Polyester film, its manufacturing method and membrane electrode assembly including same
A polyester film with specific diol and dicarboxylic acid composition addresses the limitations of conventional gaskets by enhancing flexibility, adhesion, and durability, improving the stability and reliability of hydrogen fuel cells through low moisture absorption and resistance to thermal cycling.
Patent Information
- Application Number
- JP2023540206
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-26
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2041-12-17
AI Technical Summary
Conventional gaskets used in fuel cells, such as fluorine and silicone, have limitations in completely blocking fuel leakage and are expensive, with issues in moldability and cold resistance, particularly in hydrogen fuel cells that experience frequent thermal cycling.
A polyester film is developed using a copolymerized resin with cyclohexanedimethanol and specific ratios of terephthalic and isophthalic acid, achieving a moisture absorption rate of 0.25% or less, which enhances flexibility, adhesion, and durability, making it suitable as a subgasket film for fuel cells.
The polyester film improves the stability and reliability of hydrogen fuel cells by preventing performance deterioration due to low moisture absorption, heat resistance, and chemical resistance, while maintaining excellent sealing properties.
Smart Images

Figure 0007574456000017 
Figure 0007574456000018 
Figure 0007574456000019
Abstract
Description
[Technical field]
[0001] The implementation relates to a polyester-based film, a method for producing the same and a membrane electrode assembly including the same. [Background technology]
[0002] A fuel cell is a device that generates electrical energy by electrochemically reacting a fuel with an oxidant, and uses hydrogen, methanol, butane, etc. as the fuel and oxygen, air, chlorine, chlorine dioxide, etc. as the oxidant. Such a fuel cell includes a plurality of unit cells, and the unit cells include a membrane electrode assembly (MEA) that can transport fuel, etc. and generate electricity.
[0003] A membrane electrode assembly may consist of an electrolyte membrane and electrodes (anode and cathode) located on both sides of the electrolyte membrane, but the performance of the membrane electrode assembly may be reduced due to the hygroscopicity of the electrolyte membrane. Therefore, a gasket is used to prevent the electrolyte membrane from being exposed to the outside and to prevent fuel, etc. from leaking out to the outside or mixing with air, etc.
[0004] Conventionally, fluorine or silicone gaskets have been mainly used because they are easy to manufacture and have excellent sealing properties, but the fluorine or silicone gaskets have limitations in completely blocking fuels, etc. In addition, fluorine-based gaskets have problems such as being expensive and having low moldability. Therefore, research is ongoing into gaskets that can replace fluorine or silicone gaskets and that also have excellent properties such as durability, heat resistance, cold resistance, and low moisture absorption.
[0005] As an example, Patent Document 1 discloses an injection-molded integrated gasket for hydrogen fuel cells that is directly injection-molded onto the separator and integrated through cross-linking to increase airtight durability. However, because it uses a fluorine-based material, it has problems such as poor cold resistance and being expensive. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent Publication No. 2014-0036536 Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the present invention provides a polyester film having excellent flexibility, adhesion, hydrolysis resistance, and durability, a method for producing the same, and a membrane electrode assembly including the same. [Means for solving the problem]
[0008] According to one embodiment, the polyester film includes a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, the diol includes cyclohexanedimethanol or a derivative thereof, the dicarboxylic acid includes 70 mol % to 99 mol % of terephthalic acid and 1 mol % to 30 mol % of isophthalic acid, and has a moisture absorption rate of 0.25% or less according to the following formula 1:
[0009] [Formula 1] JPEG0007574456000001.jpg1368 In the above formula 1, A is the weight (g) of the film measured after drying the film in an oven at 50°C for 24 hours, and B is the weight (g) of the film measured after leaving the film dried under the above conditions at a temperature of 25°C and a humidity of 100% RH for 24 hours.
[0010] Another embodiment of the method for producing a polyester film includes the steps of melt-extruding a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized to produce an unstretched sheet, stretching the unstretched sheet 2 to 5 times in a first direction at 70°C to 100°C and stretching the unstretched sheet 2 to 5 times in a second direction perpendicular to the first direction to produce a stretched sheet, heat-setting the stretched sheet at 200°C to 260°C, and relaxing the heat-set sheet to produce a polyester film, wherein the diol includes cyclohexanedimethanol or a derivative thereof, the dicarboxylic acid includes 70 mol% to 99 mol% terephthalic acid and 1 mol% to 30 mol% isophthalic acid, and the moisture absorption rate of the polyester film according to the formula 1 is 0.25% or less.
[0011] According to another embodiment, the membrane electrode assembly includes an electrolyte membrane and a subgasket surrounding an end portion of one or both sides of the electrolyte membrane, the subgasket including a copolymer polyester resin in which a diol and a dicarboxylic acid are copolymerized, the diol including cyclohexanedimethanol or a derivative thereof, the dicarboxylic acid including 70 mol % to 99 mol % of terephthalic acid and 1 mol % to 30 mol % of isophthalic acid, and the moisture absorption rate according to the formula 1 is 0.25% or less. Effect of the Invention
[0012] The polyester film according to the embodiment contains a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized with specific components and contents, and thus has excellent flexibility, adhesion, and durability. In particular, the polyester film has excellent hydrolysis resistance by satisfying the moisture absorption rate according to formula 1 of 0.25% or less, and therefore has excellent low moisture absorption.
[0013] Therefore, when the polyester-based film is used as a subgasket film for fuel cells, particularly for hydrogen fuel cells, in which low moisture absorption, heat resistance, and chemical resistance are important, the performance degradation of the fuel cell can be effectively prevented and the stability and reliability can be improved. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 shows an exploded view of a fuel cell. [Diagram 2] FIG. 2 shows a perspective view of a membrane electrode assembly according to one embodiment. [Diagram 3] FIG. 3 shows a top view of a membrane electrode assembly according to one implementation. [Figure 4] FIG. 4 shows a cross-sectional view of the membrane electrode assembly in FIG. 3 taken along line XX'. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below with reference to examples. Note that the examples are not limited to the contents disclosed below, and may be modified in various forms without departing from the spirit of the invention.
