Lithium metal battery and method for producing same

The introduction of a gel-type polymer electrolyte with a crosslinked polymer in lithium metal batteries addresses dendrite growth and conductivity issues, enhancing battery performance and stability.

WO2024205034A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD

Patent Information

Application Number
PCT/KR2024/002357
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-02-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium metal batteries face issues with lithium dendrite growth due to side reactions with the electrolyte, leading to reduced lifespan and safety concerns, and conventional gel-type polymer electrolytes have insufficient ionic conductivity and stability at high voltages.

Method used

A lithium metal battery design incorporating a gel-type polymer electrolyte with a crosslinked polymer formed from a polyfunctional crosslinker and a (meth)acrylic compound with a polyethylene glycol moiety, which includes a liquid electrolyte and a separator with a porous substrate, enhancing ionic conductivity and oxidation stability.

Benefits of technology

The solution improves the high-rate characteristics and lifespan of lithium metal batteries by suppressing lithium dendrite growth and maintaining stability across a wide voltage range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024002357_03102024_PF_FP_ABST
    Figure KR2024002357_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a lithium metal battery and a method for producing same, the lithium metal battery comprising a positive electrode, a negative electrode current collector, and a gel-type polymer electrolyte interposed between the positive electrode and negative electrode current collector, wherein the gel-type polymer electrolyte comprises a crosslinked polymer and a liquid electrolyte containing an organic solvent and lithium salt, and the crosslinked polymer is a product of a reaction between multifunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having a polyethylene glycol moiety.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium metal battery and manufacturing method thereof

[0001] It relates to a lithium metal battery and a method for manufacturing the same.

[0002] Lithium metal batteries currently on the market primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge / discharge, enhancing the stability of lithium metal batteries. However, their low capacity necessitates the use of higher-capacity anode materials.

[0003] Lithium metal, which has a much larger theoretical electric capacity than carbon-based negative electrode materials, can be used as a negative electrode material.

[0004] When lithium metal is charged and discharged, dendrites are formed on the surface of the lithium metal due to a side reaction with the electrolyte, and the growth of the dendrites can cause a short circuit between the positive and negative electrodes, which can reduce the life characteristics of a lithium metal battery containing lithium metal.

[0005] One aspect is to provide a lithium metal battery with a new structure.

[0006] Another aspect is to provide a method for manufacturing the above-described lithium metal battery.

[0007] According to one embodiment, a lithium metal battery is provided, comprising: a positive electrode; a negative electrode current collector; and an electrolyte layer disposed between the positive electrode and the negative electrode current collector, wherein the electrolyte layer includes a gel-type polymer electrolyte, wherein the gel-type polymer electrolyte includes a liquid electrolyte containing an organic solvent and a lithium salt and a crosslinked polymer, wherein the crosslinked polymer is a reaction product of a polyfunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having a polyethylene glycol moiety.

[0008] The above electrolyte layer may further include a separator.

[0009] Between the electrolyte layer and the negative electrode current collector, a negative electrode active material layer, a protective layer, or a combination thereof may be included.

[0010] A lithium metal layer is further included between the electrolyte layer and the negative electrode current collector, and the intensity of the fluorine peak in XPS analysis of the surface of the lithium metal layer may be greater than the intensity of the oxygen peak.

[0011] A gel-type polymer electrolyte may be present in the pores of the above separator.

[0012] The mixing weight ratio of the polyfunctional crosslinking agent having three or more functional groups and the (meth)acrylic compound having a polyethylene glycol moiety is 9:1 to 2:1.

[0013] The above gel-type polymer electrolyte comprises 90 to 99 parts by weight of a liquid electrolyte and 1 to 10 parts by weight of a crosslinked polymer.

[0014] In the above gel-type polymer electrolyte, the content of the liquid electrolyte is, for example, 92 to 99 parts by weight, 94 to 99 parts by weight, or 95 to 97 parts by weight, and the content of the crosslinked polymer is, for example, 1 to 8 parts by weight, 1 to 6 parts by weight, for example, 3 to 5 parts by weight.

[0015] The above separator comprises a porous substrate, wherein the porous substrate comprises polypropylene, polyethylene, or a combination thereof.

[0016] According to another aspect, a method for manufacturing a lithium metal battery is provided, including the steps of: preparing a negative electrode current collector; preparing an electrolyte layer; preparing a positive electrode; preparing an assembly by laminating the negative electrode current collector, the electrolyte layer, and the positive electrode; injecting a gel-type polymer electrolyte forming composition including a multifunctional crosslinking agent having three or more functional groups, a (meth)acrylic compound having a polyethylene glycol moiety, an organic solvent, and a liquid electrolyte containing a lithium salt into the assembly; and crosslinking the injected gel-type polymer electrolyte forming composition to prepare a lithium metal battery including the gel-type polymer electrolyte.

[0017] A negative electrode active material layer is further laminated on the above negative electrode current collector. And the cross-linking is performed by heat treatment at 40 to 120°C.

[0018] The composition for forming the above gel-type polymer electrolyte comprises a polyfunctional crosslinking agent having three or more functional groups, a (meth)acrylic compound having a polyethylene glycol moiety, a lithium salt, an organic solvent, and an initiator.

[0019] According to one aspect, a gel-type polymer electrolyte having improved ionic conductivity and enhanced oxidation stability is provided. Using this gel-type polymer electrolyte, a lithium metal battery having improved high-rate characteristics and cycle life characteristics is provided.

[0020] Figure 1 schematically illustrates the laminated structure of a lithium metal battery according to an embodiment.

[0021] Figure 2 schematically illustrates a laminated structure of a lithium metal battery according to another embodiment.

[0022] Figure 3 is a schematic diagram of a lithium metal battery according to an embodiment.

[0023] Figure 4 is a schematic diagram of a lithium metal battery according to another embodiment.

[0024] Figure 5 is a schematic diagram of a lithium metal battery according to another embodiment.

[0025] <Explanation of key symbols in the drawing>

[0026] 1: Lithium metal battery 2, 20: Cathode

[0027] 3, 10: Anode 4: Separator

[0028] 5: Battery case 6: Cap assembly

[0029] 7: Battery structure 8: Electrode tab

[0030] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.

[0031] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.

[0032] In order to clearly express various layers and regions in the drawings, the thickness is shown enlarged or reduced. Similar parts are designated by the same drawing reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.

[0033] In the present disclosure, the "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle is, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction. When the particle size is measured using a scanning electron microscope, it is determined as the average value of 30 or more randomly selected particles having a size of 1 μm or more, excluding fine particles.

[0034] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.

[0035] In this disclosure, “alloy” means a mixture of two or more metals.

[0036] In the present disclosure, “positive electrode active material” means a positive electrode material capable of undergoing lithiation and delithiation, and “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.

[0037] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material, and “delithiation” and “delithiating” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.

[0038] In the present disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery, and “discharging” and “discharging” mean a process of removing electrochemical energy from a battery.

[0039] In the present disclosure, “positive electrode” and “cathode” mean an electrode where electrochemical reduction and lithiation occur during a discharge process, and “negative electrode” and “anode” mean an electrode where electrochemical oxidation and delithiation occur during a discharge process.

[0040] Hereinafter, a lithium metal battery and a manufacturing method thereof according to embodiments will be described in more detail.

[0041] A non-cathode lithium metal battery is a battery that uses only a cathode current collector without a cathode active material layer. When charging, lithium ions transferred from the cathode are deposited on the surface of the cathode current collector, and when discharging, the lithium deposited on the cathode current collector is eluted again and inserted into the cathode, thereby operating the battery.

[0042] Non-cathode lithium metal batteries offer the advantage of maximizing energy density per volume / weight of the battery by omitting lithium metal as the anode active material. However, lithium metal precipitates during operation, and the uneven current concentration during oxidation / reduction causes lithium dendrites to grow. These dendrites not only cause lithium anode loss, reducing battery capacity and lifespan, but can also cause short-circuiting between the anode and cathode, posing safety concerns.

[0043] To solve the above-mentioned problems, a method has been proposed in which a protective film is introduced to minimize contact between lithium and the electrolyte and thereby reduce side reactions, or a method has been proposed in which a liquid electrolyte is introduced into a network of cross-linked polymers to minimize exposure of the electrolyte on the electrode surface and to create a uniform flow of lithium ions throughout the electrode, thereby suppressing lithium dendrite growth by using a gel-type polymer electrolyte.

