Electrochemical and Electronic Devices

By optimizing the composition of organic solvents, lithium salts, and additives, along with controlled negative electrode pore structures, the electrochemical device addresses the challenge of improving charging capacity and reducing charging temperature, enhancing the performance and longevity of lithium-ion batteries.

JP2024539314AActive Publication Date: 2024-10-28DONGGUAN AMPEREX TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024525183
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-09-29
Publication Date
2024-10-28
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

The challenge of improving charging capacity and reducing the rise in charging temperature in electrochemical devices, particularly lithium-ion batteries, is urgent due to the increasing demands of modern technology.

Method used

The electrochemical device incorporates a specific composition of organic solvents, lithium salts, and additives, including acetate ester compounds, carbonate compounds, and polynitrile compounds, with controlled mass fractions, along with optimized negative electrode pore structures, to enhance cycle characteristics and reduce charging temperature.

Benefits of technology

The solution improves the cycle characteristics and reduces the increase in charging temperature, resulting in enhanced performance and longevity of electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539314000001
    Figure 2024539314000001
  • Figure 2024539314000002
    Figure 2024539314000002
  • Figure 2024539314000003
    Figure 2024539314000003
Patent Text Reader

Abstract

The present invention provides an electrochemical device and an electronic device, the electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, the electrolyte comprising an organic solvent, a lithium salt and an additive, the organic solvent comprising an acetate compound and a carbonate compound, the carbonate compound comprising ethylene carbonate and propylene carbonate, and the mass fraction A of the acetate compound is 4%-50%, and the mass fraction B of the ethylene carbonate is 5%-20%, relative to the total mass of the electrolyte. The present invention optimizes the content and type of the solvent in the electrolyte and utilizes the interface modification effect of the additive to improve the charging ability of the electrochemical device and reduce the rise in charging temperature during charging.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS The present invention claims priority to a Chinese patent application having application number 202111243754.6, filing date October 25, 2021, and title "Electrochemical Device and Electronic Device", the entire content of which is incorporated herein by reference.

[0002] The present invention relates to the technical field of energy storage, in particular electrochemical and electronic devices. [Background technology]

[0003] Electrochemical devices such as lithium-ion batteries have the advantages of high operating voltage, high energy density, environmental friendliness, stable cycle and safety, and are therefore widely used in fields such as wearable devices, smartphones, drones and laptops. With the development of modern information technology and the expansion of the application of electrochemical devices, the requirements for the charging capacity and charging temperature of electrochemical devices are becoming higher and higher. For this reason, in the technical field of energy storage, improving the charging capacity of electrochemical devices and reducing the rise in charging temperature have become problems that need to be solved as soon as possible. Summary of the Invention

[0004] The present invention aims to provide electrochemical and electronic devices that reduce the rise in charging temperature.

[0005] According to a first aspect of the present invention, there is provided an electrochemical device including a positive electrode, a negative electrode, and an electrolyte, the electrolyte including an organic solvent, a lithium salt, and an additive, the organic solvent including an acetate compound and a carbonate compound, the carbonate compound including ethylene carbonate (EC) and propylene carbonate (PC), and a mass fraction A of the acetate compound is 4% to 50%, and a mass fraction B of the ethylene carbonate is 5% to 20%, relative to the total mass of the electrolyte. After extensive investigation, the present inventors have found that the inclusion of the acetate compound and the carbonate compound in the organic solvent in the above amounts improves the cycle characteristics of the electrochemical device and reduces an increase in charging temperature.

[0006] In some embodiments of the first aspect of the present invention, the acetate compound comprises at least one of methyl acetate, ethyl acetate, and propyl acetate.

[0007] In some embodiments of the first aspect of the present invention, the electrolyte further comprises a polynitrile compound, the polynitrile compound comprising at least two of succinonitrile, adiponitrile, 1,3,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, ethylene glycol (bispropionitrile) ether, and 1,4-dicyano-2-butene. By selecting the polynitrile compound, the cycle characteristics of the electrochemical device can be further improved and the rise in charging temperature can be further reduced.

[0008] In some embodiments of the first aspect of the present invention, the mass fraction C of the polynitrile compound is 0.1% to 10%.

[0009] In some embodiments of the first aspect of the present invention, the mass fraction C of the polynitrile compound and the mass fraction A of the acetate compound satisfy the relationship of 0.1≦C / A≦0.8. By controlling the value of C / A within the range, the cycle characteristics of the electrochemical device can be improved.

[0010] In some embodiments of the first aspect of the present invention, the additive comprises fluoroethylene carbonate (FEC), and a mass fraction D of the fluoroethylene carbonate and a mass fraction E of the propylene carbonate satisfy the relationship 0.2≦D / E≦1.

