Method for manufacturing semiconductor package

The method addresses miniaturization challenges in semiconductor packages by positioning conductive pillars below the semiconductor chip surface, improving handling and reliability through a structured redistribution process.

CN111293076BActive Publication Date: 2024-12-06SAMSUNG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910821027.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-07
Filing Date
2019-08-30
Publication Date
2024-12-06
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

As semiconductor chips become miniaturized, the intervals between solder balls decrease, making handling difficult and requiring improved technologies for integrating and miniaturizing semiconductor packages, particularly in fan-out wafer-level packaging.

Method used

A method for manufacturing a semiconductor package involving the formation of conductive pillars with their upper surfaces below the semiconductor chip surface, including a redistribution structure, and a sealant planarization process to expose these pillars, followed by forming a second redistribution structure connected to the pillars, ensuring the pillars' upper surfaces are lower than the semiconductor chip's upper surface.

Benefits of technology

This method allows for easier handling of solder balls and enhances the reliability and integrity of the semiconductor package by preventing contamination and corrosion, while maintaining a uniform surface finish.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111293076B_ABST
    Figure CN111293076B_ABST
Patent Text Reader

Abstract

A method for manufacturing a semiconductor package is disclosed, including: forming a first redistribution structure; forming a plurality of conductive pillars on the first redistribution structure; mounting a first semiconductor chip on the first redistribution structure; forming a sealant, the sealant being configured to cover an upper surface of the first redistribution structure, the plurality of conductive pillars, and the first semiconductor chip; planarizing the sealant; exposing the plurality of conductive pillars by forming openings in the planarized sealant; and forming a second redistribution structure on the first semiconductor chip and the sealant, the second redistribution structure being connected to the plurality of conductive pillars. The upper surfaces of the plurality of conductive pillars are located at a lower level than the upper surface of the first semiconductor chip, and the width of the upper surface of a connection through hole included in the second redistribution structure is greater than the width of the lower surface of the connection through hole.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority of Korean Patent Application No. 10-2018-0157071 filed on December 7, 2018 in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0003] Devices and methods consistent with example embodiments relate to a semiconductor package having a conductive pillar and a method of manufacturing the same. Background Art

[0004] As semiconductor devices become highly integrated, technologies for integrating and miniaturizing semiconductor chips and semiconductor packages on which the semiconductor chips are mounted are becoming prominent. A fan-out wafer-level packaging technology has been developed in which a redistribution layer is formed under the semiconductor chip instead of a printed circuit board in order to make the semiconductor package thinner. As semiconductor chips become miniaturized, the intervals between solder balls decrease, so that there is a problem that handling the solder balls becomes difficult. In order to solve this problem, a fan-out wafer-level package has been proposed. Summary of the invention

[0005] One or more example embodiments provide a semiconductor package having a conductive pillar whose upper surface is located at a lower level than an upper surface of a semiconductor chip.

[0006] Example embodiments of the present disclosure are directed to a method of manufacturing a semiconductor package, the method including grinding a sealant and forming an opening in an upper portion of the sealant such that a conductive pillar is exposed.

[0007] According to an example embodiment, a method for manufacturing a semiconductor package is provided, the method comprising: forming a first redistribution structure on a first carrier; forming a plurality of conductive pillars on the first redistribution structure by using a mask pattern; mounting a first semiconductor chip on the first redistribution structure to be adjacent to the plurality of conductive pillars; forming a sealant, the sealant being configured to cover an upper surface of the first redistribution structure, the plurality of conductive pillars, and the first semiconductor chip; planarizing the sealant so that an upper surface of the first semiconductor chip is exposed; exposing the plurality of conductive pillars by forming an opening in the planarized sealant; and forming a second redistribution structure on the first semiconductor chip and the planarized sealant, the second redistribution structure being connected to the plurality of conductive pillars. The upper surfaces of the plurality of conductive pillars may be located at a lower level than the upper surface of the first semiconductor chip. The second redistribution structure may include an interconnection pattern and a connecting via, the connecting via being configured to connect the interconnection pattern to the plurality of conductive pillars, and the width of the upper surface of the connecting via is greater than the width of the lower surface of the connecting via.

