Building board package and method for manufacturing building board package
The packaging method using interleaving paper with matched gloss and uneven shapes addresses gloss changes on building boards, ensuring consistent appearance by distributing pressure uniformly and preventing new gloss formation.
Patent Information
- Application Number
- JP2020166200
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Building boards used in constructing walls exhibit unwanted gloss changes due to pressure during transportation, especially noticeable in matte coatings, which can mar the appearance of exterior and interior walls.
A packaging method involving interleaving paper with specific gloss differences and microscopic uneven shapes is used to overlay building boards, ensuring the gloss levels of the paper and board surfaces match, allowing uniform pressure distribution and minimizing texture changes.
The packaging method effectively suppresses the formation of new gloss on building board surfaces, maintaining a consistent appearance during transportation and storage.
Smart Images

Figure 0007564673000002 
Figure 0007564673000003 
Figure 0007564673000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a package of building boards and a method for manufacturing the same. [Background technology]
[0002] Examples of building boards that make up the exterior and interior walls of buildings include ceramic siding boards and Inorganic boards such as ceramic boards are used. When constructing walls using building boards, A plurality of building boards are joined together in the vertical and horizontal directions. The building boards are packed and stored and transported in a state where the packages are loaded onto a transport pallet. The technology for packaging building boards is as follows: Patent document 1 describes how the coating surface of building boards is covered and protected with a thin sheet called interleaf paper. It is listed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-41546 A Summary of the Invention [Problem to be solved by the invention]
[0004] In some cases, the decorative surface of a building board is painted. When the coating film of the painted surface is pressed, the texture of the coating surface changes at the pressed point, creating a new This can result in a new gloss (i.e., the pressed area may have a higher gloss than the adjacent non-pressed areas). (The net reflectance of external light may be high.) This is because the coating surface has a high reflectance against a given texture. This is because the microscopic unevenness of the surface is microscopically deformed (e.g., flattened) by the pressure. It is believed that the building boards and building board packages (hereinafter referred to as packages) are stacked in multiple layers on a transport pallet. In the case of the building board (hereinafter referred to as "building board"), which is located at the bottom and receives the greatest load, This makes it easy for a new gloss to appear on the coating.
[0005] The building boards on which the above-mentioned gloss has been generated due to the pressing of the coating film are included in the building boards that make up the exterior and interior walls. When it is embedded in a wall, depending on the angle of the sunlight or lighting, the glossiness becomes noticeable and it can be seen on the exterior walls and This can damage the appearance of the interior walls. In particular, if the paint on the surface of the building board is a matte paint, The unintended gloss is easily noticeable and can mar the appearance of exterior and interior walls.
[0006] The present invention has been conceived under these circumstances, and its object is to Packaging body suitable for suppressing the occurrence of gloss caused by pressure in a coating film of the present invention, and its manufacturing method The purpose of this study is to provide the following: [Means for solving the problem]
[0007] According to a first aspect of the present invention, a package is provided. The package comprises a first building board and an interleaf paper superimposed on the first building board. The first building board has a first surface including a first coating surface and a second surface opposite the first surface. The interleaf paper has a third surface on the first building board side and a fourth surface opposite the third surface. The third surface is in contact with the first coating surface. The first coating surface and the third surface, 60 degree gloss measured in accordance with JIS Z 8741 The absolute value of the difference is 3.0 or less, and the first coating surface and the third surface, 85 degree gloss measured according to JIS Z 8741 The absolute value of the difference is less than or equal to 3.0.
[0008] In this package, the first and third coating surfaces that come into contact with each other correspond to each other's gloss. The surface has a microscopic uneven shape. In gloss measurement, the incidence angle is relatively small at 60 degrees. The difference in gloss between the first and third coating surfaces when measuring the gloss, and the gloss at a relatively large incident angle of 85 degrees The more the difference between the first and third coating surfaces is 3.0 or less, the better the first coating surface is. The microscopic uneven shape and the microscopic uneven shape of the third surface are similar to each other.
[0009] In such a package, the first coating surface of the first building board is pressed by the third surface of the interleaf paper. Even if the pressed portion is deformed microscopically, the deformation is the microscopic unevenness of the pressed portion before deformation. This is caused by the microscopic unevenness of the third surface, which is similar to the shape of the third surface (for example, The uneven shape is transferred to the first coating surface. Therefore, at the pressed part on the first coating surface, , changes in texture are suppressed and new gloss is less likely to occur.
[0010] As described above, the packaging body according to the first aspect of the present invention is a packaging material that prevents the pressure rise of the coating film on the surface of the building board. It is suitable for suppressing the occurrence of gloss, which is a cause of paint damage.
[0011] The package of the present invention preferably includes a second building board overlapped with a first building board via an interleaving paper. The second building board further includes a fifth surface on the first building board side and a sixth surface on the opposite side to the fifth surface. The fifth surface includes the second coating surface. The fourth surface of the interleaving paper on the second building board side includes the second The absolute value of the difference between the 60 degree gloss of the second coating surface and the 60 degree gloss of the fourth coating surface is 3.0 or less, and the absolute difference between the 85 degree gloss of the second coating surface and the 85 degree gloss of the fourth surface The contrast value is less than 3.0.
