A method for repairing the circular seam of the ladle slag line
A ladle slag line and ring seam technology, which is applied in the field of iron and steel metallurgical ladle lining repair, can solve the problems of slag line brick waste, heavy workload, and troublesome operation, so as to reduce the consumption of refractory materials per ton of steel and increase the continuous service life Effect
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2018-08-21
Smart Images

Figure 1 
Figure 2
Abstract
Description
technical field
[0001] The invention relates to a technology for repairing the inner lining of a ladle in iron and steel metallurgy, in particular to a method for repairing the circular seam at the slag line of the ladle. Background technique
[0002] With the continuous improvement of people's lives, the quality of traditional steel can no longer meet certain performance. In order to obtain better varieties of steel, it is forced to change the ladle refining technology. Therefore, various out-of-furnace refining methods such as LF, RH, CAS, and VOD have emerged as the times require. pregnancy. At the present stage, the aim is to improve the refining efficiency, realize optimal combination and complementary functions, and superimpose multiple refining methods, so higher requirements are put forward for the service life of the ladle working lining. At present, the slag line of the ladle is mainly made of magnesia-carbon bricks, and the main wall of the ladle is made of alumi...
Examples
Embodiment 1
[0040] This embodiment is a 120t cord steel ladle, high-carbon magnesia-carbon bricks are used for the working lining of the ladle slag line, and low-carbon magnesia-carbon bricks are used for the working lining of the ladle wall. The length of the brick is 170, the thickness is 100, the size deviation of the ladle brick is ±1mm, the width of the brick joint is not more than 1mm, and the number of furnaces used in this overhaul package is about 35 furnaces, the refining method is mainly LF, and the ladle is offline for minor repairs. It is obvious that there is a deep groove at the slag liquid level, and other parts are in good condition; the minimum residual thickness h=100mm allowed for the circular joint, the specific repair steps are as follows:
[0041]1) The residual thickness of the slag line brick and sealing brick on the upper part of the ladle is ≥150mm, and the thickness of the thinnest part of the circular joint is h1≥100mm. The mud should be mixed with water accor...
Embodiment 2
[0049] This example is a 180t ordinary carbon steel ladle. High-carbon magnesia-carbon bricks are used for the working lining of the slag line of the ladle. The working lining of the ladle wall is aluminum-magnesia-carbon bricks. The length is 200, the thickness is 100, the size deviation of ladle bricks is ±1mm, the allowed brick joint width is not more than 1mm, and the number of furnaces used for this overhaul package is about 40 furnaces, the refining method is mainly LF, and minor repairs can be obvious when the ladle is offline It can be seen that there is a deep groove on the slag liquid surface, and other parts are in good condition; the minimum residual thickness allowed by the circular joint is h=120mm, and the specific repair steps are as follows:
[0050] 1) The residual thickness of the slag line brick and sealing brick on the upper part of the ladle is ≥150mm, and the thickness of the thinnest part of the circular joint is h1≥120mm. This repair is mainly carried o...