[0011] In some embodiments of the first aspect of the present invention, the mass fraction E of the propylene carbonate is 5% to 30%, or the mass fraction D of the fluoroethylene carbonate is 0.1% to 15%. By controlling the mass fraction of the fluoroethylene carbonate or the mass fraction of the propylene carbonate within the above ranges, the cycle characteristics of the electrochemical device can be improved.

[0012] In some embodiments of the first aspect of the present invention, the lithium salt is LiPF6, and the mass fraction of the lithium salt is 10% to 20% with respect to the total mass of the electrolyte.

[0013] In some embodiments of the first aspect of the present invention, the compressed density of the negative electrode active material in the negative electrode is 1.40 g / cm 3 ~1.70g / cm 3 By controlling the compressed density of the negative electrode active material within the above range, the cycle characteristics of the electrochemical device can be further improved and the increase in charging temperature can be further reduced.

[0014] In some embodiments of the first aspect of the present invention, the negative electrode includes pores, the pores having (a) a pore diameter of 20 μm to 100 μm, (b) a pore depth range of 5 μm to 50 μm, and (c) a pore number per unit area of ​​0.5 pores / mm 2 ~100 pieces / mm 2 By controlling the pore diameter, pore depth, and number of pores per unit area of ​​the negative electrode pores within the above ranges, the cycle characteristics of the electrochemical device can be further improved and the increase in charging temperature can be further reduced.

[0015] A second aspect of the present invention provides an electronic device comprising an electrochemical device provided by the first aspect of the present invention.

[0016] The electrochemical device and electronic device of the present invention can improve the kinetic properties of the electrochemical device, increase the charging capacity, and reduce the rise in charging temperature by optimizing the content and type of the solvent in the electrolyte. The charging capacity can be further improved and the rise in charging temperature can be further reduced by adding an appropriate additive to the electrolyte.

[0017] Of course, it is not necessary for the practice of any one product or method of the present invention to achieve all of the above advantages simultaneously. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be described in more detail. Obviously, the described embodiments are only a part of the embodiments of the present invention, but are not all of the embodiments. Based on the embodiments in the present invention, all other embodiments that can be obtained by those skilled in the art without creative labor belong to the protection scope of the present invention. It should be noted that, in the present invention, the present invention is described by taking a lithium ion battery as an example of an electrochemical device, but the electrochemical device of the present invention is not limited to a lithium ion battery. Those skilled in the art should understand that the following description is merely an illustrative description and does not limit the scope of protection of the present invention.

[0019] Hereinafter, the embodiment of the present invention will be described in more detail with reference to examples and comparative examples. Various tests and evaluations are performed according to the following methods. In addition, "parts" and "%" are based on mass unless otherwise specified.

[0020] According to a first aspect of the present invention, there is provided an electrochemical device, the electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, the electrolyte comprising an organic solvent, a lithium salt and an additive, the organic solvent comprising an acetate compound and a carbonate compound, the carbonate compound comprising ethylene carbonate and propylene carbonate, a mass fraction A of the acetate compound is 4% to 50% relative to a total mass of the electrolyte, for example, the mass fraction A of the acetate compound may be 4%, 10%, 12%, 20%, 28%, 36%, 50%, or any range therebetween, and a mass fraction B of the ethylene carbonate is 5% to 20%, for example, the mass fraction B of the ethylene carbonate may be 5%, 8%, 11%, 14%, 17%, 20%, or any range therebetween.

[0021] As a result of the investigation, the inventors found that adjusting the organic solvent to contain an acetate compound and a carbonate compound and controlling the mass fraction of the acetate compound and ethylene carbonate within the above range contributes to improving the dissociation rate of the lithium salt and the stability of the solid electrolyte interface (SEI) film during the cycle process of the electrochemical device, thereby improving the kinetic characteristics of the electrochemical device, improving the cycle characteristics, and reducing the increase in charging temperature.

[0022] In some embodiments of the present invention, the acetate ester compound includes at least one of methyl acetate, ethyl acetate, and propyl acetate. Without being limited to any theory, the present inventors have found that the acetate ester compounds all have low viscosity, which is advantageous for improving the transport of lithium ions during charging and reducing the transport impedance, thereby reducing the rise in the charging temperature of the electrochemical device.

[0023] In some embodiments of the present invention, the electrolyte further comprises a polynitrile compound, the polynitrile compound comprising at least two of succinonitrile (SN), adiponitrile (AND), 1,3,6-hexanetricarbonitrile (HTCN), 1,2,3-tris(2-cyanoethoxy)propane (TCEP), ethylene glycol (bispropionitrile) ether (DENE), and 1,4-dicyano-2-butene (HEDN). Without being limited to any theory, the inventors have found that selecting a combination of at least two of the polynitrile compounds is advantageous for improving the stability of the SEI film during the cycling process of the electrochemical device, thereby improving the cycling characteristics of the electrochemical device and reducing the rise in charging temperature.