[0012] In such a configuration, the second coating surface and the second building board and the interleaving paper contact each other. The fourth surface has microscopic irregularities corresponding to the respective gloss levels. The difference in gloss between the second and fourth coating surfaces when measuring the gloss at a relatively small angle of incidence of 60 degrees is shown in Fig. When measuring gloss at a relatively large angle of incidence of 85 degrees, the difference between the second and fourth coating surfaces was 3. 0 or less, the closer the microscopic unevenness of the second coating film surface and the microscopic unevenness of the fourth coating film surface are to each other. In such a package, the second coating surface of the second building board is held in place by the fourth surface of the interleaving paper. Even if the pressed part is deformed microscopically, the deformation is the same as the deformation at the pressed part before the deformation. The microscopic unevenness of the fourth surface, which is similar to the microscopic unevenness of the fourth surface, is transferred to the second coating surface. Therefore, the change in texture is suppressed at the pressed portion of the second coating surface. This prevents new gloss from forming.
[0013] In a preferred embodiment of the first aspect of the present invention, the third surface of the interleaf paper is abutted against the first building board. The third surface of the slip sheet has a concave-convex shape with multiple evenly arranged micro-projections. The evenly-spaced configuration is suitable for the minute protrusions to come into uniform point contact with the first coating film of the first building board, 1When the first coating surface of the building board is pressed by the third surface of the interleaf paper, the pressing force is efficiently distributed. This is suitable for dispersing the pressure applied to the interleaf, and therefore is suitable for suppressing deformation of the pressed portion. The third surface has a microscopic uneven shape similar to the microscopic uneven shape of the first coating surface of the first building board. Therefore, the first coating surface of the first building board is pressed by the third surface of the interleaf paper and deforms microscopically. Even if the deformation is caused by the pressing, the deformation is a third deformation that is similar to the microscopic uneven shape of the pressed part before the deformation. The microscopic unevenness of the first coating surface is transferred to the second coating surface. As a result, the change in texture is suppressed at the pressed area on the first coating surface, and a new gloss is generated. Pile.
[0014] In a preferred embodiment of the first aspect of the present invention, the third surface of the interleaf paper is abutted against the first building board. The fourth surface has a concave-convex shape in which a plurality of minute protrusions are evenly arranged, and The third surface of the slip sheet has a concave-convex shape with multiple minute recesses arranged at positions corresponding to the portions of the slip sheet. The evenly-spaced convex portions allow the minute convex portions to come into uniform point contact with the first coating film of the first building board. When the first coating surface of the first building board is pressed by the third surface of the interleaf paper, the pressing force is This is suitable for efficient dispersion, and therefore suitable for suppressing deformation of the pressed area. The structure in which the micro recesses are evenly arranged on the fourth surface of the interleaf is such that the fourth surface of the interleaf is in contact with the second coating of the second building board. It is suitable for uniform point contact with the film, and the second coating surface of the second building board is pressed by the fourth surface of the interleaf paper. When the pressing force is applied to the pressing portion, the pressing force is efficiently distributed, and the deformation of the pressing portion is prevented. Furthermore, the third surface of the interleaving paper is suitable for suppressing the adhesion of the first coating film of the first building board in all places. Since the uneven shape is similar to the microscopic uneven shape, the first coating surface of the first building board becomes the third surface of the interleaf paper. Even if the deformation is microscopic due to pressure, the deformation is the deformation of the pressed part. The microscopic unevenness of the third surface, which is similar to the previous microscopic unevenness, is transferred to the first coating surface, for example. This is brought about by the change in texture at the pressed area on the first coating surface. The 4th side of the slip sheet is not affected by the 2nd layer of the paper. Since the uneven shape is similar to the microscopic uneven shape of the second coating film surface of the second building board, Even if the membrane surface is pressed by the fourth surface of the slip sheet and deforms microscopically, the deformation is The microscopic uneven shape of the fourth surface is similar to the microscopic uneven shape of the pressed area before deformation. The pressing force on the second coating surface is, for example, transferred to the In these areas, changes in texture are suppressed and new gloss is less likely to develop.
[0015] According to a second aspect of the present invention, there is provided a method for manufacturing a package. This manufacturing method includes a preparation step and a layering step. In the preparation step, a first building board having a first surface including a first coating surface and a second surface opposite the first surface, and an interleaf paper having a third surface and a fourth surface opposite the third surface are prepared. In the layering step, the first building board and the interleaf paper are layered so that the first coating surface and the third surface are in contact with each other. The first coating surface and the third surface, 60 degree gloss measured in accordance with JIS Z 8741 The absolute value of the difference is 3.0 or less, and the first coating surface and the third surface, 85 degree gloss measured according to JIS Z 8741 The absolute value of the difference is less than or equal to 3.0.
