Positive electrode material for lithium ion secondary battery and method for producing the same, positive electrode for lithium ion secondary battery, and lithium ion secondary battery
By using pyrolytic carbon coating in the manufacturing of cathode materials for lithium-ion secondary batteries, the problems of cathode active material adhesion to the inner wall of the rotary kiln and primary particle sintering were solved, resulting in higher discharge capacity and lower charge-discharge resistance, thus improving the electrochemical performance of the battery.
Patent Information
- Application Number
- CN201910720853.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-23
- Filing Date
- 2019-08-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-11-03
AI Technical Summary
Existing lithium-ion secondary battery cathode materials suffer from problems such as the adhesion of positive electrode active material to the inner wall, sintering between primary particles, and the formation of micro powder during the calcination process in a rotary kiln, leading to a decrease in battery characteristics and operability.
The method for manufacturing lithium-ion secondary battery cathode materials using pyrolytic carbon coating involves pyrolyzing carbon source organic compounds in a rotary kiln to form a pyrolytic carbon coating, preventing the adhesion of cathode active materials and sintering between primary particles. A mixture of dispersion medium and organic compounds is used for drying and granulation to ensure the sphericity and uniformity of the granules.
Uniform coating of the cathode material was achieved, preventing the positive electrode active material from adhering to the inner wall of the rotary kiln and sintering between primary particles, thus improving the discharge capacity and reducing the DC resistance during charging and discharging, and ensuring the electrochemical performance of the battery.
Smart Images

Figure BDA0002157140810000261
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a positive electrode material for a lithium ion secondary battery, a positive electrode material for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a lithium ion secondary battery. Background Art
[0002] Lithium ion secondary batteries, which are non-aqueous electrolyte secondary batteries, can be miniaturized, lightweight, and have high capacity, and have excellent characteristics of high output and high energy density, and are therefore commercialized as high-output power sources for electric tools, such as electric vehicles. As an electrode material for lithium ion secondary batteries, for example, an electrode material containing granules is known, which are obtained by granulating primary particles containing an electrode active material and a carbon film covering the surface of the electrode active material.
[0003] As a method for manufacturing a positive electrode material for a lithium-ion secondary battery, for example, a method is known that comprises the following steps: a step of adding electrode material particles containing carbon to the upper part of a kiln body of a rotary kiln; and a step of calcining the electrode material particles while moving them from the upper part to the lower part of the kiln body (for example, refer to Patent Document 1).
[0004] Furthermore, as a method for manufacturing a positive electrode material for a lithium-ion secondary battery, for example, a method is known that includes the following steps: a step of preparing a mixture by adding an organic compound that serves as a source of a conductive carbon coating to an electrode active material; and a step of placing the mixture in a calcining sagger and calcining it at a calcination temperature of not less than 630° C. and not more than 790° C. (for example, refer to Patent Document 2).
[0005] Patent Document 1: Japanese Patent No. 5710788
[0006] Patent Document 2: Japanese Patent No. 6128181 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] In a method of calcining a granulated body formed by a mixture of an electrode active material and an organic compound as a carbon coating source in an existing roller kiln, tubular furnace or other container, uneven film thickness of the carbon coating occurs during calcination due to uneven temperature in the granulated body and uneven volatilization of the organic components. In the calcination in a tubular furnace or roller kiln, a method of placing a heat-conducting auxiliary material in a container and calcining the container is also known. However, although this method can reduce the uneven temperature in the granulated body, the uneven film thickness of the carbon coating occurs due to the different degrees of contact between the volatilized organic components and the electrode active material.
[0009] Furthermore, studies have been conducted on uniformly calcining an electrode active material and a carbon source by calcining them using a rotary kiln.
[0010] However, when a rotary kiln is used to directly calcine a mixture of primary particles, agglomerates and carbon sources of electrode active materials, the agglomerates adhere to the inner wall surface of the rotary kiln due to their low fluidity. The primary particles agglomerate and contact with each other to facilitate sintering, so sintering between primary particles is easy. Due to the low adhesion between primary particles, problems such as the formation of fine powder during calcination arise. The powder attached to the inner wall surface cannot be calcined uniformly, and undesirable conditions such as uneven film thickness of the carbon coating of the recovered powder occur. For the sintering of primary particles, the battery characteristics decrease due to the decrease in surface area, and the operability decreases for the formation of fine powder.
[0011] The present invention is completed in view of the above situation, and its purpose is to provide a method for manufacturing a positive electrode material for a lithium ion secondary battery, a positive electrode material for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a lithium ion secondary battery, which prevents the adhesion of positive electrode active materials to the inner wall surface of a rotary kiln, sintering between primary particles, and the formation of fine powder.
[0012] Solutions for solving problems
[0013] In order to solve the above-mentioned problems, the present inventors conducted in-depth research and found that in a method for manufacturing a positive electrode material for a lithium-ion secondary battery comprising a pyrolytic carbon coating, by having a heat treatment step of using a rotary kiln to pyrolyze an organic compound that serves as a carbon source for forming a pyrolytic carbon coating, it is possible to prevent the positive electrode active material from adhering to the inner wall surface of the rotary kiln, sintering between primary particles, and the formation of fine powder, thereby completing the present invention.
[0014] The method for producing a positive electrode material for a lithium ion secondary battery of the present invention is a method for producing a positive electrode material for a lithium ion secondary battery including a pyrolytic carbon coating, and the method comprises a heat treatment step in which an organic compound as a carbon source for forming the pyrolytic carbon coating is pyrolyzed using a rotary kiln.
[0015] The positive electrode material for lithium ion secondary battery of the present invention is a positive electrode material for lithium ion secondary battery produced by the method for producing a positive electrode material for lithium ion secondary battery of the present invention, comprising a positive electrode active material and a pyrolytic carbon coating covering the surface of the positive electrode active material, and having a sphericity of 0.8 or more.
[0016] The positive electrode for lithium ion secondary battery of the present invention comprises an electrode current collector and a positive electrode mixture layer formed on the electrode current collector. In the positive electrode for lithium ion secondary battery, the positive electrode mixture layer contains the positive electrode material for lithium ion secondary battery of the present invention.
[0017] The lithium ion secondary battery of the present invention comprises a positive electrode, a negative electrode, and a non-aqueous electrolyte, and the lithium ion secondary battery comprises the positive electrode for a lithium ion secondary battery of the present invention as the positive electrode.
[0018] Effects of the Invention
[0019] According to the method for producing a positive electrode material for a lithium ion secondary battery of the present invention, it is possible to prevent the positive electrode active material from adhering to the inner wall surface of the rotary kiln, sintering of primary particles, formation of fine powder, and the like.
[0020] According to the positive electrode material for a lithium ion secondary battery of the present invention, it is possible to provide a positive electrode material for a lithium ion secondary battery capable of realizing a lithium ion secondary battery having a large discharge capacity and a low DC resistance during charge and discharge.
[0021] According to the positive electrode for a lithium ion secondary battery of the present invention, since it contains the positive electrode material for a lithium ion secondary battery of the present invention, it is possible to provide a positive electrode for a lithium ion secondary battery having no uneven composition.
[0022] According to the lithium ion secondary battery of the present invention, since it includes the positive electrode for lithium ion secondary battery of the present invention, it is possible to provide a lithium ion secondary battery having a large discharge capacity and a low DC resistance during charge and discharge. DETAILED DESCRIPTION
[0023] Embodiments of the present invention are described with respect to a method for producing a positive electrode material for a lithium ion secondary battery, a positive electrode material for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a lithium ion secondary battery.
[0024] In addition, the present embodiment will be described in detail for better understanding of the gist of the invention, but the present invention is not limited unless otherwise specified.
