Short track speed skating protective pad based on slow rebound foam material and preparation method thereof

By adopting multi-layer structure slow rebound foam protective pads on the short track speed skating competition field, combined with open and closed foam, the existing protective pads have been solved, and the athletes have been significantly improved security protection.

CN111923544BActive Publication Date: 2024-11-26DINGZHOU TIANHUA SPORTS GOODS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010768821.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-03
Publication Date
2024-11-26
Estimated Expiration
2040-08-03

AI Technical Summary

Technical Problem

The protective pads of the existing short track speed skating competition are composed of foam of a single nature, which cannot effectively buffer the impact force of athletes and is prone to rebound, which poses a major safety hazard.

Method used

Adopt a protective pad design based on slow rebound foam material. By combining open foam with slow rebound sealed foam, a multi-layer structure is formed, and a waterproof and wear-resistant wrapping layer is coated on the outside of the structural layer to increase the breathable mesh. cloth to reduce rebound force.

Benefits of technology

It improves the buffering effect of impact force, eliminates the rebound phenomenon of protective pads, greatly improves safety protection performance, and protects athletes more effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111923544B_ABST
    Figure CN111923544B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of protective props for short track speed skating competitions in winter sports, in particular to a short track speed skating protective pad based on a slow-rebound foam material and a preparation method thereof, comprising a structural layer, the outer side of the structural layer is coated with a wrapping layer, the structural layer is an open foam, the structural layer comprises a first structural layer, a second structural layer, a third structural layer and a fourth structural layer, and buffer layers are equidistantly bonded between the first structural layer and the second structural layer, between the second structural layer and the third structural layer, and between the third structural layer and the fourth structural layer, and the buffer layer is a slow-rebound closed foam. The present invention adopts an arrangement structure combining an open foam and a slow-rebound closed foam, which can improve the buffering effect of the impact force, can effectively eliminate the rebound phenomenon of the protective pad, greatly improve the safety protection performance of the protective pad, can better protect athletes, and is worthy of popularization and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of protective props for short track speed skating competitions in winter sports, and in particular to a short track speed skating protective pad based on a slow-rebound foam material and a preparation method thereof. Background Art

[0002] When athletes compete in short track speed skating, due to their very fast skating speed, once they fall or collide with others, they will be rushed to the sidelines under the action of centrifugal force. Currently, protective pads are set up around skating stadiums to cushion the impact force of athletes and protect them. However, the protective pads currently used are composed of foam of a single property, and the cushioning effect on the impact force of athletes is not ideal. At the same time, when the athlete hits the protective pad, a large rebound force is easily generated, which poses a great safety hazard to the athletes and has great limitations in use. Summary of the invention

[0003] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a short track speed skating protective pad based on a slow rebound foam material and a preparation method thereof.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] A short track speed skating protective pad is designed based on a slow rebound foam material, comprising a structural layer, the outer side of the structural layer is coated with a wrapping layer, the structural layer comprises a first open foam layer, a buffer layer, a second open foam layer, a third open foam layer and a fourth open foam layer, buffer layers are equidistantly bonded between the first open foam layer and the second open foam layer, between the second open foam layer and the third open foam layer, and between the third open foam layer and the fourth open foam layer, the buffer layer is a slow rebound closed foam, there is a 20 cm hollow space between two adjacent buffer layer foams, the hollow space height is from the bottom to the top of the protective pad foam, the first open foam layer, the second open foam layer, the third open foam layer and the fourth open foam layer are all open foams, the left portion of the front side of the wrapping layer is fixedly connected with a first Velcro patch used in conjunction with a first Velcro mother patch, and a breathable mesh is provided in the middle of the upper surface of the wrapping layer.

[0006] Preferably, a handle is symmetrically fixedly connected to the middle portion of the left side of the wrapping layer.

[0007] Preferably, a seat belt buckle is equidistantly connected to the rear side of the wrapping layer, a seat belt is inserted into the interior of the seat belt buckle, and a seat belt tensioner is fixedly connected to the left end of the seat belt.

[0008] Preferably, the upper and lower parts of the front side of the wrapping layer are respectively bonded with second Velcro tapes.

[0009] Preferably, the slow-rebound closed foam is prepared from raw materials in the following proportions: 50 parts of slow-rebound polyether 1030 polyol, 47.5 parts of TDI, 0.08-0.18 parts of T-9 stannous octoate catalyst, 0.2-0.26 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry.