[0016] In this manufacturing method, the first coating surface of the first building board and the third surface of the interleaving paper have a microscopic uneven shape. In the case of measuring the glossiness at a relatively small incidence angle of 60 degrees, The difference between the first and third coating surfaces in the case of the first coating and the third coating surface in the case of the second coating and the first coating surface in the case of ... second coating and the third coating surface in the case of the first coating surface in the case of the second coating. The smaller the difference between the first and third coating surfaces is, the more the microscopic unevenness of the first coating surface and the third coating surface are. The microscopic uneven shapes of the three surfaces are similar.
[0017] The first coating surface of the first building board and the third surface of the interleaf paper, which have similar microscopic irregularities, are in contact with each other. The first coating surface of the first building board is protected by the third surface of the interleaf paper. Even if the first coating surface of the plate is pressed by the third surface of the interleaf paper and deforms microscopically, The deformation of the third surface is similar to the microscopic uneven shape of the pressed portion before deformation. For example, the pressed portion of the first coating surface is transferred to the first coating surface. This suppresses changes in texture and makes it difficult for new gloss to develop.
[0018] In the present manufacturing method, preferably, a fifth surface including the second coating surface and a sixth surface opposite to the fifth surface are and a second building board having the above structure is attached to the second building board via the interleaf paper so that the second coating surface and the fourth surface of the interleaf paper are in contact with each other. The method further includes a step of overlapping the first building board with the second coating surface. The absolute value of the difference in gloss is 3.0 or less, and the 85 degree gloss of the second coating surface and the 4th surface are The absolute value of the difference from the 85 degree gloss is 3.0 or less.
[0019] In such a configuration, the second coating surface and the second building board and the interleaving paper contact each other. The fourth surface has microscopic irregularities corresponding to the respective gloss levels. The difference in gloss between the second and fourth coating surfaces when measuring the gloss at a relatively small angle of incidence of 60 degrees is shown in Fig. When measuring gloss at a relatively large angle of incidence of 85 degrees, the difference between the second and fourth coating surfaces was 3. 0 or less, the closer the microscopic unevenness of the second coating film surface and the microscopic unevenness of the fourth coating film surface are to each other. The second coating surface of the second building board and the fourth surface of the interleaf, which have similar microscopic irregularities, are in contact with each other. The second coating surface of the second building board is protected by the fourth side of the interleaf paper. The second coating surface of the second building board was pressed by the fourth surface of the interleaf paper and deformed microscopically. However, the deformation is a microscopic concave-convex shape of the fourth surface that is similar to the microscopic concave-convex shape of the pressed portion before deformation. The convex shape is transferred to the second coating surface. At the pressed areas, changes in texture are suppressed and new gloss is less likely to develop.
[0020] In a preferred embodiment of the first aspect of the present invention, the third surface of the interleaf paper is abutted against the first building board. The third surface of the slip sheet has a concave-convex shape with multiple evenly arranged micro-projections. The evenly-spaced configuration is suitable for the minute protrusions to come into uniform point contact with the first coating film of the first building board, 1When the first coating surface of the building board is pressed by the third surface of the interleaf paper, the pressing force is efficiently distributed. This is suitable for dispersing the pressure applied to the interleaf, and therefore is suitable for suppressing deformation of the pressed portion. The third surface has a microscopic uneven shape similar to the microscopic uneven shape of the first coating surface of the first building board. Therefore, the first coating surface of the first building board is pressed by the third surface of the interleaf paper and deforms microscopically. Even if the deformation is caused by the pressing, the deformation is a third deformation that is similar to the microscopic uneven shape of the pressed part before the deformation. The microscopic unevenness of the first coating surface is transferred to the second coating surface. As a result, the change in texture is suppressed at the pressed area on the first coating surface, and a new gloss is generated. Pile.
