Flat panel detection substrate and preparation method thereof, flat detector

By using a semiconductor layer with a thickness greater than 100nm in the photodetector directly contacting the electrode, and combining an inorganic insulating unit or a metal oxide dielectric layer, the problems of metal electrode oxidation and insulating layer uniformity are solved, and the uniformity of dark current is achieved and performance improvement.

CN109713076BActive Publication Date: 2024-11-19BOE TECHNOLOGY GROUP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN201910129999.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-02-21
Publication Date
2024-11-19
Estimated Expiration
2039-02-21

AI Technical Summary

Technical Problem

During the preparation process, existing photodetectors with metal-semiconductor-metal interdigital electrode structures are prone to problems such as metal electrode oxidation, signal transmission interruption and insulating layer film thickness uniformity, resulting in uneven dark current and degradation of performance.

Method used

The semiconductor layer with a thickness greater than 100nm is used to directly contact the bias electrode and the induction electrode, and the PI insulation layer is eliminated, and the thickness of the semiconductor layer is used as the dielectric layer to reduce dark current, and the inorganic insulating unit or metal oxide media is provided. The electrical layer further optimizes the structure.

Benefits of technology

The inhomogeneity of dark current and the dark current itself are significantly reduced, the performance and signal transmission stability of the detector are improved, the preparation process is simplified and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109713076B_ABST
    Figure CN109713076B_ABST
Patent Text Reader

Abstract

The present invention provides a flat-panel detection substrate and a method for preparing the same, and a flat detector, and belongs to the technical field of detectors. The flat-panel detection substrate of the present invention comprises: a substrate, and a plurality of detection units located on the substrate; each of the detection units comprises: a bias electrode and a sensing electrode; the flat-panel detection substrate further comprises: a semiconductor layer covering the bias electrode and the sensing electrode; and the thickness of the semiconductor layer is greater than 100 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of detectors, and in particular relates to a flat-panel detection substrate and a preparation method thereof, and a flat-panel detector. Background Art

[0002] Different from traditional PIN photodiode detectors, metal-semiconductor-metal interdigital electrode structure photodetectors do not require P-type doping, have a simple preparation process, are low-cost, compatible with thin-film transistor and field-effect transistor manufacturing processes, easy to integrate, have fast response speed, low dark current, high fill rate and many other advantages, and occupy an important position in the fields of medical imaging and industrial detection. Summary of the invention

[0003] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides a flat detection substrate and a preparation method thereof, and a flat panel detector.

[0004] The technical solution adopted to solve the technical problem of the present invention is a flat-panel detection substrate, comprising: a substrate, and a plurality of detection units located on the substrate; each of the detection units comprises: a bias electrode and a sensing electrode; the flat-panel detection substrate also comprises: a semiconductor layer covering the bias electrode and the sensing electrode; and the thickness of the semiconductor layer is greater than 100 nm.

[0005] Preferably, the semiconductor layer is in direct contact with the bias electrode and the sensing electrode.

[0006] Preferably, the material of the semiconductor layer includes a-Si.

[0007] Preferably, the semiconductor layer includes a first semiconductor layer and a second semiconductor layer sequentially arranged on the substrate; wherein the mobility of the second semiconductor layer is higher than the mobility of the first semiconductor layer.

[0008] Preferably, an insulating unit is provided between the bias electrode and the sensing electrode, and the semiconductor layer covers the bias electrode, the sensing electrode, and the insulating unit; wherein the material of the insulating unit includes: an inorganic insulating material.

[0009] Preferably, the thickness of the insulating unit is between 100 nm and 300 nm.

[0010] Preferably, a dielectric layer is further provided between the layer where the bias electrode and the sensing electrode are located and the semiconductor layer, and the material of the dielectric layer includes metal oxide.

[0011] Preferably, the material of the bias electrode and the sensing electrode comprises metal;

[0012] The material of the dielectric layer is obtained by oxidation of the metal.

[0013] Preferably, the bias electrode and the sensing electrode in each detection unit are in a cross-comb structure.

[0014] Preferably, each of the detection units further comprises: a thin film transistor; wherein a drain of the thin film transistor is electrically connected to the sensing electrode.

[0015] The technical solution adopted to solve the technical problem of the present invention is a method for preparing a flat-panel detection substrate, comprising: forming a plurality of detection units on a substrate; forming the detection units comprises: forming a bias electrode and a sensing electrode, and a semiconductor layer covering the bias electrode and the sensing electrode; wherein the thickness of the semiconductor layer is greater than 100 nm.

