Positive electrode active material and battery having the same
By using a coating material covering low electron conductivity and a lithium composite oxide with a multiphase structure in lithium-ion batteries, the problem of poor cycling characteristics of lithium-ion batteries at high potential is solved, and a battery with high capacity and high cycling characteristics is achieved performance.
Patent Information
- Application Number
- CN201910799156.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-09-05
- Filing Date
- 2019-08-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-08-28
AI Technical Summary
When used at high potentials, the circulation characteristics are poor, and electrolyte decomposition, side reactions and gas detachment are prone to capacity reduction.
The positive electrode active material containing lithium composite oxide and coating material is used to cover the surface of the lithium composite oxide through a coating material with low electron conductivity, inhibit the contact and electron accepting of the lithium composite oxide with the electrolyte, and prevent the generation of the resistive layer and the disengagement of the gas. The lithium composite oxide using a heterogeneous mixture has a structure of monoclinic, hexagonal and cubic crystals, forming a stable interface through chemical modification and solid solution.
The high capacity and high cycle characteristics of the battery at high potential are achieved, ensuring the maintenance of battery capacity and excellent circulation performance.
Smart Images

Figure CN110880585B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a positive electrode active material and a battery including the positive electrode active material. Background Art
[0002] Patent Document 1 discloses a lithium composite transition metal oxide having a chemical composition represented by the general formula LiaMOx (wherein M is at least one element selected from Ni, Co, and Mn). In the X-ray diffraction pattern of the lithium composite transition metal oxide, the integrated intensity (I 020 ) is the integrated intensity (I 003 ) ratio (I 020 / I 003 ) is 0.02~0.3.
[0003] Prior art literature
[0004] Patent Document 1: International Publication No. 2014 / 192759 Summary of the invention
[0005] An object of the present disclosure is to provide a positive electrode active material used to form a battery having high capacity and high cycle characteristics.
[0006] The positive electrode active material in the present disclosure includes a lithium composite oxide and a coating material, wherein the coating material covers the surface of the lithium composite oxide.
[0007] in,
[0008] The lithium composite oxide is a multiphase mixture including a first phase, a second phase and a third phase,
[0009] The first phase has a crystal structure belonging to a monoclinic crystal, the second phase has a crystal structure belonging to a hexagonal crystal, and the third phase has a crystal structure belonging to a cubic crystal,
[0010] And satisfy the following mathematical formula (I),
[0011] 0.05≤Integral intensity ratio I (18°-20°) / I (43°-46°) ≤0.99 (I)
[0012] in,
[0013] Integrated intensity ratio I (18°-20°) / I (43°-46°) Equal to the integrated intensity I (18°-20°) Relative to the integrated intensity I (43°-46°) The ratio,
[0014] Integral Intensity I (43°-46°) is the integrated intensity of the first peak, which is the largest peak existing in the range of diffraction angle 2θ of 43° or more and 46° or less in the X-ray diffraction pattern of the lithium composite oxide, and
[0015] Integral Intensity I (18°-20°) is the integrated intensity of the second peak, which is the largest peak existing in the range of diffraction angle 2θ of 18° or more and 20° or less in the X-ray diffraction pattern of the lithium composite oxide, and
[0016] The electronic conductivity of the coating material is 10 6 S / m or less.
[0017] The present disclosure provides a positive electrode active material for achieving high capacity and high cycle characteristics. The present disclosure also provides a battery having a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the positive electrode active material. The battery has high capacity and high cycle characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A cross-sectional view of a battery 10 as an example of a battery in the second embodiment is shown.
[0019] Figure 2 It is a graph showing the X-ray diffraction patterns of the positive electrode active materials of Example 1 and Comparative Example 1.
[0020] Figure 3 It is a graph showing the results of charge and discharge cycle tests of the batteries of Examples 1 and 2 and Reference Example 1.
[0021] Description of Reference Numerals
[0022] 10. Battery
[0023] 11 Housing
[0024] 12. Positive electrode collector
[0025] 13. Positive electrode active material layer
[0026] 14 Partition
[0027] 15 Sealing plate
[0028] 16 Negative electrode collector
[0029] 17 Negative electrode active material layer
[0030] 18 Gasket
[0031] 21 Positive electrode
[0032] 22 Negative electrode DETAILED DESCRIPTION
[0033] Hereinafter, embodiments of the present disclosure will be described.
[0034] (Implementation Method 1)
[0035] The positive electrode active material in the first embodiment includes a lithium composite oxide and a coating material, wherein the coating material covers the surface of the lithium composite oxide.
[0036] in,
[0037] The lithium composite oxide is a multiphase mixture including a first phase, a second phase and a third phase,
[0038] The first phase has a crystal structure belonging to a monoclinic crystal, the second phase has a crystal structure belonging to a hexagonal crystal, and the third phase has a crystal structure belonging to a cubic crystal,
[0039] And satisfy the following mathematical formula (I),
[0040] 0.05≤Integral intensity ratio I (18°-20°) / I (43°-46°) ≤0.99 (I)
[0041] in,
[0042] Integrated intensity ratio I (18°-20°) / I (43°-46°) Equal to the integrated intensity I (18°-20°) Relative to the integrated intensity I (43°-46°) The ratio,
[0043] Integral Intensity I (43°-46°) is the integrated intensity of the first peak, which is the largest peak existing in the range of diffraction angle 2θ of 43° or more and 46° or less in the X-ray diffraction pattern of the lithium composite oxide, and
[0044] Integral Intensity I (18°-20°) is the integrated intensity of the second peak, which is the largest peak existing in the range of diffraction angle 2θ of 18° or more and 20° or less in the X-ray diffraction pattern of the lithium composite oxide, and
[0045] The electronic conductivity of the coating material is 10 6 S / m or less.
[0046] This positive electrode active material is used to provide a battery having high capacity and high cycle performance.
[0047] The term "battery with high cycle characteristics" refers to a battery whose capacity retention rate is high even after repeated charge and discharge cycles. In other words, the term "battery with high cycle characteristics" refers to a battery whose capacity does not significantly decrease even after repeated charge and discharge cycles.
[0048] The redox potential (in terms of Li / Li) of the lithium ion battery having the positive electrode active material in the first embodiment + The capacity of the lithium ion battery is about 260 mAh / g or more. Even after 20 cycles of charge and discharge tests, the capacity retention rate of the lithium ion battery is about 90% or more.
[0049] When the conventional positive electrode active material is used at a high potential, the decomposition of the electrolyte (e.g., side reaction) is promoted to generate a resistance layer. Moreover, when the conventional positive electrode active material is used at a high potential, the anions contained in the positive electrode active material are separated in the form of gas. Therefore, there is a fear that the cycle characteristics will be reduced.
[0050] The positive electrode active material in the first embodiment includes a coating material in addition to the lithium composite oxide. The coating material covers the surface of the lithium composite oxide. The coating material has an electron conductivity of 10 6 S / m or less and a material different from the lithium composite oxide. The surface of the lithium composite oxide is coated with the coating material to suppress the contact between the lithium composite oxide and the electrolyte. Since the electronic conductivity of the coating material is low, the electron transfer between the lithium composite oxide and the electrolyte can be suppressed. Moreover, the side reaction caused by the electron transfer can be suppressed. Thus, the generation of the resistance layer or the detachment of the gas can be suppressed. Therefore, a battery with high cycle characteristics can be achieved.
[0051] That is, the battery including the positive electrode active material in the first embodiment has excellent cycle characteristics even when used at a high potential.
[0052] In the present disclosure, "a covered surface" includes a completely covered surface as well as a partially covered surface.
[0053] In Embodiment 1, the mass ratio of the coating material to the lithium composite oxide may be 0.2 or less.
[0054] If the mass ratio is 0.2 or less, it is possible to suppress electrochemical passivation of the surface of the positive electrode active material in Embodiment 1. As a result, it is possible to suppress an increase in resistance. Therefore, a battery with higher capacity and better cycle characteristics can be realized.
[0055] In order to realize a battery having high capacity and high cycle characteristics, the mass ratio may be 0.01 or more and 0.1 or less.
[0056] In order to realize a battery with high capacity and high cycle characteristics, the coating material may be in a film shape in Embodiment 1. The coating material may have a thickness of 0.1 nm to 10.0 nm.
[0057] When the thickness of the coating material is 0.1 nanometer or more, the uniformity of the thickness can be improved. When the thickness of the coating material is 0.1 nanometer or more, the insulation breakdown can be suppressed.
[0058] When the thickness of the coating material is 10.0 nm or less, the coating material is thin enough and thus does not impair the Li conductivity.
[0059] In order to further improve the cycle characteristics, in Embodiment 1, the thickness of the coating material may be 5.0 nanometers or more and 10.0 nanometers or less.
[0060] In the first embodiment, the coating material may chemically modify the surface of the lithium composite oxide.
[0061] The coating material in Embodiment 1 can form a solid solution with at least a portion of the surface of the lithium composite oxide.
[0062] Chemical modification and solid solution can further suppress the dissolution (eg, detachment) of metal elements, thereby further improving the cycle characteristics of the battery.
[0063] In Embodiment 1, the covering material is, for example, an inorganic material.
[0064] In Embodiment 1, the coating material may be at least one selected from graphite, carbon black, and fluorinated graphite. Examples of carbon black include acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black.
[0065] In Embodiment 1, the coating material may be formed of an insulating compound. The coating material may not contribute to the electrochemical reaction.
[0066] In the first embodiment, the coating material may be at least one selected from oxides, nitrogen oxides, halogen compounds, sulfides, and phosphorus compounds.
[0067] For example, as the halogen compound, AlF 3 can be used.
[0068] In the first embodiment, the covering material may be a lithium ion conductor.
[0069] Examples of lithium ion conductors are:
[0070] (i) Lithium compounds such as LiBO2, Li3PO4, LiNbO3, LiNbO2, LiAlO2, Li2SO4, Li2MoO4, Li4SiO4, Li4FeO4, Li4ZrO4, Li2CO3, LiW2O7, Li3VO4, LiCl, LiBr, LiI and Li2Se,
[0071] (ii) Lithium ion conducting glasses such as Li2O-B2O3, Li2O-Al2O3, Li2O-SiO4, Li2O-P2O5 and LiF-BF3, LiF-AlF3, LiF-VF3, and
[0072] (iii) The above lithium ion conductor in which a part of oxygen is substituted with nitrogen.
[0073] Two or more lithium ion conductors may be used.
[0074] The positive electrode active material having a coating material that is a lithium ion conductor improves the cycle characteristics of the battery.