[0021] In a preferred embodiment of the first aspect of the present invention, the third surface of the interleaf paper is abutted against the first building board. The fourth surface has a concave-convex shape in which a plurality of minute protrusions are evenly arranged, and The third surface of the slip sheet has a concave-convex shape with multiple minute recesses arranged at positions corresponding to the portions of the slip sheet. The evenly-spaced convex portions allow the minute convex portions to come into uniform point contact with the first coating film of the first building board. When the first coating surface of the first building board is pressed by the third surface of the interleaf paper, the pressing force is This is suitable for efficient dispersion, and therefore suitable for suppressing deformation of the pressed area. The structure in which the micro recesses are evenly arranged on the fourth surface of the interleaf is such that the fourth surface of the interleaf is in contact with the second coating of the second building board. It is suitable for uniform point contact with the film, and the second coating surface of the second building board is pressed by the fourth surface of the interleaf paper. When the pressing force is applied to the pressing portion, the pressing force is efficiently distributed, and the deformation of the pressing portion is prevented. Furthermore, the third surface of the interleaving paper is suitable for suppressing the adhesion of the first coating film of the first building board in all places. Since the uneven shape is similar to the microscopic uneven shape, the first coating surface of the first building board becomes the third surface of the interleaf paper. Even if the deformation is microscopic due to pressure, the deformation is the deformation of the pressed part. The microscopic unevenness of the third surface, which is similar to the previous microscopic unevenness, is transferred to the first coating surface, for example. This is brought about by the change in texture at the pressed area on the first coating surface. The 4th side of the slip sheet is not affected by the 2nd layer of the paper. Since the uneven shape is similar to the microscopic uneven shape of the second coating film surface of the second building board, Even if the membrane surface is pressed by the fourth surface of the slip sheet and deforms microscopically, the deformation is The microscopic uneven shape of the fourth surface is similar to the microscopic uneven shape of the pressed area before deformation. The pressing force on the second coating surface is, for example, transferred to the In these areas, changes in texture are suppressed and new gloss is less likely to develop. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic cross-sectional view of a package according to a first embodiment of the present invention. [Diagram 2] 1 is a partially enlarged perspective view of an example of an interleaf sheet; [Diagram 3] FIG. 3 is a schematic cross-sectional view of the interleaf paper shown in FIG. 2. [Figure 4] 2 illustrates a method for manufacturing the package shown in FIG. 1 . [Diagram 5] This shows the case where the packages shown in FIG. 1 are stacked in multiple layers on a pallet. [Figure 6] FIG. 5 is a schematic cross-sectional view of a building board package according to a second embodiment of the present invention. [Figure 7] 7 illustrates a method for manufacturing the package shown in FIG. 6. [Figure 8] This shows the case where the packages shown in FIG. 6 are stacked in multiple layers on a pallet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] FIG. 1 is a schematic cross-sectional view of a package X1 according to a first embodiment of the present invention. The building board 10 includes a first building board 10 and an interleaf paper 20 overlapped with the first building board 10.
[0024] The first building board 10 has a first surface 11 on the side of the interleaf paper 20 and a second surface 1 on the opposite side to the first surface 11. 2. The first surface 11 includes a first coated surface 11A.
[0025] The first coating surface 11A is formed by, for example, applying paint and drying it to form a coating film. Examples of paints include acrylic resin paint, silicon acrylic resin paint, and silicone paint. Examples of paints include silicone resin paints, fluororesin paints, and urethane resin paints. The coating may contain beads, pigments, and fillers. The thickness of the coating is, for example, 10 to 100 μm. The first coating surface 11A may have a laminated structure including a plurality of resin films. 1A has a laminated structure including, for example, an undercoat film, an intermediate coat film, and a clear coat film in this order. You may do so.
[0026] The interleaving paper 20 has a third surface 21 on the first building board 10 side and a fourth surface 22 on the opposite side to the third surface 21. 2. The third surface 21 is in contact with the first coating surface 11A. The third surface 21 is preferably , has an uneven shape with a plurality of evenly-spaced minute protrusions protruding toward the first building board 10 side.
[0027] The interleaf paper 20 covers the first coating surface 11A of the first building board 10 and protects the first coating surface 11A. The slip sheet 20 is a thin sheet. The slip sheet 20 is sized to cover the first coating surface 11A. It may be a single sheet, or two or more sheets stacked together, or may be in the form of a tube. The interleaf paper 20 may be arranged so as to cover only the first coating surface 11A, or It may be arranged so as to encase the entire first building board 10.
[0028] The material constituting the interleaf paper 20 is, for example, a resin film. Examples of such materials include polyethylene, polypropylene, vinyl chloride, nylon, and polyester. , polyvinyl alcohol, ethylene vinyl acetate copolymer, and triacetate. The interleaf paper 20 may be a laminate film of multiple resin films. The paper 20 may be a laminate of a resin film and cloth or paper.
[0029] The uneven shape of the interleaf paper 20 is due to the incorporation of inorganic or organic particles during the interleaf paper production process, or the use of metal rolls. Surface shape transfer, physical embossing by sand blasting, chemical etching, etc. It can be built in a way.
[0030] The thickness of the interleaf paper 20 is not particularly limited, but in the case of a resin film or a laminate film, Preferably, the thickness is 40 to 500 μm. In the case of a laminate of a resin film and a cloth or paper, , preferably 100 to 500 μm.
[0031] In the package X1, the 60 degree gloss of the first coating surface 11A and the 60 degree gloss of the third surface 21 are The absolute value of the difference between the 85 degree gloss of the first coating surface 11A and the 85 degree gloss of the third surface 21 is 3.0 or less. The absolute value of the difference from the 85 degree gloss is 3.0 or less.
[0032] FIG. 4 shows a method for manufacturing the package X1. This manufacturing method includes the following preparation steps and stacking steps. The process includes a mixing step.
[0033] In the preparation step, a first surface 11 including a first coating surface 11A and a second surface 11 on the opposite side to the first surface 11 are A first building board 10 having a first surface 12 and a second surface 21 and a second surface 22 opposite to the third surface 21. An interleaf sheet 20 having four sides 22 is provided.
[0034] In the overlapping step, the first building board 1 is placed on the first building board 1 so that the first coating surface 11A and the third surface 21 are in contact with each other. 0 and the interleaf paper 20 are overlapped. As described above, the 60 degree gloss of the first coating surface 11A and the third coating surface 11B are The absolute value of the difference between the 60 degree gloss of the first coating surface 11A and the 60 degree gloss of the second coating surface 11B is 3.0 or less, and The absolute value of the difference between the 5 degree gloss and the 85 degree gloss of the third surface 21 is 3.0 or less.