[0016] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, rather than excluding other components, unless specifically stated to the contrary.
[0017] All numbers and expressions expressing quantities of components, reaction conditions, and so forth described herein, unless otherwise indicated, should be understood to be modified in all instances by the term "about."
[0018] In this specification, terms such as first, second, primary, and secondary are used to describe various components, and the components are not limited by the terms. The terms are used only to distinguish one component from another.
[0019] In this specification, when a film, layer, etc. is described as being formed "on" or "under" another film, layer, etc., "on" and "under" include all films, layers, etc. that are formed "directly" or "indirectly via another component."
[0020] The size of each component in the drawings may be exaggerated for illustrative purposes and may differ from the actual size.
[0021] [Polyester film] According to one embodiment, the polyester film includes a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, the diol includes cyclohexanedimethanol or a derivative thereof, the dicarboxylic acid includes 70 mol % to 99 mol % of terephthalic acid and 1 mol % to 30 mol % of isophthalic acid, and has a moisture absorption rate of 0.25% or less according to the following formula 1:
[0022] [Formula 1] JPEG0007574456000002.jpg1368 In the above formula 1, A is the weight (g) of the film measured after drying the film in an oven at 50°C for 24 hours, and B is the weight (g) of the film measured after leaving the film dried under the above conditions at a temperature of 25°C and a humidity of 100% RH for 24 hours.
[0023] 1 shows an exploded view of a fuel cell. Specifically, the fuel cell 1 includes a plurality of fuel cell unit cells 10, each of which includes a membrane electrode assembly 100, a separator 200, and an end plate 300.
[0024] A membrane electrode assembly may consist of an electrolyte membrane and electrodes (anode and cathode) located on either side of the electrolyte membrane, but the performance of the membrane electrode assembly may be degraded due to the hygroscopicity of the electrolyte membrane.
[0025] Gaskets used in fuel cells are intended to prevent the electrolyte membrane from being exposed to the outside and to prevent the fuel supplied from leaking out or mixing with air, etc., and in the past, fluorine or silicone gaskets were mainly used because they are easy to manufacture and have excellent sealing properties. However, the fluorine or silicone gaskets have limitations in completely blocking fuel, etc., and film-type gaskets have been used recently. In particular, polyethylene naphthalate-based films are used as gasket films because they have excellent formability and durability, but they have limitations in improving adhesion and airtightness due to their low flexibility.
[0026] On the other hand, hydrogen fuel cells, which use hydrogen as fuel and oxygen as an oxidant, and especially automobiles using hydrogen fuel cells, are repeatedly started and stopped, generating heat and causing frequent contraction and expansion. Therefore, in addition to airtightness, durability such as low moisture absorption, heat resistance and cold resistance, and chemical resistance are very important for hydrogen fuel cell systems.
[0027] The polyester film according to the embodiment contains a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized with specific components and contents, and thus has excellent flexibility, adhesion, and durability. In particular, the polyester film has excellent hydrolysis resistance by satisfying a moisture absorption rate of 0.25% or less according to formula 1, and therefore has excellent low moisture absorption. Therefore, when the polyester film is applied as a gasket film for a hydrogen fuel cell, it can effectively prevent the performance of the hydrogen fuel cell from deteriorating, and can improve its stability and reliability.
[0028] The polyester film contains a copolymer polyester resin in which a diol and a dicarboxylic acid are copolymerized.
[0029] The diol includes cyclohexanedimethanol or a derivative thereof. For example, the diol may include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, or 1,4-cyclohexanedimethanol, and preferably includes 1,4-cyclohexanedimethanol.
[0030] The diol may contain cyclohexanedimethanol or a derivative thereof at 70 mol% or more. For example, the copolymer polyester resin may contain cyclohexanedimethanol or a derivative thereof at 72 mol% or more, 75 mol% or more, 85 mol% or more, 88 mol% or more, 90 mol% or more, 93 mol% or more, 95 mol% or more, 97 mol% or more, 99 mol% or more, or 100 mol% based on the total moles of the diol.
[0031] When the diol contains cyclohexanedimethanol or a derivative thereof within the above content range, flexibility, adhesion, durability, and hydrolysis resistance can be improved, and when the diol consists solely of cyclohexanedimethanol, heat resistance and hydrolysis resistance can be maximized.
[0032] The diol may contain one or more selected from the group consisting of ethylene glycol, neopentyl glycol, and diethylene glycol, as necessary. For example, the copolymerized polyester resin may contain one or more selected from the group consisting of ethylene glycol, neopentyl glycol, and diethylene glycol in an amount of 1 mol% to 30 mol%, 1 mol% to 20 mol%, 1 mol% to 15 mol%, 1 mol% to 10 mol%, or 1 mol% to 5 mol% based on the total moles of the diol.
[0033] The dicarboxylic acid includes 70 mol% to 99 mol% terephthalic acid and 1 mol% to 30 mol% isophthalic acid. For example, the copolymer polyester resin may include 72 mol% to 99 mol%, 75 mol% to 99 mol%, 80 mol% to 98 mol%, 83 mol% to 98 mol%, or 85 mol% to 98 mol% terephthalic acid and 1 mol% to 28 mol%, 1 mol% to 25 mol%, 1 mol% to 20 mol%, 2 mol% to 15 mol%, or 3 mol% to 13 mol% isophthalic acid, based on the total number of moles of the dicarboxylic acid.
[0034] When the contents of terephthalic acid and isophthalic acid satisfy the above ranges, flexibility, heat resistance and hydrolysis resistance can be improved.
[0035] The copolymer polyester resin may further include one or more additives selected from the group consisting of an ultraviolet stabilizer, a heat stabilizer, an antioxidant, and an inert particle.