[0024] In some embodiments of the first aspect of the present invention, the mass fraction C of the polynitrile compound is 0.1% to 10%, for example, the mass fraction C of the polynitrile compound can be 0.1%, 1%, 2%, 4%, 6%, 8%, 10%, or any range therebetween.

[0025] In some embodiments of the first aspect of the present invention, the mass fraction C of the polynitrile compound and the mass fraction A of the acetate compound satisfy the relationship 0.1≦C / A≦0.8. For example, the value of C / A can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or any range therebetween. The inventors have found that when the value of C / A is too low, for example less than 0.1, the improvement of the cycle characteristics of the electrochemical device and the improvement of the increase in the charging temperature are not significant, and when the value of C / A is too high, for example more than 0.8, the content of the polynitrile compound is too high, the content of the acetate ester is too low, or the viscosity of the electrolyte increases, resulting in large polarization during the cycle process, which affects the increase in the charging temperature and the cycle characteristics of the electrochemical device. By controlling the value of C / A within the above range, it is advantageous to further improve the cycle characteristics of the electrochemical device and further reduce the increase in the charging temperature.

[0026] In some embodiments of the present invention, the additive comprises fluoroethylene carbonate (FEC), a mass fraction of the fluoroethylene carbonate is D, and the mass fraction of the fluoroethylene carbonate, D, and the mass fraction of the propylene carbonate, E, satisfy the relationship 0.2≦D / E≦1. For example, the value of D / E can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any range therebetween. Without being limited to any theory, the present inventors have found that when the ratio of the mass fraction of FEC to the mass fraction of propylene carbonate is too low, for example, when D / E is less than 0.2, the viscosity of the solvent is high, so that the internal resistance of the lithium ion battery increases, the rise in charging temperature increases, and at the same time, the protection of the anode is insufficient, and the cycle performance is poor; when the ratio of the mass fraction of FEC to the mass fraction of propylene carbonate is too high, for example, when D / E is more than 1, the dissociation of the lithium salt is insufficient, the rise in temperature increases, and at the same time, the content of FEC is too high, the high temperature stability is poor, and the cycle performance is poor. By controlling the ratio of the mass fraction of fluoroethylene carbonate to the mass fraction of propylene carbonate within the above range, it is favorable to improve the cycle performance of the electrochemical device and reduce the rise in charging temperature.

[0027] In some embodiments of the present invention, the mass fraction E of the propylene carbonate is 5% to 30%, or the mass fraction D of the fluoroethylene carbonate is 0.1% to 15%, for example, E can be 5%, 10%, 12%, 14%, 16%, 18%, 20%, 30%, or any range therebetween, and D can be 0.1%, 1%, 3%, 5%, 7%, 9%, 11%, 15%, or any range therebetween.

[0028] In some embodiments of the present invention, the lithium salt is LiPF6, and the mass fraction of the lithium salt is 10% to 20% based on the total mass of the electrolyte. For example, the mass fraction of the lithium salt can be 10%, 12%, 14%, 16%, 18%, 20%, or any range therebetween. Without being limited to any theory, the present inventors have found that controlling the mass fraction of the lithium salt within the above range is advantageous in improving electrical conductivity during cycling of the electrochemical device, thereby improving the cycling characteristics of the electrochemical device.

[0029] In the present invention, the electrolyte may further include other non-aqueous solvents, and the present invention is not particularly limited to the other non-aqueous solvents, as long as the object of the present invention can be achieved. For example, the other non-aqueous solvents may include at least one of carboxylate compounds, ether compounds, and other organic solvents, but are not limited thereto. The carboxylate compounds may include at least one of methyl formate, ethyl formate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, and caprolactone, but are not limited thereto. The ether compounds may include at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran, but are not limited thereto. The other organic solvent may include, but is not limited to, at least one of dimethylsulfoxide, 1,2-dioxolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylmethylamide, trimethyl phosphate, triethyl phosphate, and trioctyl phosphate. The total mass fraction of the other non-aqueous solvents is 5% to 60% relative to the total mass of the electrolyte, and may be, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or any range therebetween.

[0030] In the present invention, the electrolyte may further contain other additives. The present invention is not particularly limited to the other additives as long as the object of the present invention can be achieved. For example, the other additives may include at least one of lithium tetrafluoroborate (LiBF4), vinyl sulfate (DTD), vinylidene carbonate (VC), vinyl sulfite (PS), and lithium bis(oxalato)borate (LiBOB), but are not limited thereto.