[0016] Preferably, the semiconductor layer is in direct contact with the bias electrode and the sensing electrode.

[0017] Preferably, the semiconductor layer comprises a first semiconductor layer and a second semiconductor layer sequentially arranged on the substrate; wherein the mobility of the second semiconductor layer is higher than the mobility of the first semiconductor layer; and the steps of forming the semiconductor layer comprise:

[0018] Depositing a first semiconductor layer using a first deposition rate;

[0019] A second semiconductor layer is formed by deposition using a second deposition rate; wherein the first deposition rate is greater than the second deposition rate.

[0020] Preferably, before forming the semiconductor layer, the method further comprises:

[0021] A step of forming an insulating unit between the bias electrode and the sensing electrode; wherein the material of the insulating unit comprises: an inorganic insulating material.

[0022] Preferably, the material of the bias electrode and the sensing electrode comprises metal; a dielectric layer is provided between the layer where the bias electrode and the sensing electrode are located and the semiconductor layer; the material of the dielectric layer comprises metal oxide; forming the bias electrode, the sensing electrode and the dielectric layer comprises:

[0023] forming a metal material layer;

[0024] The surface of the metal material layer is oxidized, and a pattern including the bias electrode, the sensing electrode and the dielectric layer is formed through a patterning process.

[0025] The technical solution adopted to solve the technical problem of the present invention is a flat panel detector, including the above-mentioned flat panel detection substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic structural diagram of a flat-panel detection substrate according to Embodiment 1 of the present invention;

[0027] Figure 2 It is a structural schematic diagram of another flat-panel detection substrate according to Embodiment 1 of the present invention;

[0028] Figure 3 is a schematic diagram of dark current generated by a flat panel detector of a flat panel detection substrate according to Embodiment 1 of the present invention;

[0029] Figure 4 A schematic diagram of dark current generated by an existing flat panel detector;

[0030] Figure 5 is a flow chart of a method for preparing a flat-panel detection substrate according to Example 1 of the present invention;

[0031] Figure 6 It is a structural schematic diagram of a flat-panel detection substrate according to Embodiment 2 of the present invention;

[0032] Figure 7 Schematic diagram of the structure of a flat-panel detection substrate according to Embodiment 3 of the present invention.

[0033] The figures are marked as follows: 10, substrate; 11, bias electrode; 12, sensing electrode; 13, semiconductor layer; 14, thin film transistor; 15, shading pattern; 16, interlayer insulating layer; 161, first interlayer insulating layer; 162, second interlayer insulating layer; 17, connecting electrode; 171, first connecting electrode; 172, second connecting electrode; 18, insulating unit; 19, dielectric layer. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0035] Compared with the structure of direct metal-semiconductor contact, KAI has designed a conventional metal-semiconductor-metal interdigital electrode structure, that is, a detector with a new structure that fills a polyimide (PI) insulating layer between the interdigital electrode and the semiconductor layer, which can significantly reduce dark current and improve detection efficiency. Under illumination conditions, the semiconductor layer of the detector receives light, generates charges inside, and the resistance drops significantly, thereby converting the light signal into an electrical signal through the photovoltaic effect. At this time, most of the external bias is applied to the PI insulating layer with high resistance. When the voltage is high enough, the PI insulating layer can be turned on through the FN tunneling effect of electrons, and the electrical signal generated in the semiconductor material can be read and stored through the conduction and shutdown of the thin film transistor, thereby achieving the purpose of detection.

[0036] However, this type of photodetector generally deposits metal (such as Mo / Al) as interdigital electrodes. Due to the thickness limit of the PI insulating layer (200nm-300nm) and the need to completely cover the metal, the metal is generally required to be very thin (50nm), which makes the metal electrode prone to oxidation during the preparation process. The oxide layer on the metal electrode increases the difficulty of carrier tunneling in the PI insulating layer, increases resistance, and affects the yield rate; and by depositing metal into the hole groove to achieve signal transmission by overlapping the sensing electrode and the thin film transistor drain electrode, the metal has poor climbing performance and poor deposition coverage, and is prone to fracture, causing signal transmission interruption. Generally, the metal has a columnar structure, and the corners are very steep after etching, with a large slope angle. After being thinned, it will also affect the deposition coverage of the subsequent film layer, and poor contact is prone to occur at the corners. It is difficult to achieve uniform film thickness in the manufacturing process of the PI insulating layer itself, and the Max-Min film thickness difference reaches 70nm-80nm, especially near the metal. As a dielectric layer, the PI insulating layer is required to have a uniform thickness of 20 nm, otherwise a large piece of Mura will appear in the detector product. To solve the above technical problems, the present invention provides the following embodiments.

