Polyethersulfone-grafted polyethylene glycol methacrylate copolymer, thin film and its preparation method

By grafting polyethylene glycol methacrylate monomers onto polyethersulfone membranes through gamma irradiation, the problems of material degradation and membrane pore blockage caused by ultraviolet light grafting were solved, and a polyethersulfone-grafted polyethylene glycol methacrylate copolymer film with excellent filtration performance and anti-fouling effect was prepared.

CN111732732BActive Publication Date: 2026-11-10SHANGHAI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202010487907.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-02
Publication Date
2026-11-10
Estimated Expiration
2040-06-02

AI Technical Summary

Technical Problem

In the prior art, when ultraviolet light induces the grafting of polyethylene glycol methacrylate onto the surface of polyethersulfone membranes, there are problems such as degradation of material properties and blockage of membrane pores, which affect membrane flux and filtration efficiency.

Method used

A polyethersulfone-grafted polyethylene glycol methacrylate copolymer film was prepared by grafting polyethylene glycol methacrylate monomer onto polyethersulfone material using gamma-ray irradiation technology, controlling the grafting rate within a specific range to form a uniform distribution of hydrophilic side chains, thereby improving the hydrophilicity and molecular chain flexibility of the material.

Benefits of technology

It improves the hydrophilicity and filtration performance of the membrane, increases water flux, enhances antifouling effect, and maintains the uniformity and stability of membrane pore size, making it suitable for wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111732732B_ABST
    Figure CN111732732B_ABST
Patent Text Reader

Abstract

This invention discloses a polyethersulfone-grafted polyethylene glycol methacrylate copolymer, a film, and its preparation method. The method involves a pretreatment process: the raw material polyethersulfone is washed, soaked, and then dried to constant weight. The dried polyethersulfone is then mixed with polyethylene glycol methacrylate monomer to form a homogeneous solution. In this homogeneous solution containing both polyethylene glycol methacrylate monomer and polyethersulfone, a co-radiative grafting reaction is performed on the polyethylene glycol methacrylate monomer and polyethersulfone. The resulting homogeneous solution is then post-treated: the homogeneous solution is reverse-phase precipitated in deionized water, the resulting solid is washed, soaked in deionized water, and then vacuum-dried to constant weight. This invention grafts PEGMA onto the PES material matrix, allowing for the preparation of graft copolymers with different grafting ratios as needed, providing greater application flexibility and improving the properties of the graft copolymer itself.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a polyethersulfone-grafted polyethylene glycol methyl ether methacrylate monomer copolymer, a film, and a preparation method thereof, which are applied in the field of polymer substrate technology. Background Technology

[0002] Currently, membrane separation technology is widely used in the petroleum industry, seawater desalination, wastewater treatment, and gas separation. Its advantages include high separation accuracy, environmental friendliness, and ease of operation. As the core of membrane separation technology, the membrane has therefore received widespread attention. Polyethersulfone (PES) is a widely used industrial polymer substrate with excellent mechanical properties. Its molecular structure consists of ether groups, sulfone groups, and phenylene groups. The ether groups impart flexibility to the polymer molecular chains, while the sulfone and phenylene groups give the polymer excellent thermodynamic and processing properties. Its creep resistance is outstanding; it can maintain good thermodynamic properties even under high temperatures and heavy loads for extended periods.

[0003] However, the development of polyethersulfone (PES) membranes has been constrained by many issues, the biggest of which is membrane fouling. Due to PES's strong hydrophobic properties, many large molecular proteins, colloids, and oils adsorb onto the membrane surface during filtration, clogging the pores, reducing flux, and even damaging the membrane, thus affecting filtration efficiency and increasing costs. Structurally, PES's hydrophobicity stems from its lack of hydrophilic groups. Therefore, chemical modification can be used to introduce other functional groups onto PES, thereby improving the polarity of the material, enhancing the membrane's antifouling properties, and further expanding its application areas.

[0004] Currently, commonly used modification methods include physical blending, chemical grafting, ultraviolet irradiation, and plasma irradiation. Each of these methods has its own advantages and disadvantages: physical blending is simple to operate, but because no chemical bonds are generated, the compounds are only bound together by force, resulting in poor stability of the mixed products; chemical grafting requires the addition of an initiator to initiate chain growth, which is complex to operate and the initiator is difficult to remove; ultraviolet and plasma irradiation can only modify the surface of the bulk material, and cannot modify the interior of the bulk material.

