Display substrate and manufacturing method thereof
By employing crystallized glass with controlled thermal contraction through specific heating and cooling rates, the substrate addresses thermal shrinkage issues, enhancing display resolution and resistance.
Patent Information
- Application Number
- JP2020534646
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-07-31
- Filing Date
- 2019-07-30
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2039-07-30
AI Technical Summary
Conventional glass substrates experience significant thermal shrinkage during high-temperature processes, leading to pattern deviations in thin film transistors and limiting the resolution of displays.
A display substrate with a heat shrinkage value of 10 ppm or less is achieved by heating at a rate of 5°C/min to 500°C, holding for 1 hour, and cooling at 5°C/min to room temperature, using crystallized glass with specific compositions and heat treatment to reduce thermal contraction.
The solution effectively suppresses pattern deviations in thin film transistors, enabling higher definition displays with reduced thermal shrinkage and improved thermal shock resistance.
Smart Images

Figure 0007574078000001 
Figure 0007574078000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a display substrate and a manufacturing method thereof, and more particularly to a display substrate for forming a TFT circuit in a flat panel display such as a liquid crystal display or an organic EL display, and a manufacturing method thereof.
[0002] As is well known, a liquid crystal panel comprises a color filter substrate on which a black matrix, RGB, photospacers, etc. are patterned, and a TFT substrate on which thin film transistors (TFTs), transparent electrodes, etc. are patterned. These substrates are bonded together with a sealant applied along the outer periphery, and a liquid crystal material is filled in the space surrounded by these substrates and the sealant.
[0003] Thin film transistors that drive displays are known to be made of amorphous silicon, low-temperature polysilicon, high-temperature polysilicon, etc. In recent years, with the spread of large liquid crystal displays, smartphones, tablet PCs, etc., there is a growing need for higher resolution displays. Low-temperature polysilicon TFTs can meet this need, but this technology requires a high-temperature process at 500 to 600°C. However, conventional glass substrates experience large amounts of thermal shrinkage before and after the high-temperature process, which causes pattern misalignment of thin film transistors. Therefore, low-thermal shrinkage glass substrates are required to achieve higher resolution displays. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-27894 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] Increasing the strain point of a glass substrate reduces the amount of thermal shrinkage of the glass substrate (see Patent Document 1). However, although current glass substrates have a high strain point, the amount of thermal shrinkage is not sufficiently small, and they do not fully meet the needs for high-definition displays.
[0006] The present invention has been made in view of the above circumstances, and its technical object is to devise a display substrate having a smaller amount of thermal shrinkage than conventional substrates, and a method for manufacturing the same. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that the above technical problems can be solved by restricting the thermal shrinkage of the substrate to a predetermined value or less, and propose this as the present invention. That is, the display substrate of the present invention is characterized in that the thermal shrinkage value is 10 ppm or less when the substrate is heated from room temperature to 500°C at a heating rate of 5°C / min, held at 500°C for 1 hour, and then cooled to room temperature at a cooling rate of 5°C / min. In this way, the amount of thermal shrinkage of the substrate is small before and after the high-temperature process, so that the pattern deviation of the thin film transistor can be suppressed. The "thermal shrinkage value" is measured by first imprinting linear markings in two parallel positions on a plate-shaped sample, dividing the sample in a direction perpendicular to the markings to obtain two sample pieces, performing a predetermined heat treatment on one of the sample pieces, arranging the heat-treated sample piece and the unheat-treated sample piece so that the dividing surfaces are aligned, and fixing them with adhesive tape, and then measuring the deviation amount ΔL of the markings of both the sample pieces, and finally measuring the value of ΔL / L0, which is the thermal shrinkage value. Here, L0 is the length of the sample piece before heat treatment.
[0008] In addition, the display substrate of the present invention preferably has a thermal shrinkage value of 10 ppm or less when heated from room temperature to 600°C at a heating rate of 5°C / min, held at 600°C for 10 hours, and then cooled to room temperature at a cooling rate of 5°C / min.