[0010] Preferably, the open foam is prepared from raw materials in the following proportions: 50 parts of ordinary polyether 3050 polyol, 47.5 parts of TDI, 0.08-0.18 parts of T-9 stannous octoate catalyst, 0.2-0.26 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry.

[0011] The present invention also provides a production step for producing a slow-rebound closed foam, and the production of the slow-rebound closed foam comprises the following steps:

[0012] The first step is to put the slow rebound polyether 1030 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 5-10 minutes to fully mix the raw materials;

[0013] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of slow-rebound closed foam.

[0014] The present invention also provides a production step for the open foam, and the production of the open foam comprises the following steps:

[0015] The first step is to put common polyether 3050 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 5-10 minutes to fully mix the raw materials;

[0016] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of open foam.

[0017] The short track speed skating protective pad based on slow-rebound foam material and the preparation method thereof proposed in the present invention have the beneficial effects that: the present invention adopts an arrangement structure combining open foam and slow-rebound closed foam, which can improve the buffering effect of impact force, can effectively eliminate the rebound phenomenon of the protective pad, greatly improve the safety protection performance of the protective pad, can better protect athletes, and is worthy of popularization and use.

[0018] The invention has short production process, low material viscosity, easy control, energy saving, small equipment investment and wide applicable density range. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the structure in the direction A of the short track speed skating protection pad based on the slow rebound foam material proposed by the present invention;

[0020] Figure 2 This is a schematic diagram of the three-dimensional structure of the short track speed skating protection pad based on the slow-rebound foam material proposed by the present invention;

[0021] Figure 3 This is a schematic diagram of the installation and use structure of the short track speed skating protection pad based on the slow rebound foam material proposed by the present invention.

[0022] In the figure: wrapping layer 1, structural layer 2, first open foam layer 3, buffer layer 4, second open foam layer 5, third open foam layer 6, fourth open foam layer 7, seat belt tensioner 8, first Velcro 9, seat belt buckle 10, first Velcro sub-tape 11, seat belt 12, second Velcro 13, handle 14, breathable mesh 15. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Example

[0024] Reference Figure 1-3 The short track speed skating protective pad based on slow rebound foam material includes a structural layer 2, the outer side of the structural layer 2 is covered with a wrapping layer 1, the wrapping layer 1 is sky blue, the wrapping layer 1 is waterproof, wear-resistant, and cut-resistant, and has good softness. The softness remains unchanged at low temperatures. A handle 14 is symmetrically fixedly connected to the middle of the left side of the wrapping layer 1, which is convenient for pulling the device to move, thereby improving the use effect of the device.

[0025] The rear side of the wrapping layer 1 is equidistantly connected with a safety belt buckle 10, a safety belt 12 is inserted inside the safety belt buckle 10, and a safety belt tensioner 8 is fixedly connected to the left end of the safety belt 12, so that the two sets of protective pads can be connected together, and the operation is simple and convenient.

[0026] The upper and lower front sides of the wrapping layer 1 are respectively bonded with second Velcro mother patches 13, which can be bonded with Velcro sub-patches on the advertising cloth to facilitate advertising. Moreover, the bonding method of the Velcro makes it convenient to replace the advertising cloth, which is more practical.

[0027] The structural layer 2 includes a first open foam layer 3, a buffer layer 4, a second open foam layer 5, a third open foam layer 6 and a fourth open foam layer 7. The buffer layer 4 is equidistantly bonded between the first open foam layer 3 and the second open foam layer 5, between the second open foam layer 5 and the third open foam layer 6, and between the third open foam layer 6 and the fourth open foam layer 7. The buffer layer 4 is a slow-rebound closed foam. The slow-rebound closed foam is prepared from raw materials in the following proportions: 50 parts of slow-rebound polyether 1030 polyol, 47.5 parts of TDI, 0.08 parts of T-9 stannous octoate catalyst, 0.2 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 pore opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow paste.

[0028] The density of the slow-rebound closed foam is 32.04kg / m3, the thickness of the buffer layer 4 is 16cm, and there is a 20cm hollow space between the foams of two adjacent buffer layers 4. The height of the hollow space is from the bottom to the top of the protective pad foam, ensuring that the gas in the foam is quickly discharged when the athlete collides, reducing the impact force, avoiding rebound, and better protecting the athlete. The top of the wrapping layer 1 is a breathable mesh 15, which is mainly used for exhaust and can play a buffering role together with the built-in foam layout structure. When the athlete hits the protective pad, the gas in the foam is quickly discharged through the breathable mesh, reducing the rebound force when the skater hits the protective pad, better absorbing the impact force when the skater hits the protective pad, and better protecting the athlete.