[0005] PEGs are a class of water-soluble polymers with linear, regular helical chains. They are non-toxic and have low irritation. In water, PEG chains can form numerous hydrogen bonds with water, and the CO bonds in the chain are more flexible than the C=C bonds, resulting in excellent flexibility in water. Grafting PEG-containing prepolymers onto PES can effectively improve the hydrophilicity of PES. Polyethylene glycol methacrylate (PEGMA), as a derivative of PEG, also possesses the excellent hydrophilicity and flexibility of PEG, and also contains C=C bonds, making the grafting reaction with PES easier to occur. Gamma rays have strong penetrating power, are easy to operate, and have a simple process. Currently, there are no reports on the use of gamma irradiation to modify PES and graft PEGMA, which provides a new avenue for our research.

[0006] Currently, there are reports on grafting polyethylene glycol methacrylate (PEGMA) onto the surface of polyethersulfone (PES) membranes using ultraviolet light. The main problems with this technology are twofold: firstly, certain wavelengths of ultraviolet light have a significant degradative effect on PES, affecting the material's inherent properties; secondly, grafting onto the PES surface easily forms graft chains that block the membrane pores, leading to uneven pore size and distribution, which significantly impacts the membrane flux, typically reducing it by 50-80%. This problem urgently needs to be addressed. Summary of the Invention

[0007] To address the problems of existing technologies, the present invention aims to overcome the shortcomings of existing technologies by providing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer, a film, and a method for its preparation. This invention overcomes the shortcomings of existing technologies where, when grafting polyethylene glycol methacrylate (PEGMA) monomers onto the surface of polyethersulfone (PES) films using ultraviolet light, certain wavelengths of ultraviolet light exhibit significant degradation effects on PES, affecting the material's properties. Furthermore, grafting onto the surface of PES films easily forms graft chains that block the pores of the PES film, significantly impacting the film's flux. The present invention provides a polyethersulfone-grafted polyethylene glycol methacrylate copolymer, a film, and a method for its preparation. The grafted copolymer of the present invention effectively improves its polarity and molecular chain flexibility; it is less prone to crosslinking and exhibits good dispersibility and solubility in solvents; during film preparation, it has good compatibility with pore-forming agents, resulting in a film with good hydrophilicity. Because the grafting rate of the graft copolymer is controlled within a specific range, the resulting film has a reasonable ratio of main chain to side chain structure and a uniform distribution of hydrophilic groups on the side chain, thus exhibiting better hydrophilicity. At the same time, the stability of the original main chain structure of the graft copolymer ensures the pore size of the film on a macroscopic level, resulting in a significant increase in water flux and better anti-fouling effect while maintaining excellent filtration performance.

[0008] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:

[0009] A method for preparing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer includes the following steps:

[0010] (1) Raw material pretreatment:

[0011] After washing and soaking, the raw material polyethersulfone is dried to constant weight. In order to remove impurities in the raw material polyethersulfone that affect the grafting reaction as easily as possible during the subsequent product post-processing, the present invention first performs a pretreatment operation.

[0012] (2) Co-radiative grafting reaction process:

[0013] The polyethersulfone obtained after drying in step (1) is mixed with polyethylene glycol methacrylate monomer to form a homogeneous solution. The solvent of the homogeneous solution is N,N-dimethylacetamide. The mass ratio of polyethersulfone to polyethylene glycol methacrylate monomer is 10:1 to 10:9. In the homogeneous solution containing polyethylene glycol methacrylate monomer and polyethersulfone, the polyethylene glycol methacrylate monomer and polyethersulfone are subjected to a co-radiative grafting reaction.

[0014] (3) Post-treatment of grafting reaction products:

[0015] The homogeneous solution obtained after the co-radiative grafting reaction in step (2) is then post-treated; the post-treatment is performed according to the following steps:

[0016] Following the co-radiative grafting reaction, a homogeneous solution was precipitated in deionized water. The resulting solid was washed, then soaked in deionized water, and finally vacuum dried to constant weight to obtain a polyethersulfone-grafted polyethylene glycol methacrylate copolymer. The soaking time in deionized water was 20–26 h, the vacuum drying temperature was 50–80 °C, and the vacuum degree was 0.06–0.08 MPa. More preferably, the soaking time in deionized water was 24 h; more preferably, it was 70 °C; and more preferably, it was 0.07 MPa.