[0009] In addition, the display substrate of the present invention is preferably made of crystallized glass. The strain point is generally measured by preparing a fiber of a predetermined diameter from a mother glass by a fiber elongation method, but crystallized glass cannot be made into a fiber due to its low resistance to devitrification, and the strain point cannot be measured. However, the present inventors have found that although the strain point of crystallized glass is unknown, it is difficult to thermally shrink in a high-temperature process, and that using crystallized glass as a display substrate can contribute to high-definition displays. Crystallized glass is mainly used in cooking utensils such as top plates for cooking appliances. The crystallized glass used for this purpose is transparent, has a low thermal expansion coefficient, and is difficult to break due to thermal shock.
[0010] Furthermore, the display substrate of the present invention preferably has a total light transmittance of 65% or more at a wavelength of 400 nm, calculated based on a plate thickness of 1.1 mm. This increases the visible light transmittance of the substrate, so that the output of the light source required to ensure the brightness of the display is reduced, making it possible to produce a display with low power consumption.
[0011] In addition, the display substrate of the present invention has a thermal expansion coefficient of −30×10 at 30 to 380° C. -7 ~30×10 -7 / ° C. In this way, the amount of thermal shrinkage in a high-temperature process is reduced and thermal shock resistance is improved.
[0012] In addition, the display substrate of the present invention preferably contains, in mass %, 50-70% SiO2, 10-30% Al2O3, and 0-15% Li2O. This reduces the amount of thermal shrinkage in high-temperature processes and improves resistance to devitrification, making it easier to mold into a plate. Furthermore, transparency is improved.
[0013] The display substrate of the present invention is preferably used as a TFT substrate.
[0014] The method for producing a display substrate of the present invention comprises the steps of forming molten glass into a plate shape, cutting it to obtain a display substrate, and maintaining the obtained display substrate at a temperature of 800° C. or higher, and then cooling it to room temperature at a temperature decrease rate of 200° C. / hour or less, thereby reducing the thermal shrinkage value to 10 ppm or less. Here, the thermal shrinkage value is the thermal shrinkage rate when the substrate is heated from room temperature to 500° C. at a temperature increase rate of 5° C. / minute, maintained at 500° C. for 1 hour, and then cooled to room temperature at a temperature decrease rate of 5° C. / minute. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In the display substrate of the present invention, the thermal shrinkage value when the substrate is heated from room temperature to 500°C at a heating rate of 5°C / min, held at 500°C for 1 hour, and then cooled to room temperature at a cooling rate of 5°C / min is 10 ppm or less, preferably 8 ppm or less, 6 ppm or less, 4 ppm or less, 2 ppm or less, and particularly 1 ppm or less. In addition, the thermal shrinkage value when the substrate is heated from room temperature to 600°C at a heating rate of 5°C / min, held at 600°C for 10 hours, and then cooled to room temperature at a cooling rate of 5°C / min is preferably 10 ppm or less, 8 ppm or less, 6 ppm or less, 4 ppm or less, 2 ppm or less, and particularly 1 ppm or less. If the thermal shrinkage value is too large, the amount of thermal shrinkage increases before and after the high-temperature process, which makes it easy for the pattern of the thin film transistor to shift. As a result, it becomes difficult to manufacture a high-definition display.
[0016] A common method for reducing the thermal shrinkage value is to increase the strain point of the glass, but there are also other methods, such as (1) performing a long-term annealing process and (2) precipitating a specified crystal in the glass matrix. Method (2) is preferable because it significantly reduces thermal shrinkage due to the fact that the structural relaxation of the glass progresses when precipitating the specified crystal, the degree of crystallization increases, the proportion of the remaining glass layer decreases, and the strain point of the remaining glass phase increases.
