Preparation method of graphite phase carbonized nitrogen / graphite negative electrode composite material with peapod structure
The tubular graphite phase carbonized nitrogen-coated flake graphite composite prepared by dry ball milling solves the problems of easy structural damage and insufficient conductivity of the negative electrode material of sodium ion batteries, achieves a combination of high specific capacity and high rate performance, and significantly improves The material's cycle stability and conductivity are suitable for sodium-ion battery anodes.
Patent Information
- Application Number
- CN202010938230.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The structure of existing sodium-ion battery anode material graphite is easily damaged during the deintercalation process of sodium ions, resulting in poor cycle performance. In addition, the conductivity and cycle stability of graphite-phase carbonized nitrogen are insufficient, making it difficult to achieve a combination of high specific capacity and high rate performance.
The dry ball milling method is used to prepare tubular graphite phase carbide nitride (g-C3N4) coated flake graphite composites. The inner core amorphous graphite improves the conductivity, and the outer layer g-C3N4 increases chemical stability and specific surface area, forming a composite material to improve Electronic conduction and sodium ion storage capacity.
It achieves the perfect combination of high specific capacity, high rate performance and high cycle performance of sodium-ion battery anode materials, significantly improves the material's conductivity and cycle stability, and is suitable for use as sodium-ion battery anode materials.
Smart Images

Figure CN112054175B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a method for preparing a graphite phase carbonized nitrogen / graphite composite material with a peapod structure applied to a negative electrode of a sodium ion battery. Background Art
[0002] In recent years, energy and environmental issues have become increasingly prominent, and lithium resources are limited and difficult to mine. Therefore, it is urgent to develop a safe and efficient energy storage system that has high energy conversion efficiency, long cycle life, and can replace lithium batteries. Sodium-ion batteries have a similar working principle to lithium-ion batteries, and sodium resources are abundant, widely distributed, and inexpensive, making sodium-ion batteries return to the field of vision of scientific researchers. At present, the reported negative electrode materials for sodium-ion batteries mainly include carbon-based materials, alloy materials, embedded materials, and conversion materials. However, there are few reports on commercialized graphite materials in lithium-ion batteries. This is mainly due to the fact that Na + Radius ratio Li + The radius is large, making Na + It is difficult to effectively deintercalate in graphite materials, and graphite is difficult to form stable NaC6 with sodium, so traditional graphite materials are not suitable for sodium storage.
[0003] Graphitic carbon nitride (g-C3N4) is a two-dimensional (2D) layered graphene-like carbon material composed of carbon atoms and nitrogen atoms in a certain ratio. It has attracted the attention of many researchers due to its rich porous structure, high nitrogen content, good chemical stability (resistance to acid, alkali and various organic solvents), simple preparation process, low cost, and potential high rate performance. However, g-C3N4 has poor conductivity and cycle stability, and Na + Low reversible storage (e.g., 10 mAh g -1 ), in order to improve the electronic conductivity and cycle stability, the present invention combines flake graphite with good conductivity with g-C3N4 to improve its conductivity, and further improve its electrochemical performance as a negative electrode material for sodium ion batteries.
[0004] The g-C3N4 coated flake graphite material proposed in the present invention is mainly an improvement plan for the technical problems existing in the application process of graphite and stone g-C3N4 as negative electrode materials for sodium ion batteries in the prior art. The existing graphite has low sodium storage performance, and it is easy to damage the structure during the sodium ion extraction process, showing poor cycle performance. g-C3N4 has good chemical stability and poor electrical conductivity, showing poor rate performance. The present invention designs a new composite carbon material, which has a tubular pod structure, a core of which is amorphous graphite and an outer layer of a few layers of g-C3N4. The inner core amorphous graphite increases the overall conductivity of the material, makes up for the disadvantages of g-C3N4, is more conducive to the conduction between electrons and the storage of sodium ions, and can improve the rate performance of the material; while the outer layer tubular g-C3N4 has an increased specific surface area and good chemical stability, which can alleviate the volume expansion problem of sodium ions in the process of embedding and extracting between flake graphite, and improve the cycle stability of the graphite material. Therefore, g-C3N4 coated flake graphite material achieves the perfect combination of high specific capacity, high rate performance and high cycle performance of sodium ion battery negative electrode materials. Summary of the invention
[0005] The g-C3N4 proposed by the present invention is composited with flake graphite, graphite is cheap, has good electrical conductivity, and the g-C3N4 structure is stable, which provides guarantee for the stability of the composite material, and the specific surface area of the whole composite material is moderate, and there are many active sites. In addition, it is very necessary to select an appropriate amount of graphite and a suitable ball milling rate and time. Because when the graphite content is too small, the traction force is not enough to make the g-C3N4 curl, and the excess graphite will be used as a kind of adhesive between the g-C3N4 layers to form a tight g-C3N4 nanosheet stack. The g-C3N4 bending of the larger nanosheet layer requires greater force, and at this time, the suitable ball milling rate and time are conducive to the bending of the sheet g-C3N4 and finally form a tubular structure. Its specific steps include:
[0006] The flake graphite and g-C3N4 are dry-milled and sieved to obtain a composite material of flake graphite and g-C3N4 (g-C3N4 / graphite). In a preferred embodiment, the conditions for the ball milling are: the ball size is 3-6 mm, the ball milling time is 12 to 24 hours, the rotation speed is 300 to 600 r / min, and the ball-to-material mass ratio is 20 to 40:1.