[0075] In the first embodiment, the coating material may be a Li-containing oxide having high Li conductivity, or a Li-containing oxide in which a part of oxygen is substituted with nitrogen.
[0076] Examples of Li-containing oxides include lithium borate, lithium niobate, lithium cobaltate, lithium titanate, and lithium aluminate. Two or more Li-containing oxides may be used.
[0077] The Li-containing oxide improves the diffusivity of Li ions, further increasing the battery capacity.
[0078] In the first embodiment, when the coating material can absorb Li during the charge and discharge reaction, the battery capacity is further improved. In this case, the coating material has a charge and discharge capacity. Therefore, even if the mass ratio of the lithium composite oxide to the entire positive electrode active material decreases, the high battery capacity can be maintained.
[0079] In order to further improve the cycle characteristics, in the first embodiment, the coating material may be an oxide or a nitride oxide.
[0080] Oxides and oxynitrides are chemically stable and have low reactivity with electrolytes, and therefore, it is believed that oxides and oxynitrides are likely to maintain their crystal structures during electrochemical reactions.
[0081] In order to further improve the cycle characteristics, in Embodiment 1, the coating material may be an oxide or a nitride oxide represented by the following composition formula (1).
[0082] Li a A b O c N d Formula (1)
[0083] in,
[0084] A is at least one selected from the group consisting of Mn, Co, Ni, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Si, Eu, Sm, Ce, and H,
[0085] 0≤a≤3,
[0086] 0.5≤b≤4,
[0087] 1≤c≤4, and
[0088] 0≤d≤1.
[0089] In order to further improve the cycle characteristics, in embodiment 1, the coating material can be formed by at least one oxide selected from, for example, NiO2, CoO2, MnO2, Al2O3, MgO, SiO2, ZrO2, ZnO, TiO2, H3BO3, Mn2O3, Fe2O3, CuO, NiO, Co3O4, Eu2O3, Sm2O3 and CeO2.
[0090] In order to further improve the cycle characteristics, in embodiment 1, the coating material can be selected from, for example, NiO2, CoO2, MnO2, Al2O3, MgO, SiO2, ZrO2, LiNbO3, LiBO2 and Li 3-e PO 4-f N g (wherein 0≤e≤3, 0≤f≤3, and 0≤g≤1) is formed.
[0091] In order to further improve the cycle characteristics, in the first embodiment, the coating material can be selected from, for example, LiNbO3, LiBO2 and Li 3-e PO 4-f N g At least one of (0≤e≤3, 0≤f≤3, 0≤g≤1) is formed.
[0092] In order to further improve the cycle characteristics, in Embodiment 1, the coating material may be formed of at least one selected from, for example, Al 2 O 3 , MgO, SiO 2 , and ZrO 2 .
[0093] In order to further improve the battery capacity and cycle characteristics, in Embodiment 1, the coating material may be formed of Al 2 O 3 .
[0094] In order to further improve the cycle characteristics, in Embodiment 1, the coating material may be formed of a transition metal oxide.
[0095] In Embodiment 1, the coating material may include the same metal element as the metal element included in the lithium composite oxide.
[0096] When the coating material has the same metal element as the metal element contained in the lithium composite oxide, the metal element forms a solid solution at the interface between the lithium composite oxide and the coating material, and the lithium composite oxide and the coating material are firmly bonded to each other. Therefore, the dissolution (e.g., detachment) of the metal element can be suppressed. As a result, the cycle characteristics of the battery are further improved.
[0097] In the first embodiment, the coating material may coat the current collector, the electron conduction aid, or the binder contained in the positive electrode in addition to the lithium composite oxide.
[0098] The positive electrode active material in embodiment 1 includes a lithium composite oxide, which is a multiphase mixture including a first phase, a second phase and a third phase, wherein the first phase has a monoclinic crystal structure, the second phase has a hexagonal crystal structure, and the third phase has a cubic crystal structure.
[0099] The crystal structure belonging to monoclinic (e.g., space group C2 / m) has a structure in which Li layers and transition metal layers are alternately stacked. The transition metal layer contains not only transition metals but also Li. Therefore, the crystal structure belonging to monoclinic absorbs more Li inside the crystal structure than the commonly used previous material, i.e., LiCoO2. However, when only the crystal structure belonging to monoclinic is used, as the Li in the transition metal layer moves, atomic rearrangement occurs. It is believed that the rearrangement of the atoms reduces the cycle characteristics of the battery.
[0100] The crystal structure belonging to hexagonal crystal (such as space group R-3m) has a structure in which Li layers and transition metal layers are alternately stacked. In the crystal structure belonging to hexagonal crystal, Li is separated and inserted in the two-dimensional plane of the Li layer during charge and discharge, so Li diffusivity is high. Therefore, it is believed that a battery with excellent rate characteristics can be achieved. However, compared with the crystal structure belonging to monoclinic crystal, the amount of Li in the transition metal layer contained in the crystal structure belonging to hexagonal crystal is small. Therefore, it is believed that when only the crystal structure belonging to hexagonal crystal is used, the battery capacity becomes low.
[0101] In a crystal structure belonging to a cubic crystal (e.g., space group Fm-3m or space group Fd-3m), the crystal structure changes associated with the separation and insertion of Li during charge and discharge are small. In this way, the crystal structure belonging to the cubic crystal is strong. Therefore, the cycle characteristics of the crystal structure belonging to the cubic crystal are excellent. However, it is believed that when only the crystal structure belonging to the cubic crystal is used, the amount of Li that can be contained in the crystal structure becomes less, so the battery capacity becomes lower.
[0102] In embodiment 1, the lithium composite oxide includes a first phase, a second phase and a third phase, wherein the first phase has a monoclinic crystal structure, the second phase has a hexagonal crystal structure, and the third phase has a cubic crystal structure, and the battery capacity is improved by the synergistic effect of the characteristics of these three crystal structures.
[0103] In order to further improve the battery capacity, in the lithium composite oxide, the monoclinic crystal may be of the space group C2 / m.
[0104] In order to further improve the battery capacity, in the lithium composite oxide, the hexagonal crystal may be of the space group R-3m.
[0105] In order to further improve the battery capacity, in the lithium composite oxide, the cubic crystal may be at least one selected from the space group Fm-3m and the space group Fd-3m. That is, the third phase may have a crystal structure belonging to the space group Fm-3m or the space group Fd-3m. The third phase may also have both a crystal structure belonging to the space group Fm-3m and a crystal structure belonging to the space group Fd-3m.
[0106] In implementation mode 1, the following mathematical formula (I) is satisfied.
[0107] 0.05≤Integral intensity ratio I (18°-20°) / I (43°-46°) ≤0.99 (I)
[0108] in,
[0109] Integrated intensity ratio I (18°-20°) / I (43°-46°) Equal to the integrated intensity I (18°-20°) Relative to the integrated intensity I (43°-46°) The ratio,
[0110] Integral Intensity I (43°-46°) is the integrated intensity of the first peak, which is the largest peak existing in the range of diffraction angle 2θ of 43° to 46° in the X-ray diffraction pattern of the lithium composite oxide, and
[0111] Integral Intensity I (18°-20°) It is the integrated intensity of the second peak which is the largest peak existing in the range of the diffraction angle 2θ of 20° to 23° in the X-ray diffraction pattern of the lithium composite oxide.
[0112] Integrated intensity ratio I (18°-20°) / I (43°-46°) It is a parameter that can be used as an index of the total amount of the first phase and the second phase and the existence ratio of the third phase in the lithium composite oxide. It is considered that when the existence ratio of the total amount of the first phase and the second phase increases, the integrated intensity ratio I (18°-20°) / I (43°-46°)In addition, it is considered that when the existence ratio of the third phase increases, the integrated intensity ratio I (18°-20°) / I (43°-46°) Become smaller.
[0113] In other words, the integrated intensity ratio I (18°-20°) / I (43°-46°) It is a parameter that can be used as an index of cation mixing in lithium composite oxides. "Cation mixing" in the present disclosure means a state in which lithium atoms and cation atoms such as transition metals are substituted for each other in the crystal structure of lithium composite oxides. If the cation mixing decreases, the integrated intensity ratio I (18°-20°) / I (43°-46°) In addition, if the cations are mixed more, the integrated intensity is greater than I (18°-20°) / I (43°-46°) Become smaller.
[0114] It is considered that in the lithium composite oxide in Embodiment 1, when the integrated intensity ratio I (18°-20°) / I (43°-46°) When the ratio is less than 0.05, the total amount of the first phase and the second phase becomes small, so the Li diffusibility and the amount of Li inserted and released during charge and discharge are insufficient. As a result, the battery capacity becomes insufficient.
[0115] It is considered that in the lithium composite oxide in Embodiment 1, when the integrated intensity ratio I (18°-20°) / I (43°-46°) When the ratio is greater than 0.99, the proportion of the third phase becomes smaller, so the stability of the crystal structure decreases. Therefore, it is believed that when Li is extracted, the rearrangement of atoms is promoted and the three-dimensional diffusion path of lithium is reduced. As a result, the battery capacity becomes insufficient.
[0116] As a prior art (in other words, a comparative example), Patent Document 1 discloses a lithium composite transition metal oxide. The lithium composite transition metal oxide disclosed in Patent Document 1 has both a crystal structure belonging to the space group R-3m and a crystal structure belonging to the space group C2 / m, and has a general formula of Li a MO x (wherein M is an element containing at least one selected from the group consisting of Ni element, Co element and Mn element).
[0117] However, in the prior art such as Patent Document 1, for a lithium composite oxide including all of the first phase, the second phase, and the third phase, and having an integrated intensity ratio I (18°-20°) / I (43°-46°)There is no disclosure or suggestion of a lithium composite oxide having a molecular weight of 0.05 or more and 0.99 or less, wherein the first phase has a monoclinic crystal structure, the second phase has a hexagonal crystal structure, and the third phase has a cubic crystal structure.
[0118] It is believed that the lithium composite oxide contained in the positive electrode active material in the first embodiment suppresses atomic rearrangement when Li is removed. As a result, a large amount of Li can be inserted and removed while maintaining high Li diffusivity, and a state with high stability of the crystal structure can be achieved. That is, such a lithium composite oxide is not easily conceivable from the prior art. The lithium composite oxide further improves the battery capacity.
[0119] In order to further improve the battery capacity, the integrated intensity ratio of lithium composite oxide is (18°-20°) / I (43°-46°) It may be 0.11 or more and 0.95 or less.
[0120] In order to further improve the battery capacity, the integrated intensity ratio of lithium composite oxide is (18°-20°) / I (43°-46°) It may be 0.35 or more and 0.95 or less.
[0121] In Embodiment 1, the following mathematical formula (II) may be satisfied.