[0017] In the method (2), the thermal shrinkage value can be reduced by adjusting the type of crystals to be precipitated, the degree of crystallization (the proportion of crystals to be precipitated), the composition of the crystal phase, the proportion of the glass phase, the composition of the glass phase, and the like. In order to reduce the thermal shrinkage value, the type of precipitated crystals is preferably a β-quartz solid solution or a β-eucryptite solid solution, and the degree of crystallization is preferably 72 to 80%, particularly 73 to 79%. The "degree of crystallization" can be evaluated by a powder method using an X-ray diffractometer (Rigaku RINT-2100). Specifically, the area of the halo corresponding to the mass of the amorphous material and the area of the peak corresponding to the mass of the crystal are calculated, and then the degree of crystallization can be calculated by the formula [area of the peak] x 100 / [area of the peak + area of the halo] (%).
[0018] The display substrate of the present invention preferably contains, in mass %, SiO2 50-70%, Al2O3 10-30%, and Li2O 0-15%. The reasons for limiting the range of each component as described above are as follows. In the explanation of the range of each component, % means mass %.
[0019] SiO2 is a component that forms the skeleton of glass and also constitutes crystals, and its content is preferably 50 to 70%, more preferably 60 to 70%, and even more preferably 62 to 68%. When the content of SiO2 is low, the amount of SiO2 in the remaining glass phase is low, the strain point of the remaining glass phase is low, and the amount of thermal contraction is large. In addition, in a high-temperature process, the thermal expansion coefficient tends to change or increase in the positive direction due to a structural change in the glass phase. On the other hand, when the content of SiO2 is high, the melting property is reduced, making it difficult to obtain a homogeneous glass.
[0020] Like SiO2, Al2O3 is a component that forms the glass skeleton and also constitutes crystals, and its content is preferably 10 to 30%, more preferably 15 to 25%, and even more preferably 20 to 24%. When the content of Al2O3 is reduced, the amount of Al2O3 in the remaining glass phase is reduced, the strain point of the remaining glass phase is lowered, and the amount of thermal contraction is increased. In addition, in high-temperature processes, the thermal expansion coefficient tends to change or increase in the positive direction due to structural changes in the glass phase. On the other hand, when the content of Al2O3 is increased, the melting property is reduced, making it difficult to obtain a homogeneous glass.
[0021] Li2O is a glass modifying component and also a component that constitutes crystals, and its content is preferably 0 to 15%, more preferably 1 to 13%, further preferably 2 to 10%, and particularly preferably 3 to 7%. If the Li2O content is low, it becomes difficult to precipitate the desired crystals (Li2O-Al2O3-SiO2 crystals). On the other hand, if the Li2O content is high, the amount of Li2O in the remaining glass phase increases, the strain point of the remaining glass phase decreases, and the amount of thermal contraction increases. In addition, in high-temperature processes, the thermal expansion coefficient changes due to structural changes in the glass phase, and the thermal expansion coefficient tends to increase in the positive direction.
[0022] In addition to the above components, it is preferable to incorporate the following components, for example:
[0023] Na2O and K2O are components that reduce the viscosity of glass and improve its melting and moldability, and the content of each of these components is preferably 0 to 4%, and more preferably 0 to 2%. If the content of these components is high, the strain point of the remaining glass phase is lowered and the amount of thermal shrinkage is increased. In addition, in high-temperature processes, the thermal expansion coefficient tends to change or increase in the positive direction due to structural changes in the glass phase.
[0024] MgO and ZnO are components that dissolve in the crystal, and the content of each of these components is preferably 0 to 2%, particularly preferably 0 to 1.5%. If the content of these components is high, crystals such as spinel and gahnite are likely to precipitate in addition to β-quartz solid solution or β-eucryptite solid solution, and thermal shock resistance is likely to decrease.
[0025] TiO2 and ZrO2 are nucleation components for precipitating crystals, and the contents of these components are preferably 0-4%, 0-3.5%, and particularly 1-3%, respectively, and the total amount of these components is preferably 1.5-6%. If the contents of these components are large, the glass is easily devitrified during melting or molding, making it difficult to obtain homogeneous glass. If the total amount of TiO2 and ZrO2 is small, the crystallization degree decreases or the nucleation action becomes insufficient, crystals of the desired particle size cannot be obtained, and β-quartz solid solution or β-eucryptite solid solution is easily transformed to β-spodumene solid solution at low temperatures. As a result, it becomes difficult to obtain transparent crystallized glass, and the thermal expansion coefficient of the crystallized glass increases, making it easy for the thermal contraction of the crystallized glass to increase. On the other hand, if the total amount of TiO2 and ZrO2 is large, the glass is easily devitrified during melting or molding, making it difficult to obtain homogeneous glass.