[0037] Embodiment 1:

[0038] like Figure 1 As shown, this embodiment provides a flat-panel detection substrate, which includes: a substrate 10, a plurality of detection units located on the substrate 10, and a semiconductor layer 13 arranged on the plurality of detection units; wherein each detection unit includes: a bias electrode 11 and a sensing electrode 12, and the semiconductor layer 13 covers the bias electrode 11 and the sensing electrode 12; and the thickness of the semiconductor layer 13 is greater than 100nm.

[0039] Due to the material of the semiconductor layer 13, its effective thickness to light is less than 100nm, that is, under the condition of light, the photocarriers of the semiconductor layer 13 are effectively used to a thickness of less than 100nm. If the thickness of the semiconductor layer 13 is greater than 100nm, then with the light incident surface of the semiconductor layer 13 as the reference, the portion exceeding the thickness of 100nm acts as a dielectric layer, which is insulating in the dark state and low voltage, and the thicker the semiconductor layer 13, the greater the resistance. In this embodiment, the semiconductor layer 13 with a thickness greater than 100nm is arranged on the bias electrode 11 and the sensing electrode 12 of the detection unit. At this time, the portion of the semiconductor layer 13 less than 100nm with its light incident surface as the reference is used to generate a corresponding electrical signal according to the light signal it receives, and the remaining portion is used as a dielectric layer, which plays the role of insulation and reducing leakage current.

[0040] Among them, in this embodiment, the semiconductor layer 13 is preferably designed to be in direct contact with the bias electrode 11 and the sensing electrode 12. At this time, the semiconductor layer 13 has a double-layer function, that is, the function of the photoelectric conversion layer and the dielectric layer. In this way, the setting of the polyimide (PI) insulating layer between the detection unit and the semiconductor layer 13 can be omitted, thereby avoiding the interface problem between the PI insulating layer and the semiconductor layer 13, and saving a process step. Further, in order to make the semiconductor layer 13 better play the role of a dielectric layer and reduce dark current, it is preferred that the thickness of the semiconductor layer 13 is not less than 450nm.

[0041] In the flat-panel detection substrate of the present embodiment, the bias electrode 11 and the sensing electrode 12 can both be made of metal materials, and the structures of the two are cross-comb structures.

[0042] In the flat-panel detection substrate of this embodiment, the material of the semiconductor layer 13 includes a-Si. Of course, the material of the semiconductor layer 13 is not limited to this material, and can also be a semiconductor material with the same or similar properties as a-Si. The thickness of the semiconductor layer 13 is about 100nm-600nm, and the thickness of the semiconductor layer 13 can be adjusted according to the specific application substrate. Figure 2 As shown, in the flat-panel detection substrate of the present embodiment, the semiconductor layer 13 includes a first semiconductor layer 131 and a second semiconductor layer 132 which are sequentially arranged above the substrate 10; the mobility of the second semiconductor layer 132 is higher than the mobility of the first semiconductor layer 131, that is, the mobility of the first semiconductor layer 131 is low mobility compared with the mobility of the second semiconductor layer 132, and the mobility of the second semiconductor layer 132 is high mobility compared with the mobility of the first semiconductor layer 131, so that the second semiconductor layer 132 with high mobility is used as a photoelectric conversion layer, and the first semiconductor layer 131 with low mobility is used as a dielectric layer.

[0043] Among them, in the flat-panel detection substrate of the present embodiment, each detection unit also includes a thin film transistor 14; specifically, the gate of the thin film transistor 14 is connected to the detection control line, the source is connected to the reading line, and the drain is connected to the sensing electrode 12; under light conditions, the semiconductor layer 13 receives light, generates charges inside, and the resistance drops significantly, thereby converting the light signal into an electrical signal through the photovoltaic effect. At this time, most of the external bias voltage is applied to the dielectric layer part of the semiconductor layer 13 with a very high resistance. When the voltage is high enough, the dielectric layer part of the semiconductor layer 13 can be turned on through the FN tunneling effect of electrons, and the electrical signal generated in the semiconductor material can be read and stored by controlling the conduction and closing of the thin film transistor 14 through the signal written on the detection control line, thereby achieving the purpose of detection.