[0122] 0.08≤Integral intensity ratio I (20°-23°) / I (18°-20°) ≤0.25 (II)
[0123] in,
[0124] Integrated intensity ratio I (20°-23°) / I (18°-20°) is the integrated intensity I (20°-23°) Relative to the integrated intensity I (18°-20°) ratio, and
[0125] Integral Intensity I (20°-23°) It is the integrated intensity of the third maximum peak existing in the range of the diffraction angle 2θ of 20° to 23° in the X-ray diffraction pattern of the lithium composite oxide.
[0126] Integrated intensity ratio I (20°-23°) / I (18°-20°) It is a parameter that can be used as an index of the existence ratio of the first phase and the second phase in the lithium composite oxide. It is considered that when the existence ratio of the first phase increases, the integrated intensity ratio I (20°-23°) / I (18°-20°) On the other hand, when the existence ratio of the second phase increases, the integrated intensity ratio I (20°-23°) / I (18°-20°) Become smaller.
[0127] It is considered that when the integrated intensity ratio I (20°-23°) / I (18°-20°) When it is 0.08 or more, the existence ratio of the first phase increases, so the amount of Li inserted and released during charge and discharge increases, and the battery capacity improves.
[0128] It is considered that when the integrated intensity ratio I (20°-23°) / I (18°-20°) When it is 0.25 or less, the existence ratio of the second phase increases, so the Li diffusibility is improved and the battery capacity is improved.
[0129] The integrated intensity of the X-ray diffraction peak can be calculated using, for example, software attached to the X-ray diffraction device (e.g., PDXL attached to the powder X-ray diffraction device manufactured by Rigaku Co., Ltd.). In this case, the integrated intensity of the X-ray diffraction peak is obtained by calculating the area from, for example, the height and half-value width of each diffraction peak.
[0130] In general, in the XRD pattern using CuKα rays, in the case of a crystal structure belonging to the space group C2 / m, the maximum peak of the diffraction angle 2θ in the range of 18° to 20° reflects the (001) plane. The maximum peak of the diffraction angle 2θ in the range of 20° to 23° reflects the (020) plane. The maximum peak of the diffraction angle 2θ in the range of 43° to 46° reflects the (114) plane.
[0131] Generally speaking, in the XRD pattern using CuKα rays, in the case of a crystal structure belonging to the space group R-3m, the maximum peak of the diffraction angle 2θ in the range of 18° to 20° reflects the (003) plane. The diffraction angle 2θ does not exist in the range of 20° to 23°. The maximum peak of the diffraction angle 2θ in the range of 43° to 46° reflects the (104) plane.
[0132] Generally speaking, in the XRD pattern using CuKα rays, in the case of a crystal structure belonging to the space group Fm-3m, there is no diffraction peak in the range of diffraction angle 2θ of 18° to 20°. There is no diffraction peak in the range of diffraction angle 2θ of 20° to 23°. The maximum peak of diffraction angle 2θ in the range of 43° to 46° reflects the (200) plane.
[0133] Generally speaking, in the XRD pattern using CuKα rays, in the case of a cubic crystal, for example, a crystal structure of the space group Fd-3m, the maximum peak of the diffraction angle 2θ in the range of 18° to 20° reflects the (111) plane. The diffraction angle 2θ does not exist in the range of 20° to 23°. The maximum peak of the diffraction angle 2θ in the range of 43° to 46° reflects the (400) plane.
[0134] As an example, the lithium composite oxide contained in the positive electrode active material in embodiment 1 has a first phase, a second phase and a third phase, the first phase has a crystal structure belonging to the space group C2 / m, the second phase has a crystal structure belonging to the space group R-3m, and the third phase has a crystal structure belonging to the space group Fm-3m or Fd-3m.
[0135] In embodiment 1, the lithium composite oxide has these three phases, so there is the following problem: it is not necessarily easy to completely determine the space group and surface index respectively reflected by the maximum peak with a diffraction angle 2θ in the range of greater than 18° and less than 20° and the maximum peak with a diffraction angle 2θ in the range of greater than 43° and less than 46°.
[0136] In order to solve this problem, in addition to the above-mentioned X-ray diffraction measurement, an electron beam diffraction measurement using a transmission electron microscope (hereinafter referred to as "TEM") can be performed. By observing the electron beam diffraction pattern using a known method, the space group of the lithium composite oxide can be determined. In this way, it can be confirmed that the lithium composite oxide has a first phase, a second phase and a third phase, the first phase has a crystal structure belonging to a monoclinic crystal, the second phase has a crystal structure belonging to a hexagonal crystal, and the third phase has a crystal structure belonging to a cubic crystal.
[0137] In the lithium composite oxide, a plurality of regions composed of the first phase, a plurality of regions composed of the second phase, and a plurality of regions composed of the third phase may be randomly arranged three-dimensionally.
[0138] This random arrangement increases the three-dimensional diffusion path of Li, allowing more Li to be inserted and removed, further improving the battery capacity.
[0139] In Embodiment 1, the lithium composite oxide is a multiphase mixture. For example, a layer structure consisting of a main layer and a covering layer covering the main layer does not correspond to a multiphase mixture in the present disclosure. A multiphase mixture refers to a substance containing multiple phases. When manufacturing the lithium composite oxide, a plurality of materials corresponding to these can be mixed.
[0140] As described later, whether the lithium composite oxide is a multiphase mixture can be determined by X-ray diffraction measurement and electron beam diffraction measurement. Specifically, if the spectrum of the lithium composite oxide obtained by X-ray diffraction measurement and electron beam diffraction measurement contains peaks showing characteristics of multiple phases, the lithium composite oxide is determined to be a multiphase mixture.
[0141] In order to further improve the battery capacity, in the first embodiment, the lithium composite oxide may be a three-phase mixture consisting of a first phase, a second phase, and a third phase.
[0142] In order to further improve the battery capacity, in Embodiment 1, the lithium composite oxide contains not only lithium atoms but also atoms other than lithium atoms. Examples of atoms other than lithium atoms are Mn, Co, Ni, Fe, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si, P and Al. The lithium composite oxide may contain one atom other than lithium atoms. The lithium composite oxide may also contain two or more atoms other than lithium atoms instead.
[0143] In order to further improve the battery capacity, in Embodiment 1, the lithium composite oxide may contain at least one 3d transition metal element selected from the group consisting of Mn, Co, Ni, Fe, Cu, V, Ti, Cr and Zn as atoms other than lithium atoms.
[0144] In order to further improve the battery capacity, in Embodiment 1, the lithium composite oxide may contain at least one selected from Mn, Co, Ni, Mg, and Al as atoms other than lithium atoms.
[0145] In order to further improve the battery capacity, in Embodiment 1, the lithium composite oxide may contain at least one selected from the group consisting of Mn, Co, Ni, Mg, and Al as atoms other than lithium atoms.
[0146] In Embodiment 1, the lithium composite oxide may contain Mn.
[0147] The orbital hybridization of Mn and oxygen is easily formed, so the oxygen separation during charging can be suppressed. As described above, in the crystal structure having the first phase, the second phase and the third phase, the crystal structure is further stabilized. Therefore, it is believed that more Li can be inserted and separated. Therefore, the battery capacity can be increased.
[0148] In Embodiment 1, the lithium composite oxide may contain not only Mn but also Co and Ni.
[0149] The hybrid orbit of Mn and oxygen is easily formed. The crystal structure is stabilized by Co. Li separation is promoted by Ni. Due to these three reasons, the lithium composite oxide containing not only Mn but also Co and Ni has a more stable crystal structure. Therefore, the lithium composite oxide containing not only Mn but also Co and Ni further improves the battery capacity.
[0150] In Embodiment 1, the lithium composite oxide may include at least one element selected from the group consisting of F, Cl, N, and S. The at least one element stabilizes the crystal structure of the lithium composite oxide.
[0151] A portion of the oxygen atoms of the lithium composite oxide can be replaced by electrochemically inert anions. In other words, a portion of the oxygen atoms can be replaced by at least one anion selected from F, Cl, N and S. It is believed that by this replacement, in embodiment 1, the crystal structure of the lithium composite oxide is more stabilized. It is believed that by replacing a portion of oxygen by anions having an ion radius larger than the oxygen anion radius, the lattice becomes larger and the Li diffusivity is improved. An example of an anion having an ion radius larger than the oxygen anion radius is an anion selected from at least one of F, Cl, N and S. As described above, in a crystal structure having a first phase, a second phase and a third phase, the crystal structure is more stabilized. Therefore, it is believed that more Li can be inserted and detached. In this way, the battery capacity is improved.
[0152] In Embodiment 1, the lithium composite oxide may contain F.
[0153] The electronegativity of fluorine atoms is high, so by replacing a part of oxygen with fluorine atoms, the interaction between cations and anions becomes larger, and the discharge capacity or operating voltage is improved. For the same reason, compared with the case where F is not included, electrons are localized due to the solid solution of F. Therefore, oxygen detachment during charging can be suppressed, and the crystal structure is stable. As described above, in a crystal structure having a first phase, a second phase, and a third phase, the crystal structure is more stabilized. Therefore, more Li can be inserted and detached. By these effects working in combination, the battery capacity is further improved.
[0154] Next, an example of the chemical composition of the lithium composite oxide is described.
[0155] In Embodiment 1, the average composition of the lithium composite oxide can be represented by the following composition formula (2).
[0156] Li x Me y O α Q β Formula (2)
[0157] in,
[0158] Me is at least one selected from the group consisting of Mn, Co, Ni, Fe, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si, P, and Al, and
[0159] Q is at least one selected from F, Cl, N and S.
[0160] Furthermore, in composition formula (2), the following four mathematical expressions are satisfied.
[0161] 1.05≤x≤1.5,
[0162] 0.6≤y≤1.0,
[0163] 1.2≤α≤2.0, and
[0164] 0≤β≤0.8.
[0165] The above-mentioned lithium composite oxide further improves the battery capacity.
[0166] When Me is composed of the chemical formula Me' y1 Me” y2 (wherein Me' and Me" are at least one independently selected for Me), "y=y1+y2" is satisfied. For example, if Me is Mn 0.6 Co 0.2 , then "y=0.6+0.2=0.8" is satisfied. Even when Q is composed of two or more elements, it can be calculated in the same way as in the case of Me.
[0167] When the x value is 1.05 or more, the amount of Li that can be inserted into and extracted from the positive electrode active material increases, thereby improving the capacity.
[0168] When the x value is 1.5 or less, the amount of Li inserted into and removed from the positive electrode active material increases due to the redox reaction of Me. As a result, it is not necessary to utilize a lot of oxygen redox reactions. As a result, the crystal structure is stabilized. Therefore, the capacity is improved.
