Lithium iron battery and its formation, aging and capacity separation process

By using the lithium iron phosphate battery formation, aging, and capacity testing process, a uniform and dense SEI film is formed through hot pressing, low-rate activation, and multiple aging processes. This solves the problem of the suboptimal SEI film in existing lithium batteries, improves the cycle life and safety of the cell, and reduces the cell expansion rate.

CN111987376BActive Publication Date: 2024-11-15SHANGHAI JINYU INTELLIGENT EQUIP MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010716762.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-23
Publication Date
2024-11-15
Estimated Expiration
2040-07-23

AI Technical Summary

Technical Problem

The SEI film formed in the current lithium battery manufacturing process has not yet reached an ideal state, resulting in short cell cycle life, insufficient safety and stability, and cell swelling during charging and discharging.

Method used

The lithium iron phosphate battery formation, aging, and capacity testing process includes hot-pressing of positive and negative electrode sheets and separators, low-rate activation, multiple aging and capacity testing processes. Low-rate activation promotes the uniformity and density of the SEI film, and cyclic activation forms a more complete SEI film. Finally, vacuuming and sealing are performed.

Benefits of technology

It significantly improves the cycle life and safety of the battery cells, reduces the expansion rate of the cells, and forms a denser and more stable SEI film, thereby improving the charge and discharge performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111987376B_ABST
    Figure CN111987376B_ABST
Patent Text Reader

Abstract

An iron-lithium battery and its formation, aging and capacity division process belong to the technical field of lithium battery manufacturing. The iron-lithium battery formation, aging and capacity division process firstly hot-presses the positive and negative electrode sheets and the diaphragm to obtain a battery core, performs low-rate activation while hot-pressing, then performs primary aging on the battery core, performs cycle activation after the primary aging, and then performs secondary aging. After the secondary aging, the battery core is vacuumed, vented, shaped and sealed, and finally the battery is divided. The present invention can greatly improve the cycle life of the battery core, as well as the safety and stability of the battery core, and reduce the degree of swelling of the battery core during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technology in the field of lithium battery manufacturing, in particular to an iron-lithium battery and its formation, aging and capacity separation process. Background Art

[0002] During the first charge and discharge process of liquid lithium-ion batteries, the electrode material and the electrolyte react at the solid-liquid interface to form a passivation film covering the surface of the electrode material. This passivation film can effectively prevent the passage of solvent molecules, but Li + However, it can be freely embedded and removed, and has the characteristics of a solid electrolyte, so this passivation film is called a "solid electrolyte interface film (SEI film)". However, the SEI film formed in the current lithium battery manufacturing process has not yet reached an ideal state.

[0003] In order to solve the above problems in the prior art, the present invention is provided. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes an iron-lithium battery and a formation, aging and capacity division process thereof, which can greatly improve the cycle life of the battery cell as well as the safety and stability of the battery cell and reduce the degree of swelling of the battery cell during use.

[0005] The invention relates to a formation, aging and capacity separation process for an iron-lithium battery. Firstly, positive and negative electrode sheets and a separator are hot pressed to obtain a battery core, low-rate activation is performed while hot pressing, and then the battery core is aged once. After the primary aging is completed, cycle activation is performed, and then secondary aging is performed. After the secondary aging, the battery core is vacuumed, vented, shaped and sealed, and finally the battery is separated.

[0006] Preferably, the hot pressing is carried out under the conditions of 0.5-3 kN pressure and 30-55°C heating.

[0007] Preferably, the low rate activation is to charge at a constant current rate of 0.01-0.2C for 1-10 hours under hot pressing conditions, and then stand for 0.5 hours after the low rate activation.

[0008] Preferably, the primary aging is aging at 40-55° C. for 12-72 h.