[0007] The graphite particle size is 300-600 mesh. x The mass ratio of N4 is: 2-4:1.
[0008] The technical solution of the present invention is to ball-mill the composite material of flake graphite and g-C3N4 and then sieve it to obtain a composite material with a particle size of 200 to 500 meshes.
[0009] The present invention also provides an application of the g-C3N4 / graphite composite material, which is used as a negative electrode material for a sodium ion battery.
[0010] The method for preparing a negative electrode of a sodium ion battery from a g-C3N4 / graphite composite material of the present invention comprises: uniformly mixing the g-C3N4 / graphite composite material with a conductive agent and a binder, and uniformly coating the mixed material on a copper foil current collector by a scraping coating method to serve as the negative electrode of the sodium ion battery.
[0011] The present invention discloses a method for preparing a sodium ion battery using the flake graphite and g-C3N4 composite material as a negative electrode material and a performance testing method: 50wt.% of the g-C3N4 / graphite composite material is weighed, 37.5wt.% Super P is added as a conductive agent, 12.5wt.% CMC is added as a binder, and a uniform black paste slurry is formed after sufficient grinding. The slurry is uniformly coated on a copper foil current collector as a test electrode, and a button battery is assembled with a metal sodium sheet as a comparison electrode. The electrolyte system used is 1M NaClO4 / EC∶PC (1∶1 v / v)+10% FEC, glass fiber is used as a separator, and CR2025 stainless steel is used as a battery shell to assemble the button battery.
[0012] Advantages of the present invention:
[0013] The present invention is the first to prepare a g-C3N4 / graphite composite material by dry ball milling of g-C3N4 and graphite. The method is simple and reliable, has good repeatability, strong operability, is environmentally friendly, has low raw material cost, and is easy to realize industrial production.
[0014] The tubular g-C3N4 coated flake graphite composite material of the present invention is prepared by dry ball milling using flake graphite with low sodium storage and g-C3N4 with high chemical stability as raw materials. The tubular g-C3N4 coated flake graphite composite material is prepared. g-C3N4 has poor electrical conductivity, and the electrical conductivity of the composite material is greatly improved after being compounded with flake graphite, thereby improving the rate performance of g-C3N4. During the dry ball milling process, g-C3N4 curls to form a tubular structure, and the specific surface area and active sites are increased, which is more conducive to the conduction between electrons and improves the rate performance of the composite material. After ball milling, the flake graphite is amorphized, the interlayer spacing becomes larger, and the sodium insertion capacity of the graphite is improved. The tubular g-C3N4 can alleviate the volume change caused by flake graphite during the charge and discharge process, and can store sodium at the same time, thereby improving the specific capacity and cycle stability of the material. These advantages make it particularly suitable for use as a negative electrode material for sodium ion batteries.
[0015] The tubular g-C3N4 coated flake graphite composite material of the present invention is applied to the field of sodium ion secondary batteries for the first time and has high specific capacity, high coulombic efficiency, excellent rate performance and high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a scanning electron microscope image obtained by ball milling graphite phase carbon nitride and 500 mesh flake graphite in a mass ratio of 2:1.
[0017] Figure 2 This is a transmission electron micrograph obtained by ball milling graphite phase carbon nitride and 500 mesh flake graphite in a mass ratio of 2:1.
[0018] Figure 3 The composite material was obtained by ball milling graphite carbon nitride and 500 mesh flake graphite in a mass ratio of 2:1 and used as the negative electrode of sodium ion battery. -1 Cycle 1000 times at 1.0A g -1 Cycle 5000 times. DETAILED DESCRIPTION
[0019] The following is a detailed description of the preparation method of a tubular g-C3N4 coated flake graphite composite material provided by the present invention in conjunction with specific embodiments.
[0020] Embodiment 1:
[0021] Take 10g of flake graphite and 20g of g-C3N4 and place them in a ball mill for ball milling. The ball-to-material ratio is 20:1, the rotation speed is 600rpm, and the ball milling time is 24h. The obtained powder is sieved and g-C3N4 / graphite with a particle size of 200-500 mesh is collected.