[0169] When the y value is 0.6 or more, the amount of Li inserted into and removed from the positive electrode active material increases due to the redox reaction of Me. As a result, it is not necessary to utilize a lot of oxygen redox reactions. As a result, the crystal structure is stabilized. Therefore, the capacity is improved.
[0170] When the y value is 1.0 or less, the amount of Li that can be inserted into and extracted from the positive electrode active material increases, thereby improving the capacity.
[0171] When the α value is 1.2 or more, the decrease in the charge compensation amount due to the redox of oxygen can be prevented, thereby improving the capacity.
[0172] When the α value is 2.0 or less, excess capacity due to redox of oxygen can be prevented, and the crystal structure is stabilized when Li is released, thereby improving the capacity.
[0173] When the β value is 0.8 or less, the influence of the electrochemical inertness of Q can be prevented from increasing, so that the electron conductivity is improved. Therefore, the capacity is improved.
[0174] In Embodiment 1, the "average composition" of the lithium composite oxide is a composition obtained by analyzing the elements of the lithium composite oxide without considering the difference in the composition of each phase of the lithium composite oxide. Typically, it refers to a composition obtained by elemental analysis using a sample with a size of the same degree or larger than that of the primary particles of the lithium composite oxide. The first phase, the second phase, and the third phase may have the same chemical composition as each other. Alternatively, the first phase, the second phase, and the third phase may also have different compositions from each other.
[0175] The above average composition can be determined by inductively coupled plasma emission spectrometry, inert gas fusion-infrared absorption, ion chromatography, or a combination of these analysis methods.
[0176] In order to further improve the battery capacity, in the composition formula (2), Me may contain at least one selected from Mn, Co, Ni, Fe, Cu, V, Ti, Cr and Zn (i.e., at least one 3d transition metal element).
[0177] In order to further improve the battery capacity, in the composition formula (2), Me may contain at least one selected from the group consisting of Mn, Co, Ni, Mg and Al.
[0178] In order to further improve the battery capacity, in the composition formula (2), Me may contain at least one selected from the group consisting of Mn, Co and Ni.
[0179] In the composition formula (2), Me may contain Mn. That is, Me may be Mn.
[0180] Alternatively, Me may include at least one selected from Co, Ni, Fe, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si, P and Al, as well as Mn.
[0181] As already explained, orbital hybridization of Mn and oxygen is easily formed, so oxygen detachment during charging can be suppressed. In the crystal structure having the first phase, the second phase, and the third phase, the crystal structure is further stabilized. Therefore, it is believed that more Li can be inserted and detached. Therefore, the battery capacity can be increased.
[0182] In the composition formula (2), the molar ratio of Mn to Me may be 60% or more. That is, the molar ratio of Mn to the entire Me including Mn (that is, the molar ratio of Mn / Me) may be 0.6 or more and 1.0 or less.
[0183] As already explained, orbital hybridization of Mn and oxygen is easily formed, so oxygen detachment during charging can be suppressed. In the crystal structure having the first phase, the second phase, and the third phase, the crystal structure is further stabilized. Therefore, it is believed that more Li can be inserted and detached. Therefore, the battery capacity can be increased.
[0184] In the composition formula (2), Me may contain not only Mn but also Co and Ni.
[0185] As already explained, hybrid orbits of Mn and oxygen are easily formed. The crystal structure is stabilized by Co. Li separation is promoted by Ni. For these three reasons, a lithium composite oxide containing not only Mn but also Co and Ni has a more stable crystal structure. Therefore, a lithium composite oxide containing not only Mn but also Co and Ni further improves the battery capacity.
[0186] In the composition formula (2), Me may contain at least one element selected from B, Si, P, and Al in such a manner that the molar ratio of at least one element selected from the group consisting of B, Si, P, and Al relative to Me is 20% or less.
[0187] Since B, Si, P, and Al have high covalent bonding properties, the crystal structure of the lithium composite oxide is stabilized in Embodiment 1. As a result, the cycle characteristics are improved, and the battery life can be further extended.
[0188] The following two mathematical formulas can be satisfied.
[0189] 1.166≤x≤1.33, and
[0190] 0.67≤y≤0.834.
[0191] If the above two mathematical expressions are satisfied, the battery capacity can be further increased.
[0192] The following two mathematical formulas can be satisfied.
[0193] 1.2≤α<2.0, and
[0194] 0<β≤0.8.
[0195] If the above two mathematical expressions are satisfied, the battery capacity can be further increased.
[0196] As described above, the lithium composite oxide represented by the composition formula (2) may contain Q (ie, at least one selected from F, Cl, N, and S).
[0197] A portion of the oxygen atoms of the lithium composite oxide can be replaced by an electrochemically inert anion. In other words, a portion of the oxygen atoms can be replaced by at least one anion selected from F, Cl, N and S. It is believed that by this replacement, the crystal structure of the lithium composite oxide represented by the composition formula (2) is further stabilized. It is believed that a portion of oxygen is replaced by anions whose ionic radius is larger than the oxygen anion radius, thereby expanding the lattice and improving the Li diffusivity. As described above, in a crystal structure having a first phase, a second phase and a third phase, the crystal structure is further stabilized. Therefore, it is believed that more Li can be inserted and detached. In this way, the battery capacity is improved.
[0198] Q may contain F. That is, Q may be F.
[0199] Alternatively, Q may contain not only F but also at least one element selected from Cl, N and S.
[0200] The electronegativity of fluorine atoms is high, so by replacing a portion of oxygen with fluorine atoms, the interaction between cations and anions becomes larger, and the discharge capacity or operating voltage is improved. For the same reason, compared with the case where F is not included, electrons are localized due to the solid solution of F. Therefore, oxygen detachment during charging can be suppressed, and the crystal structure is stabilized. As described above, in the crystal structure having the first phase, the second phase and the third phase, the crystal structure is further stabilized. Therefore, more Li can be inserted and detached. Through the comprehensive effect of these effects, the battery capacity is further improved.
[0201] The following two mathematical formulas can be satisfied.
[0202] 1.33≤α≤1.9, and
[0203] 0.1≤β≤0.67.
[0204] If the above two mathematical formulas are satisfied, excess capacity due to oxygen redox can be prevented. As a result, by fully exerting the influence of electrochemically inert Q, the crystal structure remains stable even when Li is separated. In this way, the battery capacity can be further improved.
[0205] The molar ratio of Li to Me is represented by the mathematical formula (x / y).
[0206] In order to further improve the battery capacity, the molar ratio (x / y) may be 1.4 or more and 2.0 or less.
[0207] When the molar ratio (x / y) is greater than 1, the ratio of the number of Li atoms in the lithium composite oxide is higher than that of the conventional lithium composite oxide represented by the composition formula LiMnO 2 , for example, so that more Li can be inserted and removed.
[0208] When the molar ratio (x / y) is 1.4 or more, the amount of available Li is large, so that a diffusion path of Li can be appropriately formed. Therefore, when the molar ratio (x / y) is 1.4 or more, the battery capacity is further improved.
[0209] When the molar ratio (x / y) is less than 2.0, it is possible to prevent the redox reaction of Me that can be used from decreasing. As a result, it is not necessary to use a lot of oxygen redox reactions. The decrease in Li insertion efficiency during discharge caused by the instability of the crystal structure during Li separation during charging is suppressed. Therefore, the battery capacity is further improved.
[0210] In order to further improve the battery capacity, the molar ratio (x / y) may be 1.4 or more and 1.5 or less.
[0211] The molar ratio of O to Q is represented by the mathematical formula (α / β).
[0212] In order to further improve the battery capacity, the molar ratio (α / β) may be 2 or more and 19 or less.
[0213] When the molar ratio (α / β) is 2 or more, the decrease in the charge compensation amount caused by the redox of oxygen can be prevented. In addition, the influence of the electrochemically inert Q can be reduced, so the electronic conductivity is improved. Therefore, the battery capacity is further improved.
[0214] When the molar ratio (α / β) is less than 19, excess capacity caused by oxygen redox can be prevented. As a result, the crystal structure is stabilized when Li is separated. Moreover, by exerting the influence of electrochemically inert Q, the crystal structure is stabilized when Li is separated. Therefore, a battery with a higher capacity can be achieved.
[0215] As described above, in Embodiment 1, the lithium composite oxide may have a composition formula of Li x Me y O α Q β The average composition represented by . Therefore, the lithium composite oxide is composed of a cation part and an anion part. The cation part is composed of Li and Me. The anion part is composed of O and Q. The molar ratio of the cation part composed of Li and Me to the anion part composed of O and Q is represented by the mathematical formula ((x+y) / (α+β)).
[0216] In order to further improve the battery capacity, the molar ratio ((x+y) / (α+β)) may be 0.75 or more and 1.2 or less.
[0217] When the molar ratio ((x+y) / (α+β)) is 0.75 or more, it is possible to prevent excessive generation of impurities during synthesis of the lithium composite oxide, and the battery capacity can be further improved.
[0218] When the molar ratio ((x+y) / (α+β)) is 1.2 or less, the amount of deficiency in the anion part of the lithium composite oxide decreases, so that even after lithium is released from the lithium composite oxide by charging, the crystal structure is stably maintained.
[0219] In order to further improve the battery capacity, the molar ratio ((x+y) / (α+β)) may be 1.0 or more and 1.2 or less.
[0220] In the lithium composite oxide, a part of Li may be substituted with an alkali metal such as Na or K.
[0221] The positive electrode active material in Embodiment 1 may contain the above-mentioned lithium composite oxide as a main component. In other words, the positive electrode active material in Embodiment 1 may contain the above-mentioned lithium composite oxide in such a manner that the mass ratio of the above-mentioned lithium composite oxide to the whole positive electrode active material is 50% or more. Such a positive electrode active material further improves the battery capacity.
[0222] In order to further increase the battery capacity, the mass ratio may be greater than 70%.
[0223] In order to further increase the battery capacity, the mass ratio may be higher than 90%.
[0224] The positive electrode active material in Embodiment 1 may contain not only the above-mentioned lithium composite oxide but also inevitable impurities.
[0225] The positive electrode active material in Embodiment 1 may include its starting material as an unreacted material. The positive electrode active material in Embodiment 1 may include a by-product generated during the synthesis of the lithium composite oxide. The positive electrode active material in Embodiment 1 may include a decomposition product generated by the decomposition of the lithium composite oxide.
[0226] The lithium composite oxide contained in the positive electrode active material in the first embodiment may be composed only of the above-mentioned lithium composite oxide except for inevitable impurities.