[0009] Preferably, the cyclic activation process is as follows: charging at a constant current and constant voltage of 0.2-1C to a cut-off voltage of 3.45-3.6V and a cut-off current of 0.01-0.05C, standing for 1-10 minutes, then discharging at a constant current of 0.2-1C to a cut-off voltage of 2.0-2.8V, and standing for 1-10 minutes; repeating the above operation 2-5 times.

[0010] Preferably, the secondary aging is aging at 40-55° C. for 12-72 h.

[0011] Preferably, the capacity division process is as follows: charging at a constant current and constant voltage of 0.2-1C to a cut-off voltage of 3.65V and a cut-off current of 0.02C, standing for 5 minutes, discharging at a constant current of 0.2-1C to a cut-off voltage of 2.5V, and standing for another 5 minutes; repeating the charge and discharge steps once to complete the capacity division.

[0012] The invention relates to an iron-lithium battery, which is manufactured by adopting the above process.

[0013] Technical Effects

[0014] Compared with the prior art, the present invention has the following technical effects:

[0015] 1) During the low-rate activation process, the low activation current plus a certain pressure can promote the uniform density of the SEI film on the interface of the iron-lithium battery cell. In the later stage of battery cell charging and discharging, it can effectively reduce the reaction between the negative electrode interface and the electrolyte, thereby improving the stability, safety and cycle performance of the battery cell;

[0016] 2) The SEI film in the prepared battery is denser and more uniform at the microscopic level, more complete and stable at the macroscopic level, the infiltration effect of the positive and negative active particles with the electrolyte is more sufficient, and the interface reaction effect is better;

[0017] 3) The prepared battery has better cycle performance and safety and stability; specifically, on the one hand, the room temperature cycle life of the battery cell is increased by 1000-1500 times on the original basis to 3700-3800 times, and on the other hand, the expansion rate of the battery cell during the cycle is about 4%-6%, which is much lower than the expansion rate of 11%-14% of the existing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a curve of the capacity retention rate of the 50Ah battery cell at room temperature and 1C charge and discharge cycles in Example 1. DETAILED DESCRIPTION

[0019] The present invention is described in detail below with reference to the accompanying drawings and specific implementation modes.

[0020] In the embodiment of the present invention, the positive and negative electrode sheets and the separator are first hot pressed to obtain the battery cell, and low-rate activation is performed while hot pressing. Then, the battery cell is aged once. After the completion of the primary aging, the battery cell is activated again in a cycle, and then aged twice. After the secondary aging, the battery cell is vacuumed, shaped and sealed, and finally the battery is divided into different capacities to obtain a battery.

[0021] Preferably, the hot pressing is carried out under the conditions of 0.5-3 kN pressure and 30-55°C heating.

[0022] Preferably, the low rate activation is to charge at a constant current rate of 0.01-0.15C for 1-8 hours under hot pressing conditions, and then stand for 0.5 hours after the low rate activation;

[0023] Preferably, the primary aging is aging at 40-55° C. for 12-72 h.

[0024] Preferably, the cyclic activation process is as follows: charging at a constant current and constant voltage of 0.2-1C to a cut-off voltage of 3.45-3.6V and a cut-off current of 0.01-0.05C, standing for 1-10 minutes, then discharging at a constant current of 0.2-1C to a cut-off voltage of 2.0-2.8V, and standing for 1-10 minutes; repeating the above operation 2-5 times.

[0025] Preferably, the secondary aging is aging at 40-55° C. for 12-72 h.

[0026] Preferably, the capacity division process is as follows: charging at a constant current and constant voltage of 0.2-1C to a cut-off voltage of 3.65V and a cut-off current of 0.02C, standing for 5 minutes, discharging at a constant current of 0.2-1C to a cut-off voltage of 2.5V, and standing for another 5 minutes; repeating the charge and discharge steps once to complete the capacity division.