[0044] The gel-type polymer electrolytes known so far have a semi-solid form and improved safety compared to pure liquid electrolytes, but they have high resistance and the characteristic of being decomposed at high voltage, making them difficult to use at high voltages. In addition, since the conventional gel-type polymer electrolytes mainly use non-ionic conductive cross-linking agents, the ionic conductivity is insufficient, and thus improvement in this is required.

[0045] According to one embodiment, a lithium metal battery includes a positive electrode; an anode current collector; and an electrolyte layer disposed between the positive electrode and the negative electrode current collector, wherein the electrolyte layer includes a gel-type polymer electrolyte, and the gel-type polymer electrolyte includes a liquid electrolyte containing an organic solvent and a lithium salt and a crosslinking polymer, and the crosslinking polymer includes a reaction product of a polyfunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having polyethylene glycol moieties. In the present disclosure, the reaction product of a polyfunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having polyethylene glycol moieties refers to a crosslinking product of a polyfunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having polyethylene glycol moieties.

[0046] A negative electrode active material layer, a protective layer, or a combination thereof may be included between the negative electrode current collector and the electrolyte layer.

[0047] A separator may further be included between the negative electrode current collector and the electrolyte layer.

[0048] The above separator comprises a porous substrate. When the lithium metal battery comprises a separator, the negative electrode active material layer, protective layer, or a combination thereof may be disposed between the negative electrode current collector and the separator. In this way, the negative electrode active material layer and / or protective layer disposed between the negative electrode current collector and the separator may be included, or the negative electrode active material layer or protective layer may be absent.

[0049] A lithium metal battery according to one embodiment comprises: a negative electrode current collector; an electrolyte layer (separator) disposed on the negative electrode current collector; a gel-type polymer electrolyte disposed on the electrolyte layer (separator); and a positive electrode disposed on the gel-type polymer electrolyte, wherein the gel-type polymer electrolyte comprises a liquid electrolyte containing an organic solvent and a lithium salt and a crosslinked polymer, and the crosslinked polymer may comprise a reaction product of a polyfunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having a polyethylene glycol moiety.

[0050] A gel-type polymer electrolyte may be present in the pores or inside of the above-mentioned separator.

[0051] The above-mentioned cross-linking agent having three or more functional groups refers to a multifunctional cross-linking agent having three or more cross-linkable functional groups. A material that is electrochemically stable at a voltage of about 4.3 V or higher is used in an operating environment of a positive electrode using a positive electrode active material having a nickel content of 90 mol% or higher. The number of cross-linkable functional groups is, for example, 3 to 10, or 3 to 6. These crosslinking agents include trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, trimethylolpropane ethoxylate triacrylate, trimethylolpropane propoxylate triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylate tetraacrylate, dipentaerythritol pentaacrylate, Dipentaerythritol hexaacrylate (DPHA), tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), propoxylated glyceryl triacrylate, or a combination thereof.

[0052] The (meth)acrylic compound having the above polyethylene glycol moiety is a compound that undergoes a crosslinking reaction with a polyfunctional crosslinking agent having three or more functional groups, and has two or more functional groups capable of undergoing a crosslinking reaction. When a crosslinking reaction is performed using such a compound, the degree of crosslinking increases, the phenomenon of decomposition at high voltage is suppressed, and not only is oxidation stability improved, but also a gel-type polymer electrolyte with improved ionic conductivity at high voltage can be obtained.

[0053] The (meth)acrylic compound having the above polyethylene glycol moiety has an ion-conducting ethylene glycol moiety, and thus the ion conductivity of a gel polymer electrolyte formed therefrom can be increased. Examples of the (meth)acrylic compound having the polyethylene glycol moiety include polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), trimethylolpropane trimethacrylate (TMPTMA), or a combination thereof.

[0054] The mixing weight ratio of the polyfunctional crosslinking agent having three or more functional groups and the (meth)acrylic compound having a polyethylene glycol moiety is 9:1 to 2:1, 9:1 to 2.5:1, 9:1 to 2.3:1, 9:1 to 3:1, or 6:1 to 4:1. When the mixing weight ratio is within the above range, not only is the degree of crosslinking increased and the oxidation stability improved, but also a gel-type polymer electrolyte having improved ionic conductivity can be obtained.

[0055] The gel-type polymer electrolyte contains 90 to 99 parts by weight, 92 to 98 parts by weight, 93 to 97 parts by weight, for example, 95 to 97 parts by weight, of a liquid electrolyte and 1 to 10 parts by weight, 1 to 8 parts by weight, 2 to 7 parts by weight, for example, 3 to 5 parts by weight, of a crosslinked polymer. When the contents of the liquid electrolyte and the crosslinked polymer in the gel-type polymer electrolyte are within the above ranges, ionic conductivity is improved.

[0056] The ionic conductivity of the above gel-type polymer electrolyte is 0.19 S / cm or more, or 0.19 S / cm to 0.5 S / cm. A lithium metal battery having a gel-type polymer electrolyte having such an ionic conductivity can have improved high-rate characteristics and output characteristics.

[0057] A gel-type polymer electrolyte containing a liquid electrolyte and a cross-linked polymer is contained within the pores of a porous substrate constituting the separator. In a separator having this structure, the liquid electrolyte is contained within a cross-linked polymer network with a cross-linked structure, thereby preventing leakage to the outside.

[0058] Referring to Fig. 1, an electrolyte layer (30) and a positive electrode (10) are laminated on a negative electrode current collector (21). The negative electrode (20) contains a negative electrode current collector (21), and a negative electrode active material layer is absent. The electrolyte layer (30) may contain a separator.

[0059] The positive electrode (10) contains a positive electrode active material layer (12) and a positive electrode current collector (11).

[0060] The electrolyte layer (30) may contain a gel-type polymer electrolyte.

[0061] When the electrolyte layer contains a separator, the gel polymer electrolyte may have a structure arranged between the separator and the positive electrode. According to another embodiment, the gel polymer electrolyte may not exist between the separator and the positive electrode, but may exist only inside the separator. Here, the inside of the separator may mean pores. According to another embodiment, the separator may have a structure in which the gel polymer electrolyte exists on at least one surface, for example, both surfaces of the separator. Alternatively, the gel polymer electrolyte may exist between the negative electrode current collector and the separator. When a negative electrode active material layer, such as a lithium metal layer, exists on the negative electrode current collector, the gel polymer electrolyte may exist between the negative electrode active material layer and the separator.

[0062] The separator may contain a porous substrate. The pores of the separator may contain a gel-type polymer electrolyte containing a liquid electrolyte and a cross-linked polymer.

[0063] The pore diameter of the separator is typically 0.01 to 10 μm, and the thickness is 5 to 20 μm. Examples of such separators include sheets or nonwoven fabrics made of olefin-based polymers such as polypropylene, glass fiber, or polyethylene. When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte may also function as the separator.

[0064] Among the above separation membranes, specific examples of olefin-based polymers include polyethylene, polypropylene, or a multilayer membrane of two or more layers thereof, and mixed multilayer membranes such as a polyethylene / polypropylene two-layer separation membrane, a polyethylene / polypropylene / polyethylene three-layer separation membrane, and a polypropylene / polyethylene / polypropylene three-layer separation membrane may be used.

[0065] In a lithium metal battery according to an embodiment, a liquid electrolyte is impregnated with a gel-type polymer electrolyte within a polymer matrix, so that there is no leakage, and electrochemical side reactions and electrolyte decomposition reactions occurring at the positive and negative electrodes are suppressed, thereby ensuring stability and improving battery characteristics.

[0066] A gel-type polymer electrolyte contains a liquid electrolyte, and the liquid electrolyte contains a lithium salt and an organic solvent.

[0067] The lithium salt includes a first lithium salt and a second lithium salt. The ionic conductivity of the gel polymer electrolyte can be improved by including the first lithium salt and the second lithium salt.

[0068] The first and second lithium salts are borate-based lithium salts. Compared to phosphorus-based lithium salts, borate-based lithium salts exhibit improved high-temperature stability and can suppress the production of hydrofluoric acid (HF). By including borate-based lithium salts in the first and second lithium salts, the high-temperature cycling characteristics of lithium batteries can be improved.

[0069] The first lithium salt and the second lithium salt may, for example, be independently a fluorine-containing borate-based lithium salt. By including a fluorine-containing borate-based lithium salt in the first lithium salt and the second lithium salt, the composition of the SEI layer formed during charge and discharge of the lithium battery can be more effectively modified. For example, by increasing the fluorine (F) content of the SEI layer, the structural stability of the SEI layer can be increased, and side reactions with organic solvents can be effectively suppressed. Consequently, the reversibility of the electrode reaction of the lithium battery can be improved.