[0036] Specifically, the UV stabilizer is at least one selected from the group consisting of benzophenone-based, benzotriazole-based, cyanoacrylate-based, and salicylic acid ester-based compounds, the heat stabilizer is an iodine-based compound, the antioxidant is a phosphorus-based antioxidant, a phenol-based antioxidant, or a sulfur-based antioxidant, and the inert particles may be, but are not limited to, silica or potassium carbonate.
[0037] The content of the additive may be 0.5 wt % to 15 wt %, 1 wt % to 13 wt %, 1.2 wt % to 12 wt %, 1.5 wt % to 10 wt %, 1.7 wt % to 8 wt %, or 1.8 wt % to 7.5 wt %, based on the total weight of the copolymerized polyester resin.
[0038] The polyester-based film according to the embodiment may be a gasket film for a fuel cell. Specifically, the polyester-based film may be a sub-gasket film for a fuel cell.
[0039] The moisture absorption rate of the polyester film according to the formula 1 may be 0.25% or less. Specifically, the moisture absorption rate of the polyester film according to the formula 1 may be 0.23% or less, 0.2% or less, 0.18% or less, 0.15% or less, 0.13% or less, or 0.1% or less. When the moisture absorption rate satisfies the above range, the polyester film has excellent hydrolysis resistance and therefore excellent low moisture absorption.
[0040] The modulus of the polyester film in the first in-plane direction is 400 kgf / mm 2 The modulus in a second direction perpendicular to the first direction is 550 kgf / mm 2 It can be the following:
[0041] For example, the modulus of the polyester film in the first in-plane direction is 390 kgf / mm 2 Below, 380kgf / mm 2 Below 350kgf / mm 2 Below 300kgf / mm 2 or less than 280kgf / mm 2 Less than 150kgf / mm 2 ~400kgf / mm 2 , 170kgf / mm 2 ~380kgf / mm 2 , 200kgf / mm 2 ~350kgf / mm 2 , 220kgf / mm 2 ~300kgf / mm 2 , or 240 kgf / mm 2 ~280kgf / mm 2 It could be.
[0042] The modulus of the polyester film in a second direction perpendicular to the first direction is 535 kgf / mm 2 Below 500kgf / mm 2 Below 450kgf / mm 2 Below 400kgf / mm 2 Below, 380kgf / mm 2 Below 350kgf / mm 2or less than 330kgf / mm 2 Less than 200kgf / mm 2 ~550kgf / mm 2 , 200kgf / mm 2 ~500kgf / mm 2 , 200kgf / mm 2 ~450kgf / mm 2 , 220kgf / mm 2 380kgf / mm 2 , 220kgf / mm 2 ~350kgf / mm 2 , 240kgf / mm 2 ~330kgf / mm 2 , or 260 kgf / mm 2 ~330kgf / mm 2 It could be.
[0043] When the modulus in the first direction and the second direction each falls within the above range, durability such as heat resistance, cold resistance, and chemical resistance is excellent.
[0044] In this specification, the first direction may be a transverse direction (TD) or a longitudinal direction (MD). Specifically, the first direction may be a longitudinal direction (MD), and a second direction perpendicular to the first direction may be a transverse direction (TD).
[0045] Furthermore, the ratio of the tensile strength in a first in-plane direction of the polyester film to the tensile strength in a second direction perpendicular to the first direction may be 0.8 to 1: 1. For example, the ratio of the tensile strength in a first in-plane direction of the polyester film to the tensile strength in a second direction perpendicular to the first direction may be 0.81 to 1: 1, 0.8 to 0.95: 1, or 0.82 to 0.94: 1. When the ratio of the tensile strengths in the first and second directions satisfies the above range, durability such as heat resistance and cold resistance is excellent.
[0046] The tensile strength of the polyester film in the first in-plane direction is 14 kgf / mm 2 For example, the tensile strength of the polyester film in the first in-plane direction may be 14.1 kgf / mm 2Above, 14.2kgf / mm 2 or more than 14.3kgf / mm 2 Above 14kgf / mm 2 ~20kgf / mm 2 , 14kgf / mm 2 ~18kgf / mm 2 , 14.2kgf / mm 2 ~16kgf / mm 2 , or 14.3 kgf / mm 2 ~15.8kgf / mm 2 It could be.
[0047] The tensile strength of the polyester film in a second direction perpendicular to the first in-plane direction is 14 kgf / mm 2 For example, the tensile strength of the polyester film in the second direction may be 14.5 kgf / mm 2 More than 15kgf / mm 2 More than 16kgf / mm 2 or more, or 16.5kgf / mm 2 Above 14kgf / mm 2 ~20kgf / mm 2 , 14.5kgf / mm 2 ~20kgf / mm 2 , 15kgf / mm 2 ~20kgf / mm 2 , 16kgf / mm 2 ~20kgf / mm 2 , 16.5kgf / mm 2 ~20kgf / mm 2 , 16.5kgf / mm 2 ~19kgf / mm 2 , 16.5kgf / mm 2 ~18.5kgf / mm 2 , or 17 kgf / mm 2 ~18kgf / mm 2 It could be.
[0048] The polyester film may have an elongation retention of 70% or more. Specifically, the polyester film may have an elongation retention of 71% or more, 72% or more, 80% or more, 85% or more, 90% or more, 93% or more, or 95% or more after being subjected to a PCT (Pressure Cooker Test, 121°C, 1.4 atm, RH 100%) for 72 hours. When the elongation retention satisfies the above range, durability such as heat resistance and cold resistance is excellent.
[0049] The elongation retention was calculated using the breaking elongation measured according to ASTM-D882 (1997). Specifically, the breaking elongation was measured five times in each of the first and second directions of the polyester film before and after the PCT at a chuck interval of 50 mm and a tensile speed of 300 m / min, the average value was obtained, and the elongation retention was calculated according to the following formula A.