[0035] In the package X1, the first building board 10 and the interleaving paper 20 are in contact with each other. The first coating surface 11A and the third surface 21 have microscopic irregularities corresponding to their respective glosses. In addition, the gloss level measured at a relatively small angle of incidence of 60 degrees was The difference between the first and third coating surfaces and the gloss of the first coating when measuring the gloss at a relatively large angle of incidence of 85 degrees are shown. The smaller the difference between the film surface and the third surface is, the smaller the microscopic uneven shape of the first coating film surface 11A is. and the microscopic uneven shape of the third surface 21 are similar to each other.
[0036] In such a package X1, for example, when the packages are stacked in multiple layers as shown in FIG. The first coating surface 11A of the first building board 10 is pressed by the third surface 21 of the interleaving paper 20, Even if the deformation is visibly observed, the deformation is different from the microscopic uneven shape of the pressed portion before the deformation. This is caused by the microscopic uneven shape of the third surface 21 which is close to the third surface 21 (for example, The target uneven shape is transferred to the first coated surface 11A. At the pressed area, the change in texture is suppressed and new gloss is unlikely to occur. 13 shows an example of a state in which packages X1 are stacked in four layers on top of each other.
[0037] As described above, the packaging body X1 suppresses the occurrence of gloss caused by pressure on the coating film on the surface of the building board. Suitable for
[0038] As described above, the third surface 21 preferably has a plurality of small protrusions protruding toward the first building board 10. The uneven shape includes a portion that is uniformly arranged. When the first coating surface 11A of the board 10 is pressed by the third surface 21 of the interleaf paper 20, the pressing It is suitable for efficiently dispersing pressure and therefore suitable for suppressing deformation of the pressed area. .
[0039] FIG. 6 is a schematic cross-sectional view of a package X2 according to a second embodiment of the present invention. The package X2 further comprises a first building board 10, an interleaf paper 20, and a second building board 30. It differs from the above-mentioned package X1 in that it includes a building board 30.
[0040] The second building board 30 has a fifth surface 31 on the first building board 10 side and a third surface 32 on the opposite side to the fifth surface 31. The fifth surface 31 is a sixth surface 32 and is superimposed on the first building board 10 via an interleaving paper 20. includes the second coating surface 31A.
[0041] In this embodiment, the fourth surface 22 of the interleaving paper 20 on the second building board 30 side is the second coating surface 31 In the present embodiment, the third surface of the interleaf paper 20 protrudes toward the first building board 10. The uneven shape includes a plurality of minute protrusions that are uniformly arranged, and The surface 22 has an uneven shape including a plurality of minute recesses at positions corresponding to the plurality of minute protrusions.
[0042] In the package X2, the 60 degree gloss of the second coating surface 31A and the 60 degree gloss of the fourth surface 22 are The absolute value of the difference between the 85 degree gloss of the second coating surface 31A and the 85 degree gloss of the fourth surface 22 is 3.0 or less. The absolute value of the difference from the 85 degree gloss is 3.0 or less.
[0043] FIG. 7 shows a method for manufacturing such a package X2. This manufacturing method includes the above-mentioned preparation process and A superposition process (first superposition process) and a superposition process (second superposition process) as shown in FIG. and a superposing step of
[0044] In the second overlapping step, the fifth surface 31 including the second coating surface 31A and the fifth surface 31 The second building board 30 having the sixth surface 32 on the opposite side is connected to the second coating surface 31A and the fourth surface of the interleaf paper 20. The first building board 10 is placed on the second building board 10 via the interleaf paper 20 so that the first building board 10 and the second building board 22 are in contact with each other. The absolute value of the difference between the 60 degree gloss of the second coating surface 31A and the 60 degree gloss of the fourth surface 22 is 3. 0 or less, and the 85 degree gloss of the second coating surface 31A and the 85 degree gloss of the fourth surface 22 are The absolute value of the difference is less than or equal to 3.0.
[0045] In the package X2 manufactured in this way, the second building board 30 and the interleaving paper 20 are interleaved. The second coating surface 31A and the fourth surface 22, which are in contact with each other, have microscopic concaves corresponding to their respective glosses. It has a convex shape. In gloss measurement, the incidence angle is relatively small at 60 degrees. The difference between the second coating surface 31A and the fourth surface 22 when the incident angle is relatively large at 85 degrees is The closer the difference between the second coating surface 31A and the fourth surface 22 is to 3.0 or less, the The microscopic irregular shape of the second coating surface 31A and the microscopic irregular shape of the fourth surface 22 are similar to each other.