[0031] Some embodiments of the invention include a negative electrode, wherein the compressed density of the negative electrode active material in the negative electrode is 1.40 g / cm 3 ~1.70g / cm 3 For example, the compressed density of the negative electrode active material is 1.40 g / cm 3 , 1.45g / cm 3 , 1.50g / cm 3 , 1.55g / cm 3 , 1.60g / cm 3 , 1.65g / cm 3 , 1.70g / cm 3 Without being limited to any theory, the inventors believe that if the compressed density of the negative electrode active material is too low, e.g., less than 1.40 g / cm 3 If it is less than 1.70 g / cm, the contact between the negative electrode materials in the electrochemical device is insufficient, the electronic conduction and ionic conduction are hindered, the charging temperature increases, and the cycle characteristics become poor. If the compressed density of the negative electrode active material is too high, e.g., 1.70 g / cm 3 It has been found that if the compressed density of the negative electrode active material is greater than 100%, the negative electrode is prone to overvoltage, the charging ability is deteriorated, the charging temperature rises rapidly, and the cycle characteristics are deteriorated, and at the same time, there is a risk of material particles being crushed due to the overvoltage. By controlling the compressed density of the negative electrode active material within the above range, the cycle characteristics of the electrochemical device can be improved and the rise in charging temperature can be reduced.

[0032] In some embodiments of the present invention, the negative electrode material in the negative electrode comprises at least one of a carbon material, silicon, a silicon-oxygen material, and a silicon-carbon material, and the carbon material comprises at least one of natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, and soft carbon.

[0033] In some embodiments of the present invention, the negative electrode comprises pores, the pores having (a) a pore diameter of 20 μm to 100 μm, e.g., the pore diameter may be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any range therebetween; (b) a pore depth range of 5 μm to 50 μm, e.g., the pore depth may be 5 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, or any range therebetween; and (c) a pore number per unit area of ​​0.5 pores / mm. 2 ~100 pieces / mm 2 For example, the number of pores per unit area is 0.5 / mm 2 , 1 piece / mm 2 , 10 pieces / mm 2 , 20 pieces / mm 2 , 30 pieces / mm 2 , 40 pieces / mm 2 , 50 pieces / mm 2 , 60 pieces / mm 2 , 70 pieces / mm 2 , 80 pieces / mm 2 , 90 pieces / mm 2 , 100 pieces / mm 2 Without being limited to any theory, the present inventors have found that controlling the intensity of the infrared laser, drilling holes on the surface of the negative electrode piece, and controlling the pore size, pore depth, and number of pores per unit area within the above ranges is favorable for the infiltration of the electrolyte and the transport of lithium ions between the materials, and reduces the transport impedance, thereby improving the cycle characteristics of the electrochemical device and reducing the increase in charging temperature.

[0034] The positive electrode piece in the present invention is not particularly limited as long as it can achieve the object of the present invention. The positive electrode piece usually includes a positive electrode current collector and a positive electrode active material. The positive electrode current collector is not particularly limited and may be any positive electrode current collector known in the art, such as copper foil, aluminum foil, aluminum alloy foil, and composite current collector. The positive electrode active material is not particularly limited and may be any positive electrode active material in the prior art, such as at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, and lithium iron manganese phosphate.

[0035] In the present invention, the thickness of the positive electrode current collector and the thickness of the positive electrode active material are not particularly limited as long as the object of the present invention can be achieved. For example, the thickness of the positive electrode current collector is 8 μm to 12 μm, and the thickness of the positive electrode active material is 30 μm to 120 μm.

[0036] In the present invention, the positive electrode active material layer may further include a conductive agent, and the present invention is not particularly limited to the conductive agent as long as the object of the present invention can be achieved. For example, the conductive agent may include at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, Ketjen black, graphene, metal materials, and conductive polymers, but is not limited thereto. The carbon nanotubes may include, but are not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The carbon fibers may include, but are not limited to, vapor grown carbon fibers (VGCF) and / or nano carbon fibers. The metal materials may include, but are not limited to, metal powder and / or metal fibers. Specifically, the metal may include, but is not limited to, at least one of copper, nickel, aluminum, and silver. The conductive polymer may include, but is not limited to, at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene, and polypyrrole.

[0037] In the present invention, the positive electrode active material layer may further contain a binder. The present invention is not particularly limited to the binder as long as the object of the present invention can be achieved. For example, the binder can include, but is not limited to, polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymer, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, (1,1-difluoroethylene) polymer, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, and nylon.