[0070] The first lithium salt and the second lithium salt may be, for example, a non-cyclic borate lithium salt and a cyclic borate lithium salt. Since the first lithium salt is a non-cyclic lithium salt, the ionic conductivity of the gel polymer electrolyte can be more effectively increased. Since the second lithium salt is a cyclic lithium salt, the aggregation of anions is increased, so that it can more effectively participate in the composition modification of the SEI layer, and the high-temperature stability of the gel polymer electrolyte can be improved.

[0071] The ionic conductivity of the gel polymer electrolyte may be reduced by not including the first lithium salt. The structural stability of the SEI layer may be reduced by not including the second lithium salt.

[0072] Fluorine-containing borate lithium salts may include, for example, LiBF4, LiBF3(C2F5), compounds represented by chemical formulas 1 to 12, or combinations thereof.

[0073] <Chemical Formula 1> <Chemical Formula 2>

[0074]

[0075] <Chemical Formula 3> <Chemical Formula 4>

[0076]

[0077] <Chemical Formula 5> <Chemical Formula 6>

[0078]

[0079] <Chemical Formula 7> <Chemical Formula 8>

[0080]

[0081] <Chemical Formula 9> <Chemical Formula 10>

[0082]

[0083] <Chemical Formula 11> <Chemical Formula 12>

[0084]

[0085] The first lithium salt may include, for example, LiBF4, and the second lithium salt may include a compound selected from compounds represented by chemical formulas 1 to 12.

[0086] The first lithium salt may include LiBF4, and the second lithium salt may include, for example, a compound of chemical formula 1.

[0087] The gel polymer electrolyte may not contain, for example, a phosphorus-based lithium salt. By not containing a phosphorus-based lithium salt, the high-temperature stability of the gel polymer electrolyte is improved and the generation of hydrofluoric acid (HF) can be suppressed.

[0088] The gel polymer electrolyte may not contain, for example, LiBOB. By not containing LiBOB in the gel polymer electrolyte, the ionic conductivity of the gel polymer electrolyte may be further improved and the solubility of the lithium salt in the carbonate solvent may be further improved.

[0089] The contents of the first lithium salt and the second lithium salt in the gel polymer electrolyte can be, for example, independently from each other, from more than 0 to 1.2 M, from 0.1 M to 1.0 M, or from 0.4 M to 0.8 M. By having the first lithium salt and the second lithium salt each having a content in this range, the gel polymer electrolyte can simultaneously provide excellent ionic conductivity and formation of a structurally stable SEI layer.

[0090] The content of the first lithium salt and the second lithium salt may be, for example, from more than 0 to 1.2 M, from 0.1 M to 1.0 M or from 0.4 M to 0.8 M, independently of each other, in the precursor composition for forming a gel-type polymer electrolyte before adding the first crosslinking monomer and the thermal initiator.

[0091] The content ratio of the first lithium salt and the second lithium salt may be, for example, 1:9 to 9:1, 3:7 to 7:3, or 4:6 to 6:4. When the first lithium salt and the second lithium salt have a content ratio within this range, the gel polymer electrolyte can simultaneously provide excellent ionic conductivity and the formation of a structurally stable SEI layer. The content ratio of the first lithium salt and the second lithium salt may be, for example, a molar ratio.

[0092] The gel polymer electrolyte includes a first organic solvent and a second organic solvent. By including the first organic solvent and the second organic solvent in the gel polymer electrolyte, the interfacial resistance between the gel polymer electrolyte and the positive electrode and / or the interfacial resistance between the gel polymer electrolyte and the lithium metal layer deposited during charging can be more effectively reduced. The first organic solvent and the second organic solvent include, for example, a carbonate-based compound. The first organic solvent and the second organic solvent are, for example, carbonate-based organic solvents. By including the first carbonate-based organic solvent and the second carbonate-based organic solvent in the gel polymer electrolyte, the first lithium salt and the second lithium salt can be easily dissolved in the organic solvent, and the viscosity of the precursor composition for forming the gel electrolyte can be lowered. The first organic solvent includes, for example, a linear carbonate compound. Since the first organic solvent is a linear carbonate solvent, the viscosity of the precursor composition before crosslinking can be lowered. The precursor composition can be easier to handle. The second organic solvent includes, for example, a cyclic carbonate compound substituted with a substituent. The substituent of the cyclic carbonate compound includes, for example, a halogen, a cyano group (CN), a nitro group (NO2), or a combination thereof. Since the second organic solvent is a cyclic carbonate solvent substituted with a substituent, the first lithium salt and the second lithium salt can be more easily dissolved in the precursor composition for forming a gel electrolyte, and the substituent can participate in the formation of the SEI layer, thereby improving the structural stability of the SEI layer. The first organic solvent can include, for example, diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, ethyl propyl carbonate, dipropyl carbonate, or a combination thereof.The second organic solvent may include, for example, vinylene carbonate substituted with one or more substituents selected from halogen, cyano group (CN), and nitro group (NO2); vinylethylene carbonate substituted with one or more substituents selected from halogen, cyano group (CN), and nitro group (NO2); fluoroethylene carbonate (FEC); fluoroethylene carbonate substituted with one or more substituents selected from halogen, cyano group (CN), and nitro group (NO2); or a combination thereof. The first organic solvent may include, for example, diethyl carbonate, and the second organic solvent may include, for example, a fluorine-substituted cyclic carbonate compound. The second organic solvent may include, for example, fluoroethylene carbonate. The gel polymer electrolyte may not include, for example, an unsubstituted cyclic carbonate solvent. By not including an unsubstituted cyclic carbonate solvent, the first lithium salt and the second lithium salt can be more easily dissolved in the precursor composition for forming a gel polymer. The volume ratio of the first organic solvent and the second organic solvent can be, for example, 5.5:4.5 to 9:1, 6:4 to 9:1, 6:4 to 8:2, or 6:4 to 7:3. When the first organic solvent and the second organic solvent have a volume ratio within this range, a composition for forming a gel electrolyte having excellent lithium salt solubility and low viscosity can be provided. A gel polymer electrolyte obtained from the composition for forming a gel electrolyte having excellent lithium salt solubility and low viscosity can provide excellent mechanical properties and enhanced ionic conductivity.

[0093] The lithium salt may be, for example, at least one selected from LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiC(FSO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, and LiB(C2O4)2.

[0094] The concentration of the lithium salt may be, for example, 1 to 5 M, for example, 1 to 2.5 M, in the liquid electrolyte. In the above range, a sufficient amount of lithium ions required for charging and discharging a lithium metal battery can be generated.

[0095] As the organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyrropionate, ethyl propionate, etc. can be used. Carbonate solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, and diethyl carbonate can be used.

[0096] According to an embodiment, when a gel-type polymer electrolyte is present in the pores of a porous substrate, the interfacial resistance between the positive electrode, negative electrode, and separator can be minimized and lithium can be easily moved.

[0097] As shown in Fig. 2, a negative electrode active material layer (22) can be placed between the negative electrode current collector (21) and the electrolyte layer (30).

[0098] The negative active material layer (22) can be formed by plating lithium metal after charging. In this way, the negative active material layer (22) can be a lithium plating layer (plated lithium layer). The lithium plating layer is a lithium metal layer.

[0099] The lithium metal layer acts as, for example, a lithium reservoir. The lithium alloy includes, but is not limited to, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., and any lithium alloy used in the art can be used. The lithium metal layer may be made of one of these alloys or lithium, or may be made of several types of alloys. The lithium metal layer is, for example, a plated layer. The lithium metal layer is deposited between the electrolyte layer (30) and the negative electrode current collector (21), for example, during the charging process of the lithium metal battery (1).

[0100] The lithium metal layer is a metal layer containing lithium or a lithium alloy. The lithium metal layer contains lithium or a lithium alloy. The lithium metal layer acts as, for example, a lithium reservoir. The lithium alloy includes, but is not limited to, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., and any lithium alloy used in the art can be used. The lithium metal layer may be made of one of these alloys or lithium, or may be made of several types of alloys. The lithium metal layer is, for example, a plated layer. The lithium metal layer is deposited between the electrolyte layer (30) and the negative electrode current collector (21), for example, during the charging process of a lithium metal battery (1).

[0101] The thickness of the lithium metal layer is not particularly limited, but is, for example, 1 to 200 μm, 1 to 150 μm, 1 to 100 μm, 1 to 50 μm, 1 to 30 μm, 1 to 22 μm, or 1 μm to 10 μm. If the thickness of the lithium metal layer is too thin, it is difficult for the lithium metal layer to perform the role of a lithium reservoir. If the thickness of the lithium metal layer is too thick, the volume of the lithium metal battery (1) may excessively increase, and the cycle characteristics of the lithium metal battery (1) may rather deteriorate.