[0025] [Method for producing positive electrode material for lithium ion secondary battery]
[0026] The method for producing a positive electrode material for a lithium ion secondary battery of the present embodiment is a method for producing a positive electrode material for a lithium ion secondary battery including a pyrolytic carbon coating, and the method comprises a heat treatment step in which an organic compound serving as a carbon source for forming the pyrolytic carbon coating is pyrolyzed using a rotary kiln.
[0027] Preferably, the manufacturing method of the positive electrode material for lithium ion secondary batteries of this embodiment comprises: a process of dispersing a mixed solution of a positive electrode active material and a dispersion medium to prepare a dispersion having a span value of a particle size distribution of the positive electrode active material of greater than 0.5 and less than 1.0; a process of drying a mixed solution of the dispersion and an organic compound as a carbon source to obtain granules having a sphericity of greater than 0.8; and a process of calcining the granules to pyrolyze the organic compound to obtain a positive electrode material for lithium ion secondary batteries having a sphericity of greater than 0.8 and a surface of the positive electrode active material coated with a pyrolytic carbon coating.
[0028] In the method for manufacturing a positive electrode material for a lithium ion secondary battery of the present embodiment, the obtained positive electrode material for a lithium ion secondary battery preferably contains an olivine-based positive electrode active material. That is, in the method for manufacturing a positive electrode material for a lithium ion secondary battery of the present embodiment, an olivine-based positive electrode active material is preferably used as the positive electrode active material.
[0029] As the olivine-based positive electrode active material, there are exemplified the general formula Li x A y D z A compound represented by PO4 (wherein A is at least one selected from the group consisting of Co, Mn, Ni, Fe, Cu and Cr, D is at least one selected from the group consisting of Mg, Ca, Sr, Ba, Ti, Zn, B, Al, Ga, In, Si, Ge, Sc, Y and rare earth elements, 0.9<x<1.1, 0<y≤1, 0≤z<1, 0.9<y+z<1.1).
[0030] By the general formula Li x A y D z Particles formed of a compound represented by PO4 (hereinafter referred to as "Li x A y D z PO4 particles".) are manufactured in the following manner.
[0031] For example, Li is preferably obtained by x A y D z PO4 particles: Li source, A source, D source and PO4 source are added to water so that their molar ratio becomes x:y+z=1:1, and stirred to make Li x A y D z A precursor solution of PO4 is placed in a pressure-resistant container and subjected to a hydrothermal treatment at high temperature and high pressure, for example, 120°C to 250°C and 0.2 MPa to a temperature of 1 hour to 24 hours.
[0032] In this case, by adjusting the temperature, pressure and time during the hydrothermal treatment, Li x A y D z The particle size of PO4 particles is controlled to a desired size.
[0033] In this case, as the Li source, for example, it is preferred to use at least one selected from the group consisting of lithium inorganic acid salts such as lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium chloride (LiCl), lithium phosphate (Li3PO4), and lithium organic acid salts such as lithium acetate (LiCH3COO), and lithium oxalate ((COOLi)2).
[0034] Among them, lithium chloride and lithium acetate are preferred because a uniform solution phase can be easily obtained.
[0035] Here, the A source is preferably at least one selected from the group consisting of a Co source including a cobalt compound, a Mn source including a manganese compound, a Ni source including a nickel compound, a Fe source including an iron compound, a Cu source including a copper compound, and a Cr source including a chromium compound. Furthermore, the D source is preferably at least one selected from the group consisting of a Mg source including a magnesium compound, a Ca source including a calcium compound, a Sr source including a strontium compound, a Ba source including a barium compound, a Ti source including a titanium compound, a Zn source including a zinc compound, a B source including a boron compound, an Al source including an aluminum compound, a Ga source including a gallium compound, an In source including an indium compound, a Si source including a silicon compound, a Ge source including a germanium compound, a Sc source including a scandium compound, and a Y source including a yttrium compound.
[0036] As a Co source, a Co salt is preferred. For example, it is preferred to use at least one selected from cobalt (II) chloride (CoCl2), cobalt (II) sulfate (CoSO4), cobalt (II) nitrate (Co(NO3)2), cobalt (II) acetate (Co(CH3COO)2) and their hydrates.
[0037] As the Mn source, a Mn salt is preferred, and for example, at least one selected from manganese (II) chloride (MnCl2), manganese (II) sulfate (MnSO4), manganese (II) nitrate (Mn(NO3)2), manganese (II) acetate (Mn(CH3COO)2) and hydrates thereof is preferably used. Among them, manganese sulfate is preferred because it is easy to obtain a uniform solution phase.
[0038] As a Ni source, a Ni salt is preferred, for example, preferably at least one selected from nickel (II) chloride (NiCl2), nickel (II) sulfate (NiSO4), nickel (II) nitrate (Ni(NO3)2), nickel (II) acetate (Ni(CH3COO)2) and their hydrates.
[0039] As an Fe source, for example, divalent iron compounds such as iron (II) chloride (FeCl2), iron (II) sulfate (FeSO4), iron (II) acetate (Fe(CH3COO)2) or their hydrates, trivalent iron compounds such as iron (III) nitrate (Fe(NO3)3), iron (III) chloride (FeCl3), iron (III) citrate (FeC6H5O7), lithium iron phosphate, etc. can be used.
[0040] As the Cu source, for example, copper (II) chloride (CuCl2), copper (II) sulfate (CuSO4), copper (II) nitrate (Cu(NO3)2), copper (II) acetate (Cu2(CH3COO)4) and their hydrates can be cited, and it is preferred to select at least one of the group consisting of them.
[0041] As Cr sources, for example, chromium (II) chloride (CrCl2), chromium (III) sulfate (Cr2(SO4)3), chromium (II) nitrate (Cr(NO3)3), chromium (II) acetate (Cr2(CH3COO)4) and their hydrates can be mentioned, and it is preferred to select at least one of the group consisting of them.
[0042] As Mg sources, for example, magnesium chloride (II) (MgCl2), magnesium sulfate (II) (MgSO4), magnesium nitrate (II) (Mg(NO3)2), magnesium acetate (II) (Mg(CH3COO)2) and their hydrates can be cited, and at least one of the group consisting of them is preferably selected.
[0043] As the Ca source, for example, calcium chloride (II) (CaCl2), calcium sulfate (II) (CaSO4), calcium nitrate (II) (Ca(NO3)2), calcium acetate (II) (Ca(CH3COO)2) and their hydrates can be cited, and it is preferred to select at least one of the group consisting of them.
[0044] Examples of the Sr source include strontium carbonate (SrCo 3 ), strontium sulfate (SrSO 4 ), and strontium hydroxide (Sr(OH) 2 ), and at least one selected from the group consisting of these is preferred.
[0045] As Ba sources, for example, barium (II) chloride (BaCl2), barium (II) sulfate (BaSO4), barium (II) nitrate (Ba(NO3)2), barium (II) acetate (Ba(CH3COO)2) and their hydrates can be cited, and at least one of the group consisting of them is preferably selected.
[0046] Examples of the Ti source include titanium chloride (TiCl 4 , TiCl 3 , TiCl 2 ), titanium oxide (TiO) and hydrates thereof, and at least one selected from the group consisting of these is preferred.
[0047] As the Zn source, Zn salts are preferred, for example, zinc (II) chloride (ZnCl2), zinc (II) sulfate (ZnSO4), zinc (II) nitrate (Zn(NO3)2), zinc (II) acetate (Zn(CH3COO)2) and their hydrates, preferably at least one selected from the group consisting of them.
[0048] Examples of the B source include boron compounds such as chlorides, sulfates, nitrates, acetates, hydroxides, and oxides, and at least one selected from the group consisting of these is preferred.