[0050] [Formula A] The glass transition temperature (Tg) of the polyester film measured by dynamic mechanical analysis (DMA) may be 100° C. or higher. For example, the glass transition temperature (Tg) of the polyester film measured by dynamic mechanical analysis may be 103° C. or higher, 110° C. or higher, 115° C. or higher, 120° C. or higher, 160° C. or lower, or 150° C. or lower, and may be 100° C. to 160° C., 105° C. to 155° C., 110° C. to 150° C., 115° C. to 160° C., 115° C. to 150° C., 115° C. to 140° C., 120° C. to 160° C., 120° C. to 150° C., or 115° C. to 140° C.
[0051] The polyester film may have a glass transition temperature (Tg) of 85° C. or higher as measured by a differential scanning calorimetry (DSC). For example, the polyester film may have a glass transition temperature (Tg) of 86° C. or higher or 88° C. or higher as measured by a differential scanning calorimetry (DSC), and may be 85° C. to 150° C., 85° C. to 130° C., 88° C. to 120° C., or 88° C. to 115° C.
[0052] The polyester film may have a melting point (Tm) of 250° C. or higher as measured by a differential scanning calorimeter (DSC). For example, the polyester film may have a melting point (Tm) of 253° C. or higher, 255° C. or higher, or 260° C. or higher as measured by a differential scanning calorimeter, and may be 250° C. to 300° C., 255° C. to 295° C., 255° C. to 290° C., 260° C. to 285° C., or 263° C. to 285° C.
[0053] The polyester film may have an intrinsic viscosity (IV) of 0.6 dl / g or more. For example, the intrinsic viscosity (IV) of the polyester film may be 0.62 dl / g or more, 0.65 dl / g or more, 0.68 dl / g or more, 0.7 dl / g or more, or 0.75 dl / g or more.
[0054] The polyester film may have a heat shrinkage rate of 3% or less in a first in-plane direction when heat-treated for 30 minutes at a temperature of 150° C. For example, the polyester film may have a heat shrinkage rate of 2.5% or less, 2% or less, 1.5% or less, or 1.2% or less in a first in-plane direction when heat-treated for 30 minutes at a temperature of 150° C.
[0055] Furthermore, the polyester film may have a heat shrinkage rate of 2% or less in a second direction perpendicular to the first direction when heat-treated for 30 minutes at a temperature of 150° C. For example, the polyester film may have a heat shrinkage rate of 1.5% or less, 1% or less, 0.8% or less, 0.5% or less, or 0.3% or less in a second direction perpendicular to the first direction when heat-treated for 30 minutes at a temperature of 150° C.
[0056] Specifically, the heat shrinkage is obtained by measuring the length (mm) of the polyester film in a first direction and a second direction perpendicular to the first direction at room temperature after heat-treating the polyester film in an oven at 150° C. for 30 minutes. More specifically, the heat shrinkage in the MD direction and the heat shrinkage in the TD direction can be calculated according to the following Equations 2 and 3.
[0057] [Formula 2] JPEG0007574456000004.jpg1582[Formula 3] JPEG0007574456000005.jpg1682 In the above formula 2 and formula 3, T MD is the thermal shrinkage rate in the MD direction (%), L MD1 is the length of the initial film in the MD direction (mm), L MD2 is the length in the MD direction after heat shrinkage (mm), T TD is the thermal shrinkage rate in the TD direction (%), L TD1 is the length of the initial film in the TD direction (mm), L TD2 is the length in the TD direction after heat shrinkage (mm).
[0058] The polyester film may have a thickness of 10 μm to 150 μm. For example, the polyester film may have a thickness of 10 μm to 145 μm, 10 μm to 130 μm, 15 μm to 120 μm, 15 μm to 100 μm, 20 μm to 80 μm, or 20 μm to 60 μm.
[0059] [Method of manufacturing polyester film] Another embodiment of the method for producing a polyester film includes the steps of melt-extruding a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized to produce an unstretched sheet, stretching the unstretched sheet 2 to 5 times in a first direction at 70°C to 100°C and stretching the unstretched sheet 2 to 5 times in a second direction perpendicular to the first direction to produce a stretched sheet, heat-setting the stretched sheet at 200°C to 260°C, and relaxing the heat-set sheet to produce a polyester film, wherein the diol includes cyclohexanedimethanol or a derivative thereof, the dicarboxylic acid includes 70 mol% to 99 mol% terephthalic acid and 1 mol% to 30 mol% isophthalic acid, and the moisture absorption rate of the polyester film according to the formula 1 is 0.25% or less.
[0060] The method for producing a polyester film can provide a polyester film having excellent flexibility, adhesion, heat resistance, durability, and hydrolysis resistance by adjusting the order, temperature, stretching ratio, and relaxation rate of the stretching and relaxation steps.
[0061] First, a copolymer polyester resin in which a diol and a dicarboxylic acid are copolymerized is melt-extruded to produce an unstretched sheet.
[0062] The copolymer polyester resin is as described above.
[0063] The copolymerized polyester resin may be in the form of chips. Specifically, a mixture of the diol component and the dicarboxylic acid component is reacted at 260° C. to 320° C., 270° C. to 310° C., or 270° C. to 295° C. for 2 to 8 hours, 3 to 7 hours, or 4 to 7 hours to produce the copolymerized polyester resin in the form of chips.
[0064] The copolymerized polyester resin is melt-extruded through a T-die and then cooled to obtain an unstretched sheet.
[0065] The melt extrusion step may be carried out at a temperature of Tm+5°C to Tm+70°C, Tm+5°C to Tm+50°C, or Tm+7°C to Tm+35°C, and the cooling step may be carried out at a temperature of Tg-120°C to Tg+20°C, Tg-110°C to Tg+10°C, Tg-105°C to Tg-30°C, Tg-105°C to Tg-50°C, Tg-105°C to Tg-65°C, or Tg-105°C to Tg-80°C.