[0017] In this invention, in step (2), if the mass ratio of polyethersulfone to polyethylene glycol methacrylate monomer exceeds 10:10, the grafting rate of the product will be too high, which will have a significant impact on the bulk structure. Therefore, considering the effectiveness of the grafting monomer reaction and the grafting effect, the mass ratio of polyethersulfone to polyethylene glycol methacrylate monomer is controlled at 10:1 to 10:9. More preferably, it is 10:3 to 15:7, and most preferably, it is 10:4 to 10:6.

[0018] As a preferred embodiment of the present invention, in step (1), the weight-average molecular weight of the polyethersulfone is 20,000 to 200,000, preferably 142,000.

[0019] As a preferred technical solution of the present invention, in step (1), during the pretreatment process, the raw material polyethersulfone is washed with deionized water, then soaked in deionized water for more than one week, during which the deionized water is replaced, and then vacuum dried to constant weight; the vacuum drying temperature is 60-80℃; the vacuum degree of the vacuum drying is 0.06-0.08MPa. A vacuum drying temperature of 70℃ is preferred; a vacuum degree of 0.07MPa is preferred.

[0020] As a preferred technical solution of the present invention, in step (2), the mass percentage concentration of the polyethylene glycol methacrylate monomer in the homogeneous solution is 1-9%, more preferably 3-7%, and most preferably 4-6%; in order to improve production efficiency, the mass percentage concentration of the polyethersulfone in the homogeneous solution is 10-15% without affecting the stirring of the homogeneous solution.

[0021] As a preferred embodiment of the present invention, in step (2), the radiation source of the co-radiative grafting reaction is a gamma-ray radiation source, and the radiation source of the co-radiative grafting reaction is... 60 Co; the total radiation dose of the co-radiative grafting reaction is 6-30 kGy; more preferably 5-15 kGy; the average dose rate of the co-radiative grafting reaction is 1-5.00 kGy / h; more preferably 1-2 kGy / h; the temperature of the co-radiative grafting reaction is 20-30°C; more preferably 25°C.

[0022] As a preferred embodiment of the present invention, in step (2), the atmosphere of the co-radiative grafting reaction is an oxygen-free atmosphere; the oxygen-free atmosphere is at least one gas atmosphere selected from nitrogen and argon. The oxygen-free atmosphere can be obtained using conventional techniques in the art, such as passing an oxygen-free atmosphere gas through the radiation-forward reaction system for more than 15 minutes to remove oxygen from the system.

[0023] A polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer is prepared using the preparation method of the polyethersulfone-grafted polyethylene glycol methacrylate copolymer of the present invention.

[0024] A polyethersulfone-grafted polyethylene glycol methacrylate copolymer film is disclosed. Using the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer of this invention as raw material, the preparation method of the polyethersulfone-grafted polyethylene glycol methacrylate copolymer film includes the following steps: dissolving the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer in an organic solvent to prepare a casting solution; then, coating the casting solution onto a substrate, performing phase reversal film formation in an aqueous solution, and finally curing to obtain the film. Preferably, the coating operation and conditions are conventional operations and conditions in the art. Preferably, during the coating operation, it is generally necessary to ensure that the casting solution is uniformly coated onto the substrate. Preferably, the substrate can be a conventional substrate used for film formation in the art, generally a glass plate.

[0025] As a preferred embodiment of the present invention, in its preparation method, the mass percentage concentration of the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer in the casting solution is 16-20%; more preferably 18%; the organic solvent in the casting solution is N,N-dimethylacetamide; the film curing conditions are: curing in water at 18-25°C for 46-50 hours; more preferably curing in water at 20°C for 48 hours.

[0026] As a preferred embodiment of the present invention, in its preparation method, the thickness of the prepared film is 180-250 μm; more preferably 250 μm.

[0027] Compared with the prior art, the present invention has the following obvious and prominent substantive features and significant advantages:

[0028] 1. This invention grafts PEGMA onto PES material, allowing for the preparation of graft copolymers with different grafting ratios as needed, thus providing greater application flexibility. Furthermore, the PEGMA monomer can form a "brush-like" graft polymer molecular structure on the PES molecule, achieving a moderate grafting ratio. The properties of the graft copolymer itself are improved, effectively enhancing its polarity and molecular chain flexibility. The graft copolymer of this invention effectively improves its polarity and molecular chain flexibility, is less prone to crosslinking, and exhibits good dispersibility and solubility in solvents.