[0227] Such positive electrode active materials further improve battery capacity and cycle characteristics.
[0228] <Method for producing lithium composite oxide>
[0229] Hereinafter, an example of a method for producing the lithium composite oxide contained in the positive electrode active material of the first embodiment will be described.
[0230] The lithium composite oxide can be produced, for example, by the following method.
[0231] A raw material containing Li, a raw material containing Me, and a raw material containing Q are prepared.
[0232] Examples of the raw material containing Li include lithium oxides such as Li 2 O and Li 2 O 2 , lithium salts such as LiF, Li 2 CO 3 and LiOH, and lithium composite oxides such as LiMeO 2 and LiMe 2 O 4 .
[0233] Examples of the raw material containing Me include metal oxides such as Me2O3, metal salts such as MeCO3 and Me(NO3)2, metal hydroxides such as Me(OH)2 and MeOOH, and lithium composite oxides such as LiMeO2 and LiMe2O4.
[0234] For example, when Me is Mn, the raw material containing Mn may include manganese oxides such as MnO2 and Mn2O3, manganese salts such as MnCO3 and Mn(NO3)2, manganese hydroxides such as Mn(OH)2 and MnOOH, or lithium manganese composite oxides such as LiMnO2 and LiMn2O4.
[0235] Examples of the raw material containing Q include lithium halide, transition metal halide, transition metal sulfide, and transition metal nitride.
[0236] When Q is F, examples of the raw material containing F include LiF and transition metal fluorides.
[0237] For example, these raw materials are prepared in such a way that the molar ratio of Li to the transition metal is in the range of 0.5 to 2.0. The prepared raw materials are mixed by, for example, a dry method or a wet method, and then mechanochemically ground for more than 30 hours in a mixing device such as a planetary ball mill to react with each other, thereby obtaining a first precursor of a lithium composite oxide.
[0238] Separately, a raw material containing Li, a raw material containing Me, and a raw material containing Q are prepared in a manner having a molar ratio different from that of the first precursor. The prepared raw materials are mixed by a dry method or a wet method, and then subjected to mechanochemical grinding for more than 30 hours in a mixing device such as a planetary ball mill to react, thereby obtaining a second precursor having a composition ratio different from that of the first precursor.
[0239] In addition, the first precursor and the second precursor are prepared in a molar ratio as shown in the composition formula (2). The prepared first precursor and the second precursor are mixed by a dry method or a wet method, and then subjected to mechanochemical grinding for more than 1 hour in a mixing device such as a planetary ball mill to react, thereby obtaining a final precursor.
[0240] The method for obtaining the final precursor is not limited to the above-mentioned preparation method. For example, the method may further include a step of obtaining a third precursor having a molar ratio different from that of the first precursor and the second precursor. In this case, the first precursor, the second precursor, and the third precursor prepared in a molar ratio shown in the composition formula (2) are mixed by a dry method or a wet method, and then mechanically chemically ground in a mixing device such as a planetary ball mill for more than 1 hour to react, thereby obtaining the final precursor.
[0241] In this way, the values of x, y, α and β can be changed within the range shown in the composition formula (2).
[0242] The obtained final precursor is subjected to heat treatment. The conditions of the heat treatment are appropriately set so as to obtain the lithium composite oxide in Embodiment 1. The optimal conditions of the heat treatment vary depending on other production conditions and the target composition.
[0243] The temperature and time of the heat treatment can be selected from, for example, the range of 200 to 900° C. and the range of 1 minute to 20 hours, respectively. Examples of the heat treatment atmosphere are air atmosphere, oxygen atmosphere, or inert atmosphere (eg, nitrogen atmosphere or argon atmosphere).
[0244] The inventors have found that the lower the heat treatment temperature or the shorter the heat treatment time, the higher the integrated intensity ratio I (18°-20°) / I (43°-46°) The manufacturer can use this tendency as a guide to determine the heat treatment conditions.
[0245] As described above, the lithium composite oxide can be obtained in Embodiment 1 by adjusting the raw materials, the mixing conditions of the raw materials, and the heat treatment conditions.
[0246] The space group of the crystal structure of the obtained lithium composite oxide can be determined by, for example, X-ray diffraction measurement or electron beam diffraction measurement. Thus, it can be confirmed that the obtained lithium composite oxide includes, for example, a first phase having a crystal structure belonging to a monoclinic crystal, a second phase having a crystal structure belonging to a hexagonal crystal, and a third phase having a crystal structure belonging to a cubic crystal.
[0247] The average composition of the obtained lithium composite oxide can be determined by using, for example, ICP emission spectrometry, inert gas fusion-infrared absorption, ion chromatography, or a combination of these analysis methods.
[0248] By using a lithium transition metal composite oxide as a raw material, the energy of element mixing can be reduced. Thus, in the first embodiment, the purity of the lithium composite oxide can be increased.
[0249] As described above, in the first embodiment, the method for producing a lithium composite oxide includes the step (a) of preparing raw materials, the step (b) of subjecting the raw materials to a mechanochemical milling reaction to obtain a precursor of the lithium composite oxide, and the step (c) of obtaining the lithium composite oxide by heat treating the precursor.
[0250] The raw material may be a mixed raw material, and in the mixed raw material, the ratio of Li to Me may be 1.4 or more and 2.0 or less.
[0251] The lithium compound used as a raw material can be produced by a known method.
[0252] In the above step (b), the operation of reacting the raw materials by mechanochemical grinding using a ball mill may be repeated two or three times.
[0253] As described above, in Embodiment 1, to obtain a lithium composite oxide, raw materials (such as LiF, Li2O, transition metal oxide or lithium composite transition metal) may be mixed by a mechanochemical milling reaction using a planetary ball mill to obtain a precursor, and then the obtained precursor may be heat treated.
[0254] An example of a method for coating the surface of a lithium composite oxide with a coating material is described below.
[0255] The method for coating the lithium composite oxide obtained as described above with a coating material is not limited, and the method may include atomic layer deposition, neutralization reaction, silane coupling reaction, sol-gel method or planetary ball milling.
[0256] An example of a coating material is a metal oxide. In the method of coating a lithium composite oxide with a metal oxide, a neutralization reaction can be used. For example, a salt of an acidic metal oxide can be added to an alkaline aqueous solution in which the lithium composite oxide is dissolved. A neutralization reaction occurs by the addition, and a metal oxide film can be formed on the surface of the lithium composite oxide. Examples of salts of acidic metal oxides are, for example, manganese nitrate, magnesium nitrate, aluminum sulfate, calcium nitrate, sodium nitrate, potassium nitrate, and titanium sulfate.
[0257] As a method for coating the lithium composite oxide with a coating material, for example, an atomic layer deposition method can be used. In this way, the surface of the lithium composite oxide can be coated with the coating material. Examples of the coating material are aluminum oxide, titanium oxide, zirconium oxide, zinc oxide, and tantalum oxide.
[0258] The positive electrode active material in Embodiment 1 includes a lithium composite oxide and a coating material (specifically, the surface of the lithium composite oxide is coated with the coating material), and can be observed using, for example, X-ray electron spectroscopy, a scanning electron microscope, or a transmission electron microscope.
[0259] (Implementation Method 2)
[0260] Hereinafter, Embodiment 2 will be described. Matters described in Embodiment 1 may be omitted as appropriate.
[0261] The battery in the second embodiment includes a positive electrode, a negative electrode, and an electrolyte, and the positive electrode includes the positive electrode active material in the first embodiment.
[0262] The battery in Embodiment 2 has high capacity and high cycle characteristics.
[0263] In the battery in Embodiment 2, the positive electrode may include a positive electrode active material layer. The positive electrode active material layer may contain the positive electrode active material in Embodiment 1 as a main component. That is, the mass ratio of the positive electrode active material to the entire positive electrode active material layer is 50% or more.
[0264] Such a positive electrode active material layer further improves the battery capacity and cycle characteristics.
[0265] The mass ratio may be 70% or more.
[0266] Such a positive electrode active material layer further improves the battery capacity and cycle characteristics.
[0267] The mass ratio may be 90% or more.
[0268] Such a positive electrode active material layer further improves the battery capacity and cycle characteristics.
[0269] The battery in Embodiment 2 is, for example, a lithium ion secondary battery, a nonaqueous electrolyte secondary battery, or an all-solid battery.
[0270] In the battery of Embodiment 2, the negative electrode may contain a negative electrode active material capable of absorbing and releasing lithium ions. Alternatively, the negative electrode may contain a material from which lithium metal dissolves into the electrolyte during discharge and into which the lithium metal precipitates during charge.
[0271] In the battery in Embodiment 2, the electrolyte may be a non-aqueous electrolyte (eg, a non-aqueous electrolytic solution).
[0272] In the battery in Embodiment 2, the electrolyte may be a solid electrolyte.
[0273] Figure 1 A cross-sectional view of a battery 10 in Embodiment 2 is shown.
[0274] like Figure 1 As shown, the battery 10 includes a positive electrode 21 , a negative electrode 22 , a separator 14 , a case 11 , a sealing plate 15 , and a gasket 18 .
[0275] The separator 14 is disposed between the positive electrode 21 and the negative electrode 22 .
[0276] The positive electrode 21 , the negative electrode 22 , and the separator 14 are impregnated with, for example, a nonaqueous electrolyte (eg, a nonaqueous electrolytic solution).
[0277] The positive electrode 21 , the negative electrode 22 , and the separator 14 form an electrode group.
[0278] The electrode group is housed in the case 11 .
[0279] The housing 11 is sealed by a sealing gasket 18 and a sealing plate 15 .
[0280] The positive electrode 21 includes a positive electrode current collector 12 and a positive electrode active material layer 13 disposed on the positive electrode current collector 12 .
[0281] The positive electrode current collector 12 is made of, for example, a metal material (for example, at least one selected from aluminum, stainless steel, nickel, iron, titanium, copper, palladium, gold, and platinum) or an alloy thereof.
[0282] There is a case where the positive electrode current collector 12 is not provided. In this case, the case 11 is used as the positive electrode current collector.
[0283] The positive electrode active material layer 13 contains the positive electrode active material in the first embodiment.
[0284] The positive electrode active material layer 13 may contain additives (conductive agent, ion conductive auxiliary agent or binder) as necessary.
[0285] The negative electrode 22 includes a negative electrode current collector 16 and a negative electrode active material layer 17 disposed on the negative electrode current collector 16 .
[0286] The negative electrode current collector 16 is made of, for example, a metal material (for example, at least one selected from aluminum, stainless steel, nickel, iron, titanium, copper, palladium, gold, and platinum) or an alloy thereof.