[0066] For example, the melt extrusion temperature may be 260° C. to 320° C., 270° C. to 310° C., or 270° C. to 295° C., and the cooling temperature may be −20° C. to 100° C., 0° C. to 90° C., 5° C. to 75° C., 10° C. to 60° C., 10° C. to 50° C., or 15° C. to 45° C. When the melt extrusion temperature satisfies the above range, the copolymer polyester resin can be smoothly melted, and the viscosity of the extrudate can be appropriately maintained and controlled.
[0067] Thereafter, the unstretched sheet is stretched 2 to 5 times in a first direction at 70° C. to 100° C., and then stretched 2 to 5 times in a second direction perpendicular to the first direction to produce a stretched sheet.
[0068] Specifically, the unstretched sheet is preheated while being transported at a speed of 10 m / min to 110 m / min, 20 m / min to 90 m / min, or 20 m / min to 70 m / min, and then primarily stretched in a first direction.
[0069] The preheating step may be performed for 0.01 to 1 minute at 70° C. to 120° C. For example, the preheating temperature may be 72° C. to 120° C., 75° C. to 115° C., or 80° C. to 100° C., and the preheating time may be 0.02 to 1 minute, 0.05 to 0.5 minutes, or 0.08 to 0.2 minutes.
[0070] The primary stretching may be performed at a temperature of 75° C. to 100° C. and an elongation ratio of 2 to 5 times. For example, the primary stretching step may be performed at a temperature of 75° C. to 98° C., 75° C. to 95° C., 80° C. to 95° C., or 85° C. to 93° C. and an elongation ratio of 2 to 4.8 times, 2 to 4.5 times, 2.5 to 4 times, 2.5 to 3.5 times, or 2.8 to 3.3 times. When the temperature and elongation ratio of the primary stretching satisfy the above ranges, the heat resistance and hydrolysis resistance can be improved.
[0071] According to another embodiment, heat may be applied using a far-infrared heater (R / H) at a position 40 mm to 150 mm away from the preheated unstretched sheet prior to the first stretching. For example, the far-infrared heater may be located 55 mm to 150 mm, 70 mm to 150 mm, 70 mm to 100 mm, 85 mm to 120 mm, or 100 mm to 150 mm away from one side of the preheated unstretched sheet, and the far-infrared heater may apply heat at 650°C to 800°C, 700°C to 800°C, or 730°C to 780°C.
[0072] After the primary stretching, the film is secondarily stretched in a second direction perpendicular to the first direction. The secondary stretching may be performed at a temperature 10°C to 30°C higher than the preheating temperature and at an elongation rate of 2 to 5 times. For example, the secondary stretching may be performed at a temperature of 100°C to 140°C, 110°C to 130°C, or 120°C to 130°C and at an elongation rate of 2 to 4.8 times, 2.5 to 4.5 times, 2.5 to 4 times, or 2.8 to 4 times.
[0073] The ratio (d1 / d2) of the stretch ratio (d1) in the first direction to the stretch ratio (d2) in the second direction may be 0.5 to 1. For example, the ratio (d1 / d2) of the stretch ratio (d1) in the first direction to the stretch ratio (d2) in the second direction may be 0.5 to 0.9 or 0.6 to 0.8. When the stretch ratios in the first and second directions are within the above ranges, hydrolysis resistance and low moisture absorption can be improved.
[0074] In addition, a coating step may be performed before the second stretching. Specifically, the coating step may be performed by in-line coating to impart functionality such as antistatic properties to the polyester film, but is not limited thereto.
[0075] Thereafter, the stretched sheet is heat-set at 200°C to 260°C.
[0076] Specifically, the heat setting is annealing, and may be performed at 200° C. to 260° C. for 0.01 to 1 minute. For example, the heat setting step may be performed at a temperature of 205° C. to 260° C., 210° C. to 255° C., 225° C. to 250° C., 238° C. to 248° C., or 238° C. to 245° C. for 0.01 to 0.8 minutes, 0.05 to 0.5 minutes, 0.08 to 0.2 minutes, or 0.08 to 0.15 minutes. When the temperature and time of the heat setting step are within the above ranges, the heat shrinkage rate of the polyester film can be easily adjusted.
[0077] Finally, the heat-set sheet is relaxed to produce a polyester film.
[0078] Specifically, the heat-set sheet may be relaxed in a first direction or a second direction perpendicular to the first direction.
[0079] For example, when the heat-set sheet is relaxed in a first direction or a second direction perpendicular to the first direction, the relaxation step may be performed at a temperature of 100°C to 180°C or 110°C to 175°C with a relaxation rate of 0.5% to 5%, 0.8% to 4%, 0.8% to 3.5%, or 0.8% to 3.2%.
[0080] Alternatively, the heat-set sheet may be primarily relaxed in a first direction and then secondly relaxed in a second direction, or the heat-set sheet may be primarily relaxed in a second direction and then secondly relaxed in a first direction. For example, the heat-set sheet may be primarily relaxed in a TD direction and then secondly relaxed in a MD direction.
[0081] Specifically, the relaxation step may include a primary relaxation at a relaxation rate of 1% to 10% in the second direction and a secondary relaxation at a relaxation rate of 0.5% to less than 2% in the first direction. Specifically, when the heat-set sheet is subjected to a primary relaxation and then a secondary relaxation, the primary relaxation step may be performed at a temperature of 150°C to 200°C and a relaxation rate of 1% to 10%, and the secondary relaxation step may be performed at a temperature of 110°C to 190°C and a relaxation rate of 0.5% to less than 2%.
[0082] For example, the first relaxation step is performed at a temperature of 150°C to 190°C, 155°C to 200°C, 160°C to 180°C, or 165°C to 175°C with a relaxation rate of 1% to 9.5%, 1% to 9%, 1.5% to 8%, 1.5% to 7%, 2% to 6%, or 2% to 5%, and the second relaxation step is performed at a temperature of 110°C to 185°C, 110°C to 180°C, or 110°C. The relaxation may be performed at a temperature of 0.5% to less than 2%, 0.5% to 1.95%, 0.7% to 1.8%, 0.85% to 1.65%, 0.9% to 1.6%, 0.9% to 1.4%, or 0.95% to 1.2%.
