecylaminomethyleneamine, dodecylaminodimethyleneamine, dodecylaminotrimethyleneamine (N-stearyl-1,3-propanediamine), and the tetradecyl, hexadecyl and octadecyl compounds corresponding to these polyamines, octadecenylaminotrimethyleneamine, octadecenylaminodi-(trimethylamino)-trimethyleneamine, palmitylaminotrimethyleneamine and the like. Of these, N-oleyl-1,3-propanediamine (i.e., N-octadecenylpropane-3-diamine), which is readily available with sufficient purity, is preferred.
[0034] These polyamines may be dissolved in a solvent such as methanol, ethanol, isopropanol, etc. and then added to the steam or feed water, but it is preferable to make an aqueous emulsion and add this to the steam or boiler feed water.
[0035] The polyamines may be used alone or in combination of two or more kinds.
[0036] Furthermore, long-chain aliphatic amines such as octadecylamine and oleylamine may be used in combination within a range that does not cause clogging.
[0037] The polyamine is preferably present in an amount of 0.01 to 10 ppm, particularly 0.1 to 1 ppm, based on the amount of steam. If the amount of polyamine is less than this range, the polyamine cannot fully suppress the formation of a condensed water film and improve the heating efficiency, whereas if the amount is too much, sticky deposits may form in the system.
[0038] The term "ppm" refers to the weight ratio of polyamine to water corresponding to the amount of steam, and corresponds to "mg / L-water."
[0039] As the sarcosines, unsaturated and saturated C6 to C24 alkyl sarcosines, in particular oleyl sarcosine, beef tallow sarcosine and mixtures thereof can be used.
[0040] In the present invention, a scale inhibitor may be added to the cooling water. A (meth)acrylic acid-based polymer is suitable as the scale inhibitor. The (meth)acrylic acid-based polymer is preferably a copolymer containing (meth)acrylic acid and an unsaturated monomer having a sulfonic acid group, or a salt thereof. The polymer is preferably an AA / AMPS (acrylic acid / 2-acrylamido-2-methylpropanesulfonic acid copolymer)-based polymer having a sulfonic acid group, or an AA / HAPS (acrylic acid / hydroxyallyloxypropanesulfonic acid copolymer)-based polymer. The molecular weight is preferably 4,000 to 30,000, more preferably 5,000 to 20,000. The AA / AMPS ratio and the AA / HAPS ratio are both preferably 60 to 95:40 to 5, more preferably 75 to 90:25 to 10.
[0041] In the present invention, a tracer substance of the scale inhibitor may further be added to the cooling water.
[0042] The method of the present invention is preferably applied when the temperature rise rate of the metal member is 10° C. / hour or more.
[0043] In the present invention, it is preferable to start the above-mentioned corrosion prevention method after removing rust from the metal member, so that an anticorrosive film is easily formed on the metal surface, and the corrosion prevention effect can be improved.
[0044] In this case, after removing the rust, and before starting the corrosion prevention method, a high concentration of phosphorus or zinc (for example, a total phosphorus concentration of 70 to 120 mgPO4 / L, a zinc concentration of 10 to 30 mgZn / L) may be added to the water that will be in contact with the metal member. In this way, a strong corrosion prevention film can be formed on the metal surface in advance, and a high corrosion prevention effect is likely to be maintained for a long period of time. Furthermore, a corrosion prevention film may be formed in advance by adding the above-mentioned corrosion prevention film forming substance before starting the corrosion prevention method.
[0045] The order of removing rust from the metal components before starting the corrosion prevention method, adding high concentrations of phosphorus or zinc, and adding the corrosion prevention film-forming substance may be reversed, or none of them may be performed.
[0046] In the present invention, the concentration of the corrosion-resistant film-forming substance in the cooling water may be controlled in proportion to one or more of the temperature, electrical conductivity, pH, dispersant concentration, tracer substance concentration, and Langelier index of the cooling water in the heat exchanger or at the outlet of the heat exchanger through which the cooling water passes.
[0047] In the present invention, the calcium hardness of the cooling water in the heat exchanger may be calculated from the calcium hardness and electrical conductivity of the cooling tower make-up water and the electrical conductivity of the cooling water in the heat exchanger, and when the calcium hardness is a predetermined concentration or less (e.g., 30 mg / L or less), the concentration of the film-forming substance in the cooling water in the heat exchanger may be controlled to be a predetermined concentration or more (e.g., 0.1 mg / L or more).When the calcium hardness having an anticorrosive effect in the cooling water is low and the anticorrosive effect is reduced, the anticorrosive effect can be improved by increasing the concentration of the remaining film-forming substance.
[0048] In the present invention, a corrosion-resistant film-forming substance may be added to the cooling water in batches. By adding a film-forming substance to the cooling water in addition to the film-forming substance derived from steam and remaining therein, the corrosion prevention effect can be improved.
[0049] In the present invention, the film-forming substance may be added in batches to the cooling water in the piping immediately prior to the metal member immediately prior to the start of the temperature increasing step for the metal member.
[0050] Furthermore, in the present invention, when the piping in the system is made of carbon steel, the accumulation of iron carried over from the piping to the heat exchanger can be reduced, and the inhibition of heat transfer in the heat exchanger can be reduced. EXAMPLES
[0051] [Corrosion prevention evaluation tests 1 to 3 (simulating examples)] <Experimental conditions> <Preparation of test water 1> Pure water (30°C) was placed in a 1L glass beaker, and the calcium hardness and acid consumption (pH 4.8) were adjusted to 150mgCaCO3 / L using a sodium bicarbonate solution and a calcium chloride solution. As a corrosion inhibitor, 6mgPO4 / L of the phosphorus compound in Table 2 and 3mgZn / L of zinc chloride as a zinc compound were added, and 10mg / L of AA / AMPS polymer (monomer ratio 80:20, weight average molecular weight 20,000) was added as a scale inhibitor (test water 1: cooling water in Table 1).