[0287] The negative electrode current collector 16 may not be provided. In this case, the sealing plate 15 is used as the negative electrode current collector.
[0288] The negative electrode active material layer 17 contains a negative electrode active material.
[0289] The negative electrode active material layer 17 may contain additives (conductive agent, ion conductive auxiliary agent or binder) as necessary.
[0290] Examples of the negative electrode active material are metal materials, carbon materials, oxides, nitrides, tin compounds, and silicon compounds.
[0291] The metal material may be a single metal. Alternatively, the metal material may be an alloy. Examples of the metal material include lithium metal and lithium alloys.
[0292] Examples of the carbon material include natural graphite, coke, partially graphitized carbon, carbon fiber, spherical carbon, artificial graphite, and amorphous carbon.
[0293] From the viewpoint of capacity density, as the negative electrode active material, silicon (i.e., Si), tin (i.e., Sn), a silicon compound, or a tin compound can be used. The silicon compound and the tin compound can be an alloy or a solid solution.
[0294] Examples of the silicon compound include SiO x (where 0.05 < x < 1.95). A compound obtained by substituting a part of the silicon atoms of SiO x with other elements can also be used. The compound is an alloy or a solid solution. The other elements are at least one element selected from boron, magnesium, nickel, titanium, molybdenum, cobalt, calcium, chromium, copper, iron, manganese, niobium, tantalum, vanadium, tungsten, zinc, carbon, nitrogen, and tin.
[0295] Examples of the tin compound include Ni2Sn4, Mg2Sn, SnO x (where 0 < x < 2), SnO2, and SnSiO3. One kind of tin compound selected therefrom can be used alone. Alternatively, a combination of two or more tin compounds selected therefrom can be used.
[0296] The shape of the negative electrode active material is not limited. As the negative electrode active material, a negative electrode active material having a known shape (e.g., granular or fibrous) can be used.
[0297] The method for allowing lithium to be occluded (i.e., absorbed) in the negative electrode active material layer 17 is not limited. Specifically, examples of the method are (a) a method of depositing lithium on the negative electrode active material layer 17 by a vapor phase method such as a vacuum evaporation method, or (b) a method of bringing a lithium metal foil into contact with the negative electrode active material layer 17 and heating the two. In any method, lithium diffuses into the negative electrode active material layer 17 due to heat. A method of electrochemically occluding lithium into the negative electrode active material layer 17 can also be used. Specifically, a battery is assembled using a negative electrode 22 that does not have lithium and a lithium metal foil (negative electrode). Thereafter, the battery is charged to occlude lithium in the negative electrode 22.
[0298] Examples of the binder for the positive electrode 21 and the negative electrode 22 are polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aromatic polyamide resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, methyl polyacrylate, ethyl polyacrylate, hexyl polyacrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyhexyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, polyhexafluoropropylene, styrene-butadiene rubber, and carboxymethyl cellulose.
[0299] Other examples of binders are copolymers of two or more materials selected from tetrafluoroethylene, hexafluoroethane, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. A mixture of two or more binders selected from the above materials can be used.
[0300] Examples of the conductive agent of the positive electrode 21 and the negative electrode 22 are graphite, carbon black, conductive fiber, graphite fluoride, metal powder, conductive whisker, conductive metal oxide, and organic conductive material.
[0301] Examples of graphite include natural graphite and artificial graphite.
[0302] Examples of carbon black include acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black.
[0303] An example of the metal powder is aluminum powder.
[0304] Examples of the conductive whiskers include zinc oxide whiskers and potassium titanate whiskers.
[0305] An example of the conductive metal oxide is titanium oxide.
[0306] Examples of organic conductive materials include phenylene derivatives.
[0307] A conductive agent may be used to coat at least a portion of the surface of the binder. For example, the surface of the binder may be coated with carbon black. This can increase the battery capacity.
[0308] The material of the partition 14 is a material having a large ion permeability and sufficient mechanical strength. Examples of the material of the partition 14 include microporous films, woven fabrics and non-woven fabrics. Specifically, the partition 14 is preferably made of a polyolefin such as polypropylene or polyethylene. The partition 14 made of polyolefin not only has excellent durability, but also can perform a shutdown function when overheated. The thickness of the partition 14 is in the range of, for example, 10 to 300 μm (or 10 to 40 μm). The partition 14 can be a single-layer film composed of one material. Alternatively, the partition 14 can be a composite film (or a multilayer film) composed of two or more materials. The porosity of the partition 14 is in the range of, for example, 30 to 70% (or 35 to 60%). The term "porosity" refers to the proportion of the volume of pores in the total volume of the partition 14. The porosity is measured by, for example, mercury intrusion.
[0309] The nonaqueous electrolyte contains a nonaqueous solvent and a lithium salt dissolved in the nonaqueous solvent.
[0310] Examples of the nonaqueous solvent are cyclic carbonate solvents, chain carbonate solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents, and fluorine solvents.
[0311] Examples of the cyclic carbonate solvents are ethylene carbonate, propylene carbonate, and butylene carbonate.
[0312] Examples of the chain carbonate solvent are dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
[0313] Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dihydrofuran, Alkanes and 1,3-dioxolane.
[0314] As examples of the chain ether solvent, there are 1,2-dimethoxyethane and 1,2-diethoxyethane.
[0315] An example of a cyclic ester solvent is gamma-butyrolactone.
[0316] An example of the chain ester solvent is methyl acetate.
[0317] As examples of the fluorine solvent, there are fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate and fluorodimethyl carbonate.
[0318] As the non-aqueous solvent, one non-aqueous solvent selected from these may be used alone, or two or more non-aqueous solvents selected from these may be used in combination.
[0319] The non-aqueous electrolyte may contain at least one fluorine solvent selected from the group consisting of fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, ethyl fluoromethyl carbonate, and dimethyl fluorocarbonate.
[0320] When the non-aqueous electrolyte contains the at least one fluorinated solvent, the oxidation resistance of the non-aqueous electrolyte is improved.
[0321] As a result, even when the battery 10 is charged at a high voltage, the battery 10 can be operated stably.
[0322] In the battery of Embodiment 2, the electrolyte may be a solid electrolyte.
[0323] Examples of the solid electrolyte are organic polymer solid electrolytes, oxide solid electrolytes, and sulfide solid electrolytes.
[0324] An example of an organic polymer solid electrolyte is a compound of a polymer compound and a lithium salt. An example of such a compound is lithium polystyrene sulfonate.
[0325] The polymer compound may have an ethylene oxide structure. When the polymer compound has an ethylene oxide structure, a large amount of lithium salt can be contained. As a result, the ion conductivity can be further improved.
[0326] Examples of oxide solid electrolytes are:
[0327] (i) NASICON solid electrolytes such as LiTi2(PO4)3 or its substitutes,
[0328] (ii) Perovskite solid electrolytes such as (LaLi)TiO3,
[0329] (iii)Li 14 ZnGe4O 16 , LISICON solid electrolytes such as Li4SiO4, LiGeO4 or their substitutes,
[0330] (iv)Li7La3Zr2O 12 Garnet solid electrolytes such as garnet or its substitutes,
[0331] (v) Li3N or its H-substituted product, or
[0332] (vi) Li3PO4 or its N-substituted form.
[0333] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4 and Li 10 GeP2S 12 LiX (X is F, Cl, Br or I), MO y or Li x MO y (M is any of P, Si, Ge, B, Al, Ga, and In, and x and y are respectively independent natural numbers).
[0334] Among them, sulfide solid electrolytes are excellent in formability and have high ion conductivity. Therefore, by using a sulfide solid electrolyte as a solid electrolyte, the energy density of the battery can be further improved.
[0335] Among sulfide solid electrolytes, Li2S-P2S5 has high electrochemical stability and high ion conductivity. Therefore, if Li2S-P2S5 is used as a solid electrolyte, the energy density of the battery can be further improved.
[0336] The solid electrolyte layer contained in the solid electrolyte may further contain the above-mentioned nonaqueous electrolyte solution.
[0337] Since the solid electrolyte layer contains a non-aqueous electrolyte, lithium ions can easily move between the active material and the solid electrolyte, thereby further improving the energy density of the battery.
[0338] The solid electrolyte layer may contain a gel electrolyte or an ionic liquid.
[0339] Examples of gel electrolytes are polymer materials impregnated with a non-aqueous electrolyte. Examples of polymer materials are polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate. Other examples of polymer materials are polymers having ethylene oxide bonds.
[0340] Examples of cations contained in ionic liquids are:
[0341] (i) cations of aliphatic chain quaternary ammonium salts such as tetraalkylammonium,
[0342] (ii) Tetraalkyl That kind of aliphatic chain The cation of the salt,
[0343] (iii) Pyrrolidine Morpholine Imidazolin Tetrahydropyrimidine Piperazine or piperidine Such aliphatic cyclic ammonium, or
[0344] (iv) Pyridine or imidazole Such nitrogen-containing heterocyclic aromatic cations.
[0345] The anion that makes up the ionic liquid is PF6 - 、BF4 - 、SbF6 - 、AsF6 - 、SO3CF3 - 、N(SO2CF3)2 - 、N(SO2C2F5)2 - 、N(SO2CF3)(SO2C4F9) - or C(SO2CF3)3 - The ionic liquid may contain a lithium salt.
[0346] Examples of lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3. As the lithium salt, one lithium salt selected from these may be used alone. Alternatively, as the lithium salt, a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 to 2 mol / liter.
[0347] Regarding the battery shape in Embodiment 2, the battery is a coin-type battery, a cylindrical battery, a square battery, a sheet battery, a button-type battery (ie, a button-type unit cell), a flat battery, or a laminated battery.
[0348] (Example)
[0349] <Example 1>
[0350] [Preparation of positive electrode active material]
[0351] A mixture of LiF, LiMnO2, LiCoO2 and LiNiO2 was obtained in a Li / Mn / Co / Ni / O / F molar ratio of 1.25 / 0.56 / 0.12 / 0.12 / 1.9 / 0.1.
[0352] The mixture was placed in a 45 ml container together with an appropriate amount of zirconia balls having a diameter of 3 mm, and the container was sealed in an argon glove box. The container was made of zirconia.
[0353] Next, the container was taken out from the argon glove box, and the mixture contained in the container was processed in an argon atmosphere at 600 rpm for 30 hours using a planetary ball mill to prepare a first precursor.
[0354] The obtained first precursor was subjected to powder X-ray diffraction measurement. As a result, the space group of the first precursor was determined to be Fm-3m.
[0355] On the other hand, a mixture of LiF, LiMnO2, MnO2 and NiO was obtained in a Li / Mn / Ni / O / F molar ratio of 1.0 / 1.5 / 0.5 / 3.8 / 0.2.