[0102] The thickness of the lithium metal layer may be, for example, smaller than the thickness of the positive electrode active material layer (12). The thickness of the lithium metal layer may be, for example, 70% or less, 60% or less, 50% or less, 40% or less, or 30% or less of the thickness of the positive electrode active material layer (12). The thickness of the lithium metal layer may be, for example, 1 to 70%, 1 to 60%, 1 to 50%, 1 to 40%, or 1 to 30% of the thickness of the positive electrode active material layer (12). Since the thickness of the lithium metal layer is smaller than the thickness of the positive electrode active material layer, a volume change during charge and discharge of the lithium battery (1) can be suppressed. As a result, deterioration due to a volume change of the lithium metal battery (1) can be suppressed.

[0103] A gel-type polymer electrolyte can effectively prevent deterioration of a lithium battery by suppressing side reactions with a lithium metal layer during charge / discharge of the lithium battery. For example, a solid electrolyte interphase (SEI) layer may be formed between a gel-type polymer electrolyte and a precipitated lithium metal layer during charge / discharge of a lithium metal battery. By modifying the composition of the SEI layer to have an increased content of lithium salt decomposition products, side reactions between the gel-type polymer electrolyte and the lithium metal layer can be more effectively suppressed. In addition, the gel-type polymer electrolyte and / or the modified SEI layer can effectively prevent internal short circuits of a lithium battery by more effectively suppressing the growth of lithium dendrites from the lithium metal layer.

[0104] The separator is disposed on the upper portion of the negative electrode current collector, and further includes a lithium metal layer between the negative electrode current collector and the separator, and in an XPS (X-ray photoelectron spectroscopy) analysis of the surface of the lithium metal layer, for example, a peak intensity derived from a fluorine (F) element may be greater than a peak intensity derived from an oxygen (O) element. In an XPS analysis of the surface of the lithium metal layer, for example, a peak intensity derived from a fluorine (F) element may be greater than 100%, 105% or more, 110% or more, or 120% or more of the peak intensity derived from an oxygen (O) element. In an XPS analysis of the surface of the lithium metal layer, for example, a peak intensity derived from a fluorine (F) element may be greater than 100% to 200%, 105% to 200%, 110% to 200%, or 120% to 200% of the peak intensity derived from an oxygen (O) element. The structural stability of the SEI layer formed on the surface of the lithium metal layer can be improved by mainly including an inorganic compound containing fluorine (F). As a result, the cycle characteristics of the lithium metal battery (1) can be improved. In contrast, when the SEI layer formed on the surface of the lithium metal layer mainly includes an organic compound containing oxygen (O), the structural stability of the SEI layer can be reduced. The peak derived from the fluorine (F) element can be, for example, a peak derived from the fluorine (F) 1s orbital. The peak derived from the oxygen (O) element can be, for example, a peak derived from the oxygen (O) 1s orbital.

[0105] After assembling the lithium metal battery (1), a lithium metal layer is deposited by charging, and since the lithium metal layer is not included during the assembly of the lithium metal battery (1), the energy density of the lithium metal battery (1) increases. When a lithium metal layer is additionally deposited by charging after assembling the lithium metal battery (1), the region between the negative electrode (20), i.e., the negative electrode current collector (21), and the electrolyte layer (30) is a Li-free region that does not include lithium (Li), for example, in the initial state of the lithium metal battery (1) or in the state after complete discharge.

[0106] Alternatively, the negative electrode active material layer (22) can be arranged during assembly of the lithium metal battery. The thickness of the negative electrode active material layer is 1 to 500 um, 3 to 500 um, 5 to 500 um, or 10 to 500 um. When the thickness of the negative electrode active material layer is within the above range, a lithium metal battery with improved cycle characteristics can be manufactured without a decrease in energy density.

[0107] Instead of the negative active material layer, a protective layer can be formed. The thickness of the protective layer is 1 μm to 20 μm. The protective layer contains a polymer such as polyvinyl alcohol, polyimide, vinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, carboxymethyl cellulose, styrene butylene rubber, or a polymer and an inorganic filler. Inorganic fillers include, for example, SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, AIN(Aluminum Nitride), SiC(Silicon Carbide), BoN(Boron Nitride), or a combination thereof. Introducing an additional protective layer in this way can minimize the contact between lithium and the electrolyte, thereby reducing side reactions, and can suppress lithium dendrite growth by creating a uniform flow of lithium ions throughout the electrode.

[0108] The above-mentioned negative electrode active material layer (22) includes lithium metal or a lithium alloy. Alternatively, when the negative electrode active material layer is placed during battery assembly, the negative electrode active material layer may include a carbon-based material alone, a carbon-based material, and at least one selected from metals and metalloids.

[0109] The carbon-based material includes amorphous carbon, and the average particle size of the amorphous carbon is 10 nm to 100 nm. The carbon-based material may include, for example, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or a combination thereof.

[0110] According to one embodiment, the negative active material layer may include lithium foil, lithium powder, or a combination thereof.

[0111] The lithium foil may include, for example, lithium metal foil, lithium alloy foil, or a combination thereof. The lithium powder may include lithium metal powder, lithium alloy powder, or a combination thereof. A lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, and the lithium alloy contains lithium and a first metal. The first metal may be indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

[0112] Lithium alloys include, for example, lithium-silver alloys, lithium-zinc alloys, lithium-magnesium alloys, and lithium-tin alloys. The negative electrode active material layer including a lithium metal foil may be, for example, a lithium metal layer. The negative electrode active material layer including a lithium alloy foil may be, for example, a lithium alloy layer. The negative electrode active material layer including lithium metal powder and / or lithium alloy powder may be introduced by coating a slurry including lithium powder and a binder onto a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer may be formed of a metal-based negative electrode active material.

[0113] The negative electrode current collector is composed of a material that does not react with lithium, i.e., does not form an alloy or compound. The material constituting the negative electrode current collector includes, but is not limited to, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), and any material that is used as an electrode current collector in the relevant technical field may be used. The negative electrode current collector may be composed of one of the above-mentioned metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode current collector is, for example, in the form of a plate or foil.

[0114] The negative electrode active material layer may contain a negative electrode active material and a binder.

[0115] The negative active material has, for example, a particle form. The average particle diameter of the negative active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 3 ㎛, 10 nm to 2 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 300 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative active material has an average particle diameter in this range, reversible plating and / or dissolution of lithium can be facilitated during charge and discharge. The average particle diameter of the negative active material is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.

[0116] The negative electrode active material may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of the carbon-based negative electrode active material include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material classified as amorphous carbon in the relevant technical field may be used. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium, and therefore is not a metal negative electrode active material in the present specification. The negative electrode active material layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight.The negative electrode active material included in the negative electrode active material layer may include a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 50 wt%, 15 to 40 wt%, 20 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, a lithium metal battery are further improved.

[0117] The binder included in the negative electrode active material layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode active material layer does not include a binder, the negative electrode active material layer can be easily separated from the ceramic coating layer (21) or the negative electrode current collector (21). The content of the binder included in the negative electrode active material layer may be, for example, 1 to 20 wt% based on the total weight of the negative electrode active material layer.

[0118] The thickness of the negative electrode active material layer may be, for example, 1 ㎛ to 200 ㎛, 5 ㎛ to 100 ㎛, or 10 ㎛ to 50 ㎛. The thickness of the negative electrode active material layer may be, for example, 1% to 50%, 1% to 30%, 1% to 10%, or 1% to 5% of the thickness of the positive electrode active material layer. If the thickness of the negative electrode active material layer is too thin, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the thickness of the negative electrode active material layer is excessively increased, the energy density of the lithium metal battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics.

[0119] When the thickness of the negative electrode active material layer decreases, the charge capacity of the negative electrode active material layer also decreases, for example. The charge capacity of the negative electrode active material layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode active material layer is too small, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the charge capacity of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery using the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode active material layer is also calculated in the same way. That is, the charge capacity of the negative electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer. When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the negative electrode active material layer. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is the estimated capacity using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode active material layer are directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode active material layer may be the initial charge capacity measured at the first charge cycle.