[0044] In order to more clearly illustrate that a flat-panel detection substrate using only a semiconductor layer with a thickness greater than 100 nm has better performance than a flat detection substrate using a PI insulating layer and a semiconductor layer in the prior art, flat-panel detectors using the flat-panel detection substrates in this embodiment and in the prior art are tested below, wherein the semiconductor material in the flat-panel detection substrate is a-Si.

[0045] Specifically, Figure 3 and 4 As shown, the horizontal axis and the vertical axis in the figure respectively represent the column position and the row position of the detection unit on the flat panel detector substrate.

[0046] for Figure 3 It shows that the flat panel detector using the flat panel detection substrate of this embodiment, when a voltage of about 5-10V is applied to the bias electrode and the window time (illumination time, such as X-ray illumination time) is 0.4-4.4s, the dark current generated by each detection unit in the flat panel detection substrate is uniform, and the average dark current Avg Ioff is 45.603fA. Figure 4 It shows that, for a flat-panel detector using an existing flat-panel detection substrate, when a voltage of about 200V is applied to the bias electrode and the window time is 0.4-4.4s, the dark current generated by each detection unit in the flat-panel detection substrate is very uneven, and the average dark current Avg Ioff is 99.01fA.

[0047] In summary, compared with the prior art, the dark current of the flat panel detector using the flat panel detection substrate of this embodiment is obviously uniform and the dark current is small, so the performance of the flat panel detector using the flat panel detection substrate of this embodiment is better.

[0048] Moreover, according to the above test conditions, when the linearity of the dark current of the flat panel detector using the flat panel detection substrate of this embodiment is tested, it is found that compared with the prior art, the linearity of the dark current of this embodiment is 0.999796, while the linearity of the dark current of the prior art is 0.999659. It is obvious that the linearity of the dark current of this embodiment is better, so the image detection of the flat panel detector using the flat panel detection substrate of this embodiment is more accurate. Correspondingly, in this embodiment, a method for preparing the above flat panel detection substrate is also provided, such as Figure 5 As shown, the method may specifically include the following steps:

[0049] Step 1: On the substrate 10, various layers of the thin film transistor 14 in each detection unit are formed by a patterning process.

[0050] Step 2: forming an interlayer insulating layer 16 on the substrate 10 after completing step 1, etching a via hole at a position of the interlayer insulating layer 16 corresponding to the drain of the thin film transistor 14, and then forming a connecting electrode 17 covering the via hole through a patterning process.

[0051] Among them, the thin film transistor 14 formed in step one can be a top-gate thin film transistor 14 or a bottom-gate thin film transistor 14. When the thin film transistor 14 is a bottom-gate thin film transistor 14, in order to prevent light from irradiating the active layer of the thin film transistor 14 and destroying the switching characteristics of the thin film transistor 14, a light shielding pattern 15 corresponding to the active layer of the thin film transistor 14 is also formed on the layer where the thin film transistor 14 is located. When the light shielding pattern 15 is made of metal material, it is necessary to first form a first interlayer insulating layer 161 and a first buffer layer in sequence on the layer where the thin film transistor 14 is located, and then form the light shielding pattern 15 through a composition process; after forming the light shielding pattern 15, a second interlayer insulating layer 162 is formed. That is to say, the interlayer insulating layer 16 formed in step two includes the aforementioned first interlayer insulating layer 161 and the second interlayer insulating layer 162. In order to ensure that the light shielding pattern 15 of the metal material generates leakage current, the thickness of the first interlayer insulating layer 161 and the second interlayer insulating layer 162 is relatively thick. Therefore, when the second interlayer insulating layer 162 is formed, a via hole is etched through the first interlayer insulating layer 161 and the second interlayer insulating layer 162, and then the connection electrode 17 covering the via hole is formed, it is very likely to cause the connection electrode 17 to break. Therefore, the first via hole can be etched after the first interlayer insulating layer 161 is formed, and the first connection electrode 171 connected to the drain of the thin film transistor 14 is formed after the first connection electrode 171 is formed; after the first connection electrode 171 is formed, the second interlayer insulating layer 162 is formed, and the second via hole is etched in the second interlayer insulating layer 162, and the first connection electrode 171 is exposed at the position of the second via hole, and then the second connection electrode 172 covering the second via hole is formed, and the second connection electrode 172 is electrically connected to the first connection electrode 171. That is, the first via hole and the second via hole constitute the via hole formed in step 2; the first connection electrode 171 and the second connection electrode 172 constitute the connection electrode 17 formed in step 2.