[0356] The mixture and an appropriate amount of zirconia balls with a diameter of 3 mm were placed in a 45 ml container, and the container was sealed in an argon glove box. The container was made of zirconia.
[0357] Next, the container was taken out from the argon glove box, and the mixture contained in the container was processed at 600 rpm for 5 hours using a planetary ball mill under an argon atmosphere to prepare a second precursor.
[0358] The obtained second precursor was subjected to powder X-ray diffraction measurement. As a result, the space group of the second precursor was determined to be Fm-3m.
[0359] The third precursor was obtained as follows: A mixture of LiF, LiMnO2, LiCoO2 and LiNiO2 was obtained in a Li / Mn / Co / Ni / O / F molar ratio of 1.0 / 0.15 / 0.5 / 0.35 / 1.9 / 0.1.
[0360] The mixture and an appropriate amount of zirconia balls with a diameter of 3 mm were placed in a 45 ml container, and the container was sealed in an argon glove box. The container was made of zirconia.
[0361] Next, the container was taken out from the argon glove box, and the mixture contained in the container was processed in an argon atmosphere at 600 rpm using a planetary ball mill for 5 hours to prepare a third precursor.
[0362] The obtained third precursor was subjected to powder X-ray diffraction measurement. As a result, the space group of the obtained third precursor was determined to be Fm-3m.
[0363] Next, a mixture of the first precursor, the second precursor, and the third precursor was obtained in such a manner that the molar ratio of Li / Mn / Co / Ni / O / F was 1.2 / 0.54 / 0.13 / 0.13 / 1.9 / 0.1.
[0364] The mixture and an appropriate amount of zirconia balls with a diameter of 3 mm were placed in a 45 ml container, and the container was sealed in an argon glove box. The container was made of zirconia.
[0365] Next, the container was taken out from the argon glove box, and the mixture contained in the container was processed in an argon atmosphere at 450 rpm using a planetary ball mill for 5 hours to prepare a final precursor.
[0366] The final precursor was heat-treated in an air atmosphere at 700° C. for 1 hour. In this way, a lithium composite oxide was obtained.
[0367] The lithium composite oxide was subjected to powder X-ray diffraction measurement.
[0368] The results of powder X-ray diffraction measurements are shown in Figure 2 .
[0369] The lithium composite oxide was also subjected to electron diffraction measurement. Based on the results of the powder X-ray diffraction measurement and the electron diffraction measurement, the crystal structure of the lithium composite oxide was analyzed.
[0370] As a result, it was determined that the lithium composite oxide was a multiphase mixture including a phase belonging to the space group C2 / m, a phase belonging to the space group R-3m, and a phase belonging to the space group Fm-3m.
[0371] Based on the results of powder X-ray diffraction measurement obtained using an X-ray diffractometer (manufactured by Rigaku Corporation), the integrated intensity of the X-ray diffraction peak was calculated using software (trade name: PDXL) attached to the X-ray diffractometer. The integrated intensity ratio I in the lithium composite oxide (18°-20°) / I (43°-46°) It is 0.91.
[0372] Next, the surface of the lithium composite oxide was treated by atomic layer deposition. In the surface treatment, trimethylaluminum and water (i.e., water vapor) were alternately stacked in a vacuum atmosphere at 120 degrees Celsius, thereby forming a film of aluminum oxide (i.e., Al2O3) on the surface of the lithium composite oxide. In this way, the positive electrode active material in Example 1 was obtained.
[0373] X-ray photoelectric spectroscopy was performed on the positive electrode active material in Example 1. The results of the X-ray photoelectric spectroscopy confirmed the presence of Al2O3 on the surface of the lithium composite oxide. The thickness of the Al2O3 film was 5 nanometers.
[0374] In the X-ray photoelectric spectroscopy, almost no peak related to the Al2O3 film was confirmed. The reason for this is believed to be that the Al2O3 film is thin and in an amorphous state.
[0375] [Battery production]
[0376] Next, 70 parts by mass of the positive electrode active material in Example 1, 20 parts by mass of acetylene black, 10 parts by mass of polyvinylidene fluoride (hereinafter referred to as "PVDF") and an appropriate amount of N-methyl-2-pyrrolidone (hereinafter referred to as "NMP") were mixed. Thus, a positive electrode mixture slurry was obtained. Acetylene black acts as a conductive agent. Polyvinylidene fluoride acts as a binder.
[0377] The positive electrode mixture slurry was applied on one side of a positive electrode current collector formed of an aluminum foil having a thickness of 20 μm.
[0378] The positive electrode mixture slurry was dried and rolled to obtain a positive electrode plate having a positive electrode active material layer with a thickness of 60 micrometers.
[0379] The present inventors have confirmed that the effect of improving the cycle characteristics can be obtained by obtaining a positive electrode plate using a positive electrode active material without an Al2O3 coating and then forming an Al2O3 coating on the entire positive electrode active material layer using the above-mentioned atomic deposition method.
[0380] The obtained positive electrode plate was punched to obtain a circular positive electrode having a diameter of 12.5 mm.
[0381] A circular negative electrode with a diameter of 14 mm was obtained by punching a lithium metal foil with a thickness of 300 μm.
[0382] Separately, fluoroethylene carbonate (hereinafter referred to as "FEC"), ethylene carbonate (hereinafter referred to as "EC"), and ethyl methyl carbonate (hereinafter referred to as "EMC") were mixed at a volume ratio of 1:1:6 to obtain a nonaqueous solvent.
[0383] LiPF6 was dissolved in the non-aqueous solvent at a concentration of 1.0 mol / liter, thereby obtaining a non-aqueous electrolyte solution.
[0384] The obtained non-aqueous electrolyte was allowed to infiltrate the separator. The separator was a product of Celgard (No. 2320, thickness 25 μm). The separator was a three-layer separator consisting of a polypropylene layer, a polyethylene layer and a polypropylene layer.
[0385] Using the above-mentioned positive electrode, negative electrode and separator, a coin-type battery having a diameter of 20 mm and a thickness of 3.2 mm was produced in a drying oven maintained at a dew point of -50°C.
[0386] <Example 2>
[0387] In Example 2, a positive electrode active material and a coin-type battery using the positive electrode active material were obtained in the same manner as in Example 1 except for the following item (i).
[0388] (i) The thickness of the Al2O3 film is 10 nm instead of 5 nm.
[0389] <Examples 3 to 5>
[0390] In Examples 3 to 5, a positive electrode active material and a coin-type battery using the positive electrode active material were obtained in the same manner as in Example 1 except for the following item (i).
[0391] (i) In Examples 3, 4 and 5, the materials of the coating material are MgO, SiO2 and ZrO2, respectively.
[0392] <Examples 6 to 14>
[0393] In Examples 6 to 14, positive electrode active materials and coin-type batteries using the positive electrode active materials were prepared in the same manner as in Example 1 except for the following matters (i) and (ii).
[0394] (i) Changing the preparation conditions and mixing ratio of each precursor.
[0395] (ii) The heating conditions were changed within the range of 500 to 900° C. and 10 minutes to 5 hours.
[0396] Table 1 shows the average composition of the lithium composite oxides of Examples 6 to 14.
[0397] It was confirmed that each of the lithium composite oxides of Examples 6 to 14 was a multiphase mixture including a first phase belonging to the space group C2 / m, a second phase belonging to the space group R-3m, and a third phase belonging to the space group Fd-3m or Fm-3m.
[0398] <Comparative Example 1>
[0399] In Comparative Example 1, a positive electrode active material having a composition represented by the chemical formula LiCoO 2 (ie, lithium cobalt oxide) was obtained by a known method.
[0400] Unlike Example 1, in Comparative Example 1, no Al 2 O 3 film was formed.
[0401] The obtained positive electrode active material was subjected to powder X-ray diffraction measurement.
[0402] The results of powder X-ray diffraction measurements are shown in Figure 2 .
[0403] The results of powder X-ray diffraction analysis revealed that the space group of the obtained positive electrode active material was R-3m.
[0404] The integrated intensity ratio I in the positive electrode active material in Comparative Example 1 (18°-20°) / I (43°-46°) is 1.27.
[0405] A coin-type battery of Comparative Example 1 was produced in the same manner as in Example 1 using the positive electrode active material of Comparative Example 1.
[0406] <Reference Example 1>
[0407] In Reference Example 1, a positive electrode active material and a coin-type battery using the positive electrode active material were prepared in the same manner as in Example 1 except that no Al 2 O 3 film was formed.
[0408] <Battery Evaluation>
[0409] At 0.5 mA / cm 2 The batteries of Examples 1 to 14 and Reference Example 1 were charged at a current density of until the voltage reached 4.7V.
[0410] Then, at 0.5 mA / cm 2 The batteries of Examples 1 to 14 and Reference Example 1 were discharged at a current density of 2.5 V until the voltage reached 2.5 V.
[0411] At 0.5 mA / cm 2 The battery of Comparative Example 1 was charged at a current density of until the voltage reached 4.3 V.
[0412] Then, at 0.5 mA / cm 2The battery of Comparative Example 1 was discharged at a current density of 2.5 V until the voltage reached 2.5 V.
[0413] Furthermore, the above-mentioned charge and discharge test was repeated 20 times (ie, 20 cycles), and then the battery capacity retention rates of Examples 1 to 14, Comparative Example 1, and Reference Example 1 were measured.
[0414] Figure 3 It is a graph showing the charge and discharge cycle test results of the batteries of Examples 1 and 2 and Reference Example 1.
[0415] The initial discharge capacities of the batteries of Example 1, Example 2 and Reference Example 1 were 280 mAh / g, 276 mAh / g and 282 mAh / g, respectively.
[0416] The capacity retention rates of the batteries of Example 1 and Example 21 after 20 cycles were 96.4% and 97.2%, respectively.
[0417] On the other hand, the initial discharge capacity of the battery of Comparative Example 1 was 150 mAh / g, the capacity retention rate of the battery of Comparative Example 1 after 20 cycles was 80.0%, and the capacity retention rate of the battery of Reference Example 1 after 20 cycles was 86.8%.
[0418] In Tables 1 to 3, the results of Examples 1 to 14, Comparative Example 1, and Reference Example 1 are shown in Table 1.
[0419] Table 1
[0420]
[0421] Table 2
[0422]
[0423] Table 3
[0424]
[0425] As shown in Tables 1 to 3, in the batteries of Examples 1 to 14 and Reference Example 1, the initial discharge capacity was 260 to 282 mAh / g.