[0027] Example 1

[0028] This embodiment takes the preparation of a 50Ah square aluminum shell lithium iron battery cell as an example, and includes the following steps:

[0029] S1, place the positive and negative electrodes and the separator in a hot pressing fixture for hot pressing, with a pressure of 2kN and a temperature of 45°C; while hot pressing, charge at a constant current of 0.5A for 8h or 7.5A for 2h for low rate activation, and then let it stand for 0.5h;

[0030] S2, take out the static battery cells in S1 and place them in the aging room, aging at 45℃ for 24h;

[0031] S3, after the aging in S2 is completed, the battery cell is taken out and placed in a formation cabinet for cyclic activation, and the number of cycles is 3 times; the single process is as follows: charge at a constant current and constant voltage of 25A to a cut-off voltage of 3.6V and a cut-off current of 1A, stand for 5 minutes, then discharge at a constant current of 25A to a cut-off voltage of 2.5V, and stand for another 5 minutes;

[0032] S4, take out the battery cells in S3 and place them in an aging room at 45℃ for 36h;

[0033] S5, after the aging in S4 is completed, the battery cells are taken out, vacuumed, shaped and sealed, and then placed on the capacity division cabinet for capacity division; the capacity division process is as follows: first charge with 10A constant current and constant voltage, cut-off voltage 3.65V, cut-off current 1A, stand for 5 minutes, then discharge with 25A constant current, cut-off voltage 2.5V, and stand for 5 minutes; then charge with 25A constant current and constant voltage, cut-off voltage 3.65V, cut-off current 1A, stand for 5 minutes, then discharge with 25A constant current, cut-off voltage 2.5V, and stand for 5 minutes;

[0034] S6, finally conduct capacity internal resistance screening and electrical performance spot check test.

[0035] In this embodiment, hot pressing and low-rate activation are performed simultaneously, so that the positive and negative electrodes are effectively and closely contacted with the diaphragm, the heat conduction efficiency is increased, high-temperature activation is performed, the rapid formation of the SEI film is promoted, and the volume expansion of the battery cell during the formation process is suppressed, so that the formed SEI film is denser and more stable, thereby avoiding the rupture and generation of the SEI film in the initial stage of the battery charge and discharge cycle, resulting in rapid capacity decay and gas expansion of the battery cell; several subsequent cycles of activation are performed to make the formed SEI film more sufficient and complete, thereby significantly reducing the capacity decay rate of the battery cell in the initial stage; at the same time, the above process can form a good negative electrode interface, avoiding the safety hazards and capacity decay caused by spotty lithium deposition at the negative electrode interface during the charge and discharge process.

[0036] In the electrical performance test, the battery 1C charge and discharge cycle capacity retention rate is as follows Figure 1 As shown, according to the prediction, the final cycle life of the battery cell at room temperature will be increased by 1000-1500 times on the original basis, reaching 3700-3800 times.

[0037] Example 2

[0038] This embodiment takes the preparation of a 50Ah square aluminum shell lithium iron battery cell as an example, and includes the following steps:

[0039] S1, place the positive and negative electrodes and the separator in a hot pressing fixture for hot pressing at a pressure of 0.5 kN and a temperature of 50 °C; while hot pressing, charge at a constant current of 5A for 1 hour for low rate activation, and then let it stand for 0.5 hour;

[0040] S2, take out the static battery cells in S1 and place them in the aging room, aging at 45℃ for 24h;

[0041] After aging in S3 and S2, the battery is taken out and placed in a formation cabinet for cyclic activation. The number of cycles is 5. The single process is as follows: charge at a constant current and constant voltage of 40A to a cut-off voltage of 3.5V and a cut-off current of 2.4A, stand for 5 minutes, then discharge at a constant current of 40A to a cut-off voltage of 2.5V, and stand for another 5 minutes.