[0049] Examples of the Al source include aluminum compounds such as chlorides, sulfates, nitrates, acetates, and hydroxides, and at least one selected from the group consisting of these is preferred.
[0050] Examples of the Ga source include gallium compounds such as chlorides, sulfates, nitrates, acetates, and hydroxides, and at least one selected from the group consisting of these is preferred.
[0051] Examples of the In source include indium compounds such as chlorides, sulfates, nitrates, acetates, and hydroxides, and at least one selected from the group consisting of these is preferred.
[0052] Examples of the Si source include sodium silicate, potassium silicate, silicon tetrachloride (SiCl 4 ), silicates, and organic silicon compounds, and at least one selected from the group consisting of these is preferred.
[0053] Examples of the Ge source include germanium compounds such as chlorides, sulfates, nitrates, acetates, hydroxides, and oxides, and at least one selected from the group consisting of these is preferred.
[0054] Examples of the Sc source include scandium compounds such as chlorides, sulfates, nitrates, acetates, hydroxides, and oxides, and at least one selected from the group consisting of these is preferred.
[0055] Examples of the Y source include yttrium compounds such as chlorides, sulfates, nitrates, acetates, hydroxides, and oxides, and at least one selected from the group consisting of these is preferred.
[0056] As a PO4 source, for example, it is preferably selected from at least one of phosphoric acid such as orthophosphoric acid (H3PO4), metaphosphoric acid (HPO3), diammonium phosphate (NH4H2PO4), diammonium hydrogen phosphate ((NH4)2HPO4), ammonium phosphate ((NH4)3PO4), lithium phosphate (Li3PO4), dilithium hydrogen phosphate (Li2HPO4), lithium dihydrogen phosphate (LiH2PO4) and their hydrates.
[0057] In particular, orthophosphoric acid is preferred because it easily forms a uniform solution phase.
[0058] Next, a positive electrode active material (e.g., Li x A y D z PO4 particles) and a dispersion medium are used to prepare a mixed solution, and the mixed solution is subjected to a dispersion treatment to prepare a dispersion solution in which the span value of the particle size distribution of the positive electrode active material is 0.5 or more and 1.0 or less (a step of preparing a dispersion solution).
[0059] The span value of the particle size distribution of the positive electrode active material in the dispersion is preferably 0.5 or more and 3.0 or less, more preferably 0.6 or more and 2.0 or less, and even more preferably 0.7 or more and 1.0 or less.
[0060] If the span value of the particle size distribution of the positive electrode active material in the dispersion is less than 0.5, the porosity increases due to the small difference in particle size in the granules, resulting in a decrease in energy density. On the other hand, if the span value of the particle size distribution of the positive electrode active material in the dispersion exceeds 3.0, the particles remain in the granules through aggregation and sinter during calcination, resulting in a decrease in capacitance due to a decrease in surface area.
[0061] The span value of the particle size distribution of the positive electrode active material in the dispersion refers to the value calculated by the following formula based on the particle size (D90) with a cumulative volume percentage of 90 volume%, the particle size (D50) with a cumulative volume percentage of 50 volume%, and the particle size (D10) with a cumulative volume percentage of 10 volume% in the volume particle size distribution of the positive electrode active material.
[0062] Span value = (D90-D10) / D50
[0063] The volume particle size distribution of the positive electrode active material is measured by a method in accordance with JIS Z8825 "Particle size analysis-Laser diffraction / scattering method".
[0064] The dispersion method of the mixed solution of the positive active material and the dispersion medium is not particularly limited, but it is preferred to use a device that can give a loose positive active material a cohesive state so that the positive active material is uniformly dispersed in the dispersion medium, and the span value of the particle size distribution of the positive active material in the dispersion liquid can be set to a dispersion energy of more than 0.5 and less than 3.0. As such a device, for example, in addition to a stirrer, a bead mill, a ball mill, a homogenizer, an ultrasonic disperser, a mixer, a three-roll mill, a rotation / revolution mixer, etc. using zirconia beads can also be cited. In particular, in the case of using a disperser based on a continuous bead mill, it is possible to sample the liquid in the middle of the dispersion, so that the time point at which the span value falls within a specified range can be set as the end point, and the span value can be easily adjusted.
[0065] The time required for the dispersion treatment may be a time sufficient to uniformly disperse the positive electrode active material in the dispersion medium.
[0066] The mixing ratio of the positive electrode active material and the dispersion medium (positive electrode active material / dispersion medium) is preferably 1 / 9 to 7 / 3, more preferably 2 / 8 to 6 / 4, in terms of mass ratio.
[0067] The dispersion medium is not particularly limited as long as it can uniformly disperse the positive electrode active material, but a solvent containing water as a main component is preferred.
[0068] The solvent containing water as a main component refers to any of water alone or water-based solvents containing water as a main component and containing an aqueous solvent such as alcohol as needed.
[0069] The aqueous solvent is not particularly limited as long as it is a solvent that can dissolve lithium salts, metal salts containing Fe, metal salts containing Mn, metal salts containing M, and phosphoric acid compounds. For example, alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol: IPA), butanol, pentanol, hexanol, octanol, and diacetone alcohol; esters such as ethyl acetate, butyl acetate, ethyl lactate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and γ-butyrolactone can be cited. ; ethers such as diethyl ether, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monomethyl ether and diethylene glycol monoethyl ether; ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetylacetone and cyclohexanone; amides such as dimethylformamide, N,N-dimethylacetoacetamide and N-methylpyrrolidone; and glycols such as ethylene glycol, diethylene glycol and propylene glycol. These may be used alone or in combination of two or more.
[0070] Next, the dispersion and an organic compound as a carbon source are mixed to prepare a mixed solution (slurry), and the mixed solution is dried to obtain granules having a sphericity of 0.8 or more (step of producing granules).
[0071] The mixing method of the dispersion liquid and the organic compound is not particularly limited, but it is preferred to use a device that can uniformly mix the dispersion liquid and the organic compound. Such a device, for example, in addition to a stirrer, can also include a bead mill using zirconium oxide beads, a ball mill, a homogenizer, an ultrasonic disperser, a kneading machine, a three-roll mill, a rotation / revolution mixer, etc.
[0072] The time required for the mixing treatment may be a time sufficient to uniformly mix the dispersion and the organic compound.
[0073] The organic compound is preferably mixed so that carbon in the organic compound is 2 parts by mass or more and 20 parts by mass or less, more preferably 4 parts by mass or more and 10 parts by mass or less, based on 100 parts by mass of the positive electrode active material.
[0074] Examples of the organic compound include polyvinyl alcohol, polyvinyl pyrrolidone, cellulose, starch, gelatin, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, polystyrene sulfonic acid, polyacrylamide, polyvinyl acetate, glucose, fructose, galactose, mannose, maltose, sucrose, lactose, glycogen, pectin, alginic acid, glucomannan, chitin, hyaluronic acid, chondroitin, agarose, polyethers, and polyols.
[0075] Examples of the polyol include polyethylene glycol, polypropylene glycol, polyglycerol, and glycerol.
[0076] The mixed solution of the dispersion and the organic compound is dried to obtain granules having a sphericity of 0.8 or more.
[0077] The drying method is not particularly limited as long as the dispersion medium can be dispersed from the mixed liquid.
[0078] In addition, when agglomerated particles are produced, the granules may be dried by a spray decomposition method using a spray dryer, etc. For example, the mixed solution may be sprayed in a high temperature atmosphere of 50° C. to 300° C. and dried to produce a granular dried body or a granular dried body.
[0079] The sphericity of granules is a value obtained by dividing the circumference of a circle having the same area as the projected area of the particle image by the circumference of the particle image. In the case of a perfect circle, the sphericity is 1, and decreases as the shape deviates from a sphericity.