[0038] The positive electrode may also optionally include a conductive layer located between the positive electrode current collector and the positive electrode active material layer. The present invention is not particularly limited to the composition of the conductive layer, and may be a conductive layer commonly used in the art, for example, the composition of the conductive layer may include the conductive agent and the binder, but is not limited thereto.

[0039] The negative electrode current collector in the present invention is not particularly limited, and may be a foil or porous plate of a metal such as copper, nickel, titanium, or iron or an alloy thereof, for example, a metal foil such as copper foil or a porous metal plate. The negative electrode active material layer includes a negative electrode active material, a conductive agent, an adhesive, and a thickener. The adhesive may be at least one of styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, and carboxymethylcellulose (CMC), and the thickener may be sodium carboxymethylcellulose (CMC). In the present invention, there is no particular limit to the thickness of the negative electrode current collector, and may be any material that can achieve the object of the present invention. For example, the thickness of the negative electrode current collector is 4 μm to 12 μm.

[0040] In the present invention, the negative electrode active material layer may further contain a conductive agent, and the present invention is not particularly limited to the conductive agent as long as the object of the present invention can be achieved.

[0041] In the present invention, the negative electrode active material layer may further contain an adhesive, and the present invention is not particularly limited to the adhesive, so long as the object of the present invention can be achieved.

[0042] The negative electrode may also optionally include a conductive layer located between the negative electrode current collector and the negative electrode active material layer. The present invention is not particularly limited to the composition of the conductive layer, which may be any conductive layer commonly used in the art.

[0043] The separator in the present invention is not particularly limited, and may be any material that can achieve the object of the present invention. The separator may include a substrate layer and a surface treatment layer. The present invention is not particularly limited to the material of the substrate layer, and for example, the material of the substrate layer may include at least one of polyethylene (PE), polypropylene (PP), polytetrafluoroethylene-based polyolefin (PO), polyester (e.g., polyethylene terephthalate (PET)), cellulose, polyimide (PI), polyamide (PA), spandex, and aramid, but is not limited thereto, and the type of the substrate layer may include at least one of woven film, nonwoven film (nonwoven fabric), microporous membrane, composite membrane, membrane paper, laminate film, and spun film, but is not limited thereto, and the material of the substrate layer is preferably PP. The separator of the present invention may have a porous structure, and the pore size is not particularly limited, and may be any material that can achieve the object of the present invention, and for example, the pore size may be 0.01 μm to 1 μm. In the present invention, the thickness of the separator is not particularly limited as long as the object of the present invention can be achieved, and the thickness of the separator can be, for example, 5 μm to 500 μm.

[0044] In the present invention, a surface treatment layer may be provided on at least one surface of the substrate layer, and the present invention is not particularly limited to the surface treatment layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or may be a layer formed by mixing a polymer and an inorganic material. The inorganic layer may include, but is not limited to, inorganic particles and an inorganic layer adhesive. The present invention is not particularly limited to the inorganic particles, and for example, the inorganic particles may include, but are not limited to, at least one of alumina, silica, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium oxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. The present invention is not particularly limited to the inorganic layer adhesive, and for example, the inorganic layer adhesive may include at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylic acid ester, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene, but is not limited thereto. The polymer layer includes a polymer, and the polymer material may include at least one of polyamide, polyacrylonitrile, acrylic acid ester polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene), but is not limited thereto.

[0045] The electrochemical device of the present invention is not particularly limited and may include any device that undergoes an electrochemical reaction. In some embodiments, the electrochemical device may include, but is not limited to, a lithium ion battery.

[0046] The manufacturing process of the electrochemical device is well known to those skilled in the art, and the present invention is not particularly limited, and may include, for example, a step of stacking a positive electrode piece, a separator, and a negative electrode piece in this order, and performing operations such as winding and folding as necessary to obtain an electrode assembly with a rolled structure, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag and sealing it to obtain an electrochemical device, or a step of stacking a positive electrode, a separator, and a negative electrode in order, fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly with a stacked structure, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag and sealing it to obtain an electrochemical device, but is not limited thereto. In addition, an overcurrent protection element, a lead plate, etc. may be placed in the packaging bag as necessary, which can prevent pressure rise and overcharge / overdischarge inside the electrochemical device.

[0047] A second aspect of the present invention provides an electronic device comprising an electrochemical device according to any of the above-mentioned embodiments of the present invention. The electrochemical device provided by the present invention has good cycle characteristics and low charging temperature rise, so that the electronic device provided by the present invention has a long life and good performance.