[0008] According to an example embodiment, a method for manufacturing a semiconductor package is provided, the method comprising: forming a first redistribution structure on a first carrier; forming a plurality of conductive pillars on the first redistribution structure by using a mask pattern; mounting a first semiconductor chip on the first redistribution structure to be adjacent to the plurality of conductive pillars; forming a sealant, the sealant being configured to cover an upper surface of the first redistribution structure, the plurality of conductive pillars and the first semiconductor chip; planarizing the sealant so that an upper surface of the first semiconductor chip is exposed; exposing the plurality of conductive pillars by forming an opening in the planarized sealant; forming an anti-corrosion layer on the plurality of exposed conductive pillars; and forming a second redistribution structure on the planarized sealant, the second redistribution structure being connected to the plurality of conductive pillars. The upper surfaces of the plurality of conductive pillars may be located at a lower level than the upper surface of the first semiconductor chip. The second redistribution structure may include an interconnection pattern and a connecting through hole, the connecting through hole being configured to connect the interconnection pattern to the plurality of conductive pillars, and the width of the upper surface of the connecting through hole is greater than the width of the lower surface of the connecting through hole.

[0009] According to an example embodiment, a semiconductor package is provided, including: a first redistribution structure; a first semiconductor chip disposed on the first redistribution structure; a plurality of conductive pillars disposed on the first redistribution structure to be adjacent to the first semiconductor chip; a sealant configured to cover an upper surface of the first redistribution structure, the plurality of conductive pillars, and a side surface of the first semiconductor chip; and a second redistribution structure disposed on the sealant and connected to the plurality of conductive pillars. The upper surfaces of the plurality of conductive pillars may be located at a lower level than the upper surface of the first semiconductor chip. The second redistribution structure may include an interconnection pattern and a connecting through hole, the connecting through hole being configured to connect the interconnection pattern to the plurality of conductive pillars, and the width of the upper surface of the connecting through hole being greater than the width of the lower surface of the connecting through hole. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] These and / or other aspects will become more apparent and more easily understood through the description of the embodiments in conjunction with the accompanying drawings, in which:

[0011] Figures 1 to 9 is a cross-sectional view for illustrating a method of manufacturing a semiconductor package according to an embodiment;

[0012] Fig.10 yes Fig. 9 A partial enlarged view of the semiconductor package shown;

[0013] Figures 11 to 14 is a cross-sectional view for describing a method of manufacturing a semiconductor package according to an embodiment;

[0014] Fig.15 is a cross-sectional view for describing a method of manufacturing a semiconductor package according to an embodiment;

[0015] Fig.16 yes Fig.15 A partial enlarged view of

[0016] Fig.17 is a partially enlarged view of a semiconductor package according to an example embodiment; and

[0017] Fig.18 is a partially enlarged view of a semiconductor package according to example embodiments. DETAILED DESCRIPTION

[0018] Hereinafter, a method for manufacturing a semiconductor package according to an example embodiment configured as described above will be described with reference to the accompanying drawings. Aspects of the example embodiments will be more clearly understood according to the following embodiments described in detail with reference to the accompanying drawings. Throughout the drawings and detailed description, unless otherwise described, the same reference numerals will be understood to refer to the same elements, features, and structures. For clarity, illustration, and convenience, the relative sizes and plotting of these elements may be exaggerated.

[0019] It should be understood that although the terms first, second, etc. can be used to describe various elements in this article, these elements should not be limited by these terms. These terms are only used to distinguish elements from each other. Unless explicitly stated, any reference to the singular form can include plural. In addition, unless otherwise explicitly stated, expressions such as "including" or "comprising" will be understood to mean including the elements described, but do not exclude any other elements. In addition, terms such as "components", "units" or "modules" etc. should be understood as units that perform at least one function or operation and can be implemented as hardware, software or a combination thereof.

[0020] Figures 1 to 9 and Figures 11 to 14 is a cross-sectional view for illustrating a method of manufacturing a semiconductor package according to an embodiment.

[0021] The method for manufacturing a semiconductor package according to an example embodiment may include: providing a first carrier; forming a first redistribution structure on the first carrier; forming a conductive pillar on the first redistribution structure by using a mask pattern; mounting a first semiconductor chip on the first redistribution structure to be adjacent to a plurality of conductive pillars; forming a sealant surrounding an upper surface of the first redistribution structure, a plurality of conductive pillars, and the first semiconductor chip; flattening the sealant so that an upper surface of the first semiconductor chip is exposed; exposing a plurality of conductive pillars by forming an opening in an upper portion of the flattened sealant; and forming a second redistribution structure connected to the conductive pillars on the first semiconductor chip and the flattened sealant. In addition, the method for manufacturing a semiconductor package according to an example embodiment may further include: mounting a second semiconductor chip on the second redistribution structure, and forming a sealant covering the upper surface of the second redistribution structure and the second semiconductor chip. This is merely an example embodiment, and the present disclosure is not limited thereto.

[0022] In the following, reference will be made to Figures 1 to 9 and Figures 11 to 14 A method of manufacturing the semiconductor package 100 according to the example embodiment configured as described above is described.