[0029] The first open foam layer 3, the second open foam layer 5, the third open foam layer 6 and the fourth open foam layer 7 are all open foams, and the open foams are prepared from raw materials containing the following proportions: 50 parts of ordinary polyether 3050 polyol, 47.5 parts of TDI, 0.08 parts of T-9 stannous octoate catalyst, 0.2 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry. The density of the open foam is 22.4kg / m3, the thickness of the first foam layer 3 is 16cm, and the thickness of the second foam layer 5, the third foam layer 6 and the fourth foam layer 7 is 12cm.

[0030] A first Velcro sub-tape 11 used in conjunction with the first Velcro female tape 9 is fixedly connected to the left portion of the front side of the wrapping layer 1 , and a breathable mesh 15 is provided in the middle portion of the upper surface of the wrapping layer 1 .

[0031] The present invention also provides a method for preparing a slow-rebound closed foam. The method comprises the following steps:

[0032] The first step is to put the slow rebound polyether 1030 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 5 minutes to fully mix the raw materials;

[0033] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of slow-rebound closed foam.

[0034] The present invention also provides a production step for the open foam, and the production of the open foam comprises the following steps:

[0035] The first step is to put common polyether 3050 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 5 minutes to fully mix the raw materials;

[0036] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of open foam. Example

[0037] Reference Figure 1-3 The short track speed skating protective pad based on slow rebound foam material includes a structural layer 2, the outer side of the structural layer 2 is covered with a wrapping layer 1, the wrapping layer 1 is sky blue, the wrapping layer 1 is waterproof, wear-resistant, and cut-resistant, and has good softness. The softness remains unchanged at low temperatures. A handle 14 is symmetrically fixedly connected to the middle of the left side of the wrapping layer 1, which is convenient for pulling the device to move, thereby improving the use effect of the device.

[0038] The rear side of the wrapping layer 1 is equidistantly connected with a safety belt buckle 10, a safety belt 12 is inserted inside the safety belt buckle 10, and a safety belt tensioner 8 is fixedly connected to the left end of the safety belt 12, so that the two sets of protective pads can be connected together, and the operation is simple and convenient.

[0039] The upper and lower front sides of the wrapping layer 1 are respectively bonded with second Velcro mother patches 13, which can be bonded with Velcro sub-patches on the advertising cloth to facilitate advertising. Moreover, the bonding method of the Velcro makes it convenient to replace the advertising cloth, which is more practical.

[0040] The structural layer 2 includes a first open foam layer 3, a buffer layer 4, a second open foam layer 5, a third open foam layer 6 and a fourth open foam layer 7. The buffer layer 4 is equidistantly bonded between the first open foam layer 3 and the second open foam layer 5, between the second open foam layer 5 and the third open foam layer 6, and between the third open foam layer 6 and the fourth open foam layer 7. The buffer layer 4 is a slow-rebound closed foam. The slow-rebound closed foam is prepared from raw materials containing the following proportions: 50 parts of slow-rebound polyether 1030 polyol, 47.5 parts of TDI, 0.13 parts of T-9 stannous octoate catalyst, 0.23 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 pore opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow paste.

[0041] The density of the slow-rebound closed foam is 32.04kg / m3, the thickness of the buffer layer 4 is 16cm, and there is a 20cm hollow space between the foams of two adjacent buffer layers 4. The height of the hollow space is from the bottom to the top of the protective pad foam, ensuring that the gas in the foam is quickly discharged when the athlete collides, reducing the impact force, avoiding rebound, and better protecting the athlete. The top of the wrapping layer 1 is a breathable mesh 15, which is mainly used for exhaust and can play a buffering role together with the built-in foam layout structure. When the athlete hits the protective pad, the gas in the foam is quickly discharged through the breathable mesh, reducing the rebound force when the skater hits the protective pad, better absorbing the impact force when the skater hits the protective pad, and better protecting the athlete.