[0046] In such a package X2, for example, when the package X2 is stacked in multiple layers as shown in FIG. The second coating surface 31A of the second building board 30 is pressed by the fourth surface 22 of the interleaving paper 20, and Even if the deformation is visibly observed, the deformation is different from the microscopic uneven shape of the pressed portion before the deformation. This is caused by the microscopic uneven shape of the fourth surface 22 which is similar to the second coating surface 31. At the pressed area in A, the change in texture is suppressed and new gloss is unlikely to occur. 1 shows an example of a state in which packages X2 are stacked in four layers on a pallet P.
[0047] In addition to the above-mentioned technical effects of the package X1, the package X2 has the following technical effects: The results are achieved.
[0048] In addition, in the interleaving paper 20 of the present embodiment, as described above, the third surface 21 is the first building board 1 The uneven shape includes a plurality of minute protrusions protruding toward the 0 side and are evenly arranged, In addition, the fourth surface 22 has an uneven shape including a plurality of minute recesses at positions corresponding to the plurality of minute protrusions. In this configuration, the first coating surface 11A of the first building board 10 is in contact with the third surface 21 of the interleaving paper 20. When the second coating surface 31A of the second building board 30 is pressed against the fourth surface 22 of the interleaf paper 20, When the pressing force is applied by the pressing force, the pressing force is efficiently distributed. Suitable for suppressing deformation of pressure points. EXAMPLES
[0049] Example 1 (Manufacturing of building boards) First, we used an inorganic board (1820mm x 470mm x 16mm) with a flat design surface. The design surface of the 17 kg acrylic paint is applied and dried to create a 20 μm thick undercoat. Next, a silicone acrylic paint containing resin beads was applied on the intermediate coating film. Then, the coating was dried to form a matte clear coating film having a thickness of 10 μm. Two building boards B1 with a matte clear coating were prepared.
[0050] <Creating the packaging> First, a slip sheet S1 (50 μm thick, polyester) was applied to the non-gloss clear coating of one of the building boards B1. The interleaf S1 was placed so that the back surfaces of the two sheets of polyethylene film ( The embossing process is performed, and multiple small convex portions (evenly distributed) are formed by the embossing process. The surface has an uneven shape including a plurality of minute projections, and the plurality of minute projections are disposed at positions corresponding to the plurality of minute projections. The back surface of the interleaf S1 has an uneven shape including small recesses. The top surface has minute protrusions with a height of 42 μm, which are arranged in a staggered pattern at approximately equal intervals, forming a uniform unevenness. The back side of the interleaf S1 has a 310 x 410 μm pattern at the position corresponding to the minute convex portion. The surface has an elliptical bottom and minute recesses with a depth of 38 μm arranged in a staggered pattern at approximately equal intervals, creating a uniform unevenness. Next, one building board B1 is laminated on the other building board B1 via a slip sheet S1. The other building board B1 was placed on the other side of the interleaving paper S1 with its matte clear coating film facing the other side of the interleaving paper S1. In this manner, a laminated structure similar to that shown in FIG. A package consisting of the following components was produced.
[0051] [Example 2 and Comparative Examples 1 and 2] Instead of the interleaving paper S1, the interleaving paper S2 (Example 2), the interleaving paper S3 (Comparative Example 1), or the interleaving paper S4 ( The packaging body of Example 2 and Comparative Example 2 were prepared in the same manner as that of Example 1, except that Comparative Example 2 was used. We created packages 1 and 2.
[0052] The interleaf paper S2 is an interleaf paper (thickness 80 μm, polyester) with a matte finish created by embossing. The interleaf paper S2 is a embossed sheet with a concave-convex shape. The surface has a matte finish (including multiple evenly-spaced micro-projections) and can accommodate multiple micro-projections. The back surface has an uneven shape including a plurality of minute recesses at the positions indicated.
[0053] The interleaf paper S3 is an interleaf paper containing calcium carbonate particles (thickness 56 μm, calcium carbonate The film is a polyethylene film containing microparticles.
[0054] S4 is a paper made by laminating both sides of kraft paper with polyethylene resin (thickness 20 0 μm).
[0055] Example 3 (Manufacturing of building boards) First, we used an inorganic board (1820mm x 470mm x 16mm, 1 7 kg) on the design surface, acrylic paint is applied and dried to form a 50 μm thick undercoat film. Next, a silicone acrylic paint containing resin beads was applied on the intermediate coating film. After drying, a matte clear coating film with a thickness of 40 μm was formed. Two building boards B2 having a matte clear coating were prepared.
[0056] <Creating the packaging> On one of the building boards B2, a slip sheet S1 (thickness 50 μm, polyethylene) is applied to the matte clear coating. The interleaf paper S1 was placed so that the back surfaces of the two sheets of the film were in contact with each other. The other building board B2 was placed on top of the other building board B2 with the interleaf S1 between them. 2 was placed so that its matte clear coating film faced and contacted the other side of the slip sheet S1. In this manner, a package having the same layered structure as that shown in FIG. 6 was produced.
[0057] Comparative Example 3 The same packaging as in Example 3 was carried out except that the interleaf paper S4 was used instead of the interleaf paper S1. A package of Comparative Example 3 was produced.