[0052] <Preparation of test water 2> Test water (temperature 80°C) was prepared by diluting the same chemicals so that the concentration of each component was 1 / 5 (test water 2: steam system in Table 1). After adding the scale inhibitor, 0.3 mg / L of N-octadecenylpropane-1,3-diamine (OLDA) was added as a polyamine, which is a film-forming substance, to test water 2.
[0053] <Test piece> The test specimens used were SPCC (50 mm x 30 mm x 1 mm).
[0054] <Test procedure> The test piece was hung on a copper wire covered with vinyl chloride and immersed in the test water 1. Beaker 1 of test water 1 was placed in a thermostatic bath set at 30°C, and stirred for 20 hours by rotating the stirrer at 250 rpm using a magnetic stirrer.
[0055] Thereafter, the test piece was removed from the beaker 1 and transferred to a beaker 2 of test water 2 placed in a thermostatic bath set at 80° C., and stirred with a magnetic stirrer at 250 rpm for 5 hours.
[0056] After the test, the test piece was removed from the beaker 2, and the corrosion products adhering to the surface of the test piece were washed off with acid, then the test piece was dried and weighed. The corrosion weight loss was calculated from the difference between the dry weight of the test piece after the test and the weight before the test. The results are shown in Table 2.
[0057] [Test Examples 4 to 6 (simulating comparative examples)] Tests were conducted in the same manner as in Test Examples 1 to 3, except that the presence or absence and types of phosphorus compounds and zinc compounds in Test Waters 1 and 2, and the presence or absence of polyamine in Test Water 2 were as shown in Table 2, and the corrosion weight loss was calculated. The results are shown in Table 2.
[0058] [Table 1]
[0059] [Table 2]
[0060] <Results / Discussion> As shown in Table 2, in Test Examples 1 to 3, in which a phosphorus compound, a zinc salt, and a polyamine were used in combination, sufficient corrosion inhibition effects were obtained even at low corrosion inhibitor concentrations and in high-temperature environments, and this can contribute to maintaining the heat transfer efficiency of heat exchangers and equipment maintenance.
[0061] [Residual evaluation test of anticorrosive film forming substances when used in combination with scale inhibitors] 1000 mL of room temperature pure water was placed in a 1 L glass beaker, and 0.3 mg / L of N-octadecenylpropane-1,3-diamine (OLDA) was added as a corrosion-resistant film-forming substance, and AA / AMPS polymer (monomer ratio 80:20, weight average molecular weight 20,000) was added as a scale inhibitor to the concentration shown in Table 3. The mixture was stirred for 30 minutes to prepare test waters 1 to 6.
[0062] After each test water 1 to 6 was left to stand for 30 minutes, the residual OLDA concentration in the supernatant was measured. The OLDA concentration was analyzed by the Bengal Rose method described in Power Plant Chemistry 2015, 17(1). The results are shown in Table 3.
[0063] [Table 3]
[0064] <Results / Discussion> As shown in Table 3, when OLDA is used in combination with AA / AMPS polymer, the OLDA and AA / AMPS polymer co-precipitate, decreasing the OLDA concentration. It was presumed that by setting the [AA / AMPS] / [OLDA] value to 6 or less, especially 3 or less, the concentration of OLDA remaining in the cooling water increases, improving the corrosion prevention effect.
Claims
1. A method for preventing corrosion of a metal member that is alternately in contact with cooling water and steam, comprising the steps of: A method for preventing corrosion of metal members, comprising adding a phosphorus compound and / or a zinc compound to cooling water and adding a substance for forming a corrosion-resistant film to steam.
2. 2. The method for preventing corrosion of a metal member according to claim 1, wherein the metal member is a steel reaction vessel or a molding machine.
3. 2. The method for preventing corrosion of a metal member according to claim 1, wherein the phosphorus compound is at least one of hexametaphosphoric acid, tripolyphosphoric acid, orthophosphoric acid, phosphonobutanetricarboxylic acid, hydroxyethylidene diphosphonic acid (HEDP), and aminotrimethylphosphonic acid.
4. 2. The method for protecting metal members against corrosion according to claim 1, wherein the anticorrosive film-forming substance is an anodic inhibitor.
5. 2. The method for protecting metal members against corrosion according to claim 1, wherein the anticorrosive film-forming substance is a polyamine represented by the following formula: R 1 -[NH-(CH 2 ) m ] n -NH 2 …(1) (In the formula, R 1 represents a saturated or unsaturated hydrocarbon group having 10 to 22 carbon atoms, m is an integer of 1 to 8, and n is an integer of 1 to 7. When n is 2 or more, a plurality of NH-(CH 2 ) m may be the same or different.)
6. 6. The method for preventing corrosion of a metal member according to claim 1, further comprising adding a (meth)acrylic acid-based polymer as a scale inhibitor to the cooling water.
7. 7. The method for protecting metal members against corrosion according to claim 6, wherein a ratio A / B of an amount A of the scale inhibitor to an amount B of the anticorrosive film-forming substance is set to 6 or less.
Citation Information
Patent Citations
System for automatically controlling heating and cooling of high-pressure reaction kettle
CN210022050U
Method for providing corrosion protection in a water-steam circuit
JP2022532692A
Method for providing corrosion protection to a pressurized water-steam system
WO2021246367A1
Metal corrosion suppression method of water system
JP2009299161A
Corrosion suppressing method and corrosion suppressing device for boiler device
JP2011033301A