[0120] [Lithium metal battery]

[0121] According to one embodiment, a lithium metal battery includes a positive electrode; a negative electrode; and a separator disposed between the positive electrode and the negative electrode. Such a lithium metal battery can simultaneously provide excellent life characteristics. The lithium metal battery may be, but is not limited to, a lithium primary battery, a lithium secondary battery, a lithium-sulfur battery, a lithium-air battery, etc., and any lithium metal battery used in the relevant technical field may be used.

[0122] Lithium metal batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.

[0123] (anode)

[0124] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.

[0125] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A1 - b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E1 - b B b O2 - c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE2- b B b O4 - c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni1 -b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni1 -b- c Co b B c O2 - α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni1 -b- c Co b B c O2 - α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni1 -b- c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni1 -b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni1 -b- c Mn b B c O2 -α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.

[0126] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0127] The cathode active material is, for example, Li a Ni x Co y M z O2 - b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O2 - b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O2 - b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO4 - b X b (Here, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).

[0128] Conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.

[0129] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.

[0130] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.

[0131] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium metal battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0132] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.

[0133] In one embodiment of the present invention, the positive electrode collector (11) may include, for example, a base film and a metal layer disposed on one or both sides of the base film.

[0134] The positive electrode collector uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The thickness of the positive electrode collector is, for example, 1 ㎛ to 100 ㎛, 1 ㎛ to 50 ㎛, 5 ㎛ to 25 ㎛, or 10 ㎛ to 20 ㎛.

[0135] The cathode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The base film may be, for example, an insulator. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film may soften or liquefy, thereby blocking battery operation and suppressing a sudden increase in current. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The metal layer can act as an electrochemical fuse and cut off in case of overcurrent to prevent short circuits. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the positive electrode current collector decreases, thereby improving the stability of the lithium battery in case of a short circuit. A lead tab can be added to the metal layer for external connection. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melt, so that the metal layer can be electrically connected to the lead tab. To strengthen the welding between the metal layer and the lead tab, a metal chip can be added between the metal layer and the lead tab.The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be easily bonded to the lead tab during the welding process by melting. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. Since the metal layer has a thickness within this range, the stability of the electrode assembly can be secured while maintaining conductivity. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure as the cathode current collector, the weight of the cathode can be reduced, and as a result, the energy density of the cathode and lithium metal battery can be improved.

[0136] (Separator)

[0137] Next, a separator to be inserted between the anode and cathode is prepared.

[0138] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion transport and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in nonwoven or woven form. For lithium-ion batteries, rollable separators, such as polyethylene or polypropylene, are used, while for lithium-ion polymer batteries, separators with excellent organic electrolyte absorption capacity are used.

[0139] The membrane is manufactured by the following exemplary method, but is not limited to this method and may be adjusted according to required conditions.

[0140] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast onto a support and dried, and then a separator film peeled from the support is laminated onto the electrode to form a separator.

[0141] The polymer used in membrane manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.

[0142] (cathode)

[0143] The cathode contains a cathode current collector.

[0144] In one embodiment of the present invention, although not shown in the drawings, the negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The polymer may be an insulating polymer. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film softens or liquefies, thereby blocking battery operation and suppressing a sudden increase in current. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may correspond to, for example, the first metal substrate. The metal layer may additionally include a coating layer including a second metal. The negative electrode current collector (21) may additionally include a metal piece and / or a lead tab. For more specific details on the base film, metal layer, metal chip, and lead tab of the negative electrode current collector (21), refer to the positive electrode current collector. By having such a structure, the negative electrode current collector (21) can reduce the weight of the negative electrode, thereby improving the energy density of the negative electrode and the lithium battery.

[0145] A negative electrode active material layer may be formed on the negative electrode current collector. The negative electrode active material layer may be formed as a lithium deposition layer after charging. Alternatively, the negative electrode active material layer may be formed using a negative electrode active material during battery assembly.

[0146] The method of forming a negative electrode active material layer using a negative electrode active material can be manufactured in the same manner as described above, except that the negative electrode active material is used instead of the positive electrode active material when forming the positive electrode active material layer.

[0147] A lithium metal battery may further include, for example, a thin film comprising an element capable of forming an alloy with lithium on one surface of an anode current collector. The thin film is disposed between the anode current collector and the anode active material layer. The thin film includes, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By disposing the thin film on one surface of the anode current collector, for example, the deposition shape of the first anode active material layer deposited between the thin film and the anode active material layer becomes flatter, and the cycle characteristics of the lithium metal battery may be further improved.

[0148] (Separator)

[0149] A separation membrane according to the embodiment is used.

[0150] Organic electrolytes are manufactured, for example, by dissolving lithium salts in organic solvents.

[0151] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0152] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x + 1SO2)(C y F 2y + 1SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.

[0153] A lithium metal battery according to one embodiment may further include a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof. The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0154] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li1 +x+ y (Al, Ga) x (Ti, Ge)2 - x Si y P3 - y O 12 (0≤x≤1 0≤y≤1), Li x La yTiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li3 + x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li3 + x La3Zr2 - a M a O 12 A garnet-type solid electrolyte selected from (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10).

[0155] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1??x GeO4("LISICON", 0≤x<1), Li3 + y PO4 - x N x ("LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O5 ( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n (0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcination) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.

[0156] The polymer solid electrolyte may, for example, comprise a mixture of a lithium salt and a polymer, or a polymer having ion-conducting functional groups. The polymer solid electrolyte may, for example, be a polymer electrolyte that is solid at 25°C and 1 atm. The polymer solid electrolyte may, for example, not comprise a liquid.The polymer solid electrolyte comprises a polymer, and the polymer is, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), Polyacrylonitrile (PAN), polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. +) or a combination thereof, but is not limited thereto, and any lithium salt that can be used in polymer electrolytes in the relevant technical field is possible. The lithium salt can be any lithium salt that can be used in the relevant technical field. The lithium salt is, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x + 1SO2)(C y F 2y + 1SO2) (x and y are each 1 to 20), LiCl, LiI or a mixture thereof, etc. The polymer included in the polymer solid electrolyte may be, for example, a compound including 10 or more, 20 or more, 50 or more or 100 or more repeating units. The weight average molecular weight of the polymer included in the polymer solid electrolyte may be, for example, 1000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more or 1,000,000 Dalton or more.

[0157] A gel electrolyte is, for example, a polymer gel electrolyte. A gel electrolyte can have a gel state without containing a polymer, for example.

[0158] A polymer gel electrolyte may include, for example, a liquid electrolyte and a polymer, or an organic solvent and a polymer having an ion-conducting functional group. The polymer gel electrolyte may be, for example, a polymer electrolyte that is in a gel state at 25°C and 1 atm. The polymer gel electrolyte may, for example, have a gel state without containing a liquid. The liquid electrolyte used in the polymer gel electrolyte may be, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent; a mixture of a lithium salt and an organic solvent; a mixture of an ionic liquid and an organic solvent; or a mixture of a lithium salt, an ionic liquid, and an organic solvent. The polymer used in the polymer gel electrolyte may be selected from among the polymers used in solid polymer electrolytes. The organic solvent may be selected from among the organic solvents used in liquid electrolytes. The lithium salt may be selected from among the lithium salts used in solid polymer electrolytes. An ionic liquid refers to a salt that has a melting point below room temperature, is composed solely of ions, and is liquid at room temperature or a molten salt at room temperature. The ionic liquid may include, for example, one or more cations selected from among a) ammonium compounds, pyrrolidinium compounds, pyridinium compounds, pyrimidinium compounds, imidazolium compounds, piperidinium compounds, pyrazolium compounds, oxazolium compounds, pyridazinium compounds, phosphonium compounds, sulfonium compounds, triazolium compounds, and mixtures thereof, and b) one or more anions selected from among BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-. A polymer solid electrolyte can form a polymer gel electrolyte, for example, by being impregnated into a liquid electrolyte in a secondary battery. The polymer gel electrolyte may further include inorganic particles. The polymer included in the polymer gel electrolyte may be, for example, a compound containing 10 or more, 20 or more, 50 or more, or 100 or more repeating units.The weight average molecular weight of the polymer included in the polymer gel electrolyte may be, for example, 500 Dalton or more, 1000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more, or 1,000,000 Dalton or more.

[0159] (lithium metal battery)

[0160] Referring to FIG. 3, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). A gel-type polymer electrolyte (not shown) is disposed between the separator and the positive electrode. The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium metal battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0161] Referring to FIG. 3, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.

[0162] A gel-type polymer electrolyte (not shown) can be placed between the separator (4) and the anode (3).