[0023] refer to Figure 1 , a process of providing the first carrier 102 is performed. A release film 104 may be disposed on the first carrier 102. The first carrier 102 may be a glass carrier, a ceramic carrier, a silicon wafer, etc. The release film 104 may be composed of multiple layers, and may include, for example, an adhesive layer and a release layer. The release film 104 may be used to bond a structure to be formed on the release film 104 to the first carrier 102. In addition, the release film 104 may be removed from the upper structure to be described below together with the first carrier 102, and may include a polymer-based material. In an exemplary embodiment, the release film 104 may include a light-to-heat conversion (LTHC) release coating material, and may be thermally released by heating. In an exemplary embodiment, the release film 104 may include an ultraviolet (UV) adhesive released by UV light. In addition, the release film 104 may be released by a physical method. The release film 104 may be applied in a liquid state or a cured state, or may be a laminated film laminated on the first carrier 102. The upper surface of the release film 104 may be flat and may have high coplanarity.

[0024] refer to Figure 2 , a process of forming a first redistribution structure 110 on the first carrier 102 is performed. For example, the first redistribution structure 110 may be disposed on the release film 104. The first redistribution structure 110 may include an interlayer insulating layer 112, an interconnection pattern 114, and a through hole 116.

[0025] The interlayer insulating layer 112 and the interconnection pattern 114 may be stacked in at least one layer. The through hole 116 may electrically connect the interconnection patterns 114 of different layers to each other, and may have various shapes, such as but not limited to a cylindrical shape and / or a conical shape. In addition, the through hole 116 may be provided to be integrated with the interconnection pattern 114. The interlayer insulating layer 112 may electrically insulate the interconnection pattern 114 and the through hole 116 from the outside.

[0026] The interlayer insulating layer 112 may include a photosensitive material that can be patterned using a photolithography process. For example, the interlayer insulating layer 112 may include a polymer such as polybenzoxazole (PBO), polyimide, benzocyclobutene (BCB), etc. In example embodiments, the interlayer insulating layer 112 may include silicon nitride, silicon oxide, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), or a combination thereof. The interlayer insulating layer 112 may be formed by processes such as a chemical vapor deposition (CVD) process, a lamination process, a spin coating process, and the like.

[0027] The process of forming the first redistribution structure 110 may include forming an interconnection pattern 114 on the release film 104. The formation of the interconnection pattern 114 may include: forming a barrier layer and a seed layer (not shown) on the interlayer insulating layer 112, forming a patterned mask (not shown) such as a photoresist on the seed layer, and forming a conductive material on the exposed seed layer. The formation of the conductive material may include a plating process. Thereafter, the patterned mask and the portions of the barrier layer and the seed layer covered by the patterned mask are removed, and the interconnection pattern 114 is formed. By repeating the process of forming the interconnection pattern 114 and the through hole 116 and covering the interconnection pattern 114 and the through hole 116 with the interlayer insulating layer 112, the interconnection pattern 114 and the through hole 116 may be formed as shown in FIG. Figure 2 As shown, a first redistribution structure 110 is formed.

[0028] The barrier layer may include at least one selected from Ta, Ti, W, Ru, V, Co, and Nb. The seed layer may include at least one selected from Al, Ti, Cr, Fe, Co, Ni, Cu, Zn, Pd, Pt, Au, and Ag. In example embodiments, the barrier layer may include Ti, and the seed layer may include Cu. The barrier layer and the seed layer may be formed by a physical vapor deposition (PVD) process, a CVD process, or an atomic layer deposition (ALD) process.

[0029] The interconnection pattern 114 and the through hole 116 may include a metal such as Al, Ti, Cr, Fe, Co, Ni, Cu, Zn, Pd, Pt, Au, or Ag. In an example embodiment, the interconnection pattern 114 and the through hole 116 may include copper. The interconnection pattern 114 and the through hole 116 may be formed by an electrochemical plating process, an electroless plating process, a PVD process, a CVD process, a spin coating process, or a combination thereof. In an example embodiment, the interconnection pattern 114 and the through hole 116 may be formed by a damascene process.

[0030] refer to Figure 3 and Figure 4 , a process of forming the conductive pillars 122 on the first redistribution structure 110 is performed. For example, a plurality of conductive pillars 122 may be disposed on the first redistribution structure 110. A plurality of conductive pillars 122 may be disposed on the uppermost interconnection pattern 114 of the first redistribution structure 110.

[0031] refer to Figure 3 , the mask pattern 120 may be disposed on the upper surface of the first redistribution structure 110. A portion of the upper surface of the first redistribution structure 110 may be exposed by the mask pattern 120. For example, the interconnection pattern 114 to be connected to the conductive pillar 122 may be exposed by the mask pattern 120. Figure 4, the conductive pillars 122 may be disposed on portions of the upper surface of the first redistribution structure 110 exposed by the mask pattern 120 .