[0083] When the temperature and relaxation rate of the first and second relaxation steps are within the above ranges, the heat resistance and hydrolysis resistance can be improved.
[0084] Furthermore, the ratio of the primary relaxation rate to the secondary relaxation rate may be 1:0.1 to 1.0. For example, the ratio of the primary relaxation rate to the secondary relaxation rate may be 1:0.1 to 0.9, 1:0.1 to 0.8, 1:0.2 to 0.7, or 1:0.25 to 0.65. When the ratio of the primary relaxation rate to the secondary relaxation rate satisfies the above range, heat resistance and hydrolysis resistance can be maximized.
[0085] Specifically, the second relaxation step may be divided into two or more sections, and the second relaxation rate may be the sum of the relaxation rates of the sections. For example, if the second relaxation step is divided into four sections and the relaxation rates of the four sections are 0%, 0.5%, 0.5%, and 1%, respectively, the second relaxation rate is 2%. By dividing the second relaxation step into sections as described above, it is easier to adjust the relaxation rate, and thus the heat resistance and hydrolysis resistance can be maximized.
[0086] The film transport speed in the second relaxation step may be 1% to 10% slower than the film transport speed in the first relaxation step. For example, the film transport speed in the second relaxation step may be 2% to 10% or 2% to 8% slower than the film transport speed in the first relaxation step.
[0087] [Membrane-electrode assembly] According to another embodiment, the membrane electrode assembly includes an electrolyte membrane and a subgasket surrounding an end portion of one or both sides of the electrolyte membrane, the subgasket including a copolymer polyester resin in which a diol and a dicarboxylic acid are copolymerized, the diol including cyclohexanedimethanol or a derivative thereof, the dicarboxylic acid including 70 mol % to 99 mol % of terephthalic acid and 1 mol % to 30 mol % of isophthalic acid, and the moisture absorption rate according to the formula 1 is 0.25% or less.
[0088] Specifically, the subgasket may include a first subgasket film and a second subgasket film.
[0089] 2 is a perspective view of a membrane electrode assembly according to an embodiment of the present invention, specifically illustrating a membrane electrode assembly 100 including an electrolyte membrane 140, a first electrode 150 and a second electrode 160 on either side of the electrolyte membrane, a first subgasket film 110 on the top of the first electrode, and a second subgasket film 120 on the bottom of the second electrode.
[0090] Fig. 3 shows a top view of a membrane electrode assembly according to one embodiment. Specifically, Fig. 3 shows a top view of the membrane electrode assembly of Fig. 2, in which a first electrode 150 is located at the center and a first subgasket film 110 is located surrounding the first electrode.
[0091] Fig. 4 is a cross-sectional view of the membrane electrode assembly of Fig. 3 taken along X-X'. Specifically, Fig. 4 illustrates a membrane electrode assembly including an electrolyte membrane 140 located at the center, a first electrode 150 and a second electrode 160 located at the top and bottom of the electrolyte membrane, a first subgasket film 110 located at the top of both ends of the electrolyte membrane, a second subgasket film 120 located at the bottom of both ends of the electrolyte membrane, and an adhesive layer 130 interposed between the first subgasket film 110 and the second subgasket film 120.
[0092] The membrane electrode assembly according to the embodiment includes a subgasket surrounding an end portion of one or both sides of the electrolyte membrane, thereby improving the stability and reliability of the fuel cell. Specifically, the subgasket surrounds and seals an end portion of one or both sides of the electrolyte membrane, thereby effectively preventing fuel from leaking to the outside or mixing with other substances such as air. In addition, it is possible to prevent the performance of the membrane electrode assembly from being deteriorated due to the hygroscopicity of the electrolyte membrane.
[0093] The first subgasket film may be the polyester-based film described above. Specifically, the first subgasket film and the second subgasket film may be the polyester-based film described above, and the components and contents thereof may be the same or different from each other.
[0094] Furthermore, the ratio of the thickness of the first subgasket film to the thickness of the second subgasket film may be 0.5 to 1.5: 1. For example, the ratio of the thickness of the first subgasket film to the thickness of the second subgasket film may be 0.5 to 1.4: 1, 0.7 to 1.2: 1, or 0.9 to 1.1: 1.
[0095] The adhesive layer may include at least one selected from the group consisting of an acrylic resin, a silicone resin, and a urethane resin. Specifically, the adhesive layer may be formed by coating a resin composition including at least one selected from the group consisting of an acrylic resin, a silicone resin, and a urethane resin, but is not limited thereto.
[0096] The adhesive layer may have a thickness of 5 μm to 80 μm. For example, the adhesive layer may have a thickness of 5 μm to 75 μm, 7 μm to 70 μm, 10 μm to 65 μm, 15 μm to 50 μm, 15 μm to 45 μm, or 15 μm to 30 μm.
[0097] The subgasket may have a tensile strength of 105 MPa or more. For example, the subgasket may have a tensile strength of 108 MPa or more, 110 MPa or more, 115 MPa or more, or 120 MPa or more.
[0098] The electrolyte membrane may act as a separator to transport fuel or the like and to prevent direct mixing with air. The electrolyte membrane may include one or more resins selected from the group consisting of perfluorosulfonic acid-based resins, polyimide-based resins, polyethersulfone-based resins, polyphenylene oxide-based resins, polyethylene naphthalate-based resins, and polyester-based resins.
[0099] The first electrode and the second electrode may face each other and have the same area. Specifically, the first electrode and the second electrode may be located facing each other in the center of the electrolyte membrane, and the first electrode and the second electrode may contact 60% to 90% or 65% to 95% of the area of one side of the electrolyte membrane, respectively.
[0100] The first electrode may be an anode or a cathode, and the second electrode may be a cathode or an anode. Specifically, the first electrode may be an anode, and the second electrode may be a cathode.