[0026] P2O5 is a component that facilitates nucleation, and its content is preferably 0 to 4%, particularly preferably 0 to 3%. If the P2O5 content is too high, the glass tends to undergo phase separation, making it difficult to obtain a homogeneous glass.
[0027] BaO is a component that reduces the viscosity of glass and improves its meltability and formability, and its content is preferably 0 to 2%, particularly preferably 0 to 1.8%. If the BaO content is too high, the glass is more likely to devitrify during melting or forming, making it difficult to obtain homogeneous glass.
[0028] In order to improve meltability and moldability, B2O3, SrO, CaO, etc. may be introduced in a total amount of up to 5%, and in order to improve clarity, SnO2, Cl, Sb2O3, As2O3, etc. may be introduced in a total amount of up to 2%. If the content of these components is high, the thermal expansion coefficient tends to change or become larger in the positive direction due to structural changes in the glass phase in high-temperature processes. Furthermore, it becomes difficult to precipitate the desired crystals.
[0029] Fe2O3 is a component mixed in as an impurity, and its content is preferably 0.03% or less, 0.025% or less, and particularly preferably 0.02% or less. If the Fe2O3 content is high, coloring becomes stronger and visible light transmittance tends to decrease.
[0030] The display substrate of the present invention preferably has the following properties.
[0031] The thermal expansion coefficient at 30 to 380°C is preferably -30×10 -7 ~30×10 -7 / ℃, -25×10 -7 ~25×10 -7 / ℃, -20×10 -7 ~20×10 -7 / ℃, -15×10 -7 ~15×10 -7 / ℃, -10×10 -7 ~10×10 -7 / ℃, -8×10 -7 ~8×10 -7 / ℃, -6×10 -7 ~6×10 -7 / ℃, -4×10 -7 ~4×10 -7 / ℃, -2×10 -7 ~2, ×10 -7 / ℃, especially -1×10 -7 ~1×10 -7 / °C. If the thermal expansion coefficient is outside the above range, the time and effort required to determine the patterning positioning from the dimensions of the substrate at room temperature while taking into account the thermal expansion during a high-temperature process increases, making film formation design difficult. If a β-quartz solid solution or a β-eucryptite solid solution having a negative thermal expansion coefficient is precipitated as the main crystal in the glass matrix and the crystallinity is restricted to 73 to 79%, the negative thermal expansion coefficient of the crystal phase and the positive thermal expansion coefficient of the glass phase are easily offset, making it easier to restrict the thermal expansion coefficient to within the above range.
[0032] The total light transmittance at a wavelength of 400 nm, calculated based on a plate thickness of 1.1 mm, is preferably 65% or more, 70% or more, 75% or more, 80% or more, or 85% or more. If the total light transmittance is too low, the image on the display tends to become unclear. Furthermore, the output of the light source to ensure a certain brightness tends to increase, and the power consumption of the display tends to increase. In addition, if the particle size of the precipitated crystals in the crystallized glass, the refractive index difference between the crystal phase and the glass phase, and the amount of precipitated crystals are appropriately controlled, the total light transmittance can be increased.
[0033] The density is preferably 2.60 g / cm 3 Below, 2.58g / cm 3 The following, especially 2.56 g / cm 3 If the density is too high, it becomes difficult to make the display lightweight.
[0034] The Young's modulus is preferably 85 GPa or more, 88 GPa or more, 90 GPa or more, 92 GPa or more, particularly 94 GPa or more. If the Young's modulus is too low, the amount of bending of the substrate increases, making it difficult to handle the substrate in the display manufacturing process, etc.