[0029] 2. In the preparation of the film, the present invention exhibits good compatibility with the pore-forming agent, resulting in a film with good hydrophilicity. Because the grafting rate of the graft copolymer is controlled within a specific range, the resulting film has a reasonable ratio of main chain to side chain structure and a uniform distribution of hydrophilic groups on the side chains, thus exhibiting better hydrophilicity. Simultaneously, the stability of the original main chain structure of the graft copolymer macroscopically ensures the pore size of the film, resulting in a significant increase in water flux while maintaining excellent filtration performance and superior resistance to protein fouling, demonstrating excellent prospects for wastewater treatment applications.

[0030] 3. The method of the present invention is simple, easy to implement, and low in cost, making it suitable for widespread use. Attached Figure Description

[0031] Figure 1 This is the infrared spectrum of the product obtained in Example 1 of the present invention.

[0032] Figure 2 This is the infrared spectrum of the product obtained in Example 2 of this invention.

[0033] Figure 3 This is the infrared spectrum of the product obtained in Example 3 of the present invention.

[0034] Figure 4 This is the infrared spectrum of the product obtained in Example 4 of this invention.

[0035] Figure 5 This is the infrared spectrum of the product obtained in the comparative example of this invention.

[0036] Figure 6 This is an analysis diagram of the static water contact angle test results of the thin film obtained in Example 5 of the present invention.

[0037] Figure 7 This is an analysis chart of the pure water flux detection results of the thin film obtained in Example 5 of this invention.

[0038] Figure 8 This is a graph showing the performance analysis of the membrane filter for bovine serum albumin (BSA) obtained in Example 5 of this invention.

[0039] Figure 9 This is a graph showing the pure water recovery rate, i.e., the anti-fouling effect, of the thin film obtained in Example 5 of this invention. Detailed Implementation

[0040] In the following examples and comparative examples, N,N-dimethylacetamide was of analytical grade and purchased from Sinopharm Group. In Examples 1-5 and the comparative examples, the polyethersulfone (PES) used was model 049, purchased from Rainbow High-Tech Materials (Laiyang) Co., Ltd., with a weight-average molecular weight of 142,000. Before the irradiation reaction, all materials underwent the following pretreatment: the raw material polyethersulfone was washed with deionized water, then soaked in deionized water for more than one week, with the deionized water being changed multiple times. The raw material polyethersulfone was then vacuum dried to constant weight at 70°C and a vacuum degree of 0.07 MPa in a vacuum drying oven to obtain polyethersulfone (PES) powder, which was used as the pretreated raw material.

[0041] The above solution will be further described below with reference to specific embodiments. The preferred embodiments of the present invention are described in detail below:

[0042] Example 1:

[0043] In this embodiment, a method for preparing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer includes the following steps:

[0044] a. Co-radiative grafting reaction process:

[0045] Weigh 10g of pretreated polyethersulfone (PES) powder, dissolve it in 89g of DMAc solvent, add 1g of polyethylene glycol methacrylate monomer (PEGMA) monomer, stir for 24h to obtain a homogeneous solution of the reactants, purge with N2 for at least 15min, and then place the homogeneous solution in a container. 60 C O Under the source, a co-radiation reaction was carried out at 25°C with a radiation dose rate of 1.67 kGy / h and a total radiation dose of 10 kGy for the co-radiation grafting reaction.

[0046] b. Post-treatment of grafting reaction products:

[0047] After the irradiation reaction is complete, the homogeneous solution obtained after the co-radiation grafting reaction in step a will undergo post-treatment; the post-treatment will be carried out according to the following steps:

[0048] After the co-radiative grafting reaction, a homogeneous solution was obtained and precipitated in deionized water. The resulting solid was washed and then soaked in deionized water for 24 hours. The deionized water was then discarded, and the resulting solid was vacuum dried in a vacuum oven at 70°C and 0.07 MPa to constant weight, thereby obtaining polyethersulfone-grafted polyethylene glycol methacrylate copolymer.