[0101] In addition, the membrane electrode assembly may further include a catalyst layer and a gas diffusion layer that can improve performance. The catalyst layer and the gas diffusion layer are not particularly limited as long as they are used in membrane electrode assemblies in the art.
[0102] (Example) The above contents will be described in more detail with reference to the following examples. Note that the following examples are only for illustrating the present invention, and the scope of the examples is not limited to these examples.
[0103] [Production of copolymer polyester resin] (Production Example 1-1) 100 mol% cyclohexanedimethanol (CHDM) as the diol component, and 96 mol% terephthalic acid (TPA) and 4 mol% isophthalic acid (IPA) as the dicarboxylic acid components were mixed and reacted at 285°C for 6 hours to produce chip-shaped copolymer polyester resin.
[0104] (Production Examples 1-2 to 1-6) Chip-shaped copolymer polyester resins were produced in the same manner as in Production Example 1-1, except that the components and contents were changed as shown in Table 1 below.
[0105] JPEG0007574456000006.jpg86164
[0106] [Production of polyester film] Example 1 The copolymer polyester resin of Preparation Example 1-1 prepared above was put into an extruder and melt-extruded at 290° C., and then cooled with a casting roll at 25° C. to prepare an unstretched sheet.
[0107] The unstretched sheet was preheated at 92°C while being transported at a speed of 30 m / min, and heat of 750°C was applied to the preheated unstretched sheet by a far-infrared heater (R / H) at a position 80 mm from the preheated unstretched sheet while being transported at a speed of 30 m / min.
[0108] Thereafter, the unstretched sheet was first stretched in the MD direction at 90° C. at an elongation ratio of 3.1 times, and secondly stretched in the TD direction at 125° C. at an elongation ratio of 3.9 times, and then heat-set at 240° C. for 0.1 minutes.
[0109] The heat-set sheet was then primarily relaxed at a relaxation rate of 3% in the TD at a temperature of 170° C. and a transport speed of 50 m / min, and then secondary relaxed at a relaxation rate of 1.0% in the MD at a temperature of 120° C. and a transport speed of 50 m / min to produce a polyester film having a thickness of 25 μm. The secondary relaxation in the MD was performed in four sections, and the relaxation rates of the four sections were 0%, 0%, 0.5%, and 0.5%, respectively.
[0110] (Example 2 and Comparative Examples 1 to 4) Polyester films were produced in the same manner as in Example 1, except that the copolymer polyester resins of Production Examples 1-2 to 1-6 were used instead of Production Example 1-1, and the process conditions were as shown in Table 2 below.
[0111] In the case of Comparative Example 4 in which the copolymer polyester resin of Production Example 1-6 was used, film formation was impossible, and therefore a film could not be produced.
[0112] JPEG0007574456000007.jpg94161
[0113] (Experimental Example) (Experimental Example 1: Glass transition temperature (Tg) and melting point (Tm)) For the films (10 mg) of Examples 1 and 2 and Comparative Examples 1 to 3, the glass transition temperature (Tg) and melting point (Tm) were measured using a differential scanning calorimeter (Q2000, manufactured by TA Instruments).
[0114] (Experimental Example 2: Intrinsic Viscosity (IV)) The films (10 mg) of Examples 1 and 2 and Comparative Examples 1 to 3 were each dissolved in o-chlorophenol at 100° C., and then the relative viscosity was measured by determining the drop time of the sample using an Ostwald viscometer in a thermostatic bath at 35° C. The obtained relative viscosity was converted to intrinsic viscosity (IV) based on a relative viscosity-intrinsic viscosity conversion table, and the values rounded off to two decimal places are shown in Table 3 below.
[0115] (Experimental Example 3: Hygroscopicity) The films of Examples 1 and 2 and Comparative Examples 1 to 3 were dried in an oven at 50° C. for 24 hours, and the weight (A) of the film was measured. The films dried under the above conditions were left at a temperature of 25° C. and a humidity of 100% RH for 24 hours, and the weight (B) of the film was measured. The moisture absorption rate was calculated according to the following Equation 1.
[0116] [Formula 1] JPEG0007574456000008.jpg1368 In the above formula 1, A is the weight (g) of the film measured after drying the film in an oven at 50°C for 24 hours, and B is the weight (g) of the film measured after leaving the film dried under the above conditions at a temperature of 25°C and a humidity of 100% RH for 24 hours.
[0117] (Experimental Example 4: Elongation retention rate) The films of Examples 1 and 2 and Comparative Examples 1 to 3 were subjected to a PCT (Pressure Cooker Test, 121° C., 1.4 atmospheric pressure, RH 100%) for 72 hours, and the elongation retention rate was measured.
[0118] Specifically, before and after the PCT, the polyester film was measured for elongation at break five times in each of the first and second directions at a chuck distance of 50 mm and a tensile speed of 300 m / min in accordance with ASTM-D882 (1997), the average value was calculated, and the elongation retention rate was calculated according to the following formula A.
[0119] [Formula A] JPEG0007574456000009.jpg14128 (Experimental Example 5: Modulus) For the films of Examples 1 and 2 and Comparative Examples 1 to 3, the modulus in the MD and TD directions was measured according to KS B 5521.
[0120] (Experimental Example 6: Heat shrinkage rate) The films of Examples 1 and 2 and Comparative Examples 1 to 3 were cut into a length of 100 mm and a width of 100 mm, and heat-treated in an oven at 150° C. for 30 minutes. The lengths (mm) in the TD and MD directions were then measured at room temperature, and the thermal shrinkage rates were calculated using the following Equations 2 and 3.
[0121] [Formula 2] JPEG0007574456000010.jpg1582[Formula 3] JPEG0007574456000011.jpg1682 In the above formula 2 and formula 3, T MD is the thermal shrinkage rate in the MD direction (%), L MD1 is the length of the initial film in the MD direction (mm), L MD2 is the length in the MD direction after heat shrinkage (mm), T TD is the thermal shrinkage rate in the TD direction (%), L TD1 is the length of the initial film in the TD direction (mm), L TD2is the length in the TD direction after heat shrinkage (mm).