[0163] A pouch-type lithium metal battery corresponds to the lithium metal battery of FIG. 4, which uses a pouch as a battery case. The pouch-type lithium metal battery includes one or more battery structures. A separator is disposed between the positive electrode and the negative electrode to form the battery structure. A gel-type polymer electrolyte (not shown) may be disposed between the separator and the positive electrode. The battery structure may be impregnated with the electrolyte, accommodated and sealed in a pouch, thereby completing the pouch-type lithium metal battery. For example, although not shown in the drawing, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. An organic electrolyte may be used as the electrolyte.

[0164] The lithium metal battery of the present disclosure may be, for example, an all-solid-state lithium metal battery.

[0165] The lithium metal battery of the present disclosure has excellent discharge capacity and cycle life characteristics, as well as high energy density, and is therefore used in, for example, electric vehicles (EVs). For example, it is used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). It is also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0166] Lithium metal batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.

[0167] [Method for manufacturing lithium metal batteries]

[0168] According to one embodiment, a lithium metal battery comprises the steps of: preparing an anode current collector; preparing a separator; preparing an anode; preparing an assembly by laminating the anode current collector, the separator, and the anode; injecting a composition for forming a gel-type polymer electrolyte, which includes a monomer for forming a crosslinked polymer, an organic solvent, and a liquid electrolyte containing a lithium salt, into the assembly; and crosslinking the injected composition for forming a gel-type polymer electrolyte to prepare a lithium metal battery including a gel-type polymer electrolyte.

[0169] The monomer for forming a crosslinked polymer includes a polyfunctional crosslinking agent having three or more functional groups and a (meth)acrylic compound having a polyethylene glycol moiety. The composition for forming the gel-type polymer electrolyte may contain an initiator.

[0170] The step of injecting a composition for forming a gel-type polymer electrolyte into the above assembly may be performed as an impregnation step under vacuum so that the composition for forming a gel-type polymer electrolyte can sufficiently penetrate into the pores of the porous substrate.

[0171] Methods for forming a gel-type polymer electrolyte include curing using heat, UV, or high-energy radiation (electron beam, γ-ray). The curing reaction using heat can be performed at a temperature of 40 to 120°C, for example, 50 to 90°C, with a heat treatment for 30 to 120 minutes.

[0172] The above heat treatment varies depending on the type of the (meth)acrylic compound having a polyfunctional crosslinking agent having three or more functional groups and a polyethylene glycol moiety, but is performed at a temperature of, for example, 40 to 120°C.

[0173] The weight average molecular weight of the polyfunctional crosslinking agent having three or more functional groups may be in the range of 200 to 2,000, and may be in the range of 200 to 1,000, for example, in the range of 200 to 800. And the weight average molecular weight of the (meth)acrylic compound having a polyethylene glycol moiety is 300 to 600. If the weight average molecular weight of the polyfunctional crosslinking agent having three or more functional groups and the (meth)acrylic compound having a polyethylene glycol moiety is smaller than the above range, the density of crosslinking points within the molecular structure of the polymer after crosslinking may be too high, so that the movement of the lithium salt may not be free, and if it is larger than the above range, the density of crosslinking points within the molecular structure of the polymer after crosslinking may be too low, so that the electrolyte blocking ability may be reduced. In the present disclosure, the weight average molecular weight is determined using gel permeation chromatography.

[0174] The content of the polyfunctional crosslinking agent having three or more functional groups as the monomer for forming the crosslinked polymer and the (meth)acrylic compound having a polyethylene glycol moiety is 3 to 5 parts by weight based on 100 parts by weight of the composition for forming a gel-type polymer electrolyte. If the total content of the monomer for forming the crosslinked polymer is less than the above range, the degree of crosslinking during crosslinking is too low, so that the crosslinking characteristics cannot be sufficiently expressed, and the electrolyte moisture absorption capacity and mechanical characteristics may be poor, and if it exceeds the above range, the internal resistance within the electrode plate increases, which may act as a cause of capacity reduction during high-rate charge / discharge.

[0175] The composition for forming the above gel-type polymer electrolyte may further include a crosslinking agent, a photoinitiator, etc. to assist in crosslinking of the crosslinkable monomer. The crosslinking agent, initiator, etc. are not particularly limited as long as they are commonly used in the relevant technical field.

[0176] The initiator can be, for example, benzoin ethyl ether.

[0177] The content of the crosslinking agent, initiator, etc. may be within a typical range. For example, the content of the initiator may be used in a range of 0.1 to 10 parts by weight, 0.1 to 5 parts by weight, or 0.2 to 3 parts by weight based on 100 parts by weight of the total content of the monomer for forming the crosslinking polymer. Using the gel polymer electrolyte formed in this way, the ionic conductivity can be maintained at a value close to that of the liquid electrolyte, and the gel polymer electrolyte inside the positive and negative electrodes can play a role in preventing leakage of the liquid electrolyte. The electrolyte can be trapped in the polymer matrix of the gel polymer electrolyte and maintained within the polymer matrix, thereby helping the smooth movement of lithium ions. In addition, the excellent electrochemical properties of the polymer can suppress the electrolyte decomposition reaction within the range of -1 V to 5 V.

[0178] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0179] Example 1: 3 wt% of cross-linked polymer content in TMPTA / PEG-DA (8:2) GPE (hereinafter: 3 wt% of cross-linked polymer)

[0180] A polyethylene single film having a thickness of 20 μm was laminated as a separator on top of a copper foil having a thickness of 10 μm, which is a negative current collector, and a positive electrode was laminated on the other side of the separator to manufacture a laminate. After injecting the composition for forming a gel-type polymer electrolyte manufactured in Manufacturing Example 1 into the prepared laminate, a lithium metal battery including a gel-type polymer electrolyte was manufactured by thermally cross-linking in an oven at 70°C for 1 hour and 30 minutes.

[0181] Lithium metal batteries have a cathode / gel polymer electrolyte (separator) / negative current collector structure. The pores of the separator contain a gel polymer electrolyte.

[0182] The composition for forming the above gel-type polymer electrolyte was prepared by mixing trimethylolpropane triacrylate (TMPTA), a multifunctional crosslinking agent having three or more functional groups, polyethyleneglycol diacrylate (PEG-DA), a liquid electrolyte, and benzoin ethyl ether (Sigma-Aldrich, 240.30 g / mol) as an initiator.

[0183] As a liquid electrolyte, a 2:1 volume ratio mixed solvent of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC) was used, in which 0.6 M LiBF4 and 0.6 M lithium difluoro(oxalate)borate (LiDFOB) were added.

[0184] The composition for forming the above gel-type polymer electrolyte includes 2.4 parts by weight of TMPTA, 0.6 parts by weight of PEG-DA, and 95 parts by weight of a liquid electrolyte based on 100 parts by weight of the total weight of the composition for forming the above gel-type polymer electrolyte, and the content of the initiator was 5 parts by weight based on 100 parts by weight of the total weight of the above multifunctional crosslinking agent and polyethylene glycol diacrylate.

[0185] The mixing weight ratio of the above TMPTA and PEG-DA is 7:3, and the weight average molecular weight of PEG-DA is about 550. In addition, the content of the cross-linked polymer in the gel-type polymer electrolyte is 3 wt%, and the content of the liquid electrolyte is 97 wt%.

[0186] The above anode was manufactured according to the following method.

[0187] Li1 . 04 Ni0 . 88 Co0 . 1Al0 . 02 O2 powder and carbon conductive material (Super-P; Timcal Ltd.) were uniformly mixed at a weight ratio of 90:5, and then a PVDF (polyvinylidene fluoride) binder solution was added to prepare a positive electrode active material slurry with a weight ratio of active material:carbon conductive material:binder = 90:5:5.

[0188] The manufactured slurry was coated on a 15 ㎛ thick aluminum substrate using a doctor blade, dried under reduced pressure at 120°C, and rolled using a roll press to form a sheet to manufacture a positive electrode.

[0189] Example 2: TMPTA / PEG-DA (9:1), 3 wt% crosslinked polymer

[0190] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of TMPTA and PEG-DA was changed to 9:1.

[0191] Example 3: TMPTA / PEG-DA (7:3), 3 wt% crosslinked polymer

[0192] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of TMPTA and PEG-DA was changed to 7:3.

[0193] Example 4: TMPTA / PEG-DA (3:1), 3 wt% cross-linked polymer

[0194] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of TMPTA and PEG-DA was changed to 3:1.