[0049] Example 2:

[0050] This embodiment is basically the same as Embodiment 1, except that:

[0051] In this embodiment, a method for preparing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer includes the following steps:

[0052] a. Co-radiative grafting reaction process:

[0053] Weigh 10g of pretreated polyethersulfone (PES) powder, dissolve it in 85g of DMAc solvent, add 5g of polyethylene glycol methacrylate monomer (PEGMA) monomer, stir for 24h to obtain a homogeneous solution of the reactants, purge with N2 for at least 15min, and then place the homogeneous solution in a container. 60 C O Under the source, a co-radiation reaction was carried out at 25°C with a radiation dose rate of 1.67 kGy / h and a total radiation dose of 10 kGy for the co-radiation grafting reaction.

[0054] b. This step is the same as in Example 1.

[0055] Example 3:

[0056] This embodiment is basically the same as the previous embodiments, except that:

[0057] In this embodiment, a method for preparing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer includes the following steps:

[0058] a. Co-radiative grafting reaction process:

[0059] Weigh 10g of pretreated polyethersulfone (PES) powder, dissolve it in 81g of DMAc solvent, add 9g of polyethylene glycol methacrylate monomer (PEGMA) monomer, stir for 24h to obtain a homogeneous solution of the reactants, purge with N2 for at least 15min, and then place the homogeneous solution in a container. 60 C O Under the source, a co-radiation reaction was carried out at 25°C with a radiation dose rate of 1.67 kGy / h and a total radiation dose of 10 kGy for the co-radiation grafting reaction.

[0060] b. This step is the same as in Example 1.

[0061] Example 4:

[0062] This embodiment is basically the same as the previous embodiments, except that:

[0063] In this embodiment, a method for preparing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer includes the following steps:

[0064] a. Co-radiative grafting reaction process:

[0065] Weigh 10g of pretreated polyethersulfone (PES) powder, dissolve it in 81g of DMAc solvent, add 9g of polyethylene glycol methacrylate monomer (PEGMA) monomer, stir for 24h to obtain a homogeneous solution of the reactants, purge with N2 for at least 15min, and then place the homogeneous solution in a container. 60 C O Under the source, a co-radiation reaction was carried out at 25°C with a radiation dose rate of 1 kGy / h, and the total radiation dose of the co-radiation grafting reaction was 6 kGy.

[0066] b. This step is the same as in Example 1.

[0067] Comparative Example

[0068] Accurately weigh 10g of pretreated PES powder, dissolve it in 90g of DMAc solvent, stir for 24h to obtain a homogeneous solution, purge with N2 for at least 15min, and then place the homogeneous solution in a container. 60 C O Under the source, radiation was carried out at 25°C with a dose rate of 1.67 kGy / h and an absorbed dose of 10 kGy.

[0069] After irradiation, the resulting solution undergoes post-processing, which is performed under the same conditions and procedures as in Example 1.

[0070] Example 5:

[0071] In this embodiment, the polyethersulfone-grafted polyethylene glycol methacrylate copolymer products obtained in Examples 1 to 3 and the comparative example were used to prepare corresponding films. The film preparation method included the following steps: dissolving the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer in N,N-dimethylacetamide organic solvent to prepare a casting solution, wherein the mass percentage concentration of the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer in the casting solution was 18%; then, the casting solution was coated onto a substrate, and after phase inversion film formation in an aqueous solution, it was cured in water at 18°C ​​for 24 hours to obtain the corresponding polyethersulfone-grafted polyethylene glycol methacrylate copolymer films, all with a film thickness of 250 μm.

[0072] Experimental test analysis:

[0073] I. Using Fourier transform infrared spectrometer to detect grafting effect:

[0074] The products obtained in Examples 1 to 4 and the comparative example were used as samples for FT-IR testing, and the results are as follows: Figures 1-5 As shown.

[0075] FT-IR testing: The products from Examples 1 to 4 and the comparative example were dried, ground into powder, and made into potassium bromide tablets. These tablets were then placed on a NICOLETAVATAR-370 Fourier transform infrared spectrometer, and the transmission spectra of the samples were scanned in ATR mode, with a scanning range of 4000–400 cm⁻¹. -1 The number of scans was 32.