[0058] Example 4 (Manufacturing of building boards) First, we used an inorganic board (1820mm x 470mm x 16mm) with a flat design surface. The design surface of the 17 kg (17 kg) is coated with acrylic paint and dried to create a 40 μm thick undercoat. Next, a silicone acrylic paint that does not contain resin beads was applied on the intermediate coating film. The coating was then dried to form a glossy clear coating with a thickness of 5 μm. In this manner, two building boards B3 each having a glossy clear coating on one side were prepared. Ta.
[0059] <Creating the packaging> On one of the building boards B3, a laminate S5 (thickness 60 μm, polyethylene) is applied to the glossy clear coating. The interleaf S5 was placed so that the back surfaces of the two sheets of the interleaf film (film) faced each other and were in contact with each other. The embossing process is performed, and multiple small convex portions (equally arranged) are formed by the embossing process. The surface has a concave-convex shape including a plurality of minute recesses at positions corresponding to the plurality of minute protrusions. Specifically, the surface of the interleaf S5 has a rhombus shape of about 4×2 mm. The micro-projections, each 70 μm high, have a top surface with a uniform unevenness. On the top surface of each micro-projection, there is an even smaller elliptical projection of about 300 x 500 μm. The back surface of the interleaf sheet S5 has a plurality of micro-projections formed thereon, forming a concave-convex pattern. The diamond-shaped micro recesses are arranged in a staggered pattern at approximately equal intervals on the surface, forming uniform unevenness. One building board B3 was placed on the other building board B3 with interleaving paper S5 between them. The building board B3 is placed so that its glossy clear coating faces and contacts the other side of the interleaf S5. In this manner, a package having the same layered structure as that shown in FIG.
[0060] [Comparative Examples 4 to 6] Instead of the interleaving paper S5, the interleaving paper S4 (Comparative Example 4), the interleaving paper S6 (Comparative Example 5), or the interleaving paper S7 ( Each of the packages of Comparative Examples 4 to 6 was prepared in the same manner as the package of Example 4, except that Comparative Example 6 was used. The body was created.
[0061] The interleaf paper S6 is a non-oriented polypropylene sheet (thickness: 100 μm).
[0062] S7 is a polyethylene film containing calcium carbonate particles, which is shaped like a tube. The resulting interleaf paper (thickness: 76 μm)
[0063] <Measurement of Glossiness> The surfaces of the matte clear coatings of the above-mentioned building boards B1 and B2, and the glossy clear coating of the building board B3 The surface of the coating film and the surface and back of each of the slip sheets S1 to S7 are The 60 degree gloss and 85 degree gloss were measured in accordance with 8741. Product name: "micro-TRI-gloss with standard holder, model 4430", manufactured by BYK Gardner was used.
[0064] For the surface of the matte clear coating of building board B1, 60 degree gloss level G 60 is 4.0 , 85 degree gloss G 85The surface of the matte clear coating of the building board B2 was 1.7. 60 degree gloss G 60 is 3.3, and the gloss level at 85 degrees is G 85 was 3.2. Building board B 3. Glossy clear coating surface, 60 degree gloss level G 60 is 12.7, and 85 degrees Glossiness G 85 was 12.8.
[0065] In addition, for each of Examples 1 to 4 and Comparative Examples 1 to 6, the surface and Back side gloss level G at 60 degrees 60 , the 85 degree glossiness G of the front and back of the slip sheet used 85 , construction Absolute value of the difference in 60 degree gloss between the surface of the board coating and the surface or back of the slip sheet, ΔG 60 , and Absolute value of the difference in 85 degree gloss between the surface of the architectural board coating and the surface or back of the interleaf paper, ΔG 85 Table 1 As shown in.
[0066] Evaluation of Gloss Generation For each of the packages in Examples 1 to 4 and Comparative Examples 1 to 6, the coating film of the building board was The surface gloss was evaluated. First, 25 packages were stacked in multiple layers. Next, After 24 hours, the packages were opened and the coating surface of each building board in the package placed at the bottom was The results are shown in Table 1.
[0067] [Table 1]
[0068] In Example 1, the absolute difference in 60-degree gloss between the coating surface of the building board B1 and the surface of the interleaf paper S1 was Value G 60 The absolute value of the difference in glossiness at 85 degrees G 85The thickness of the slip sheet S1 is also 3.0 or less. No new gloss was observed on the coating surface of building board B1, which was placed in In Example 1, the difference in gloss at 60 degrees between the coating surface of the building board B1 and the back surface of the interleaf S1 was The absolute value of G 60 The absolute value of the difference in glossiness at 85 degrees G 85 The thickness of the interleaf S1 is also 3.0 or less. No new gloss was observed on the coating surface of building board B1, which was placed on the reverse side. It was.
[0069] In Example 2, the absolute difference in 60-degree gloss between the coating surface of the building board B1 and the back surface of the interleaf paper S2 was Value G 60 The absolute value of the difference in glossiness at 85 degrees G 85 The thickness of the back side of the interleaf S2 is also 3.0 or less. No new gloss was observed on the coating surface of building board B1, which was placed in .