[0032] The formation of the conductive pillar 122 may include forming a barrier layer and a seed layer (not shown), forming a mask pattern 120 on the seed layer, and filling a portion exposed by the mask pattern 120 with a conductive material. Thereafter, the mask pattern 120 and the portions of the barrier layer and the seed layer covered by the mask pattern 120 may be removed.

[0033] Although not shown, a barrier layer and a seed layer may be formed on an upper surface of the first redistribution structure 110. In example embodiments, the barrier layer may include Ti, and the seed layer may include Cu. The barrier layer and the seed layer may be formed by a PVD process, a CVD process, an ALD process, or the like.

[0034] The mask pattern 120 may be formed on the seed layer. The mask pattern 120 may be formed by a spin coating process or the like, and may be exposed to light for patterning. The mask pattern 120 may define an area where the conductive pillar 122 is to be provided. A conductive material may be formed in the opening of the mask pattern 120 and on the exposed portion of the seed layer. The conductive material may be formed, for example, by plating such as electroplating, electroless plating, etc. The conductive material may include metals such as Cu, Ti, W, Al, etc. In an example embodiment, the conductive material may include Cu. The mask pattern 120 and a portion of the seed layer on which the conductive material is not formed may be removed. The mask pattern 120 may be removed by a release process using oxygen plasma or the like. After removing the mask pattern 120, the barrier layer and the exposed portion of the seed layer may be removed by wet etching or dry etching. The barrier layer, the remaining portion of the seed layer, and the conductive material may form the conductive pillar 122.

[0035] like Figure 3 and Figure 4 As shown, since the conductive pillars 122 are formed by using the mask pattern 120, the conductive pillars 122 can be arranged in various forms compared to the case where the provided connection structure is provided on the first redistribution structure 110. For example, the intervals between the conductive pillars 122 can be varied, and the arrangement of the conductive pillars 122 can be varied according to the size or width of the semiconductor chip. In addition, the conductive pillars 122 can be formed to have different diameters.

[0036] Reference Figure 5 , a process of mounting the first semiconductor chip 130 on the first redistribution structure 110 to be adjacent to the conductive pillars 122 is performed. For example, when viewed from above, a plurality of conductive pillars 122 may be disposed to surround the first semiconductor chip 130.

[0037] The first semiconductor chip 130 may include a bonding pad 132 disposed under the first semiconductor chip 130 and a bump 134 disposed under the bonding pad 132. The bonding pad 132 may be electrically connected to the interconnection pattern 114 of the first redistribution structure 110 through the bump 134. In example embodiments, the bonding pad 132 may include Cu, and the bump 134 may include Sn.

[0038] The upper surface of the first semiconductor chip 130 may be located at a higher level than the upper surface of the conductive pillar 122. Figure 5 , the first semiconductor chip 130 is shown to be bonded on the first redistribution structure 110 in the form of a flip chip, but the present disclosure is not limited thereto, and the first semiconductor chip 130 may be connected to the first redistribution structure 110 by wire bonding. In the case where the first semiconductor chip 130 is connected to the first redistribution structure 110 by wire bonding, the upper surface of the first semiconductor chip 130 may be located at a level higher than that of the upper surface of the conductive pillar 122.

[0039] Reference Figure 6 , a process of forming a sealant 140 surrounding the upper surface of the first redistribution structure 110, the conductive pillars 122, and the first semiconductor chip 130 is performed. In an example embodiment, the sealant 140 may be formed by an underfill method of molding, and may fill a space between the upper surface of the first redistribution structure 110 and the lower surface of the first semiconductor chip 130. In an example embodiment, before forming the sealant 140, an underfill may be formed between the upper surface of the first redistribution structure 110 and the lower surface of the first semiconductor chip 130. The sealant 140 may not be affected by external influences such as impact on the conductive pillars 122 and the first semiconductor chip 130.

[0040] The sealant 140 may be a resin including epoxy resin or polyimide. For example, the sealant 140 may include bisphenol-based epoxy resin, polycyclic aromatic epoxy resin, o-cresol novolac epoxy resin, biphenyl epoxy resin, naphthyl epoxy resin, and the like.

[0041] Reference Figure 7 , a process of planarizing the sealant 140 so that the upper surface of the first semiconductor chip 130 is exposed is performed. The sealant 140 may be planarized to form a sealant 142. The sealant 142 may be planarized by partially grinding the upper portion of the sealant 142. Since the upper surface of the conductive pillar 122 is located at a lower level than the upper surface of the first semiconductor chip 130, the conductive pillar 122 may not be exposed by the planarization process.