[0076] Figures 1-4 The infrared spectra of the products obtained in Examples 1 to 4 are shown in sequence. Figure 5 The image shows the infrared spectrum of the product obtained for comparison. Figure 5 It can be seen that at 848cm -1 740cm -1 The peaks at the left and right are the out-of-plane stretching vibration peaks of the CH bonds on the benzene ring; at 1150 cm⁻¹... -1 The peaks around 1240 cm⁻¹ are the stretching vibration peaks within the plane of symmetry of SO₂; while those at 1240 cm⁻¹ are... -1 The peaks around 1578 cm⁻¹ are in-plane stretching vibration peaks of the ether group CO; the peaks at 1578 cm⁻¹ are the stretching vibration peaks within the symmetry plane of the ether group CO. -1 1486cm -1 The peak corresponds to the bending vibration of the entire benzene ring. (And...) Figure 5 The comparison shows that the graft-modified copolymer of polyethersulfone grafted with polyethylene glycol methacrylate monomer, Figures 1-4The main difference is that it is located at 1720cm. -1 A new absorption peak appeared around the [position missing], which is the absorption vibration peak of the carbonyl C=O group on the grafted monomer. Furthermore, [the text abruptly ends here]. Figures 1-3 It can be seen that the absorption peak at this point increases significantly with the continuous increase of monomer (PEGMA) concentration, indicating that the grafting rate increases with the increase of monomer concentration, which proves the reaction effectiveness of the graft copolymer and the linear relationship between the grafting rate and the concentration.

[0077] II. Static water contact angle detection of thin films:

[0078] The contact angles of Examples 1-3 and the comparative examples were tested using the Attension Theta System. The testing method for the contact angle is conventional in the art and generally follows these steps: 5 μL of deionized water is dropped onto the membrane surface using a needle, magnified images of the droplet are collected, the contact angle is calculated using a corresponding program, and the average of the three measurements is taken. Specific contact angle data are as follows... Figure 6 As shown, the specific data for the contact angle are presented in Table 1. From Figure 6 As can be seen, the static water contact angle of the membrane decreases with increasing concentration of grafted monomers, indicating that the membrane's hydrophilicity is improving.

[0079] Table 1. Specific data on the contact angle of the products prepared in Examples 1 to 3 and comparative examples.

[0080]

[0081] III. Membrane Pure Water Flux Detection

[0082] The pure water flux of the membrane obtained in Example 5 was measured, which is to say, the pure water flux of the membranes prepared using the products obtained in Examples 1 to 3 and the comparative example as raw materials was measured. The methods for measuring the pure water capacity of the three membranes obtained in Example 5 are as follows:

[0083] (1) The membrane obtained in Example 5 was cut into pieces with an area of ​​35.3 cm². 2 A circular thin film was placed in the membrane pressing component of the membrane flux tester, and the film was pressed with deionized water for 20 minutes at a pressure of 0.01 MPa.

[0084] (2) When testing the pure water flux of the membrane, the membrane filters pure water at 0.01 MPa, and the pure water flux of the membrane is obtained from the software of the membrane flux tester.

[0085] Figure 7 This is a graph showing the pure water flux detection results of the membrane obtained in Example 5. Specific data are shown in Table 2. Figure 7It is evident that the pure water flux of the membranes obtained in Examples 1 to 3 is significantly greater than that of the membranes prepared from the ungrafted polyethersulfone material in the comparative examples. Furthermore, the higher the concentration of the grafted monomer, the more pronounced the increase in pure water flux. However, many small molecules, after modifying PES, exhibit a decreasing water flux with increasing grafting rate, as seen in patent CN107641178A, where the modified membrane's pure water flux decreases. Similarly, after PES is modified with PMAA, the water flux also decreases with increasing grafting rate. Therefore, the pure water flux modified by this method increases significantly with increasing grafting rate, which can improve filtration efficiency and save production capacity in industrial applications, thus possessing significant importance.

[0086] Table 2. Results of pure water flux detection for thin films prepared using the products obtained in Examples 1-3 and the comparative examples as raw materials.

[0087]

[0088] IV. Performance testing and analysis of bovine serum albumin (BSA) membrane filtration:

[0089] The membrane used in Example 5 to filter bovine serum albumin was analyzed to evaluate its filtration performance. Specifically, membranes prepared from the products of Examples 1-3 and the comparative example were used to filter bovine serum albumin, and their filtration performance was evaluated. The detection methods are as follows:

[0090] (1) Prepare 1L of phosphate buffer solution, adjust the pH to 7.4, add 1g of bovine serum albumin to prepare bovine serum albumin solution, abbreviated as BSA solution, Mw=20000, 500ppm;

[0091] (2) The membrane from Example 5 was cut into pieces with an area of ​​approximately 35.3 cm². 2 A circular membrane is placed in a membrane flux meter. The BSA solution is refluxed in the membrane flux meter at a rate of 2 kg / h. The pressure of the membrane flux meter is adjusted to 0.01 MPa. Filtration is performed, and the medium flux is obtained from the membrane flux meter. The filtered liquid is collected from the filtrate outlet of the membrane flux meter.