[0052] Step 3: On the substrate 10 after completing step 2, a pattern including the bias electrode 11 and the sensing electrode 12 in the detection unit is formed by a composition process; wherein the sensing electrode 12 in each detection unit is connected to the drain of the thin film transistor 14 through the connecting electrode 17 in the detection unit.

[0053] The bias electrode 11 and the sensing electrode 12 are usually made of metal materials. Therefore, before forming the patterns of the bias electrode 11 and the sensing electrode 12 , it is preferred to form a second buffer layer on the interlayer insulating layer 16 before forming the bias electrode 11 and the sensing electrode 12 .

[0054] Step 4: forming a semiconductor layer 13 on the substrate 10 after completing step 3; wherein the thickness of the semiconductor layer 13 is greater than 100 nm.

[0055] Specifically, the semiconductor layer 13 may include a first semiconductor layer 131 and a second semiconductor layer 132 sequentially disposed on the substrate 10; wherein the mobility of the second semiconductor layer 132 is higher than the mobility of the first semiconductor layer 131. That is, the mobility of the first semiconductor layer 131 is low mobility, and the mobility of the second semiconductor layer 132 is high mobility; wherein the high mobility is greater than 0.75 cm / vs, and the low mobility is less than 0.5 cm / vs.

[0056] For the convenience of preparation, a-Si can be used as the material of the first semiconductor layer 131 and the second semiconductor layer 132. The method of forming the second semiconductor layer 132 with high mobility and the first semiconductor layer 131 with low mobility is described below.

[0057] First, a low-mobility a-Si material layer is deposited at a first deposition rate to form a first semiconductor layer 131; then, a high-mobility a-Si material layer is deposited at a second deposition rate to form a second semiconductor layer 132; wherein the first deposition rate is greater than the second deposition rate. At this time, the high-mobility second semiconductor layer 131 is equivalent to the photoelectric conversion layer; the low-mobility first semiconductor layer 131 is equivalent to the dielectric layer, so the preparation of the PI insulating layer can be omitted in the preparation method of this embodiment, so the preparation process can be simplified.

[0058] Embodiment 2:

[0059] like Figure 6 As shown, this embodiment provides a flat panel detector substrate, the structure of which is substantially the same as that of the flat panel detector substrate in Embodiment 1, except that an insulating unit 18 is provided between the bias electrode 11 and the sensing electrode 12 (it should be noted that the insulating unit 18 usually covers the edge of the bias electrode 11 and the edge of the sensing electrode 12 adjacent thereto due to process reasons); the material of the insulating unit 18 includes an inorganic insulating material. The semiconductor layer 13 of the flat detector is above the bias electrode 11, the sensing electrode 12, and the insulating unit 18.

[0060] Since the flat-panel detection substrate of this embodiment includes an insulating unit 18 disposed between the bias electrode 11 and the sensing electrode 12, and the material of the insulating unit 18 includes an inorganic material, the insulating unit 18 of the inorganic material is easier to level at the edge of the bias electrode 11 and the sensing electrode 12 than the PI insulating layer, thereby avoiding the uniformity problem of the PI insulating layer. Moreover, in this embodiment, it is not necessary to set a PI insulating layer, which can greatly reduce the difficulty of preparing the flat-panel detection substrate and improve the production capacity. In particular, in the prior art, a voltage of more than 200V is required to drive the flat-panel detector to work. By omitting the PI insulating layer, only a working voltage of 10-20V is required, thereby greatly reducing power consumption.

[0061] In this embodiment, the insulating unit 18 can be a silicon oxide film, a silicon nitride film, or a silicon oxide and silicon nitride composite film. The thickness of the insulating unit 18 is about 100nm-300nm. Of course, the specific thickness value can be set according to the specific substrate structure.

[0062] The remaining structures of the flat-panel detection substrate in this embodiment may be the same as those in Embodiment 1, and thus will not be described one by one here.

[0063] Correspondingly, a method for preparing the above-mentioned flat-panel detection substrate is also provided in this embodiment. The preparation method is substantially the same as the preparation method in Example 1, except that a step of forming an insulating unit 18 through a composition process is added between step three and step four; wherein the material of the insulating unit 18 includes an inorganic insulating material.