[0042] The first open foam layer 3, the second open foam layer 5, the third open foam layer 6 and the fourth open foam layer 7 are all open foams, and the open foams are prepared from raw materials containing the following proportions: 50 parts of ordinary polyether 3050 polyol, 47.5 parts of TDI, 0.13 parts of T-9 stannous octoate catalyst, 0.23 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry. The density of the open foam is 22.4kg / m3, the thickness of the first foam layer 3 is 16cm, and the thickness of the second foam layer 5, the third foam layer 6 and the fourth foam layer 7 is 12cm.

[0043] A first Velcro sub-tape 11 used in conjunction with the first Velcro female tape 9 is fixedly connected to the left portion of the front side of the wrapping layer 1 , and a breathable mesh 15 is provided in the middle portion of the upper surface of the wrapping layer 1 .

[0044] The present invention also provides a production step for producing a slow-rebound closed foam, and the production of the slow-rebound closed foam comprises the following steps:

[0045] The first step is to put the slow-rebound polyether 1030 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 8 minutes to fully mix the raw materials;

[0046] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of slow-rebound closed foam.

[0047] The present invention also provides a process for making an open foam, and the process for making the open foam comprises the following steps:

[0048] The first step is to put common polyether 3050 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 8 minutes to fully mix the raw materials;

[0049] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of open foam. Example

[0050] Reference Figure 1-3 The short track speed skating protective pad based on slow rebound foam material includes a structural layer 2, the outer side of the structural layer 2 is covered with a wrapping layer 1, the wrapping layer 1 is sky blue, the wrapping layer 1 is waterproof, wear-resistant, and cut-resistant, and has good softness. The softness remains unchanged at low temperatures. A handle 14 is symmetrically fixedly connected to the middle of the left side of the wrapping layer 1, which is convenient for pulling the device to move, thereby improving the use effect of the device.

[0051] The rear side of the wrapping layer 1 is equidistantly connected with a safety belt buckle 10, a safety belt 12 is inserted inside the safety belt buckle 10, and a safety belt tensioner 8 is fixedly connected to the left end of the safety belt 12, so that the two sets of protective pads can be connected together, and the operation is simple and convenient.

[0052] The upper and lower front sides of the wrapping layer 1 are respectively bonded with second Velcro mother patches 13, which can be bonded with Velcro sub-patches on the advertising cloth to facilitate advertising. Moreover, the bonding method of the Velcro makes it convenient to replace the advertising cloth, which is more practical.

[0053] The structural layer 2 includes a first open foam layer 3, a buffer layer 4, a second open foam layer 5, a third open foam layer 6 and a fourth open foam layer 7. The buffer layer 4 is equidistantly bonded between the first open foam layer 3 and the second open foam layer 5, between the second open foam layer 5 and the third open foam layer 6, and between the third open foam layer 6 and the fourth open foam layer 7. The buffer layer 4 is a slow-rebound closed foam. The slow-rebound closed foam is prepared from raw materials in the following proportions: 50 parts of slow-rebound polyether 1030 polyol, 47.5 parts of TDI, 0.18 parts of T-9 stannous octoate catalyst, 0.26 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 pore opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow paste.

[0054] The density of the slow-rebound closed foam is 32.04kg / m3, the thickness of the buffer layer 4 is 16cm, and there is a 20cm hollow space between the foams of two adjacent buffer layers 4. The height of the hollow space is from the bottom to the top of the protective pad foam, ensuring that the gas in the foam is quickly discharged when the athlete collides, reducing the impact force, avoiding rebound, and better protecting the athlete. The top of the wrapping layer 1 is a breathable mesh 15, which is mainly used for exhaust and can play a buffering role together with the built-in foam layout structure. When the athlete hits the protective pad, the gas in the foam is quickly discharged through the breathable mesh, reducing the rebound force when the skater hits the protective pad, better absorbing the impact force when the skater hits the protective pad, and better protecting the athlete.

[0055] The first open foam layer 3, the second open foam layer 5, the third open foam layer 6 and the fourth open foam layer 7 are all open foams, and the open foams are prepared from raw materials containing the following proportions: 50 parts of ordinary polyether 3050 polyol, 47.5 parts of TDI, 0.18 parts of T-9 stannous octoate catalyst, 0.26 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry. The density of the open foam is 22.4kg / m3, the thickness of the first foam layer 3 is 16cm, and the thickness of the second foam layer 5, the third foam layer 6 and the fourth foam layer 7 is 12cm.