[0048] The electronic device of the present invention is not particularly limited and may be any electronic device known in the prior art. For example, the display device includes, but is not limited to, a notebook computer, a pen-input computer, a mobile computer, an electronic book player, a mobile phone, a portable facsimile, a portable copy machine, a portable printer, a stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini disc, a transceiver, an electronic organizer, a calculator, a memory card, a portable tape recorder, a radio, a backup power source, a motor, an automobile, a motorcycle, an assisted bicycle, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flashlight, a camera, a large-scale household storage battery, and a lithium ion capacitor.

[0049] Measurement method and device: Lithium Deposition Test: The battery was charged at 3C at 25°C up to 4.45V, then charged at a constant voltage of 0.05C at 4.45V, and discharged at a constant current of 1.0C up to 3.0V. After repeating this charge / discharge cycle 10 times, the battery was disassembled and the degree of lithium deposition was observed. Here, cases where no lithium deposition was found or the lithium deposition area was less than 2% are referred to as no lithium deposition, cases where the lithium deposition area was between 2% and 20% are referred to as slight lithium deposition, and cases where the lithium deposition area was more than 20% are referred to as heavy lithium deposition.

[0050] Temperature Rise Test: At a test temperature of 25°C, the battery was charged at a constant current of 0.5C to 4.45V, then charged at a constant voltage of 0.05C, and left to stand for 60 minutes. The lithium-ion battery was then discharged at a constant current of 0.5C to 3V, and left to stand for 60 minutes. The lithium-ion battery was then charged at a constant current of 6C to 4.45V, then charged at a constant voltage of 0.05C, and the temperature during this high current charging was monitored, and the test temperature of 25°C was subtracted to obtain the increase in charging temperature at 6C.

[0051] High temperature cycle test: The battery was placed in a thermostatic chamber at 45°C, charged at a constant current of 1.5C to 4.45V, charged at a constant voltage of 0.05C at 4.45V, and then discharged at a constant current of 1.0C to 3.0V, forming one charge / discharge cycle. This charge / discharge cycle was repeated 800 times, and the capacity retention rate was monitored. The 45°C cycle capacity retention rate = (discharge capacity at the 800th cycle / initial discharge capacity) x 100%.

[0052] Electrolyte content test: The cell was discharged and centrifuged, and the liquid obtained by centrifugation was subjected to GC-MS testing to detect the mass fraction of each component (acetate ester, EC, PC, and additives).

[0053] Compressed density test of negative electrode active material: The compressed density of the negative electrode active material was measured by the following method. Negative double-sided pole piece with an area of ​​1540.25 mm 2The weight and thickness of 20 small wafers were measured, and the compressed density of the negative electrode active material=(weight of small wafer−weight of substrate) / (1540.25×(thickness of both sides of small wafer−thickness of substrate))×1000 was calculated, and the average value was taken as the compressed density of the negative electrode in this example. The weight and thickness of the substrate (copper foil) were obtained by measuring the weight and thickness using an area without active material. The weights of the small wafer and the substrate were in mg. The thicknesses of both sides of the small wafer and the thickness of the substrate were in μm.

[0054] Pore ​​characteristic test on negative electrode strip: Pore ​​characteristic data (pore size, pore depth, number of pores per unit area) on the negative electrode pieces were obtained by scanning tunneling microscope examination.

[0055] Example 1 (1) Preparation of negative electrode pieces: The negative electrode active materials artificial graphite, styrene butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) were mixed in a mass ratio of 97.4:1.2:1.4, and then deionized water was added as a solvent to prepare a slurry with a solid content of 70 wt%, which was then uniformly stirred. The slurry was uniformly applied to one surface of a copper foil with a thickness of 8 μm, dried under conditions of 110 ° C, and cold rolled to obtain a negative electrode piece with a negative electrode active material layer applied on one side with a thickness of 150 μm, and then the above application process was repeated on the other surface of this negative electrode piece to obtain a negative electrode piece with a negative electrode active material layer applied on both sides. The negative electrode piece was cut to the specifications of (74 mm × 867 mm) and a tab was welded. It was set aside until it was used later.

[0056] (2) Preparation of positive electrode pieces: The positive electrode active material lithium cobalt oxide (LiCoO2), the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 96:2:2, N-methylpyrrolidone (NMP) was added as a solvent, and the mixture was stirred with a vacuum stirrer until the system became uniform, to obtain a positive electrode slurry with a solid content of 75 wt%. The positive electrode slurry was uniformly applied to an aluminum foil positive electrode current collector with a thickness of 12 μm, dried under conditions of 85 ° C, and cold rolled to obtain a positive electrode piece with a positive electrode active material layer thickness of 100 μm, and then the above application process was repeated on the other surface of this positive electrode piece to obtain a positive electrode piece with a positive electrode active material layer applied on both sides. The positive electrode piece was cut to a specification of 74 mm × 867 mm, and a tab was welded. It was set aside until it was used later.