[0195] Example 5: TMPTA / PEG-MA (8:2), 3 wt% cross-linked polymer

[0196] A lithium metal battery was manufactured in the same manner as in Example 1, except that polyethylene glycol monoacrylate (PEG-MA) was used instead of polyethylene glycol diacrylate when manufacturing a composition for forming a gel-type polymer electrolyte.

[0197] Example 6: TMPTA / PEG-MA (9:1), 3 wt% cross-linked polymer

[0198] A lithium metal battery was manufactured in the same manner as in Example 2, except that polyethylene glycol monoacrylate (PEG-MA) was used instead of polyethylene glycol diacrylate when manufacturing a composition for forming a gel-type polymer electrolyte.

[0199] Example 7: TMPTA / PEG-MA (7:3), 3 wt% cross-linked polymer

[0200] A lithium metal battery was manufactured in the same manner as in Example 3, except that polyethylene glycol monoacrylate (PEG-MA) was used instead of polyethylene glycol diacrylate when manufacturing a composition for forming a gel-type polymer electrolyte.

[0201] Example 8: TMPTA / PEG-MA (3:1), 3 wt% cross-linked polymer

[0202] A lithium metal battery was manufactured in the same manner as in Example 4, except that polyethylene glycol monoacrylate (PEG-MA) was used instead of polyethylene glycol diacrylate when manufacturing a composition for forming a gel-type polymer electrolyte.

[0203] Example 9: PETTA / PEG-MA (8:2), 3 wt% cross-linked polymer

[0204] A lithium metal battery was manufactured in the same manner as in Example 1, except that pentaerythritol tetramethacrylate (PETTA) was used instead of TMPTA when manufacturing a composition for forming a gel-type polymer electrolyte.

[0205] Comparative Example 1: TMPTA, 3 wt% cross-linked polymer

[0206] A gel-type polymer electrolyte and a lithium metal battery were manufactured in the same manner as in Example 1, except that the composition for forming a gel-type polymer electrolyte was prepared by mixing trimethylolpropane triacrylate (TMPTA), a mixed solvent (weight ratio 1:1:0.5) of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in which 1.3 M LiPF6 was dissolved as an electrolyte, and benzoin ethyl ether (Sigma-Aldrich, 240.30 g / mol) as an initiator.

[0207] Comparative Example 2: Liquid electrolyte (LE)

[0208] A lithium metal battery was prepared in the same manner as Example 1, except that a liquid electrolyte was injected instead of the composition for forming a positive electrode prepared in Manufacturing Example 1 and the thermal cross-linking process was omitted.

[0209] As a liquid electrolyte, a 2:1 volume ratio mixed solvent of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC) was used, in which 0.6 M LiBF4 and 0.6 M LiDFOB (lithium difluoro(oxalate)borate) were added.

[0210] Evaluation Example 1: Lifespan at room temperature (25℃)

[0211] The charge / discharge characteristics of the lithium metal batteries of Example 1 and Comparative Example 1-2 were evaluated under the following conditions.

[0212] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).

[0213] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 300 th The cycle was repeated under the same conditions.

[0214] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 1 below, and the capacity retention rate is defined by Equation 1 below.

[0215] <Formula 1>

[0216] Capacity retention rate [%] = [300 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100

[0217] Electrolyte capacity retention rate (%) @ cycle 0.2C discharge 100 cycles 200 cycles 300 cycles Example 1 TMPTA / PEG-DA (8:2) 7 1.47 8.96 6.2 Comparative example 1 TMPTA 3% (GPE) 9 1.17 8.16 4.7 Comparative example 2 LE 8 6.47 2.25 4.6

[0218] As shown in Table 1, the lithium metal battery of Comparative Example 2 had a reduced capacity retention rate due to lithium and electrolyte side reactions caused by dendrite growth, while the lithium metal battery of Comparative Example 1 had a gel-type polymer electrolyte containing a cross-linked polymer of TMPTA, which reduced the phenomenon of deterioration in capacity retention rate due to positive electrode interfacial side reactions and negative electrode dendrite formation compared to Comparative Example 1. In contrast, the lithium metal battery of Example 1 had an improved capacity retention rate, unlike the lithium metal batteries of Comparative Examples 1 and 2. This improved capacity retention rate is because the gel-type polymer electrolyte containing a cross-linked polymer of TPMPTA and PEG-DA physically suppressed dendrite growth, thereby improving long-term life characteristics.

[0219] Evaluation Example 2: Lifespan at room temperature (25℃)

[0220] The charge / discharge characteristics of the lithium metal batteries of Examples 4, 8 and Comparative Example 2 were evaluated under the following conditions.

[0221] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).

[0222] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 100 th The cycle was repeated under the same conditions.

[0223] In all charge / discharge cycles, a 10-minute pause was observed after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 2 below.

[0224] Electrolyte capacity retention rate (%)%@100cy (0.2C)Example 4TMPTA / PEG-DA(3:1)98.7Example 8TMPTA / PEG-MA(3:1)97.5Comparative example 2LE95.4

[0225] As shown in Fig. 3, the lithium metal battery of Comparative Example 2 had a reduced capacity retention rate due to lithium and electrolyte side reactions resulting from dendrite growth. In contrast, the lithium metal batteries of Examples 4 and 8 had improved capacity retention rates, unlike the lithium metal battery of Comparative Example 2. In particular, the lithium metal battery of Example 4 had better capacity retention rate and capacity characteristics than the lithium metal battery of Example 8. This is because the crosslinking degree increased due to the increase in the crosslinking agent having a trifunctional group and the crosslinked functional groups, thereby further increasing stability and improving long-term life characteristics by physically suppressing dendrite growth with the gel-type polymer electrolyte.

[0226] Evaluation Example 3: High-rate characteristics

[0227] The lithium metal batteries manufactured in Examples 3, 6 and Comparative Example 1 were charged at a constant current of 0.1 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut-off was achieved at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C until the voltage reached 2.8 V (vs. Li) (1 st cycle, Mars (formation) cycle).

[0228] 1 stThe cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C until the voltage reached 2.8 V (vs. Li) (2 nd cycle).

[0229] 2 nd Cycle 7 th The cycle was repeated under the same conditions.

[0230] 7 th The cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C until the voltage reached 2.8 V (vs. Li) (8 rd cycle).

[0231] 8th cycle 17 th The cycle was repeated under the same conditions.

[0232] 17 th The cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 1 C until the voltage reached 2.8 V (vs. Li) (18 th cycle).

[0233] 18 th Cycle 25 th The cycle was repeated under the same conditions.

[0234] 25 stThe cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 2 C until the voltage reached 2.8 V (vs. Li) (26 th cycle).

[0235] In all the above charge / discharge cycles, a pause of 10 minutes was allowed after each charge / discharge cycle.

[0236] Some of the results of the above charge-discharge experiment are shown in Table 3 below. The high-rate characteristics are defined by Equation 2 below.

[0237] <Formula 2>

[0238] High rate characteristic [%] = [26 st Discharge capacity in cycle (1C rate) /

[0239] 1 st Discharge capacity in cycle (0.1C rate)] × 100

[0240] Electrolyte separation rate characteristics (%) Example 3 TMPTA / PEG-DA (7:3) 40.2 Example 6 TMPTA / PEG-MA (9:1) 35.1 Comparative example 1 TMPTA 3% 31.7

[0241] Referring to Table 3, it was found that the donor characteristics of the bifunctional PEG-DA were superior to those of the monofunctional PEG-MA. In addition, it was found that the lithium metal batteries of Examples 3 and 6 were improved compared to that of Comparative Example 1, and the lithium metal battery of Example 3 having a gel-type polymer electrolyte containing a cross-linked polymer obtained by the reaction of TMPTMA and PEG-DA had a higher rate characteristic than the lithium metal battery of Example 6 having a gel-type polymer electrolyte containing a cross-linked polymer obtained by the reaction of TMPTMA and PEG-MA. This result is because PEG-DA increased the oxidation stability and physical strength due to the increased cross-linking degree of TMPTMA, thereby further increasing stability, and the gel-type polymer electrolyte improved the long-term life characteristic by physically suppressing dendrite growth.

[0242] Evaluation Example 4: Ionic Conductivity

[0243] The ionic conductivity of the gel polymer electrolyte in the lithium metal batteries manufactured according to Examples 1-3 and Comparative Example 1 was measured by the AC impedance method. The interfacial resistance and bulk resistance of the cell were measured as impedance changes over time. The ionic conductivity of each gel polymer electrolyte was calculated using Equation 3 below, and the results are shown in Table 4 below.

[0244] <Formula 3>

[0245] σ= 1 / Rb x t / A Equation (1)

[0246] In Equation 3, Rb is the resistance of the electrolyte, t is the thickness of the electrolyte film, and A is the area of ​​the electrolyte film.