[0122] (Experimental Example 7: Tensile strength) The films of Examples 1 and 2 and Comparative Examples 1 to 3 were cut to a length of 100 mm and a width of 15 mm, and were subjected to an experiment using an INSTRON universal testing machine (4206-001, manufacturer: UTM) based on ASTM D 882, with the chuck spacing set to 50 mm, at a tensile speed of 500 mm / min, and the tensile strength was measured using a program built into the machine.
[0123] JPEG0007574456000012.jpg59156
[0124] JPEG0007574456000013.jpg69156
[0125] As shown in Tables 3 and 4 above, the polyester films of Examples 1 and 2 exhibited superior results in both hydrolysis resistance and durability compared to the films of Comparative Examples 1-3.
[0126] Specifically, the polyester films of Examples 1 and 2 have intrinsic viscosity, moisture absorption, elongation retention, modulus, heat shrinkage, and tensile strength all within the preferred ranges, and therefore have excellent durability such as heat resistance and excellent hydrolysis resistance, and therefore have excellent low moisture absorption. [Explanation of symbols]
[0127] 1: Fuel cell 10: Fuel cell unit cell 100: Membrane electrode assembly 200: Separator 300: End plate 110: First subgasket film 120: Second subgasket film 130: Adhesive layer 140: Electrolyte membrane 150: 1st electrode 160:Second electrode
Claims
1. A polyester film comprising: The polyester resin includes a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, the diol comprises cyclohexanedimethanol or a derivative thereof; the dicarboxylic acid comprises 70 mol % to 99 mol % terephthalic acid and 1 mol % to 30 mol % isophthalic acid; The ratio of the tensile strength in a first in-plane direction of the polyester film to the tensile strength in a second direction perpendicular to the first direction is 0.8 to 1:1; The first direction is a machine direction (MD), the second direction is a transverse direction (TD), and the moisture absorption rate according to the following formula 1 is 0.25% or less: [Formula 1] In the above formula 1, A is the weight (g) of the film measured after drying the film in an oven at 50°C for 24 hours, and B is the weight (g) of the film measured after leaving the film dried under the above conditions at a temperature of 25°C and a humidity of 100% RH for 24 hours.
2. The polyester film according to claim 1 , which is a film for a subgasket of a fuel cell.
3. 2. The polyester film according to claim 1, wherein the diol comprises 70 mol % or more of cyclohexanedimethanol or a derivative thereof.
4. The tensile modulus of the polyester film in the first in-plane direction is 400 kgf / mm 2 The modulus in a second direction perpendicular to the first direction is 550 kgf / mm or less. 2 2. The polyester film according to claim 1, wherein:
5. The polyester film according to claim 1, which has an elongation retention rate of 70% or more after being subjected to a PCT (Pressure Cooker Test, 121° C., 1.4 atm, RH 100%) for 72 hours.
6. A step of melt-extruding a copolymer polyester resin obtained by copolymerizing a diol and a dicarboxylic acid to produce an unstretched sheet; stretching the unstretched sheet by 2 to 5 times in a first direction at 70° C. to 100° C., and then stretching the unstretched sheet by 2 to 5 times in a second direction perpendicular to the first direction to produce a stretched sheet; heat fixing the stretched sheet at 200°C to 260°C; and relaxing the heat-set stretched sheet to produce a polyester film. the diol comprises cyclohexanedimethanol or a derivative thereof; the dicarboxylic acid comprises 70 mol % to 99 mol % terephthalic acid and 1 mol % to 30 mol % isophthalic acid; The ratio of the tensile strength in a first in-plane direction of the polyester film to the tensile strength in a second direction perpendicular to the first direction is 0.8 to 1:1; The first direction is a machine direction (MD), and the second direction is a transverse direction (TD), and the moisture absorption rate of the polyester film is 0.25% or less according to the following formula 1: [Formula 1] In the above formula 1, A is the weight (g) of the polyester film measured after drying the polyester film in an oven at 50°C for 24 hours, and B is the weight (g) of the polyester film measured after leaving the polyester film dried under the above conditions at a temperature of 25°C and a humidity condition of 100% RH for 24 hours.
7. the ratio (d1 / d2) of the stretch ratio (d1) in the first direction to the stretch ratio (d2) in the second direction is 0.5 to 1; 7. The method of claim 6, wherein the relaxation step comprises a primary relaxation at an elongation rate of 1% to 10% in the second direction and a secondary relaxation at an elongation rate of 0.5% to less than 2% in the first direction.
8. An electrolyte membrane; a subgasket film surrounding an end portion of one or both sides of the electrolyte membrane; The subgasket film contains a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, the diol comprises cyclohexanedimethanol or a derivative thereof; the dicarboxylic acid comprises 70 mol % to 99 mol % terephthalic acid and 1 mol % to 30 mol % isophthalic acid; a ratio of a tensile strength in a first in-plane direction of the subgasket film to a tensile strength in a second direction perpendicular to the first direction is 0.8 to 1:1; The first direction is a machine direction (MD), the second direction is a transverse direction (TD), and the moisture absorption rate according to the following formula 1 is 0.25% or less. [Formula 1] In the above formula 1, A is the weight (g) of the polyester film measured after drying the subgasket film in an oven at 50°C for 24 hours, and B is the weight (g) of the subgasket film measured after leaving the subgasket film dried under the above conditions at a temperature of 25°C and a humidity condition of 100% RH for 24 hours.
9. 9. The membrane electrode assembly according to claim 8, wherein the subgasket film has a tensile strength of 105 MPa or more.
Citation Information
Patent Citations
Seal material
JP2015026571A
KR2014-0036536
Polyester resin composition and biaxially oriented polyester film comprising same
WO2019103370A1