[0056] A first Velcro sub-tape 11 used in conjunction with the first Velcro female tape 9 is fixedly connected to the left portion of the front side of the wrapping layer 1 , and a breathable mesh 15 is provided in the middle portion of the upper surface of the wrapping layer 1 .

[0057] The present invention also provides a method for preparing a slow-rebound closed foam. The method comprises the following steps:

[0058] The first step is to put the slow-rebound polyether 1030 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 10 minutes to fully mix the raw materials;

[0059] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of slow-rebound closed foam.

[0060] The present invention also provides a production step for the open foam, and the production of the open foam comprises the following steps:

[0061] The first step is to put common polyether 3050 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 10 minutes to fully mix the raw materials;

[0062] The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of open foam.

[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A short track speed skating protective pad based on a slow rebound foam material, comprising a structural layer (2), the outer side of the structural layer (2) being coated with a wrapping layer (1), characterized in that: The structural layer (2) comprises a first open foam layer (3), a buffer layer (4), a second open foam layer (5), a third open foam layer (6) and a fourth open foam layer (7); the buffer layer (4) is equidistantly bonded between the first open foam layer (3) and the second open foam layer (5), between the second open foam layer (5) and the third open foam layer (6), and between the third open foam layer (6) and the fourth open foam layer (7); the buffer layer (4) is a slow-rebound closed foam; there is a 20 cm hollow space between the foams of two adjacent buffer layers (4); the hollow space has a height from the bottom to the top of the protective pad foam; the first open foam layer (3), the second open foam layer (5), the third open foam layer (6) and the fourth open foam layer (7) are all open foams; the left portion of the front side of the wrapping layer (1) is fixedly connected to a first Velcro (11) used in conjunction with the first Velcro mother tape (9); and a breathable mesh (15) is provided in the middle of the upper surface of the wrapping layer (1).

2. The short track speed skating protective pad based on slow rebound foam material according to claim 1, characterized in that: A handle (14) is symmetrically fixedly connected to the middle portion of the left side of the wrapping layer (1).

3. The short track speed skating protective pad based on slow rebound foam material according to claim 1, characterized in that: Safety belt buckles (10) are equidistantly connected to the rear side of the wrapping layer (1), a safety belt (12) is inserted into the interior of the safety belt buckle (10), and a safety belt tensioner (8) is fixedly connected to the left end of the safety belt (12).

4. The short track speed skating protective pad based on slow rebound foam material according to claim 1, characterized in that: The upper and lower front portions of the wrapping layer (1) are respectively bonded with second Velcro tapes (13).

5. The short track speed skating protective pad based on slow rebound foam material according to claim 1, characterized in that: The slow-rebound closed foam is prepared from raw materials in the following proportions: 50 parts of slow-rebound polyether 1030 polyol, 47.5 parts of TDI, 0.08-0.18 parts of T-9 stannous octoate catalyst, 0.2-0.26 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry.

6. The short track speed skating protective pad based on slow rebound foam material according to claim 1, characterized in that: The open foam is prepared from raw materials in the following proportions: 50 parts of common polyether 3050 polyol, 47.5 parts of TDI, 0.08-0.18 parts of T-9 stannous octoate catalyst, 0.2-0.26 parts of Dabco33-LV amine catalyst, 2.5 parts of MK-01 cell opener, 1 part of B8002 silicone oil, 2.6 parts of water, and 0.04 parts of yellow slurry.

7. The method for preparing a short track speed skating protective pad based on a slow rebound foam material according to claim 5, characterized in that: The preparation of the slow-rebound closed foam comprises the following steps: The first step is to put the slow rebound polyether 1030 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 5-10 minutes to fully mix the raw materials; The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of slow-rebound closed foam.

8. The method for preparing a short track speed skating protective pad based on a slow rebound foam material according to claim 6, characterized in that: The preparation of the open foam comprises the following steps: The first step is to put common polyether 3050 polyol, TDI, T-9 stannous octoate catalyst, Dabco33-LV amine catalyst, MK-01 cell opener, B8002 silicone oil, water and yellow slurry into a high-speed stirring device and stir at high speed for 5-10 minutes to fully mix the raw materials; The second step is to quickly put the mixed raw materials into a molding box, complete the chain growth, foaming, cross-linking and curing reactions in the molding box, and complete the production of open foam.