[0035] Specific Young's modulus is preferably 30 GPa / g cm -3 Above, 32GPa / g cm -3 Above, 34GPa / g cm -3 Above, especially 36 GPa / g cm -3That is all. Since the amount of bending of the substrate increases, it becomes difficult to handle the substrate during the display manufacturing process, etc. The "specific Young's modulus" is the value obtained by dividing the Young's modulus by the density.
[0036] The Vickers hardness is preferably 550 or more, 600 or more, and particularly preferably 650 or more. If the Vickers hardness is too low, the substrate is easily scratched, and there is a risk that the substrate may be scratched by contact with other members during the display manufacturing process, etc., and the image on the display may become unclear. Note that "Vickers hardness" refers to a value measured by a method conforming to JIS Z2244-1992.
[0037] In the display substrate of the present invention, the plate thickness is preferably 5 mm or less, 4 mm or less, 3 mm or less, 2 mm or less, 1 mm or less, 0.8 mm or less, 0.7 mm or less, 0.55 mm or less, 0.5 mm or less, and particularly preferably 0.4 mm or less. If the plate thickness is too thick, the mass of the display becomes too large. Furthermore, it becomes difficult to apply the plate to existing manufacturing equipment, and the manufacturing cost of the display tends to rise.
[0038] The substrate size is preferably 100 mm or more, 150 mm or more, 200 mm or more, 300 mm or more, 500 mm or more, 800 mm or more, 1000 mm or more, 1500 mm or more, 2000 mm or more, 2500 mm or more, 3000 mm or more, and particularly preferably 3500 mm or more. If the substrate size is too small, it becomes difficult to produce multiple panels, which can lead to high display manufacturing costs.
[0039] The surface roughness Ra is preferably 5 nm or less, 3 nm or less, 2 mm or less, 1 nm or less, and particularly preferably 0.5 nm or less. If the surface roughness Ra is too large, the quality of the film formed on the substrate surface is likely to decrease. Here, "surface roughness Ra" refers to a value measured by a method conforming to SEMI D7-94 "Method of measuring surface roughness of FPD glass substrates".
[0040] The display substrate of the present invention can be produced as follows. First, a glass batch prepared to have a predetermined glass composition is put into a continuous melting furnace, melted at 1600 to 1750°C, clarified, and then fed to a molding device, where the molten glass is formed into a plate shape and then cut to obtain a crystalline glass substrate. Here, various molding methods such as a float method, a press method, and a roll-out method can be applied as the molding method. Among them, the roll-out method is preferable because devitrified crystals are unlikely to precipitate during molding and a glass substrate with a relatively large area can be produced.
[0041] Next, the crystallizable glass substrate is held at a temperature of 800°C or higher, and then cooled to room temperature at a temperature drop rate of 200°C / hour or less. More specifically, the substrate is heat-treated at 600-800°C for 1-10 hours to form crystal nuclei (crystal nucleation stage), and then heat-treated at 800-950°C for 0.5-6 hours (crystal growth stage) to precipitate crystals and form a crystallized glass substrate. In this way, the thermal shrinkage value is reduced. The temperature drop rate from the temperature in the crystal growth stage to room temperature is preferably 200°C / hour or less, 100°C / hour or less, 50°C / hour or less, and particularly 30°C / hour or less. If the temperature drop rate is too fast, the structure of the glass phase does not relax, making it difficult to reduce the thermal shrinkage rate.
[0042] When Li2O-Al2O3-SiO2 crystals are precipitated as the main crystals, Li2O-Al2O3-SiO2 transparent crystallized glass substrates can be obtained. When the Li2O-Al2O3-SiO2 crystallized glass substrate is heat-treated at a high temperature of 1000°C or higher, particularly 1100°C or higher, in the crystal growth stage, β-spodumene solid solution crystals are precipitated as the main crystals, and the crystallized glass substrate becomes opaque. Therefore, the heat treatment temperature in the crystal growth stage is preferably 1000°C or lower. The heat treatment time in the crystal growth stage is preferably adjusted appropriately between, for example, 0.5 to 6 hours so that the crystals grow sufficiently and do not become coarse.