[0426] That is, the initial discharge capacity of the batteries of Examples 1 to 14 and Reference Example 1 is much greater than the initial discharge capacity of the battery of Comparative Example 1.
[0427] The reason for this is that the lithium composite oxide contained in the positive electrode active material of the batteries of Examples 1 to 14 and Reference Example 1 is a multiphase mixture including a first phase, a second phase, and a third phase, wherein the first phase has a monoclinic crystal structure, the second phase has a hexagonal crystal structure, and the third phase has a cubic crystal structure, and the integrated intensity ratio I (18°-20°) / I (43°-46°) It is 0.05 or more and 0.99 or less. Therefore, it is believed that a lot of Li can be inserted and removed, and the Li diffusibility and stability of the crystal structure are high. Therefore, it is believed that the initial discharge capacity is significantly improved.
[0428] In Comparative Example 1, the integrated intensity ratio I (18°-20°) / I (43°-46°) Greater than 0.99. Moreover, in Comparative Example 1, the crystal structure is a single phase of space group R-3m. Therefore, it is believed that the amount of Li inserted and removed during charge and discharge and the stability of the crystal structure are reduced. The x / y value is a relatively small value such as 1. Therefore, it is believed that the amount of Li that can participate in the reaction is reduced, and the diffusivity of Li ions is reduced. Therefore, it is believed that the initial discharge capacity is significantly reduced.
[0429] As shown in Tables 1 to 3, the initial discharge capacity of the batteries of Examples 6 and 7 is smaller than the initial discharge capacity of the battery of Example 1.
[0430] The reason for this is that the integrated intensity ratio I (18°-20°) / I (43°-46°) It is smaller than that in Example 1. Therefore, it is considered that the amount of cation mixing increases, thereby reducing the Li diffusivity during charge and discharge. Therefore, it is considered that the initial discharge capacity decreases.
[0431] As shown in Tables 1 to 3, the initial discharge capacity of the batteries of Examples 8 and 9 is smaller than the initial discharge capacity of the battery of Example 1.
[0432] The reason for this is that in Examples 8 and 9, the x / y value was 1.4, which was smaller than that in Example 1. Therefore, the amount of Li that could participate in charge and discharge was reduced. Therefore, the initial discharge capacity was reduced.
[0433] As shown in Tables 1 to 3, the initial discharge capacity of the battery of Example 10 is smaller than the initial discharge capacity of the battery of Example 1.
[0434] The reason for this is that the F content in Example 10 is greater than that in Example 1 (i.e., α / β=9). Therefore, it is believed that the electron conductivity is reduced compared with Example 1. In addition, it is believed that the diffusivity of Li bonded to F in the crystal structure may be reduced. Therefore, it is believed that the initial discharge capacity is reduced.
[0435] As shown in Tables 1 to 3, the initial discharge capacity of the batteries of Examples 11 and 12 is smaller than the initial discharge capacity of the battery of Example 1.
[0436] The reason for this is that the contents of Co and Ni in Examples 11 and 12 are smaller than those in Example 1. Therefore, the crystal structure is considered to be unstable. Therefore, the initial discharge capacity is considered to be reduced.
[0437] As shown in Tables 1 to 3, the initial discharge capacity of the batteries of Examples 13 and 14 is smaller than the initial discharge capacity of the battery of Example 1.
[0438] As a reason for this, it is believed that in Example 13 and Example 14, the x / y value is a large value of 2.0 compared to Example 1. Therefore, it is believed that the crystal structure after Li is separated is unstable. It is believed that the F content in Example 13 and Example 14 is greater than that in Example 1 (that is, α / β=2). Therefore, it is believed that the electronic conductivity decreases. Moreover, it is believed that the diffusivity of Li combined with F in the crystal structure may decrease. Therefore, it is believed that the initial discharge capacity decreases.
[0439] As shown in Tables 1 to 3, the capacity retention rates of the batteries of Examples 1 to 14 after 20 cycles are higher than the capacity retention rates of the batteries of Comparative Example 1 and Reference Example 1 after 20 cycles.
[0440] As a reason for this, it is believed that in the batteries of Examples 1 to 14, the surface of the lithium composite oxide contains a coating material. That is, it is believed that the direct contact between the surface of the lithium composite oxide and the electrolyte is suppressed by the coating material. As a result, it is believed that, for example, the generation of gas associated with the side reaction between the lithium composite oxide and the electrolyte, the detachment of oxygen, and the generation of side reaction products on the surface of the positive electrode active material are suppressed. Therefore, it is believed that the capacity retention rate after 20 cycles is improved.
[0441] As shown in Tables 1 to 3, the battery of Example 2 has a lower initial discharge capacity and a higher capacity retention rate after 20 cycles than the battery of Example 1.
[0442] The reason for this is that the thickness of Al2O3, which functions as a coating material, is larger in the battery of Example 2 than in the battery of Example 1. This is believed to suppress the side reaction between the lithium composite oxide and the electrolyte, but on the other hand, the resistance related to Li conduction increases.
[0443] As shown in Tables 1 to 3, the capacity retention rate of the batteries of Example 1 and Examples 3 to 5 after 20 cycles is higher than the capacity retention rate of the battery of Reference Example 1 after 20 cycles. In the batteries of Example 1 and Examples 3 to 5, the coating materials are Al2O3, MgO, SiO2, and ZrO2, respectively. It can be seen that in the present disclosure, the material of the coating material is not limited to Al2O3, and various oxides can be used as the material of the coating material. In order to achieve a battery with higher capacity and high cycle characteristics, Al2O3 is suitable as the coating material used in the present disclosure.
[0444] Industrial Applicability
[0445] The positive electrode active material disclosed herein can be used in batteries such as secondary batteries.
Claims
1. A positive electrode active material comprising a lithium composite oxide and a coating material coating the surface of the lithium composite oxide, in, The lithium composite oxide is a multiphase mixture including a first phase, a second phase and a third phase, The first phase has a crystal structure belonging to a monoclinic crystal, the second phase has a crystal structure belonging to a hexagonal crystal, and the third phase has a crystal structure belonging to a cubic crystal, And the lithium composite oxide satisfies the following mathematical formula (I): 0.05≤Integral intensity ratio I (18°-20°) / I (43°-46°) ≤0.99(I) in, Integrated intensity ratio I (18°-20°) / I (43°-46°) Equal to the integrated intensity I (18°-20°) Relative to the integrated intensity I (43°-46°) The ratio, Integral Intensity I (43°-46°) is the integrated intensity of the first peak, which is the largest peak existing in the diffraction angle 2θ range of 43° to 46° in the X-ray diffraction pattern of the lithium composite oxide, and Integral Intensity I (18°-20°) is the integrated intensity of the second peak, which is the largest peak existing in the diffraction angle 2θ range of 18° to 20° in the X-ray diffraction pattern of the lithium composite oxide, and The electronic conductivity of the coating material is 10 6 S / m or less, The average composition of the lithium composite oxide is represented by the composition formula Li x Me y O α Q β express, in, Me is at least one selected from the group consisting of Mn, Co, Ni, Fe, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si, P, and Al, Q is at least one selected from F, Cl, N and S, 1.05≤x≤1.5, 0.6≤y≤1.0, 1.2≤α≤2.0, and 0≤β≤0.8。 2. The positive electrode active material according to claim 1, The coating material is an inorganic material.
3. The positive electrode active material according to claim 1 or 2, The mass ratio of the coating material to the lithium composite oxide is 0.2 or less.
4. The positive electrode active material according to claim 3, The mass ratio of the coating material to the lithium composite oxide is 0.01 to 0.
1.
5. The positive electrode active material according to claim 1 or 2, The coating material has a thickness of 0.1 nanometers or more and 10.0 nanometers or less.
6. The positive electrode active material according to claim 1 or 2, The coating material forms a solid solution with at least a portion of the surface of the lithium composite oxide.
7. The positive electrode active material according to claim 1 or 2, The coating material is formed of an oxide or an oxynitride.
8. The positive electrode active material according to claim 7, The coating material has a composition formula of Li a A b O c N d express, in, A is at least one selected from the group consisting of Mn, Co, Ni, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Si, Eu, Sm, Ce and H, 0≤a≤3, 0.5≤b≤4、 1≤c≤4, and 0≤d≤1。 9. The positive electrode active material according to claim 8, The coating material is selected from NiO2, CoO2, MnO2, Al2O3, MgO, SiO2, ZrO2, LiNbO3, LiBO2 and Li 3-e PO 4-f N g At least one of the following is formed, wherein 0≤e≤3, 0≤f≤3 and 0≤g≤1.
10. The positive electrode active material according to claim 9, The coating material is formed of at least one selected from Al2O3, MgO, SiO2 and ZrO2.
11. The positive electrode active material according to claim 1 or 2, The monoclinic crystal is of space group C2 / m.
12. The positive electrode active material according to claim 1 or 2, The hexagonal crystal is of space group R-3m.
13. The positive electrode active material according to claim 1 or 2, The cubic crystal is at least one selected from the group consisting of a space group Fm-3m and a space group Fd-3m.
14. The positive electrode active material according to claim 1 or 2, Integrated intensity ratio I (18°-20°) / I (43°-46°) It is 0.11 or more and 0.95 or less.
15. The positive electrode active material according to claim 14, Integrated intensity ratio I (18°-20°) / I (43°-46°) It is 0.35 or more and 0.95 or less.
16. The positive electrode active material according to claim 1 or 2, The lithium composite oxide contains Mn.
17. The positive electrode active material according to claim 1 or 2, The lithium composite oxide contains at least one selected from F, Cl, N, and S.
18. The positive electrode active material according to claim 17, The lithium composite oxide contains F.
19. The positive electrode active material according to claim 1 or 2, The lithium composite oxide is contained as a main component.
20. The positive electrode active material according to claim 1 or 2, The multiphase mixture is a three-phase mixture consisting of the first phase, the second phase, and the third phase.
21. A battery comprising a positive electrode, a negative electrode and an electrolyte. The positive electrode includes the positive electrode active material according to any one of claims 1 to 20.
22. The battery according to claim 21, The negative electrode comprises at least one selected from the following (i) and (ii), (i) a negative electrode active material capable of absorbing and releasing lithium ions, (ii) a material from which lithium metal dissolves into an electrolyte during discharge and from which lithium metal precipitates during charge, and The electrolyte is a non-aqueous electrolyte.
23. The battery according to claim 21, The negative electrode comprises at least one selected from the following (i) and (ii), (i) a negative electrode active material capable of absorbing and releasing lithium ions, (ii) a material from which lithium metal dissolves into an electrolyte during discharge and from which lithium metal precipitates during charge, and The electrolyte is a solid electrolyte.