[0070] In Example 3, the absolute difference in 60-degree gloss between the coating surface of the building board B2 and the surface of the interleaf paper S1 was Value G 60 The absolute value of the difference in glossiness at 85 degrees G 85 The thickness of the slip sheet S1 is also 3.0 or less. No new gloss was observed on the coating surface of building board B2, which was placed in In Example 3, the difference in gloss at 60 degrees between the coating surface of the building board B2 and the back surface of the interleaf S1 was The absolute value of G 60 The absolute value of the difference in glossiness at 85 degrees G 85 The thickness of the interleaf S1 is also 3.0 or less. No new gloss was observed on the coating surface of building board B2, which was located on the reverse side. It was.
[0071] In Example 4, the absolute difference in 60-degree gloss between the coating surface of the building board B3 and the surface of the interleaf paper S5 was Value G 60The absolute value of the difference in glossiness at 85 degrees G 85 The thickness of the interleaf S5 is also 3.0 or less. No new gloss was observed on the coating surface of building board B3, which was placed in In Example 4, the difference in gloss at 60 degrees between the coating surface of the building board B3 and the back surface of the interleaf paper S5 was The absolute value of G 60 The absolute value of the difference in glossiness at 85 degrees G 85 The thickness of the interleaf S5 is also 3.0 or less. No new gloss was observed on the coating surface of building board B3, which was located on the reverse side. It was. [Explanation of symbols]
[0072] X1, X2 packaging 10 1st Building Board 11 Page 1 11A 1st coating film 12 Side 2 20 slip paper 21 Page 3 22 Page 4 30 1st Building Board 31 Page 5 31A 2nd coating 32 Page 6
Claims
1. A building board package comprising a first building board and an interleaving paper overlapped with the first building board, The first building board has a first surface including a first coating surface and a second surface opposite to the first surface, The interleaving paper has a third surface on the first building board side and a fourth surface opposite to the third surface, the third surface is in contact with the first coated surface; the absolute value of the difference in 60 degree gloss between the first coating surface and the third surface, as measured in accordance with JIS Z 8741, is 3.0 or less; and the absolute value of the difference in 85 degree gloss between the first coating surface and the third surface, as measured in accordance with JIS Z 8741, is 3.0 or less.
2. Further, a second building board is overlapped with the first building board via the interleaving paper, The second building board has a fifth surface on the first building board side and a sixth surface on the opposite side to the fifth surface. the fifth surface includes a second coating surface; The fourth surface of the interleaving paper on the second building board side is in contact with the second coating surface, The absolute value of the difference between the 60 degree gloss of the second coating surface and the 60 degree gloss of the fourth surface is 3. 0 or less, and the 85 degree gloss of the second coating surface and the 85 degree gloss of the fourth surface are 2. The building board package according to claim 1, wherein the absolute value of the difference is 3.0 or less.
3. The third surface has an uneven shape in which a plurality of minute protrusions protruding toward the first building board are evenly arranged. The building board package according to claim 1 or 2, comprising:
4. The third surface has an uneven shape in which a plurality of minute protrusions protruding toward the first building board are evenly arranged. having The fourth surface has an uneven shape including a plurality of minute recesses at positions corresponding to the plurality of minute protrusions. The building board package according to claim 2 .
5. A step of preparing a first building board having a first surface including a first coating surface and a second surface opposite to the first surface, and an interleaf paper having a third surface and a fourth surface opposite to the third surface; and overlapping the first building board and the interleaf paper so that the first coating surface and the third surface are in contact with each other, a difference in 60 degree gloss between the first coating surface and the third surface, measured in accordance with JIS Z 8741, of 3.0 or less, and a difference in 85 degree gloss between the first coating surface and the third surface, measured in accordance with JIS Z 8741, of 3.0 or less, is an absolute value.
6. A second building board having a fifth surface including a second coating surface and a sixth surface opposite to the fifth surface. The second coating surface is brought into contact with the fourth surface of the interleaf paper via the interleaf paper. The method further includes a step of overlapping the board with a building board. The absolute value of the difference between the 60 degree gloss of the second coating surface and the 60 degree gloss of the fourth surface is 3. 0 or less, and the 85 degree gloss of the second coating surface and the 85 degree gloss of the fourth surface are 6. The method for manufacturing a building board package according to claim 5, wherein the absolute value of the difference is 3.0 or less.
7. The third surface has an uneven shape in which a plurality of minute protrusions protruding toward the first building board are evenly arranged. The method for manufacturing a building board package according to claim 5 or 6, comprising the steps of:
8. The third surface has an uneven shape in which a plurality of minute protrusions protruding toward the first building board are evenly arranged. having The fourth surface has an uneven shape including a plurality of minute recesses at positions corresponding to the plurality of minute protrusions. The method for manufacturing a building board package according to claim 6 .
Citation Information
Patent Citations
Slip sheet for stacking painted member
JP1998338262A
Slip sheet for ceramic siding material and method for laminating ceramic siding material
JP1999278547A
Slip sheet for packing
JP2005041546A
Method for manufacturing embossed decorative sheet
JP2010082872A
Structure for loading ceramic building material
JP2011025989A