[0057] (3) Preparation of electrolyte: In a glove box with an argon atmosphere and a water content of <10 ppm, ethylene carbonate (EC), propylene carbonate (PC), ethyl acetate (EA) and ethyl propionate (EP) were mixed uniformly, and then the fully dried lithium salt LiPF6 was dissolved in the non-aqueous solvent, and the additive fluoroethylene carbonate was added to finally obtain a basic electrolyte. Of these, the mass fraction of the lithium salt was 10%, the mass fractions of EC, PC, EA and FEC were 10%, 15%, 4% and 7.5%, respectively, and the remaining part in the electrolyte was ethyl propionate, where the ratio of the mass fraction of fluoroethylene carbonate to the mass fraction of ethylene carbonate was 0.5.

[0058] (4) Separator: A PE porous polymer film was used as the separator.

[0059] (5) Preparation of lithium-ion battery: A positive electrode piece, a separator, and a negative electrode piece were laminated in this order, a separator film was interposed between the positive electrode piece and the negative electrode piece to function as a separator, and then the resultant was wound up to obtain a bare battery. The bare battery was placed in an exterior foil, and the electrolyte prepared above was injected into the dried battery. The battery was then vacuum sealed, left to stand, formed, shaped, and other processes to complete the preparation of the lithium-ion battery.

[0060] In Examples 2 to 21, the process for preparing the negative electrode pieces, the process for preparing the positive electrode pieces, the process for preparing the electrolyte, the process for preparing the separator, and the process for preparing the lithium ion battery are all the same as those in Example 1, and the changes in the relevant preparation parameters and performance parameters are shown in Table 1.

[0061] Examples 22 to 43 and 46 were similar to Example 3, except that a polynitrile compound was added to the electrolytic solution of Example 3, and the type and content of the polynitrile compound, the total content of the polynitrile compound, and the ratio of the content of the polynitrile compound to the content of the acetate ester compound were adjusted as shown in Table 2.

[0062] Example 44 was the same as Example 2, except that a polynitrile compound was added to the electrolytic solution of Example 2, and the type and content of the polynitrile compound, the total content of the polynitrile compound, and the ratio of the content of the polynitrile compound to the content of the acetate ester compound were adjusted as shown in Table 2.

[0063] Example 45 was the same as Example 10, except that a polynitrile compound was added to the electrolytic solution of Example 10, and the type and content of the polynitrile compound, the total content of the polynitrile compound, and the ratio of the content of the polynitrile compound to the content of the acetate ester compound were adjusted as shown in Table 2.

[0064] In Examples 47 to 55, the compressed density of the negative electrode active material, and the pore diameter, pore depth, and number of pores per unit area of ​​the pores on the negative electrode pieces were adjusted based on the electrolytes of Examples 23 to 31 as shown in Table 3, and were otherwise similar to Examples 23 to 31.

[0065] In Comparative Example 1 to Comparative Example 7, the process for preparing the negative electrode pieces, the process for preparing the positive electrode pieces, the process for preparing the electrolyte, the process for preparing the separator, and the process for preparing the lithium ion battery are all the same as in Example 1, and the relevant preparation parameters and performance changes are shown in Table 1.

[0066] Tables 1 to 3 show the preparation parameters and performance tests for each of the Examples and Comparative Examples.

[0067] [Table 1] In Table 1, " / " indicates that the corresponding preparation parameter does not exist.

[0068] [Table 2]

[0069] [Table 3]

[0070] From Examples 1 to 10 and Comparative Examples 1 to 3, it can be seen that with an increase in the content of ethyl acetate, the lithium precipitation state and the rise in charging temperature are improved, but when the content of ethyl acetate is high, the cycle characteristics are degraded; when an acetate ester compound is not contained, lithium precipitation is deteriorated, the cycle characteristics are deteriorated, and the rise in charging temperature is significantly increased; when the content of acetate ester compound is too low, lithium is severely precipitated, the cycle characteristics are deteriorated, and the rise in charging temperature is increased; and when the content of acetate ester compound is too high, cycling is not possible, gas is generated, and capacity diving occurs.

[0071] From Example 3, Examples 11 to 13, Comparative Example 4, and Comparative Example 5, it can be seen that when the EC content is low, the interfacial stability is improved due to dissociation of the lithium salt, and the dynamic characteristics are improved, thereby improving the cycle characteristics; when the EC content is too high, the viscosity increases and the stability is deteriorated, and when the EC content is too low, the cycle characteristics are deteriorated and lithium is severely precipitated; and when the EC content is too high, the cycle characteristics are deteriorated and lithium is severely precipitated.