[0064] The preparation process of the remaining structures of the flat-panel detection substrate is the same as that in Example 1, and thus will not be described one by one here.

[0065] Embodiment 3:

[0066] like Figure 7 As shown, this embodiment provides a flat panel detector substrate, the structure of which is substantially the same as that of the flat panel detector substrate in Embodiment 1, except that a dielectric layer 19 is provided between the layer where the bias electrode 11 and the sensing electrode 12 are located and the semiconductor layer 13, and the material of the dielectric layer 19 is a metal oxide. Since the dielectric layer 19 of the metal oxide is provided between the layer where the bias electrode 11 and the sensing electrode 12 are located and the semiconductor layer 13, the dark current generated by the semiconductor layer 13 of the flat panel detector substrate can be reduced, and during operation, the metal oxide will be broken down, thereby realizing current transmission.

[0067] Specifically, when the bias electrode 11 and the sensing electrode 12 are made of metal materials in this embodiment, the metal oxide material of the dielectric layer 19 can be obtained by oxidizing the metal materials used by the bias electrode 11 and the sensing electrode 12. In this way, process steps can be saved and costs can be reduced.

[0068] The metal material may include any one of copper (Cu), molybdenum (Mo) and aluminum (Al). Of course, the metal material is not limited thereto, and a specific metal material may be selected according to process conditions.

[0069] The remaining structures of the flat-panel detection substrate in this embodiment may be the same as those in Embodiment 1, and thus will not be described one by one here.

[0070] Accordingly, a method for preparing the above-mentioned flat-panel detection substrate is also provided in this embodiment. The preparation method is substantially the same as the preparation method in Example 1, except that a step of forming a dielectric layer 19 is added between step three and step four; wherein the dielectric layer material is metal oxide.

[0071] When the bias electrode 11 and the sensing electrode 12 are made of metal materials in this embodiment, the metal oxide material of the dielectric layer can be obtained by oxidizing the metal materials used by the bias electrode 11 and the sensing electrode 12 .

[0072] The steps of forming the bias electrode 11, the sensing electrode 12 and the dielectric layer 19 specifically include:

[0073] A metal material layer is formed on the substrate 10 on which the interlayer insulating layer 16 is formed; a metal oxide layer is formed by thermal oxidation; it should be noted that only the portion of the metal material layer away from the substrate 10 is oxidized, and the remaining portion is not oxidized. Finally, a pattern including a bias electrode 11, a sensing electrode 12 and a dielectric layer 19 is formed by a patterning process; wherein the dielectric layer covers the bias electrode 11 and the sensing electrode 12. Moreover, the metal oxide layer formed by thermal oxidation has a high density, and has a better insulation effect than insulating layers such as silicon oxide and silicon nitride deposited on metals.

[0074] The metal material may include any one of copper (Cu), molybdenum (Mo) and aluminum (Al). Of course, the metal material is not limited thereto, and a specific metal material may be selected according to process conditions. The thickness of the metal material layer is about 3000, and the thickness of the formed dielectric layer is about 5nm-20nm.

[0075] The preparation process of the remaining structures of the flat-panel detection substrate is the same as that in Example 1, and thus will not be described one by one here.

[0076] Embodiment 4:

[0077] This embodiment provides a flat panel detector, which includes any one of the flat panel detection substrates in Embodiments 1-3. The flat panel detector may further include a planarization layer and other structures disposed on the semiconductor layer 13 .

[0078] In this embodiment, the flat panel detector may be an X-ray flat panel detector.

[0079] Since the flat-panel detector in this embodiment includes any one of the flat-panel detection substrates in Embodiments 1-3, wherein the semiconductor layer 13 having a thickness greater than 100 nm is disposed on the bias electrode 11 and the sensing electrode 12 of the detection unit, at this time, the portion of the semiconductor layer 13 less than 100 nm based on its light incident surface is used to generate a corresponding electrical signal according to the received light signal, and the remaining portion is used as a dielectric layer to perform insulation and reduce leakage current.

[0080] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A flat panel detection substrate, comprising: A substrate, and a plurality of detection units located on the substrate; Each of the detection units comprises: a bias electrode and a sensing electrode; characterized in that the flat detection substrate further comprises: a semiconductor layer covering the bias electrode and the sensing electrode; and the thickness of the semiconductor layer is greater than 100nm; The material of the semiconductor layer includes a-Si; based on the light incident surface of the semiconductor layer, the portion of the semiconductor layer with a thickness less than 100 nm is used for photoelectric conversion, and the remaining portion is used as a dielectric layer, and the dielectric layer is insulated in a dark state and at low voltage.