[0043] After the crystallized glass substrate is obtained, the surface may be polished to improve the surface smoothness, and chamfering may be performed to increase the strength of the edge surface.
[0044] In the display substrate of the present invention, a film for preventing the diffusion of alkaline components may be formed on the surface on which the TFT is formed. The alkaline component diffusion prevention film is preferably made of, for example, SiOx, SiN, or a combination thereof, and has a thickness of preferably 100 to 1000 nm, particularly preferably 200 to 800 nm. EXAMPLES
[0045] The present invention will be described in detail below based on examples. However, the following examples are merely illustrative and the present invention is not limited to the following examples.
[0046] Table 1 shows the compositions and properties of the samples used in the examples.
[0047] [Table 1]
[0048] Each sample in the table was prepared as follows. First, glass raw materials were prepared and mixed uniformly to obtain the glass composition shown in the table, and then the glass raw materials were placed in a platinum crucible and melted at 1600°C for 20 hours. Next, the molten glass was poured onto a carbon platen and formed into a plate shape with a thickness of 5 mm using a roller, and then cooled from 700°C to room temperature at a temperature drop rate of 100°C / hour using an annealing furnace to obtain each crystallizable glass substrate.
[0049] Next, the obtained crystallizable glass substrate was heat-treated at 785°C for 8 hours to generate crystal nuclei in the glass matrix, and then heat-treated at 910°C for 4 hours to grow crystals from the crystal nuclei, and then cooled to room temperature to obtain a crystallized glass substrate. The heating rate from room temperature to 785°C (nucleation temperature) was 168°C / hour, the heating rate from 785°C (nucleation temperature) to 910°C (crystal growth temperature) was 62°C / hour, and the cooling rate from 910°C (crystal growth temperature) to room temperature was 29°C / hour.
[0050] The thermal shrinkage value of the obtained crystallized glass substrate was measured as follows. First, linear markings were engraved in two parallel positions on the crystallized glass substrate, and then the substrate was divided in a direction perpendicular to the markings to obtain two crystallized glass pieces. Next, one of the crystallized glass pieces was heated from room temperature to 500°C at a heating rate of 5°C / min, held at 500°C for 1 hour, and then cooled to room temperature at a heating rate of 5°C / min. Next, the heat-treated crystallized glass piece and the unheat-treated crystallized glass piece were arranged so that the divided surfaces matched, and fixed with adhesive tape, and the deviation amount ΔL of the markings of both was measured. Finally, the value of ΔL / L0 was measured, and this was taken as the thermal shrinkage value. Note that L0 is the length of the glass piece before heat treatment. Using the same method, the heat shrinkage value was also measured when the temperature was raised from room temperature to 600°C at a heating rate of 5°C / min, held at 600°C for 10 hours, and then cooled to room temperature at a heating rate of 5°C / min.
[0051] The thermal expansion coefficient α at 30 to 380° C. is an average value measured with a dilatometer.
[0052] The total light transmittance at a wavelength of 400 nm converted into a plate thickness of 1.1 mm was measured using a spectrophotometer.
[0053] The density is a value measured by the well-known Archimedes method.
[0054] The Young's modulus, rigidity modulus, and Poisson's ratio were measured by the bending resonance method. The specific Young's modulus is the value obtained by dividing the Young's modulus by the density.
[0055] The Vickers hardness was measured by a method in accordance with JIS Z2244-1992.
[0056] As is clear from Table 1, samples Nos. 1 to 4 had a thermal shrinkage value of 0 ppm when heated from room temperature to 500°C at a heating rate of 5°C / min, held at 500°C for 1 hour, and then cooled to room temperature at a cooling rate of 5°C / min, and are therefore believed to contribute to higher resolution displays.
[0057] Table 2 shows the compositions and properties of the samples used in the comparative examples.