[0042] S4, take out the battery cells in S3 and place them in an aging room at 45℃ for 36h;

[0043] S5, after the aging in S4 is completed, the battery cells are taken out, vacuumed, shaped and sealed, and then placed on the capacity division cabinet for capacity division; the capacity division process is as follows: first charge with a constant current and constant voltage of 45A, a cut-off voltage of 3.65V, a cut-off current of 1A, stand for 5 minutes, then discharge with a constant current of 45A, a cut-off voltage of 2.5V, and then stand for 5 minutes; then charge with a constant current and constant voltage of 45A, a cut-off voltage of 3.65V, a cut-off current of 1A, stand for 5 minutes, then discharge with a constant current of 45A, a cut-off voltage of 2.5V, and then stand for 5 minutes;

[0044] S6, finally conduct capacity internal resistance screening and electrical performance spot check test.

[0045] Example 3

[0046] This embodiment takes the preparation of a 50Ah square aluminum shell lithium iron battery cell as an example, and includes the following steps:

[0047] S1, place the positive and negative electrodes and the separator in a hot pressing fixture for hot pressing at a pressure of 3kN and a temperature of 35°C; while hot pressing, charge at a constant current of 3A for 5h for low rate activation, and then let it stand for 0.5h;

[0048] S2, take out the static battery cells in S1 and place them in the aging room, aging at 45℃ for 24h;

[0049] S3, after the aging in S2 is completed, the battery cell is taken out and placed in a formation cabinet for cyclic activation, and the number of cycles is 2; the single process is as follows: charge at a constant current and constant voltage of 20A to a cut-off voltage of 3.5V and a cut-off current of 2.0A, stand for 5 minutes, then discharge at a constant current of 20A to a cut-off voltage of 2.3V, and stand for another 5 minutes;

[0050] S4, take out the battery cells in S3 and place them in an aging room at 45℃ for 36h;

[0051] S5, after the aging in S4 is completed, the battery cells are taken out, vacuumed, shaped and sealed, and then placed on the capacity division cabinet for capacity division; the capacity division process is as follows: first charge with 30A constant current and constant voltage, cut-off voltage 3.65V, cut-off current 1A, stand for 5 minutes, then discharge with 30A constant current, cut-off voltage 2.5V, and stand for 5 minutes; then charge with 30A constant current and constant voltage, cut-off voltage 3.65V, cut-off current 1A, stand for 5 minutes, then discharge with 30A constant current, cut-off voltage 2.5V, and stand for 5 minutes;

[0052] S6, finally conduct capacity internal resistance screening and electrical performance spot check test.

[0053] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A formation, aging and capacity separation process for lithium iron batteries, characterized in that: First, the positive and negative electrodes and the separator are hot-pressed under a pressure of 0.5-3kN and a heating condition of 30-55°C to obtain a battery cell. During the hot-pressing, the battery cell is charged at a constant current of 0.01-0.2C for 1-10h for low-rate activation, and then left to stand after the low-rate activation. Then, the battery cell is aged for 12-72h at 40-55°C, and then cycle activation is performed after the primary aging is completed. After that, the battery cell is aged for 12-72h at 40-55°C for a second time. After the secondary aging, the battery cell is vacuumed, vented, shaped and sealed, and finally the battery cell is divided into different capacities. The cyclic activation process is as follows: charging at a constant current and constant voltage of 0.2-1C to a cut-off voltage of 3.45-3.6V and a cut-off current of 0.01-0.05C, standing for 1-10 minutes, then discharging at a constant current of 0.2-1C to a cut-off voltage of 2.0-2.8V, and standing for 1-10 minutes; repeating the above operation 2-5 times.

2. The iron-lithium battery formation aging capacity separation process according to claim 1 is characterized in that: The capacity division process is as follows: charging at a constant current and constant voltage of 0.2-1C to a cut-off voltage of 3.65V and a cut-off current of 0.02C, standing for 5 minutes, discharging at a constant current of 0.2-1C to a cut-off voltage of 2.5V, and standing for another 5 minutes; repeating the charge and discharge steps once to complete the capacity division.

3. An iron-lithium battery, characterized in that: The invention is manufactured by the process described in claim 1 or 2.