[0080] The sphericity of the granules was calculated from the average value of the sphericity of each granule by measuring the area and the perimeter of 100 particles in a scanning electron microscope image by image analysis.
[0081] Next, a rotary kiln is used to calcine (heat treat) the above-mentioned granules, and the organic compound serving as the carbon source for forming the pyrolytic carbon coating is pyrolyzed (heat treatment step) to obtain a positive electrode material for a lithium ion secondary battery having a sphericity of greater than 0.8 and the surface of the positive electrode active material being coated with a pyrolytic carbon coating.
[0082] As the rotary kiln, for example, a rotary kiln including a heat treatment section having a cylindrical kiln body, an input section for inputting granules (processed material) into the kiln body, and a discharge section for discharging the granules from the kiln body can be used.
[0083] As a method for calcining granules using a rotary kiln, for example, the following method can be mentioned.
[0084] Granulated bodies are put into the upper part of the kiln main body, positive pressure gas is flowed inside the kiln main body, and granulated bodies are calcined while being moved from the upper part to the lower part of the kiln main body, and the calcined granulated bodies are discharged from the lower part of the kiln main body. Granulated bodies discharged from the lower part of the kiln main body are passed through a cooler and cooled.
[0085] The method of feeding the granules into the rotary kiln is not particularly limited, but the feeding method differs depending on the repose angle of the granules. If the repose angle of the granules is large, the granules cannot be smoothly fed into the kiln body due to the bridging phenomenon between the granules and the feeding device in the feeding part of the rotary kiln. The form of the feeding device is not particularly limited, but examples thereof include a stud form, a vibration form, a push form, and an empty delivery form.
[0086] The calcination temperature of the granules in the kiln main body is preferably 400°C or higher and 1000°C or lower, and more preferably 600°C or higher and 800°C or lower.
[0087] This is because: if the calcination temperature is less than 400°C, the decomposition reaction of the organic compound contained in the granules cannot be fully carried out, the carbonization of the organic compound becomes insufficient, and the generated decomposition reaction product becomes an organic decomposition product with high resistance, which is not preferred. On the other hand, if it exceeds 1000°C, not only the components constituting the granules, such as lithium (Li), evaporate and cause deviation in the composition, but also the particle growth is promoted in the granules, the discharge capacity at a high charge and discharge rate decreases, and it becomes difficult to achieve sufficient charge and discharge rate performance, which is not preferred.
[0088] The time for which the granules remain in the kiln main body (ie, the calcination time) is preferably 0.5 hours to 6 hours, and more preferably 0.5 hours to 2 hours.
[0089] If the calcination time is more than 0.5 hours, the granules can be fully calcined, and the granules are in contact with the positive pressure gas for a long time, so the crystallinity of the granules increases, and the unreacted products and moisture content decrease. When it is used as a positive electrode material, the tap density of the positive electrode mixture layer increases, and the bonding strength between the positive electrode mixture layer and the electrode collector increases.
[0090] The kiln body is arranged to be inclined, and the granules are calcined while being conveyed from the upper part (top side) to the lower part (bottom side) of the kiln body. In addition, a positive pressure gas (pressure higher than atmospheric pressure) is supplied to the kiln body, but in the kiln body, the positive pressure gas preferably has a pressure higher than atmospheric pressure by 0.01 kPa to 1 kPa.
[0091] If the pressure in the kiln body is lower than the atmospheric pressure, the external air containing impurities such as moisture and oxygen flows into the kiln body. However, if the granules calcined in an environment with a high moisture content are used as positive electrode materials, the bonding force between the positive electrode mixture layer and the electrode current collector will decrease. In addition, oxygen not only oxidizes the positive electrode material to reduce the electrochemical properties, but also oxidizes the kiln body to reduce the durability. On the other hand, if the pressure in the kiln body is too high, it is not preferred from the perspective of safety.
[0092] The positive pressure gas supplied to the kiln body is discharged through the positive pressure gas upper outlet provided at the upper part (top side) of the heat treatment part or the positive pressure gas lower outlet provided at the lower part (bottom side) of the heat treatment part. Here, the upper side of the heat treatment part refers to the side (upper part) where the input part of the object to be treated exists, with the center of the long side direction of the heat treatment part as a reference, and the lower side of the heat treatment part refers to the side (lower part) where the discharge part of the object to be treated exists. More than 50% of the total amount of the discharged positive pressure gas is discharged through the positive pressure gas upper outlet, which is conducive to removing the moisture present in the kiln body.
[0093] It is preferred that the positive pressure gas flows from the lower part of the kiln body to the upper part. The positive pressure gas is supplied to the lower part of the kiln body and discharged from the upper part of the kiln body. The positive pressure gas is injected and discharged in the kiln body in a direction opposite to the flow of the processed object, which is conducive to collecting and removing carbon powder and other powders. Carbon powder can be contained in the positive electrode active material or generated by etching the kiln body formed of carbon material.
[0094] The positive pressure gas is at least one selected from the group consisting of nitrogen (N2), carbon dioxide (CO2), hydrogen (H2), helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe) and radon (Rn). As the positive pressure gas, a mixture of nitrogen and butane can also be used.
[0095] A carbon compound in a gaseous state may be mixed in the positive pressure gas. In this case, there is an advantage that the surface of the positive electrode active material that is incompletely coated with the pyrolytic carbon film can be improved.
[0096] Furthermore, the gaseous carbon compound plays a role in preventing damage caused by oxidation of the positive electrode active material and oxidation of the kiln body. Examples of such gaseous carbon compounds include hydrocarbon gases such as methane, ethane, butane, and propane.
[0097] The oxygen concentration in the kiln main body is preferably 200 ppm or less, more preferably 100 ppm or less.
[0098] When the oxygen concentration in the kiln body is 200 ppm or less, there will be no problem of oxidation of the positive electrode active material or the kiln body.
[0099] The material of the kiln body includes metal, ceramic, carbon, etc. During the calcination of the granules, the inner wall of the kiln body that rubs against the granules is sometimes worn to generate fine powder, and the fine powder is mixed into the granules as impurities. Therefore, in order to prevent this, it is preferred that the inner surface of the kiln body that contacts the granules is made of carbon.
[0100] The sphericity of the positive electrode material for lithium ion secondary batteries is a value obtained by dividing the circumference of a circle having the same area as the projected area of the positive electrode material by the circumference of the positive electrode material. In the case of a perfect circle, the sphericity is 1, and decreases as the shape deviates from a sphericity.
[0101] The sphericity of the positive electrode material for lithium ion secondary batteries is measured by the same method as the sphericity of the granules described above.
[0102] According to the method for manufacturing a positive electrode material for a lithium-ion secondary battery of the present embodiment, by forming a granulation body comprising a positive electrode active material and an organic compound as a carbon source and maintaining the fluidity of the granulation body, it is possible to prevent the positive electrode active material from adhering to the inner wall surface of a rotary kiln, and to prevent the primary particles comprising the positive electrode active material (primary particles) and the pyrolytic carbon coating covering the surface thereof from sticking together.
[0103] Thus, sintering between primary particles can be prevented, and granules can be prevented from breaking. In addition, by using a rotary kiln to calcine the granules, the granules are stirred by the rotation of the rotary kiln, and can be uniformly contacted with the ambient gas, and the granules can be homogenized. By homogenizing the granules, the fluctuation of characteristics caused by uneven calcination caused by the recovery part, which is a problem in a tubular furnace, can be reduced.
[0104] Furthermore, according to the method for manufacturing a positive electrode material for a lithium ion secondary battery of the present embodiment, a dispersion is prepared by dispersing a mixed solution of a positive electrode active material and a dispersion medium, and the dispersion is mixed with an organic compound as a carbon source to prepare a mixed solution, so that when the mixed solution is dried to form a granule, the primary particles of the positive electrode active material can be prevented from bonding to each other due to agglomeration. Furthermore, since the organic compound plays the role of a binder, the granule is not easily broken.