[0058] [Table 2]
[0059] The samples in the table were prepared as follows. First, the glass raw materials were prepared so as to obtain the glass composition shown in the table, and after uniformly mixing, the glass raw materials were charged into a continuous melting furnace and melted at 1600°C. Next, after each process such as fining, supplying, and stirring, the glass was formed into a plate shape by the overflow downdraw method. The obtained glass substrate was evaluated for each characteristic in the same manner as in the examples. The strain point was measured based on the method of ASTM C336, and while it was not measurable in the examples, it was measurable in the comparative examples.
[0060] As is clear from Table 2, the substrate of the comparative example had a thermal shrinkage value of 12 ppm when heated from room temperature to 500°C at a heating rate of 5°C / min, held at 500°C for 1 hour, and then cooled to room temperature at a cooling rate of 5°C / min, and therefore is considered unlikely to contribute to high-definition displays. EXAMPLES
[0061] First, glass raw materials were prepared and mixed uniformly to obtain the glass composition shown in Table 1, and then melted in a tank furnace. Next, the molten glass was formed into a plate shape having a width of 2000 mm, a length of 2000 mm, and a thickness of 2 mm using a roll forming machine, and then cooled to room temperature in an annealing furnace to obtain each crystallizable glass substrate.
[0062] Next, the obtained crystallizable glass substrate was heat-treated at 785°C for 8 hours to generate crystal nuclei in the glass matrix, and then heat-treated at 910°C for 4 hours to grow crystals from the crystal nuclei, and then cooled to room temperature to obtain a crystallized glass substrate. The heating rate from room temperature to 785°C (nucleation temperature) was 168°C / hour, the heating rate from 785°C (nucleation temperature) to 910°C (crystal growth temperature) was 62°C / hour, and the cooling rate from 910°C (crystal growth temperature) to room temperature was 29°C / hour.
[0063] Furthermore, the obtained crystallized glass substrate was ground until the plate thickness became 0.5 mm, and then the surface was optically polished.
[0064] Finally, when the thermal shrinkage value of the optically polished crystallized glass substrate was measured by the same method as above, the same results as those shown in Table 1 were obtained.
Claims
1. It is made of crystallized glass and has a thermal expansion coefficient of -30x10 at 30 to 380°C. -7 ~30 x 10 -7 / °C, the surface roughness Ra of the surface is 5 nm or less, and the heat shrinkage value when heated from room temperature to 500°C at a heating rate of 5°C / min, held at 500°C for 1 hour, and then cooled to room temperature at a cooling rate of 5°C / min is 10 ppm or less, and the display substrate is used for a liquid crystal display or an organic EL display.
2. 2. The display substrate according to claim 1, wherein the heat shrinkage value is 10 ppm or less when the substrate is heated from room temperature to 600°C at a heating rate of 5°C / min, held at 600°C for 10 hours, and then cooled to room temperature at a cooling rate of 5°C / min.
3. The composition is, in mass%, SiO 2 50-70%, Al 2 O 3 10-30%, Li 2 3. The display substrate according to claim 1, further comprising 0 to 15% O.
4. Thermal expansion coefficient at 30 to 380°C is -20 x 10 -7 ~20 x 10 -7 4. The display substrate according to claim 1, wherein the temperature is 100°C.
5. 5. The display substrate according to claim 1, wherein the total light transmittance at a wavelength of 400 nm is 65% or more when converted into a plate thickness of 1.1 mm.
6. The composition is, in mass%, SiO 2 50-70%, Al 2 O 3 10-30%, Li 2 6. The display substrate according to claim 1, further comprising 1 to 15% of O.
7. 7. The display substrate according to claim 1, which is used as a TFT substrate.
Citation Information
Patent Citations
Production of transparent glass ceramic having dimensional stability at high temperature
JP1999335139A
Display and its manufacture
JP1999354021A
Process for production of glass substrates and glass substrates
JP2009196879A
Aluminosilicate glass having high strain point
JP2018027894A
Glass substrate and slow-cooling method for same
WO2014163130A1