[0042] Typically, in the grinding process, when the conductive pillar 122 is planarized simultaneously with the semiconductor chip, the upper surface of the conductive pillar 122 may be partially removed and residues and / or burrs may be formed. The residues and / or burrs may cause the reliability of the redistribution layer formed on the semiconductor chip to be reduced. In the method of manufacturing the semiconductor package of the present disclosure, since the conductive pillar 122 is not exposed to the outside during the planarization process of the sealant 140, contamination problems caused by the residues and / or burrs may be prevented or suppressed.

[0043] Since the upper surface of the conductive pillar 122 is located at a lower level than the upper surface of the first semiconductor chip 130, the sealant 140 and the upper silicon of the first semiconductor chip 130 can be removed during the grinding process. In the method for manufacturing a semiconductor package according to an exemplary embodiment of the present disclosure, since the conductive pillar 122 is not removed during the grinding process, the upper surface of the sealant 140 can be uniformly cut during the grinding process. For example, the surface roughness Ra (arithmetic mean roughness) of the upper surface of the sealant 142 can be 0.1 μm or less. In the following, 'surface roughness' means arithmetic mean roughness unless otherwise described.

[0044] Reference Figure 8 , a process of exposing the conductive pillar 122 by forming an opening 145 in the upper portion of the seal 142 is performed. The upper portion of the seal 142 may be partially removed. For example, the upper portion of the seal 142 may be partially removed by using a laser drilling process. A carbon dioxide gas laser beam, a UV laser beam, or an excimer laser beam may be used in the laser drilling process. The opening 145 may have a shape that tapers downward from the upper surface of the seal 142. The upper surface of the conductive pillar 122 may be exposed through the opening 145.

[0045] Reference Fig. 9 , a process of forming a second redistribution structure 150 on the first semiconductor chip 130 and the sealant 142, the second redistribution structure 150 being connected to the conductive pillars 122. A detailed description of a configuration of the second redistribution structure 150 similar to or identical to that of the first redistribution structure 110 may be omitted.

[0046] Fig.10 yes Fig. 9 A partial enlarged view of the semiconductor package shown in FIG. Fig.10 Corresponds to Fig. 9 The area R shown in FIG. Fig.10 , the second redistribution structure 150 may include an interlayer insulating layer 152, interconnection patterns 154 and 155, a via 156, and a connection via 157. The interlayer insulating layer 152 and the interconnection patterns 154 and 155 may be stacked in at least one layer. The via 156 may electrically connect the interconnection patterns 154 and 155 of different layers to each other.

[0047] The interlayer insulating layer 152 may be formed on the first semiconductor chip 130 and the sealant 142. The interlayer insulating layer 152 may be patterned, and positions where interconnection patterns 154 and 155, through holes 156, and connection through holes 157 are formed may be defined. Although not shown, a barrier layer and a seed layer may be formed on the interlayer insulating layer 152 and the conductive pillars 122. The interconnection patterns 154 and 155 and the connection through holes 157 may be formed by filling the seed layer with a conductive material. The interconnection patterns 154 and 155, the through holes 156, and the connection through holes 157 may be formed by processes such as CVD, ALD, plating, and the like.

[0048] The connecting via 157 may completely fill the opening 145 and may connect the conductive pillar 122 to the interconnection pattern 155. The interconnection pattern 155 and the connecting via 157 may be integrally formed. For example, the interconnection pattern 155 and the connecting via 157 may be formed by a damascene process. The connecting via 157 may have a truncated cone shape. For example, the first diameter D1 may be greater than the second diameter D2. Here, the first diameter D1 may refer to Fig.10 , and the second diameter D2 may refer to the diameter of the upper surface of the connecting through-hole 157 shown in , and the second diameter D2 may refer to the diameter of the lower surface of the connecting through-hole 157. The upper surface of the connecting through-hole 157 may be located at a higher level than the upper surface of the sealant 142, and the lower surface of the connecting through-hole 157 may be located at a lower level than the upper surface of the sealant 142. Here, the upper surface of the sealant 142 may refer to a portion where the opening 145 is not formed after the grinding process. In addition, the second diameter D2 may refer to the diameter of the upper portion of the guide electric column 122, and the third diameter D3 may refer to the diameter of the lower portion of the guide electric column 122. The second diameter D2 may be substantially the same as the third diameter D3, but the present disclosure is not limited thereto. In example embodiments, the second diameter D2 may be greater than the third diameter D3.

[0049] In the method of manufacturing a semiconductor package according to an exemplary embodiment of the present disclosure, since the upper surface of the conductive pillar 122 is formed at a lower level than the upper surface of the first semiconductor chip 130, the first thickness T1 may be greater than the second thickness T2. Here, the first thickness T1 may refer to a distance from the lower surface of the conductive pillar 122 to the upper surface of the sealant 142, and the second thickness T2 may refer to a distance from the lower surface of the conductive pillar 122 to the surface of the connecting through hole 157. The ratio of the second thickness T2 to the first thickness T1 may be 0.8 or less.