[0105] [Positive electrode materials for lithium-ion secondary batteries]
[0106] The positive electrode material for lithium ion secondary battery of this embodiment is produced by the method for producing the positive electrode material for lithium ion secondary battery of this embodiment, and comprises a positive electrode active material and a pyrolytic carbon coating covering the surface of the positive electrode active material, and has a sphericity of 0.8 or more.
[0107] The positive electrode material for lithium ion secondary battery of the present embodiment preferably contains an olivine-based positive electrode active material. That is, the positive electrode material for lithium ion secondary battery of the present embodiment preferably contains an olivine-based positive electrode active material as the positive electrode active material.
[0108] The positive electrode material for lithium ion secondary battery of the present embodiment comprises a granulated body obtained by granulating primary particles containing a positive electrode active material (primary particles) and a pyrolytic carbon coating covering the surface thereof. Hereinafter, the primary particles containing a positive electrode active material (primary particles) and a pyrolytic carbon coating covering the surface thereof are sometimes referred to as primary particles of a carbonaceous coated positive electrode active material.
[0109] The sphericity of the positive electrode material for lithium ion secondary batteries according to the present embodiment is preferably 0.8 or more, and more preferably 0.9 or more.
[0110] When the sphericity of the positive electrode material for a lithium ion secondary battery is 0.8 or more, handling during electrode production becomes favorable and an improvement in electrode density can be achieved.
[0111] Regarding the positive electrode material for lithium ion secondary batteries of this embodiment, the average particle size of primary particles of the carbonaceous coated positive electrode active material is 30 nm to 500 nm, preferably 50 nm to 400 nm, and more preferably 50 nm to 300 nm.
[0112] Here, the reason for setting the average particle size of the primary particles of the carbonaceous coated positive electrode active material within the above range is as follows. If the average primary particle size is 30 nm or more, the increase in the amount of carbon caused by the excessive specific surface area can be suppressed. On the other hand, if the average primary particle size is 500 nm or less, the electronic conductivity and ion diffusivity can be improved according to the size of the specific surface area.
[0113] The average particle size of the primary particles of the carbonaceous coated positive electrode active material is determined by taking the number average of the particle sizes of 200 or more primary particles randomly measured by observation with a scanning electron microscope (SEM).
[0114] Regarding the positive electrode material for lithium ion secondary batteries of this embodiment, the average particle size of the granulated body obtained by granulating primary particles of the carbonaceous coated positive electrode active material is 0.5 μm to 60 μm, preferably 1 μm to 20 μm, and more preferably 1 μm to 10 μm.
[0115] Here, the reasons for setting the average particle size of the granules within the above range are as follows. If the average particle size of the granules is 0.5 μm or more, the mixing of the positive electrode material, the conductive aid, the binder resin (binder) and the solvent can be suppressed, and the amount of the conductive aid and the binder when preparing the positive electrode material paste for lithium ion secondary batteries can be increased. The battery capacity of the lithium ion secondary battery per unit mass of the positive electrode mixture layer for lithium ion secondary batteries can be increased. On the other hand, if the average particle size of the granules is 60 μm or less, the dispersibility and uniformity of the conductive aid and the binder contained in the positive electrode mixture layer for lithium ion secondary batteries can be improved. As a result, the lithium ion secondary battery using the positive electrode material for lithium ion secondary batteries of the present embodiment can increase the discharge capacity under high-speed charge and discharge.
[0116] The average particle size of the granules was measured by suspending the positive electrode material for lithium ion secondary batteries of the present embodiment in a dispersion medium prepared by dissolving 0.1 mass % of polyvinyl pyrrolidone in water, and using a laser diffraction particle size analyzer.
[0117] Regarding the positive electrode material for lithium ion secondary batteries of this embodiment, the carbon content in the primary particles of the carbonaceous coated positive electrode active material is preferably 0.5 mass % to 2.5 mass %, more preferably 0.8 mass % to 1.3 mass %, and further preferably 0.8 mass % to 1.2 mass %.
[0118] Here, the reason for setting the carbon content in the primary particles of the carbonaceous coated positive electrode active material within the above range is as follows. If the carbon content in the primary particles is 0.5% by mass or more, the electronic conductivity can be fully improved. On the other hand, if the carbon content in the primary particles of the carbonaceous coated positive electrode active material is 2.5% by mass or less, the electrode density can be increased.
[0119] The carbon content in the primary particles of the carbonaceous coated positive electrode active material was measured using a carbon analyzer (carbon-sulfur analyzer: EMIA-810W (trade name), manufactured by HORIBA, Ltd.).
[0120] In the positive electrode material for lithium ion secondary batteries of the present embodiment, the coverage rate of the carbonaceous coating on the primary particles of the carbonaceous coated positive electrode active material is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more.
[0121] Here, the reason why the coverage rate of the carbonaceous film in the primary particles of the carbonaceous coated positive electrode active material is set within the above range is as follows: If the coverage rate of the carbonaceous film in the primary particles of the carbonaceous coated positive electrode active material is 80% or more, the covering effect of the carbonaceous coating can be fully obtained.
[0122] The coverage rate of the carbonaceous film on the primary particles of the carbonaceous coated positive electrode active material is measured using a transmission electron microscope (TEM), an energy dispersive X-ray microanalyzer (EDX), or the like.
[0123] Regarding the positive electrode material for lithium ion secondary batteries of this embodiment, the thickness of the carbonaceous coating in the primary particles of the carbonaceous coated positive electrode active material is preferably 0.8 nm to 5.0 nm, more preferably 0.9 nm to 4.5 nm, and even more preferably 0.8 nm to 4.0 nm.
[0124] Here, the reason for setting the film thickness of the carbonaceous film in the primary particles of the carbonaceous coated positive electrode active material within the above range is as follows. If the film thickness of the carbonaceous film in the primary particles is 0.8nm or more, it is possible to suppress the inability to form a carbonaceous film with a desired resistance value due to the thickness of the carbonaceous film being too thin. On the other hand, if the film thickness of the carbonaceous film in the primary particles of the carbonaceous coated positive electrode active material is 5.0nm or less, it is possible to suppress the decrease in battery capacity per unit mass of the electrode material.
[0125] The film thickness of the carbonaceous film on the primary particles of the carbonaceous coated positive electrode active material is measured using a transmission electron microscope (TEM), an energy dispersive X-ray microanalyzer (EDX), or the like.
[0126] In addition, the positive electrode material for lithium ion secondary battery of the present embodiment may also include components other than the above-mentioned granules. As components other than the granules, for example, conductive aids such as a binder including a binder resin, carbon black, acetylene black, graphite, Ketjen black, natural graphite, and artificial graphite may be cited.
[0127] The specific surface area of the granules of the positive electrode material for lithium ion secondary batteries of the present embodiment is preferably 6 m 2 / g or more and 30m 2 / g or less, more preferably 10m 2 / g or more and 20m 2 / g or less.
[0128] Here, the reason why the specific surface area of the positive electrode material for lithium ion secondary batteries of this embodiment is limited to the above range is as follows. 2 / g or more, the diffusion rate of lithium ions in the positive electrode material can be increased, and the battery characteristics of the lithium ion secondary battery can be improved. On the other hand, if the specific surface area is 30m 2 / g or less, the electronic conductivity can be improved.
[0129] The specific surface area of the positive electrode material for lithium ion secondary batteries of the present embodiment is measured by the BET method based on nitrogen (N 2 ) adsorption using a specific surface area meter.