[0092] (3) The BSA content in the solution before and after filtration is obtained by ultraviolet spectrophotometer, and the membrane rejection rate is calculated.

[0093] Figure 8 Table 3 shows the retention rates of films with different grafted monomer concentrations obtained in Example 4. Figure 8 It can be seen that the retention rates of the products obtained in Examples 1 to 3 are not significantly different from those of the unmodified pure polyethersulfone membrane, and their retention rates are all above 90%. Therefore, it can be concluded that the membrane products prepared from the grafted products of the present invention have good filtration performance.

[0094] Table 3. Retention rate data of films with different grafted monomer concentrations

[0095]

[0096] V. Analysis of the pure water recovery rate and antifouling effect of the membrane:

[0097] The membrane obtained in Example 5 was analyzed to evaluate its filtration performance. Specifically, membranes prepared from the products of Examples 1-3 and the comparative examples were evaluated for their filtration performance. The detection methods are as follows:

[0098] (1) The membrane from Example 5 was cut into pieces with an area of ​​approximately 35.3 cm². 2 A circular membrane was placed in a membrane flux analyzer and compacted with pure water at a pressure of 0.1 MPa and a flow rate of 2 kg / h for half an hour. The pure water flux was then obtained from the flux analyzer.

[0099] (2) Prepare 1L of phosphate buffer solution, adjust the pH to 7.4, add 1g of bovine serum albumin to prepare bovine serum albumin solution, abbreviated as BSA solution, Mw=20000, 500ppm;

[0100] (3) Replace the reflux liquid of the flux tester with BSA solution, and filter the BSA solution through the membrane at a rate of 2 kg / h and a pressure of 0.1 MPa for half an hour;

[0101] (4) Change the reflux liquid of the membrane flux tester to pure water, with a flow rate of 5 kg / h and a pressure of 0 MPa, and reflux for half an hour to achieve the effect of cleaning the membrane surface.

[0102] (5) Replace the cleaned pure water and measure the second pure water flow rate at a speed of 2 kg / h and a pressure of 0.1 MPa.

[0103] Figure 9 Table 4 shows the pure water flux, media flux, and pure water recovery rate of membranes prepared with different concentrations of grafted monomers obtained in Example 5. It can be seen that the pure water flux and media flux of the grafted membrane both increase significantly, and the pure water recovery rate is also very high, indicating that the modified membrane has excellent antifouling effect.

[0104] Table 4. Data on pure water, dielectric flux, and pure water recovery rate for membranes prepared with different graft monomer concentrations.

[0105]

[0106] In summary, the graft copolymer of this invention effectively improves its polarity and molecular chain flexibility, making it less prone to cross-linking and exhibiting good dispersibility and solubility in solvents. When preparing films, it shows good compatibility with pore-forming agents, resulting in films with good hydrophilicity. Because the grafting rate of the graft copolymer is controlled within a specific range, the resulting film has a reasonable ratio of main chain to side chain structure and a uniform distribution of hydrophilic groups on the side chains, thus exhibiting better hydrophilicity. Simultaneously, the stability of the original main chain structure of the graft copolymer macroscopically ensures the pore size of the film, resulting in a significant increase in water flux while maintaining excellent filtration performance and superior resistance to protein fouling, showing great promise for wastewater treatment applications. This invention grafts PEGMA onto the PES material matrix, allowing for the preparation of graft copolymers with different grafting rates as needed, providing greater application flexibility, and also improving the performance of the graft copolymer itself.