[0050] In the method of manufacturing a semiconductor package according to an exemplary embodiment of the present disclosure, since the conductive pillar 122 connecting the first redistribution structure 110 to the second redistribution structure 150 is formed on the first redistribution structure 110 by using the mask pattern 120, the conductive pillar 122 may have a columnar shape. In addition, the diameter of the conductive pillar 122 may be substantially constant, and the conductive pillar 122 may not have a protrusion protruding in the radial direction.

[0051] Reference Fig.11 , the first carrier 102 may be separated from the first redistribution structure 110, and the second carrier 160 may be formed on the second redistribution structure 150. The first carrier 102 may be separated by a peeling process of the release film 104, and Fig. 9 In example embodiments, the peeling process may include a process of projecting light (eg, laser or UV light) onto the release film 104. The release film 104 may be decomposed by the heat of the light, and the first carrier 102 may be separated from the first redistribution structure 110.

[0052] The second carrier 160 may be formed before the first carrier 102 is separated. A release film 162 may also be disposed between the second carrier 160 and the second redistribution structure 150. The second carrier 160 may be located on a surface opposite to a surface of the second redistribution structure 150 that contacts the first semiconductor chip 130. The second carrier 160 and the release film 162 may include the same materials as the first carrier 102 and the release film 104, respectively.

[0053] Reference Fig.12 , an external connection member 170 may be formed on the first redistribution structure 110. The external connection member 170 may be disposed on a surface opposite to a surface on which the first semiconductor chip 130 mounted on the first redistribution structure 110 is located. The external connection member 170 may be connected to the interconnection pattern 154 of the first redistribution structure 110 through a via 174 and an under bump metal 176. An interlayer insulating layer 172 may be disposed on the interconnection pattern 114 of the first redistribution structure 110, and may cover the interconnection pattern 114 and the via 174. An under bump metal 176 may be disposed on the interlayer insulating layer 172.

[0054] The external connection member 170 may include tin (Sn), silver (Ag), copper (Cu), palladium (Pd), bismuth (Bi) or antimony (Sb). The interlayer insulating layer 172 may include the same material as the interlayer insulating layer 112, and may include, for example, a polymer (e.g., PBO, polyimide, BCB, etc.). The through hole 174 may include a metal such as Al, Ti, Cr, Fe, Co, Ni, Cu, Zn, Pd, Pt, Au or Ag. In an example embodiment, the through hole 174 may include Cu. The under bump metal 176 may include chromium / chromium copper alloy / copper (Cr / Cr-Cu / Cu), titanium tungsten copper alloy (Ti-W / Cu), aluminum / nickel / copper (Al / Ni / Cu), or nickel. The under bump metal 176 may be formed by a sputtering process, an electrolytic plating process, an electroless plating process, etc.

[0055] Reference Figures 5 to 9 Although not shown, a plurality of first semiconductor chips 130 may be arranged on the first carrier 102 at predetermined intervals, and a plurality of conductive pillars 122 may be disposed adjacent to the first semiconductor chips 130, respectively. Fig.12 As shown, after forming the external connection members 170 , a sawing process may be further performed. Singulation may be performed on the plurality of first semiconductor chips 130 by using the sawing process.

[0056] Reference Fig.13 , the second semiconductor chip 180 may be mounted on the second redistribution structure 150, and the second carrier 160 may be removed. The second semiconductor chip 180 may be mounted on the second redistribution structure 150 by wire bonding. The second redistribution structure 150 may be electrically connected to the second semiconductor chip 180 through the pads 182 and the wires 184. An adhesive may be provided on the lower surface of the second semiconductor chip 180 to fix the second semiconductor chip 180 to the second redistribution structure 150. Fig.13 , the second semiconductor chip 180 is shown as being mounted by wire bonding, but the present disclosure is not limited thereto. In example embodiments, the second semiconductor chip 180 may be connected to the second redistribution structure 150 by flip chip bonding. By irradiating laser or UV light, the second carrier 160 may be separated from the second redistribution structure 150 by heating.

[0057] The second semiconductor chip 180 may function differently from the first semiconductor chip 130. For example, the first semiconductor chip 130 may be a logic chip such as an application processor, and the second semiconductor chip 180 may be a memory chip such as a dynamic random access memory (DRAM), a static random access memory (SRAM), a non-AND (NAND) flash memory, etc.