[0130] “Olivine-based positive electrode active material”
[0131] Olivine-based positive electrode active materials include Li x A y D z A compound represented by PO4 (wherein A is at least one selected from the group consisting of Co, Mn, Ni, Fe, Cu and Cr, D is at least one selected from the group consisting of Mg, Ca, Sr, Ba, Ti, Zn, B, Al, Ga, In, Si, Ge, Sc, Y and rare earth elements, 0.9<x<1.1, 0<y≤1, 0≤z<1, 0.9<y+z<1.1).
[0132] Li x A y D zAmong PO4, from the viewpoint of high discharge capacity and high energy density, a positive electrode active material satisfying 0.9<x<1.1, 0<y≤1, 0≤z<1, and 0.9<y+z<1.1 is preferred.
[0133] From the viewpoint of being able to produce a positive electrode mixture layer that can achieve a high discharge potential and high safety, A is preferably Co, Mn, Ni, and Fe, and D is preferably Mg, Ca, Sr, Ba, Ti, Zn, and Al.
[0134] Here, the rare earth elements refer to 15 elements of the lanthanum series: La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.
[0135] The crystallite diameter of the olivine-based positive electrode active material is preferably 30 nm or more and 150 nm or less, and more preferably 50 nm or more and 120 nm or less.
[0136] If the crystallite diameter of the olivine-based positive electrode active material is less than 30nm, a large amount of carbon is required to fully coat the surface of the positive electrode active material with a pyrolytic carbon coating, and a large amount of binder is required, so sometimes the amount of positive electrode active material in the positive electrode decreases, and the capacity of the battery decreases. Similarly, the carbonaceous coating sometimes peels off due to insufficient bonding force. On the other hand, if the crystallite diameter of the olivine-based positive electrode active material exceeds 150nm, the internal resistance of the positive electrode active material increases, and when a battery is formed, the discharge capacity at a high charge and discharge rate is sometimes reduced.
[0137] The crystallite diameter of the olivine-based positive electrode active material is calculated according to the Scherrer formula using the half-value width and diffraction angle (2θ) of the diffraction peak on the (020) plane of the powder X-ray diffraction pattern measured by X-ray diffraction measurement.
[0138] "Carbon coating"
[0139] The carbonaceous film is a pyrolytic carbonaceous film obtained by carbonizing an organic compound as a raw material. The carbon source as a raw material of the carbonaceous film is preferably derived from an organic compound having a carbon purity of 42.00% or more and 60.00% or less.
[0140] The method for calculating the "carbon purity" of the carbon source that serves as the raw material for the carbonaceous coating in the positive electrode material for the lithium-ion secondary battery of this embodiment can be the following method: when using multiple organic compounds, based on the blending amount (mass %) of each organic compound and the known carbon purity (%), calculate the carbon amount (mass %) in the blending amount of each organic compound and add them up, and calculate from the total blending amount (mass %) of the organic compounds and the total carbon amount (mass %) according to the following formula (1).
[0141] Carbon purity (%) = total carbon content (mass %) / total blending amount (mass %) × 100 ... (1)
[0142] According to the positive electrode material for lithium ion secondary batteries of the present embodiment, since it is manufactured by the manufacturing method of the positive electrode material for lithium ion secondary batteries of the present embodiment, it is possible to provide a positive electrode material for lithium ion secondary batteries in which the surface of the positive electrode active material is uniformly coated with a pyrolytic carbon coating and the primary particles of the positive electrode active material are not bonded to each other due to agglomeration. Therefore, according to the positive electrode material for lithium ion secondary batteries of the present embodiment, a lithium ion secondary battery with a large discharge capacity and a low DC resistance of charge and discharge can be realized.
[0143] [Positive electrode for lithium-ion secondary battery]
[0144] The positive electrode for lithium ion secondary battery of the present embodiment includes an electrode current collector and a positive electrode mixture layer (electrode) formed on the electrode current collector, and the positive electrode mixture layer contains the positive electrode material for lithium ion secondary battery of the present embodiment.
[0145] That is, the positive electrode for lithium ion secondary batteries of the present embodiment is obtained by forming a positive electrode mixture layer on one main surface of an electrode current collector using the positive electrode material for lithium ion secondary batteries of the present embodiment.
[0146] The method for manufacturing the positive electrode for lithium ion secondary batteries of the present embodiment is not particularly limited as long as it is a method that can form a positive electrode mixture layer on one main surface of an electrode current collector using the positive electrode material for lithium ion secondary batteries of the present embodiment. As the method for manufacturing the positive electrode for lithium ion secondary batteries of the present embodiment, for example, the following method can be cited.
[0147] First, a positive electrode material paste for lithium ion secondary batteries is prepared by mixing the positive electrode material for lithium ion secondary batteries of the present embodiment, a binder, a conductive auxiliary agent, and a solvent.
[0148] "Binder"
[0149] The binder is not particularly limited as long as it can be used in an aqueous system, and for example, at least one selected from the group consisting of polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, vinyl acetate copolymer, styrene-butadiene latex, acrylic latex, acrylonitrile-butadiene latex, fluorine latex, silicone latex, etc. can be cited.
[0150] When the total mass of the positive electrode material, binder and conductive aid for lithium ion secondary battery of this embodiment is set to 100 mass %, the content of the binder in the positive electrode material paste for lithium ion secondary battery is preferably 1 mass % to 10 mass %, and more preferably 2 mass % to 6 mass %.
[0151] "Conductive additive"
[0152] The conductive additive is not particularly limited, but for example, at least one selected from the group consisting of fibrous carbons such as acetylene black, Ketjen black, furnace black, vapor grown carbon fiber (VGCF), and carbon nanotubes can be used.
[0153] When the total mass of the positive electrode material, binder and conductive aid for lithium ion secondary battery of this embodiment is set to 100 mass %, the content of the conductive aid in the positive electrode material paste for lithium ion secondary battery is preferably 1 mass % to 15 mass %, and more preferably 3 mass % to 10 mass %.
[0154] "Solvent"
[0155] The positive electrode material paste for lithium ion secondary batteries containing the positive electrode material for lithium ion secondary batteries of the present embodiment may contain a solvent as appropriate in order to facilitate coating on an object to be coated such as an electrode current collector.
[0156] Although the main solvent is water, an aqueous solvent such as alcohols, glycols, or ethers may be contained within a range that does not impair the characteristics of the positive electrode material for lithium ion secondary batteries of the present embodiment.
[0157] When the total mass of the positive electrode material for lithium ion secondary batteries, the binder and the solvent of the present embodiment is set to 100 parts by mass, the content of the solvent in the positive electrode material paste for lithium ion secondary batteries is preferably 60 parts by mass or more and 400 parts by mass or less, and more preferably 80 parts by mass or more and 300 parts by mass or less.
[0158] By containing the solvent in the above range, a positive electrode material paste for lithium ion secondary batteries having excellent electrode formability and excellent battery characteristics can be obtained.
[0159] As a method for mixing the positive electrode material, binder, conductive additive and solvent for lithium ion secondary battery of the present embodiment, there is no particular limitation as long as it is a method that can uniformly mix these components. For example, a method using a kneading machine such as a ball mill, a sand mixer, a planetary mixer, a paint stirrer, a homogenizer, etc. can be cited.
[0160] Next, the positive electrode material paste for lithium ion secondary batteries is applied to one main surface of the electrode collector to form a coating, and the coating is dried. Then, it is pressurized and crimped, thereby obtaining a positive electrode for lithium ion secondary batteries having a positive electrode mixture layer formed on one main surface of the electrode collector.
[0161] According to the positive electrode for lithium ion secondary batteries of the present embodiment, since the positive electrode material for lithium ion secondary batteries of the present embodiment is contained, it is possible to provide a positive electrode for lithium ion secondary batteries having no uneven composition.