2. The flat panel detection substrate according to claim 1, characterized in that: The semiconductor layer is in direct contact with the bias electrode and the sensing electrode.

3. The flat panel detection substrate according to claim 1, characterized in that: The semiconductor layer includes a first semiconductor layer and a second semiconductor layer sequentially disposed on the substrate; wherein the mobility of the second semiconductor layer is higher than the mobility of the first semiconductor layer.

4. The flat panel detection substrate according to claim 3, characterized in that: The mobility of the first semiconductor layer is less than 0.5 cm / vs; the mobility of the second semiconductor layer is greater than 0.75 cm / vs.

5. The flat panel detection substrate according to claim 1, characterized in that: An insulating unit is provided between the bias electrode and the sensing electrode, and the semiconductor layer covers the bias electrode, the sensing electrode, and the insulating unit; wherein the material of the insulating unit includes: an inorganic insulating material.

6. The flat panel detection substrate according to claim 5, characterized in that: The thickness of the insulating unit is between 100nm and 300nm.

7. The flat panel detection substrate according to claim 1, characterized in that: A metal oxide is also arranged between the layer where the bias electrode and the sensing electrode are located and the semiconductor layer.

8. The flat panel detection substrate according to claim 7, characterized in that: The materials of the bias electrode and the sensing electrode include metal; The metal oxide is obtained by oxidizing the metal.

9. The flat panel detection substrate according to claim 1, characterized in that: The bias electrode and the sensing electrode in each detection unit are in a cross-comb structure.

10. The flat panel detection substrate according to claim 1, characterized in that: Each of the detection units further includes a thin film transistor; wherein a drain of the thin film transistor is electrically connected to the sensing electrode.

11. A method for preparing a flat panel detection substrate, comprising: A plurality of detection units are formed on a substrate; the formation of the detection units comprises: forming a bias electrode and a sensing electrode, and a semiconductor layer covering the bias electrode and the sensing electrode; wherein the thickness of the semiconductor layer is greater than 100 nm; wherein the material of the semiconductor layer comprises a-Si; based on the light incident surface of the semiconductor layer, a portion of the semiconductor layer with a thickness less than 100 nm is used for photoelectric conversion, and the remaining portion is used as a dielectric layer, and the dielectric layer is insulated in a dark state and at low voltage.

12. The method for preparing a flat panel detection substrate according to claim 11, characterized in that: The semiconductor layer is in direct contact with the bias electrode and the sensing electrode.

13. The method for preparing a flat panel detection substrate according to claim 11, characterized in that: The semiconductor layer comprises a first semiconductor layer and a second semiconductor layer sequentially arranged on the substrate; wherein the mobility of the second semiconductor layer is higher than the mobility of the first semiconductor layer; and the steps of forming the semiconductor layer comprise: Depositing a first semiconductor layer using a first deposition rate; A second semiconductor layer is formed by deposition using a second deposition rate; wherein the first deposition rate is greater than the second deposition rate.

14. The method for preparing a flat panel detection substrate according to claim 11, characterized in that: Before forming the semiconductor layer, the method further comprises: A step of forming an insulating unit between the bias electrode and the sensing electrode; wherein the material of the insulating unit comprises: an inorganic insulating material.

15. The method for preparing a flat panel detection substrate according to claim 11, characterized in that: The materials of the bias electrode and the sensing electrode include metal; a metal oxide is provided between the layer where the bias electrode and the sensing electrode are located and the semiconductor layer; Forming the bias electrode, the sensing electrode and the metal oxide comprises: forming a metal material layer; The surface of the metal material layer is oxidized, and a pattern including the bias electrode, the sensing electrode and the metal oxide pattern is formed through a patterning process.

16. A flat panel detector, characterized in that: The invention comprises the flat-panel detection substrate according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Detection substrate, fabrication method thereof and detector

    CN105097860A

  • Array substrate and preparation method therefor, sensor and detection equipment

    CN105720063A

  • Apparatus for radiation detection in a digital imaging system

    CN106535768A

  • Multi-sensor pixel architecture for use in digital imaging system

    CN107831523A

  • Flat panel detection substrate and flat panel detector

    CN209571423U