[0058] Reference Fig.14 , a process of forming a sealant 185 surrounding the upper surface of the second redistribution structure 150 and the second semiconductor chip 180 is performed. The upper surface of the sealant 185 may be located at a higher level than the upper surface of the second semiconductor chip 180, and the sealant 185 may cover the entire second semiconductor chip 180 and the entire conductive line 184. The sealant 185 may be a resin including epoxy resin or polyimide.

[0059] The semiconductor package 100 according to the example embodiment of the present disclosure may be completed by covering the second semiconductor chip 180 with a sealant 185. The semiconductor package 100 may include a lower package 10 and an upper package 20. The lower package 10 may include a first redistribution structure 110, a conductive pillar 122, a first semiconductor chip 130, a sealant 142, and a second redistribution structure 150. The upper package 20 may include a second semiconductor chip 180 and a sealant 185.

[0060] Fig.15 is a cross-sectional view for describing a method of manufacturing a semiconductor package 200 according to an embodiment of the present disclosure. Fig.16 yes Fig.15 A partial enlarged view of . Fig.15 Can correspond to Fig. 9 ,and Fig.16 Can correspond to Fig.15 The area shown in R.

[0061] refer to Fig.15 and Fig.16 , the semiconductor package 200 may include a second redistribution structure 250. The second redistribution structure 250 may include interconnection patterns 254 and 255, a through hole 256, and a connection through hole 257. In addition, the second redistribution structure 250 may further include an anticorrosion layer 260. Fig. 9 and Fig.15 In the process of forming the second redistribution structure 250 on the first semiconductor chip 130 and the sealant 142 , the anti-corrosion layer 260 may be disposed before forming the interconnection pattern 255 and the connection via 257 .

[0062] The interconnection patterns 254 and 255, the vias 256, and the connection vias 257 of the second redistribution structure 250 may include a conductive material different from that of the conductive pillars 122. In example embodiments, the conductive pillars 122 may include copper, and the interconnection patterns 254 and 255, the vias 256, and the connection vias 257 may include aluminum. However, the present disclosure is not limited thereto.

[0063] Generally, aluminum interconnects can form denser films than copper interconnects and do not have problems with diffusion into silicon or insulating films. However, aluminum interconnects may have a disadvantage in that they may easily cause corrosion due to poor electron mobility. Specifically, galvanic corrosion may easily occur at portions of the aluminum interconnect that contact foreign metals. Fig.15 and Fig.16 As shown, the anti-corrosion layer 260 may be disposed under the interconnection pattern 255 and the connection via 257. The anti-corrosion layer 260 may prevent corrosion of the conductive pillar 122 and the connection via 257 including different materials. The anti-corrosion layer 260 may be formed by a deposition process such as a CVD process, a PVD process, an ALD process, etc. The anti-corrosion layer 260 may include a conductive material. In example embodiments, the anti-corrosion layer 260 may include Ta, TaN, Ti, TiN, W, or a combination thereof.

[0064] Fig.17 is a partially enlarged view of a semiconductor package 300 according to example embodiments.

[0065] refer to Fig.17 , the semiconductor package 300 may include a second redistribution structure 350. The second redistribution structure 350 may include interconnection patterns 354 and 355, a through hole 356, a connection through hole 357, and an anti-corrosion layer 360. The anti-corrosion layer 360 may be formed on the conductive pillar 122 exposed by the opening 145 through a plating process. The anti-corrosion layer 360 may be disposed between the conductive pillar 122 and the connection through hole 357, and may not be disposed under the interconnection pattern 355. The anti-corrosion layer 360 may include a conductive material, and may include, for example, Ni, Pd, Au, or a combination thereof.

[0066] Fig.18 is a plan view of a semiconductor package 400 according to an embodiment. The semiconductor package 400 may include a second redistribution structure 450 .

[0067] Reference Figure 8 and Fig.18 In the process of forming the opening 145 on the upper surface of the seal 142, the opening 145 may be formed so that the lower end of the opening 145 is located at a lower level than the upper surface of the conductive pillar 122. After the opening 145 is formed, the second redistribution structure 450 may be formed on the upper surface of the seal 140. The second redistribution structure 450 may include a connection through hole 457 connected to the conductive pillar 122. The connection through hole 457 may fill the entire interior of the opening 145, and the lower end of the connection through hole 457 may be located at a lower level than the upper surface of the conductive pillar 122. The connection through hole 457 may include copper or aluminum. Although not shown, a barrier layer and a seed layer or an anti-corrosion layer may be provided between the conductive pillar 122 and the connection through hole 457.

[0068] According to example embodiments of the present disclosure, since the upper surface of the conductive pillar is located at a lower level than the upper surface of the first semiconductor chip, the conductive pillar may not be exposed during grinding of the sealant, and thus contamination problems and reliability degradation problems may be prevented.