[0162] [Lithium-ion secondary battery]
[0163] The lithium ion secondary battery of the present embodiment includes a positive electrode, a negative electrode, and a non-aqueous electrolyte, and includes the positive electrode for a lithium ion secondary battery of the present embodiment as the positive electrode.
[0164] In the lithium ion secondary battery of the present embodiment, the negative electrode, the nonaqueous electrolyte, the separator, and the like are not particularly limited.
[0165] As the negative electrode, for example, metal Li, carbon material, Li alloy, Li4Ti5O 12 Negative electrode materials.
[0166] Also, a solid electrolyte may be used instead of the nonaqueous electrolyte and the separator.
[0167] The non-aqueous electrolyte may be prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) at a volume ratio of 1:1, and adding lithium hexafluorophosphate (LiPF6) at a concentration of 1 mol / dm 3 The method is to dissolve the obtained mixed solvent in the obtained method.
[0168] As the separator, for example, porous acryl can be used.
[0169] Since the lithium ion secondary battery of the present embodiment includes the positive electrode for the lithium ion secondary battery of the present embodiment, the discharge capacity is large and the DC resistance during charge and discharge is low.
[0170] Example
[0171] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0172] [Production Example 1]
[0173] "Manufacturing of positive electrode active material (LiFePO4)"
[0174] Lithium hydroxide (LiOH) was used as a Li source, ammonium dihydrogen phosphate (NH 4 H 2 PO 4 ) was used as a P source, and iron (II) sulfate heptahydrate (FeSO 4 ·7H 2 O) was used as a Fe source.
[0175] Lithium hydroxide, ammonium dihydrogen phosphate, and iron (II) sulfate heptahydrate were mixed in water at a mass ratio of Li:Fe:P=3:1:1 and a total amount of 200 mL to prepare a uniform slurry-like mixture.
[0176] Next, the mixture was placed in a 500 mL pressure-resistant sealed container and subjected to hydrothermal synthesis at 170° C. for 12 hours.
[0177] After the reaction, the reaction solution was cooled to room temperature (25° C.), and a precipitated cake-like reaction product was obtained.
[0178] Next, the precipitate (reaction product) was washed sufficiently with distilled water several times, and pure water was added to prevent drying while maintaining the water content at 30%, thereby preparing a cake-like substance.
[0179] A small amount of the cake-like substance was collected and vacuum dried at 70° C. for 2 hours to obtain a powder, which was analyzed by X-ray diffraction measurement (X-ray diffraction apparatus: RINT2000, manufactured by RIGAKU Corporation). As a result, it was confirmed that single-phase LiFePO 4 was formed.
[0180] [Production Example 2]
[0181] "Manufacturing of positive electrode active material (LiMnPO4)"
[0182] Li[Fe] was synthesized in the same manner as in Example 1 except that a mixture of iron(II) sulfate heptahydrate (FeSO4·7H2O) and manganese(II) sulfate monohydrate (MnSO4·H2O) (FeSO4·7H2O:MnSO4·H2O=25:75 (mass ratio)) was used as an Fe source. 0.25 Mn 0.75 ]PO4.
[0183] [Example 1]
[0184] A mixed solution was prepared by mixing 20 g of LiFePO4 (positive electrode active material) obtained in Manufacturing Example 1 and 80 g of water as a dispersion medium, and 150 g of zirconia beads with a diameter of 0.1 mm as medium particles were added to the mixed solution, and a bead mill was used to disperse the mixture to prepare a uniform dispersion.
[0185] Next, 0.73 g of sucrose as a carbon source was added to the above dispersion, and a dispersion was prepared using a bead mill in the same manner as above.
[0186] Next, the obtained dispersion was dried and granulated using a spray dryer at a drying outlet temperature of 60° C. to obtain a granulated powder.
[0187] Then, the granulated powder was heat-treated at 770° C. for 4 hours using a rotary kiln to obtain the positive electrode material of Example 1 including granulated bodies obtained by granulating primary particles of the positive electrode active material coated with carbon.
[0188] [Example 2]
[0189] Prior to heat treatment in a rotary kiln, 0.5% polyvinyl alcohol was added to the granulated powder and stirred and mixed. In the same manner as in Example 1, a positive electrode material of Example 2 comprising granulated primary particles of a positive electrode active material coated with carbon was obtained.
[0190] [Example 3]
[0191] A positive electrode material of Example 3 including granulated bodies obtained by granulating primary particles of the positive electrode active material coated with carbonaceous material was obtained in the same manner as in Example 1 except that zirconia beads having a diameter of 0.3 mm were used.
[0192] [Example 4]
[0193] As the positive electrode active material, Li[Fe 0.25 Mn 0.75 ]PO4 was used instead of LiFePO4, and in the same manner as in Example 1, a positive electrode material of Example 4 including granulated bodies obtained by granulating primary particles of a positive electrode active material coated with carbon was obtained.
[0194] [Comparative Example 1]
[0195] A positive electrode material of Comparative Example 1 including granulated bodies obtained by granulating primary particles of a positive electrode active material coated with carbonaceous material was obtained in the same manner as in Example 1 except that a stirring tool was used instead of mixing with zirconia beads to prepare the dispersion.
[0196] [Comparative Example 2]
[0197] A positive electrode material of Comparative Example 2 comprising granulated bodies obtained by granulating primary particles of a positive electrode active material coated with carbon was obtained in the same manner as in Example 1, except that zirconia beads having a diameter of 1 mm were used and the granulated powder was crushed by a dry ball mill and then heat treated.
[0198] [Comparative Example 3]
[0199] A positive electrode material of Comparative Example 3 including granulated bodies obtained by granulating primary particles of a positive electrode active material coated with carbon was obtained in the same manner as in Example 1 except that the granulated powder was charged into a carbon sagger and the carbon sagger was heat-treated using a tubular furnace.
[0200] [Manufacturing of lithium-ion batteries]
[0201] The positive electrode material obtained in Examples 1 to 4 and Comparative Examples 1 to 3, polyvinylidene fluoride (PVdF) as a binding material, and acetylene black (AB) as a conductive aid were added to N-methyl-2-pyrrolidone (NMP) in a mass ratio in the paste such that positive electrode material: AB:PVdF = 90:5:5, and they were mixed to prepare a positive electrode material paste.
[0202] Next, the positive electrode material paste is applied on the surface of an aluminum foil (electrode current collector) with a thickness of 30 μm to form a coating, and the coating is dried. After a positive electrode mixture layer is formed on the surface of the aluminum foil, the positive electrode mixture layer is pressed to a specified density to make a positive electrode plate.
[0203] The obtained electrode plate was punched into a square (electrode area of 9 cm) with a length of 3 cm and a width of 3 cm using a forming machine. 2 )'s positive electrode mixture layer and the plate-shaped edge of the flat plate.
[0204] Next, an electrode flat plate was welded to the flat edge of the electrode plate to prepare a test electrode (positive electrode).
[0205] The coated electrode was placed on the test electrode as a negative electrode via a separator formed of a porous polypropylene film to prepare a battery component.
[0206] The coated electrode was formed by applying a mixture of natural graphite, acetylene black (AB), styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) at a mass ratio of natural graphite:AB:SBR:CMC=92:4:3:1 to the separator.
[0207] The prepared positive electrode and negative electrode were placed opposite each other with a separator having a thickness of 20 μm and made of porous polypropylene, and then immersed in 0.5 mL of a 1 mol / L lithium hexafluorophosphate (LiPF6) solution as a non-aqueous electrolyte (non-aqueous electrolyte solution), and then sealed with a laminated film to produce a lithium ion secondary battery.