[0247] Electrolyte ionic conductivity (S / cm) Example 1 TMPTA / PE-DA (8:2) 0.32 Example 2 TMPTA / PE-DA (9:1) 0.39 Example 3 TMPTA / PE-DA (7:3) 0.36 Comparative Example 1 TMPTA 3% 0.18

[0248] Referring to Table 4, it was found that the gel-type polymer electrolytes of Examples 1 to 3 had superior ionic conductivity compared to the gel-type polymer electrolyte of Comparative Example 1.

[0249] However, a linear increase in the ionic conductivity of the gel polymer electrolyte with increasing PEG-DA content was not observed, and the case where the mixing weight ratio of TMPTMA and PED-DA was 9:1 showed the best ionic conductivity characteristics.

[0250] Evaluation Example 5: Charge / Discharge Characteristics

[0251] In the lithium metal batteries of Examples 1-3 and Comparative Example 1, charge and discharge characteristics were evaluated under the following conditions.

[0252] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).

[0253] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 100 th The cycle was repeated under the same conditions.

[0254] In all charge / discharge cycles, a 10-minute pause was observed after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 5.

[0255] Mixed weight ratio of TMPTA and PEG-DA Capacity retention rate (%) @100cy Example 18: 291.1 Example 29: 190.7 Example 37: 390.2 Comparative example 110: 088.8

[0256] As shown in Table 5, the lithium metal batteries of Examples 1 to 3 showed improved capacity retention rates, unlike the lithium metal battery of Comparative Example 1. Among them, the lithium metal battery of Example 1 with a PEG-DA content of 20% showed the best capacity retention rate. This improved capacity retention rate is because the gel polymer electrolyte containing the cross-linked polymer of TPMPTA and PEG-DA physically inhibited dendrite growth, thereby improving long-term life characteristics.

[0257] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.

Claims

1. A positive electrode; a negative electrode current collector; and an electrolyte layer disposed between the positive electrode and the negative electrode current collector, The above electrolyte layer includes a gel-type polymer electrolyte, The above gel-type polymer electrolyte includes a liquid electrolyte containing an organic solvent and a lithium salt and a cross-linked polymer, A lithium metal battery, wherein the crosslinked polymer comprises a reaction product of a (meth)acrylic compound having a polyfunctional crosslinking agent having three or more functional groups and a polyethylene glycol moiety.

2. In the first paragraph, the polyfunctional crosslinking agent having three or more functional groups is trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, trimethylolpropane ethoxylate triacrylate, trimethylolpropane propoxylate triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylate tetraacrylate, dipentaerythritol pentaacrylate. (dipentaerythritol pentaacrylate), dipentaerythritol hexaacrylate (DPHA), tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), propoxylated glyceryl triacrylate, or a combination thereof, a lithium metal battery.

3. A lithium metal battery according to claim 1, wherein the (meth)acrylic compound having a polyethylene glycol moiety is polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), or a combination thereof.

4. A lithium metal battery in the first paragraph, wherein the mixing weight ratio of the polyfunctional crosslinking agent having three or more functional groups and the (meth)acrylic compound having a polyethylene glycol moiety is 9:1 to 2:

1.

5. A lithium metal battery comprising a negative electrode active material layer, a protective layer, or a combination thereof between the electrolyte layer and the negative electrode current collector in the first paragraph.

6. In the first paragraph, the electrolyte layer further includes a separator, A lithium metal battery, wherein the separator comprises a porous substrate.

7. In the first paragraph, the lithium salt includes a first lithium salt and a second lithium salt, The first lithium salt and the second lithium salt independently contain a fluorine-containing borate lithium salt, The above fluorine-containing borate lithium salt includes LiBF4, LiBF3(C2F5), compounds represented by the following chemical formulas 1 to 12, or a combination thereof, and the contents of the first lithium salt and the second lithium salt are each more than 0 and less than or equal to 1.2 M. A lithium metal battery, wherein the content ratio of the first lithium salt and the second lithium salt is 1:9 to 9:

1. <Chemical Formula 1> <Chemical Formula 2> <Chemical Formula 3> <Chemical Formula 4> <Chemical Formula 5> <Chemical Formula 6> <Chemical Formula 7> <Chemical Formula 8> <Chemical Formula 9> <Chemical Formula 10> <Chemical Formula 11> <Chemical Formula 12> 8. In the first paragraph, the organic solvent includes a first organic solvent and a second organic solvent, wherein the first organic solvent comprises a linear carbonate compound, The second organic solvent comprises a cyclic carbonate compound substituted with a substituent, A lithium metal battery wherein the substituent comprises a halogen, a cyano group (CN), a nitro group (NO2), or a combination thereof.

9. In the 8th paragraph, the first organic solvent includes diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, ethyl propyl carbonate, dipropyl carbonate or a combination thereof, A lithium metal battery, wherein the second organic solvent comprises vinylene carbonate substituted with one or more substituents selected from a halogen, a cyano group (CN), and a nitro group (NO2); vinylethylene carbonate substituted with one or more substituents selected from a halogen, a cyano group (CN), and a nitro group (NO2); fluoroethylene carbonate (FEC); fluoroethylene carbonate substituted with one or more substituents selected from a halogen, a cyano group (CN), and a nitro group (NO2); or a combination thereof.

10. In the first paragraph, the electrolyte layer further includes a separator, A lithium metal battery comprising: a negative electrode current collector; a separator disposed on the negative electrode current collector; a gel-type polymer electrolyte disposed on the separator; and a positive electrode disposed on the gel-type polymer electrolyte.

11. In the first paragraph, a lithium metal layer is further included between the negative electrode current collector and the electrolyte layer, A lithium metal battery in which the intensity of the fluorine peak is greater than the intensity of the oxygen peak in the XPS analysis of the surface of the lithium metal layer.

12. A lithium metal battery in the first paragraph, wherein the negative electrode collector comprises copper (Cu), nickel (Ni), nickel-coated copper, stainless steel (SUS), iron (Fe), cobalt (Co), or an alloy thereof.

13. In the first paragraph, the positive electrode includes a positive electrode current collector and a positive electrode active material layer, At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium metal battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

14. A lithium metal battery according to claim 1, wherein the ionic conductivity of the gel-type polymer electrolyte is 0.19 to 0.5 S / cm.

15. A lithium metal battery in which a gel-type polymer electrolyte exists in the pores of the separator in the first paragraph.

16. In the first paragraph, the lithium metal battery further includes an electrolyte, A lithium metal battery, wherein the electrolyte comprises a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof.

17. In the 16th paragraph, the solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof, A lithium metal battery, wherein the polymer solid electrolyte comprises a polymer gel electrolyte.

18. Step of preparing the negative electrode collector; Step of preparing an electrolyte layer; Steps to prepare the anode; A step of preparing an assembly by laminating a negative electrode collector, an electrolyte layer, and a positive electrode; A step of injecting a composition for forming a gel-type polymer electrolyte, which comprises a multifunctional crosslinking agent having three or more functional groups, a (meth)acrylic compound having a polyethylene glycol moiety, an organic solvent, and a liquid electrolyte containing a lithium salt into the above assembly; and A method for manufacturing a lithium metal battery, comprising the step of preparing a lithium metal battery including a gel-type polymer electrolyte by crosslinking the composition for forming the injected gel-type polymer electrolyte; 19. In paragraph 18, A method for manufacturing a lithium metal battery, wherein the electrolyte layer includes a separator.

20. In paragraph 18, A method for manufacturing a lithium metal battery, wherein the above cross-linking is performed by heat treatment at 40°C to 120°C.

Citation Information

Patent Citations

  • Warp Knitting Fabric of Silk Complex with Slip Preventing Property and Low Density

    KR1020200100977A

  • Modifying method for metallic compound and polymer comprising modified metallic compound for neutron shielding material in spent nuclear fuel cask

    KR102392506B1

  • Composition for preparing a gel polymer electrolyte, gel polymer electrolyte, and lithium-metal secondary battery comprising it

    WO2023002015A1

Cited By

  • Lithium metal battery and manufacturing method thereof, battery device, energy storage device and power utilization device

    CN120999143A

  • High-energy-density semi-solid lithium battery and preparation method thereof

    CN121964785A

  • High energy density semi-solid lithium battery and method of making same

    CN121964785B

  • Lithium battery

    EP4576300A1

  • Battery cell, electrode sheet and preparation method therefor, and battery device and electric device

    WO2026149495A1