[0107] The embodiments of the present invention have been described above in conjunction with the accompanying drawings. However, the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention. Any changes, modifications, substitutions, combinations or simplifications made based on the spirit and principle of the technical solution of the present invention shall be equivalent substitutions. As long as they meet the purpose of the invention and do not deviate from the technical principles and inventive concept of the polyethersulfone-grafted polyethylene glycol methacrylate copolymer, film and its preparation method, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a polyethersulfone-grafted polyethylene glycol methacrylate copolymer, characterized in that, Includes the following steps: (1) Raw material pretreatment: The raw material polyethersulfone was washed, soaked, and then dried to constant weight; (2) Co-radiative grafting reaction process: The polyethersulfone obtained after drying in step (1) is mixed with polyethylene glycol methacrylate monomer to prepare a homogeneous solution. The solvent of the homogeneous solution is N,N-dimethylacetamide. The mass ratio of polyethersulfone to polyethylene glycol methacrylate monomer is 10:5 to 10:

9. The mass percentage concentration of polyethylene glycol methacrylate monomer in the homogeneous solution is 5% to 9%. The mass percentage concentration of polyethersulfone in the homogeneous solution is 10% to 15%. In the homogeneous solution containing polyethylene glycol methacrylate monomer and polyethersulfone, the polyethylene glycol methacrylate monomer and polyethersulfone are subjected to a co-radiative grafting reaction. The radiation source for the co-radiative grafting reaction is 60 Co; the total radiation dose of the co-radiation grafting reaction is 6~30 kGy; the average dose rate of the co-radiation grafting reaction is 1.67~5.00 kGy / h; the temperature of the co-radiation grafting reaction is 20~30℃; (3) Post-treatment of grafting reaction products: The homogeneous solution obtained after the co-radiative grafting reaction in step (2) is then post-treated; the post-treatment is performed according to the following steps: After the co-radiative grafting reaction, a homogeneous solution is obtained and precipitated in deionized water. The resulting solid is washed, then soaked in deionized water, and then vacuum dried to constant weight to obtain polyethersulfone-grafted polyethylene glycol methacrylate copolymer. The soaking time in deionized water is 20-26 hours, the vacuum drying temperature is 50-80°C, and the vacuum degree of the vacuum drying is 0.06-0.08 MPa.

2. The method for preparing the polyethersulfone-grafted polyethylene glycol methacrylate copolymer according to claim 1, characterized in that: In step (1), the weight-average molecular weight of the polyethersulfone is 20,000 to 200,000.

3. The method for preparing the polyethersulfone-grafted polyethylene glycol methacrylate copolymer according to claim 2, characterized in that: In step (1), during the pretreatment process, the raw material polyethersulfone is washed with deionized water and then soaked in deionized water for more than a week, during which the deionized water is replaced, and then vacuum dried to constant weight; the temperature of the vacuum drying is 60~80℃; the vacuum degree of the vacuum drying is 0.06~0.08MPa.

4. The method for preparing the polyethersulfone-grafted polyethylene glycol methacrylate copolymer according to claim 1, characterized in that, In step (2), the atmosphere of the co-radiative grafting reaction is an oxygen-free atmosphere; the oxygen-free atmosphere is at least one of nitrogen and argon.

5. A polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer, prepared by the preparation method of the polyethersulfone-grafted polyethylene glycol methacrylate copolymer according to any one of claims 1 to 4.

6. A polyethersulfone-grafted polyethylene glycol methacrylate copolymer film, using the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer of claim 5 as raw material, characterized in that, The preparation method of polyethersulfone-grafted polyethylene glycol methacrylate copolymer film includes the following steps: dissolving the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer in an organic solvent to prepare a casting solution; then coating the casting solution onto a substrate, forming a film by phase reversal in an aqueous solution, and then curing it to obtain a film.

7. The polyethersulfone-grafted polyethylene glycol methacrylate copolymer film according to claim 6, characterized in that: In its preparation method, the mass percentage concentration of the polyethersulfone-grafted polyethylene glycol methacrylate monomer copolymer in the casting solution is 16-20%; the organic solvent in the casting solution is N,N-dimethylacetamide; and the film curing conditions are: curing in water at 18-25°C for 46-50 hours.

8. The polyethersulfone-grafted polyethylene glycol methacrylate copolymer film according to claim 6, characterized in that: In its preparation method, the thickness of the prepared film is 180~250μm.

Citation Information

Patent Citations

  • Polyether sulfone grafted N-vinylpyrrolidone copolymer, film and preparation methods

    CN107641178A

  • Copolymer comprising at least three blocks: polyamide blocks, peg blocks and other blocks

    CN107001643A

  • Modified nanofiltration membrane suitable for recycling industrial wastewater, and production method and application thereof

    CN107486039A

  • Polyether sulfone grafted acrylic monomer copolymer and preparation method thereof

    CN107641177A

  • Method for graft modification of polyethersulfone

    CN1844175A