[0208] As the LiPF6 solution, a solution prepared by mixing ethylene carbonate and ethyl methyl carbonate at a volume ratio of 1:1 and adding 2% of vinylene carbonate as an additive was used.
[0209] [Evaluation of positive electrode materials]
[0210] The positive electrode materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 and the components contained in these positive electrode materials were evaluated. The evaluation method is as follows. The results are shown in Table 1.
[0211] (1) Span of particle size distribution of positive electrode active material contained in dispersion
[0212] The particle size distribution of the positive electrode active material contained in the dispersion containing the positive electrode active material and water was measured using a particle size distribution meter (trade name: LA-920, manufactured by HORIBA, Ltd.) in accordance with JIS Z8825 "Particle size analysis-laser diffraction scattering method". Using the measurement results of the particle size distribution, the span value of the particle size distribution of the positive electrode active material contained in the dispersion was calculated according to the following formula.
[0213] Span value = (D90-D10) / D50
[0214] (2) Crystallite diameter of positive electrode active material
[0215] The crystallite diameter of the positive electrode active material was calculated using the half-width and diffraction angle (2θ) of the diffraction peak on the (020) plane of the powder X-ray diffraction pattern measured by X-ray diffraction measurement (X-ray diffraction apparatus: RINT2000 (trade name), manufactured by RIGAKU Corporation) and the Scherrer equation.
[0216] (3) Sphericity of granules
[0217] The granules after the heat treatment were observed using a scanning electron microscope, and the average value of the minor axis diameter / major axis diameter per 100 granules was defined as the sphericity of the granules.
[0218] [Evaluation of positive electrode and lithium-ion secondary battery]
[0219] The lithium ion secondary batteries obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were used to measure the discharge capacity and the direct current resistance (DCR) during charge and discharge. The evaluation method was as follows. The results are shown in Table 1.
[0220] (1) Discharge capacity
[0221] At an ambient temperature of 25°C, the cutoff voltage was set to 2.5V-3.7V (vs carbon negative electrode) in the batteries other than Example 3, and the cutoff voltage was set to 2.5V-4.2V (vs carbon negative electrode) in the batteries of Example 3, the charging current was set to 1C, and the discharging current was set to 3C, and the discharge capacity of the lithium-ion secondary battery was measured by constant current charging and discharging.
[0222] (2) DC resistance (DCR) during charge and discharge
[0223] The lithium-ion secondary battery was charged at a current of 0.1C for 5 hours at an ambient temperature of 0°C, and the depth of charge (charge rate (SOC) 50%) was adjusted. In the battery adjusted to SOC 50%, the first cycle was "1C charge for 10 seconds → stop for 10 minutes → 1C discharge for 10 seconds → stop for 10 minutes", the second cycle was "3C charge for 10 seconds → stop for 10 minutes → 3C discharge for 10 seconds → stop for 10 minutes", the third cycle was "5C charge for 10 seconds → stop for 10 minutes → 5C discharge for 10 seconds → stop for 10 minutes", and the fourth cycle was "10C charge for 10 seconds → stop for 10 minutes → 10C discharge for 10 seconds → stop for 10 minutes", and the voltage after 10 seconds was measured during each charge and discharge at this time. Each current value was plotted on the horizontal axis and the voltage after 10 seconds was plotted on the vertical axis to draw an approximate straight line, and the slopes on the approximate straight line were respectively set as the DC resistance during charging (charging DCR) and the DC resistance during discharging (discharging DCR).
[0224]
Table 1
[0225]
[0226] According to the results in Table 1, in Examples 1 to 4, a rotary kiln was used as a calcining device, the span value of the particle size distribution of the positive electrode active material was 0.58 to 2.99, and the sphericity of the granules was 0.82 to 0.93, so the 3C discharge capacity was more than 130 mAh / g, the charging DC resistance was less than 2.9Ω, and the discharge DC resistance was less than 2.5Ω.
[0227] On the other hand, in Comparative Example 1, the span value of the particle size distribution of the positive electrode active material was 26.63, so the 3C discharge capacity was 122 mAh / g or more, the charge DC resistance was 2.9Ω, and the discharge DC resistance was 2.5Ω.
[0228] In Comparative Example 2, the sphericity of the granules was 0.65, so the 3C discharge capacity was 125 mAh / g or more, the charge DC resistance was 2.9Ω, and the discharge DC resistance was 2.6Ω.
[0229] In Comparative Example 3, a tubular furnace was used as the calcination device, so the 3C discharge capacity was 120 mAh / g or more, the charge DC resistance was 3.0Ω, and the discharge DC resistance was 2.7Ω.
[0230] That is, it is found that Examples 1 to 4 have larger discharge capacities and lower DC resistances during charge and discharge than Comparative Examples 1 to 3.
[0231] Industrial Applicability
[0232] The positive electrode material for lithium ion secondary battery of the present invention is manufactured by the manufacturing method of the positive electrode material for lithium ion secondary battery of the present invention, and comprises a positive electrode active material and a pyrolytic carbon coating on the surface of the positive electrode active material, and the sphericity is above 0.8, so the positive electrode for lithium ion secondary battery made using the positive electrode material for lithium ion secondary battery has excellent electronic conductivity. Therefore, for the lithium ion secondary battery with the positive electrode for lithium ion secondary battery, the DC resistance of charge and discharge is low, and the discharge capacity is increased, so it can also be applied to the next generation of secondary batteries that expect higher voltage, high energy density, high load characteristics and high-speed charge and discharge characteristics, and in the case of the next generation of secondary batteries, the effect is very large.
Claims
1. A method for producing a positive electrode material for a lithium ion secondary battery, the positive electrode material for a lithium ion secondary battery comprising a pyrolytic carbon coating, the method comprising the following steps: A step of dispersing a mixed solution of a positive electrode active material and a dispersion medium to prepare a dispersion solution having a particle size distribution span value of the positive electrode active material of not less than 0.5 and not more than 3.0; A step of drying a mixed solution of the dispersion and an organic compound as a carbon source to obtain granules having a sphericity of 0.8 or more; and A heat treatment step is performed in which an organic compound serving as a carbon source for forming the pyrolytic carbon film is pyrolyzed using a rotary kiln.
2. The method for producing a positive electrode material for a lithium ion secondary battery according to claim 1, It is characterized in that The positive electrode material for a lithium ion secondary battery includes an olivine-based positive electrode active material.
3. The method for producing a positive electrode material for a lithium ion secondary battery according to claim 1 or 2, It is characterized in that The process is as follows: The granulated body is calcined to pyrolyze the organic compound, thereby obtaining a positive electrode material for a lithium ion secondary battery having a sphericity of 0.8 or more and a surface of the positive electrode active material covered with a pyrolytic carbon coating.
4. The method for producing a positive electrode material for a lithium ion secondary battery according to claim 1 or 2, It is characterized in that The positive electrode active material is manufactured by a hydrothermal synthesis method.
5. A positive electrode material for a lithium ion secondary battery, It is characterized in that The positive electrode material is produced by the method for producing a positive electrode material for a lithium ion secondary battery according to any one of claims 1 to 4. The positive electrode material for lithium ion secondary battery comprises a positive electrode active material and a pyrolytic carbon coating covering the surface of the positive electrode active material. The sphericity is 0.8 or more.
6. A positive electrode for a lithium ion secondary battery, comprising: an electrode current collector and a positive electrode mixture layer formed on the electrode current collector, wherein the positive electrode for a lithium ion secondary battery is characterized in that: The positive electrode mixture layer contains the positive electrode material for a lithium ion secondary battery according to claim 5 .
7. A lithium ion secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, wherein: The positive electrode for a lithium ion secondary battery according to claim 6 is provided as the positive electrode.