[0069] Although the exemplary embodiments of the present disclosure have been described with reference to the accompanying drawings, it will be appreciated by those skilled in the art that various modifications may be made without departing from the scope of the present disclosure. Therefore, the above embodiments should be considered as merely illustrative and not for the purpose of limitation.

Claims

1. A method for manufacturing a semiconductor package, the method include: forming a first redistribution structure on a first carrier; forming a plurality of conductive pillars on the first redistribution structure by using a mask pattern; mounting a first semiconductor chip on the first redistribution structure to be adjacent to the plurality of conductive pillars; forming a sealant configured to cover an upper surface of the first redistribution structure, the plurality of conductive pillars, and the first semiconductor chip; planarizing the sealant so that an upper surface of the first semiconductor chip is exposed; exposing the plurality of conductive pillars by forming openings in the planarized seal; as well as forming a second redistribution structure on the first semiconductor chip and the planarized sealant, the second redistribution structure being connected to the plurality of conductive pillars, wherein the upper surfaces of the plurality of conductive pillars are located at a lower level than the upper surface of the first semiconductor chip, The second redistribution structure includes a first interconnection pattern, a second interconnection pattern on the first interconnection pattern, a connecting via and a through hole, the connecting via being configured to connect the first interconnection pattern to the plurality of conductive pillars, and the through hole connecting the first interconnection pattern and the second interconnection pattern, The width of the upper surface of the connecting through hole is greater than the width of the lower surface of the connecting through hole, The height of the connecting through hole is greater than the height of the through hole, and A side surface of the conductive pillar and at least a portion of the connecting through hole are surrounded by the sealant.

2. The method according to claim 1, in, The planarizing includes planarizing the sealant so that the plurality of conductive pillars are not exposed.

3. The method according to claim 1, in, The exposing includes exposing portions of upper surfaces and side surfaces of the plurality of conductive pillars.

4. The method according to claim 1, further comprising: include: A second semiconductor chip is mounted on the second redistribution structure after forming the second redistribution structure, the second semiconductor chip being connected to the plurality of conductive pillars.

5. The method according to claim 1, in, The planarized upper surface of the sealant has a surface roughness Ra of 0.1 μm or less.

6. The method according to claim 1, in, Side surfaces of the plurality of conductive pillars are in contact with the sealant.

7. The method according to claim 1, in, A lower surface of the connecting through hole is located at a lower level than an upper surface of the sealant.

8. The method according to claim 1, in, An upper surface of the first interconnection pattern is formed parallel to an upper surface of the sealant.

9. The method according to claim 1, in, The opening tapers downward from the upper surface of the seal.

10. The method according to claim 1, in, The plurality of conductive pillars are formed by a plating process.

11. A method for manufacturing a semiconductor package, the method include: forming a first redistribution structure on a first carrier; forming a plurality of conductive pillars on the first redistribution structure by using a mask pattern; mounting a first semiconductor chip on the first redistribution structure to be adjacent to the plurality of conductive pillars; forming a sealant configured to cover an upper surface of the first redistribution structure, the plurality of conductive pillars, and the first semiconductor chip; planarizing the sealant so that an upper surface of the first semiconductor chip is exposed; exposing the plurality of conductive pillars by forming openings in the planarized seal; forming an anti-corrosion layer on the exposed plurality of conductive pillars; as well as forming a second redistribution structure on the planarized seal, the second redistribution structure being connected to the plurality of conductive pillars, wherein the upper surfaces of the plurality of conductive pillars are located at a lower level than the upper surface of the first semiconductor chip, The second redistribution structure includes a first interconnection pattern, a second interconnection pattern on the first interconnection pattern, a connecting via and a through hole, the connecting via being configured to connect the first interconnection pattern to the plurality of conductive pillars, and the through hole connecting the first interconnection pattern and the second interconnection pattern, The width of the upper surface of the connecting through hole is greater than the width of the lower surface of the connecting through hole, The height of the connecting through hole is greater than the height of the through hole, and A side surface of the conductive pillar and at least a portion of the connecting through hole are surrounded by the sealant.

12. The method according to claim 11, in, The plurality of conductive pillars include copper, and the first interconnection pattern and the connection via include aluminum.

13. The method according to claim 11, in, The anti-corrosion layer is disposed between the plurality of conductive pillars and the connecting through holes.

14. The method according to claim 11, in, The planarizing includes planarizing the sealant so that the plurality of conductive pillars are not exposed.

15. The method according to claim 11, in, The plurality of conductive pillars are formed by a plating process.

16. The method according to claim 11, in, The anti-corrosion layer includes Ta, TaN, Ti, TiN, W, Ni, Pd, Au and / or combinations thereof.