[0072] From Example 3, Examples 14 to 21, Comparative Example 6 and Comparative Example 7, it can be seen that when the FEC / PC value is within the range of the present invention, the lithium precipitation state and the increase in charging temperature are improved, and when the FEC / PC is too small, the cycle characteristics are deteriorated, and when the FEC / PC is too high, lithium is severely precipitated. From Examples 2, 3, 10, and 22 to 46, it is seen that the addition of a polynitrile compound further improves the stability of the SEI film during the cycle process, thereby improving the cycle characteristics.

[0073] From Example 40 and Examples 47 to 49, it is understood that the lithium deposition state and the rise in charging temperature are improved as the pore size of the pores on the negative electrode piece increases.

[0074] From Example 48, Example 50 and Example 51, it can be seen that when the pore depth range of the pores on the negative electrode piece is within the range of the present invention, the obtained lithium ion battery has slight or no lithium precipitation, the rise in charging temperature is low, and the cycle capacity retention rate is high. This shows that the lithium ion battery has good cycle characteristics, the problem of the rise in charging temperature is improved, and lithium is less likely to be precipitated during the cycle process.

[0075] From Example 48, Example 52 and Example 53, it can be seen that when the number of pores per unit area on the negative electrode piece is within the range of the present invention, the obtained lithium ion battery exhibits slight or no lithium precipitation, a low rise in charging temperature and a high cycle capacity retention rate, which indicates that the lithium ion battery has good cycle characteristics, the problem of the rise in charging temperature is improved, and lithium is less likely to be precipitated during the cycle process.

[0076] From Example 47, Example 54 and Example 55, it can be seen that when the compressed density of the negative electrode active material in the negative electrode piece is within the range of the present invention, the obtained lithium ion battery has slight or no lithium precipitation, the rise in charging temperature is low, and the cycle capacity retention rate is high. This shows that the lithium ion battery has good cycle characteristics, the problem of the rise in charging temperature is improved, and lithium is not easily precipitated during the cycle process.

[0077] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the present invention.

Claims

1. An electrochemical device comprising a positive electrode, a negative electrode, and an electrolyte, the electrolyte solution comprises an organic solvent, a lithium salt and an additive, the organic solvent comprises an acetate compound and a carbonate compound, The carbonate compound includes ethylene carbonate and propylene carbonate, an electrochemical device, wherein a mass fraction A of the acetate compound is 4% to 50%, and a mass fraction B of the ethylene carbonate is 5% to 20%, relative to a total mass of the electrolyte solution.

2. 10. The electrochemical device of claim 1, wherein the acetate compound comprises at least one of methyl acetate, ethyl acetate, and propyl acetate.

3. The electrolyte further comprises a polynitrile compound, 2. The electrochemical device of claim 1, wherein the polynitrile compound comprises at least two of succinonitrile, adiponitrile, 1,3,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, ethylene glycol (bispropionitrile) ether, and 1,4-dicyano-2-butene.

4. 4. The electrochemical device according to claim 3, wherein the mass fraction C of the polynitrile compound is 0.1% to 10%.

5. 4. The electrochemical device according to claim 3, wherein the mass fraction C of the polynitrile compound and the mass fraction A of the acetate compound satisfy 0.1≦C / A≦0.

8.

6. The additive comprises fluoroethylene carbonate; 2. The electrochemical device according to claim 1, wherein the mass fraction D of the fluoroethylene carbonate and the mass fraction E of the propylene carbonate satisfy 0.2≦D / E≦1.

7. 7. The electrochemical device of claim 6, wherein the mass fraction E of the propylene carbonate is between 5% and 30% or the mass fraction D of the fluoroethylene carbonate is between 0.1% and 15%.

8. The compressed density of the negative electrode active material in the negative electrode is 1.40 g / cm 3 ~1.70g / cm 3 2. The electrochemical device of claim 1 ,

9. The negative electrode includes pores, The pores are (a) the pore size is 20 μm to 100 μm; (b) the pore depth range is 5 μm to 50 μm; and (c) The number of pores per unit area is 0.5 / mm 2 ~100 pieces / mm 2 To be The electrochemical device according to claim 1 , wherein at least one of the following is satisfied:

10. An electronic device comprising an electrochemical device according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Lithium ion battery electrolyte and lithium ion battery using same

    CN105845984A

  • Electrolyte and lithium secondary battery comprising same

    CN107910586A

  • Lithium ion battery nonaqueous electrolyte and lithium ion battery

    CN109346772A

  • Low-temperature lithium ion battery considering both energy density and safety

    CN111525089A

  • Lithium ion battery negative electrode plate and lithium ion battery