[0022] Weigh 50wt.% of the tubular g-C3N4-coated flake graphite material prepared in this embodiment, add 37.5wt.% SuperP as a conductive agent, 12.5wt.% sodium carboxymethyl cellulose (CMC) as a binder, grind thoroughly, add a small amount of deionized water and mix to form a uniform black paste slurry, coat the slurry on a copper foil current collector as a test electrode, and use a metal sodium sheet as a comparison electrode to assemble into a button cell, which uses an electrolyte system of 1M NaClO4 / EC∶DEC (1∶1) + 5% FEC, glass fiber as a separator, and CR2025 stainless steel as a battery casing to assemble into a button cell. The rate performance of the battery was tested at different current densities such as 0.1A / g, 0.2A / g, 0.4A / g, 0.6A / g, 0.8A / g, 1.0A / g, and 0.1A / g. The battery was tested for 1000 cycles at a current density of 0.4A / g, and then continued to be tested for 5000 cycles at 1.0A / g, and 10000 cycles at a high current density of 5.0A / g. The test results show that the sodium ion battery negative electrode prepared in this example has good electrochemical properties: after 1000 cycles at a current density of 0.4A / g, the specific capacity remains at about 220mAh / g, and after 5000 cycles at a discharge density of 1.0A / g, the specific capacity can still be maintained at 186mAh / g. The charge and discharge test was carried out at a density of 5.0A / g. The first cycle discharge capacity was 172.8mAh / g. After 10,000 cycles, the capacity could still fluctuate at 84mAh / g, and the average coulomb efficiency could reach 100%.
[0023] Embodiment 2:
[0024] Take 5g of flake graphite and 20g of g-C3N4 and place them in a ball mill for ball milling with a ball-to-material ratio of 20:1, a rotation speed of 600rpm, and a ball milling time of 20h. The obtained powder is sieved and g-C3N4 / graphite with a particle size of 200-500nm is collected.
[0025] Weigh 50wt.% of the tubular g-C3N4-coated flake graphite material prepared in this embodiment, add 37.5wt.% SuperP as a conductive agent, 12.5wt.% sodium carboxymethyl cellulose (CMC) as a binder, grind thoroughly, add a small amount of deionized water and mix to form a uniform black paste slurry, coat the slurry on a copper foil current collector as a test electrode, and use a metal sodium sheet as a comparison electrode to assemble into a button cell, which uses an electrolyte system of 1M NaClO4 / EC∶DEC (1∶1) + 5% FEC, glass fiber as a separator, and CR2025 stainless steel as a battery casing to assemble into a button cell. The rate performance of the battery was tested at different current densities such as 0.1A / g, 0.2A / g, 0.4A / g, 0.6A / g, 0.8A / g, 1.0A / g, and 0.1A / g. The original battery was tested for 1000 cycles at a current density of 0.4A / g, and then the battery was tested for 5000 cycles at 1.0A / g. A long cycle test of 10,000 cycles was performed at a high current density of 5.0A / g. The test results show that the electrochemical performance of the sodium ion battery negative electrode prepared in this example is not as good as that of Example 2: after 1000 cycles at a current density of 0.4A / g, the specific capacity remains at about 180mAh / g, and after 5000 cycles at a discharge density of 1.0A / g, the specific capacity can still be maintained at 149mAh / g. The charge and discharge test was carried out at a density of 5.0A / g. The first cycle discharge capacity was 202.4mAh / g. After 5000 cycles, the specific capacity remained at 70mAh / g, and the average coulombic efficiency could reach 99.86%.
[0026] Embodiment 3:
[0027] Take 6g of flake graphite and 20g of g-C3N4 and place them in a ball mill for ball milling. The ball-to-material ratio is 30:1, the rotation speed is 400rpm, and the ball milling time is 18h. The obtained powder is sieved and g-C3N4 with a particle size of 200-500nm is collected.
[0028] Weigh 50wt% g-C3N4, add 37.5wt.% Super P as a conductive agent, 12.5wt.% sodium carboxymethyl cellulose (CMC) as a binder, grind thoroughly, add a small amount of deionized water and mix to form a uniform black paste slurry, apply these slurries on copper foil current collector as test electrodes, and use metal sodium sheets as reference electrodes to assemble button cells, which use an electrolyte system of 1M NaClO4 / EC∶DEC (1∶1)+5%FEC, glass fiber as a separator, and CR2025 stainless steel as a battery shell to assemble button cells. The rate performance of the battery is tested at different current densities such as 0.1A / g, 0.2A / g, 0.4A / g, 0.6A / g, 0.8A / g, 1.0A / g, and 0.1A / g, and a long cycle test of 5000 cycles is carried out at a high current density of 5.0A / g. The test results show that the negative electrode of the sodium ion battery prepared in this example has poor rate performance: at a current density of 0.4A / g, its first cycle coulomb efficiency is, the first cycle discharge capacity is, and after 1000 cycles, it can still maintain a specific capacity of; at a discharge density of 1.0A / g, it can cycle 5000 cycles, and can still maintain a specific capacity of. At a discharge density of 5.0A / g, it cycles 5000 cycles, the first cycle discharge capacity is 149.1mAh / g, and after 10000 cycles, the capacity remains at 65mAh / g, and the average coulomb efficiency can reach 99.38%.
Claims
1. A method for preparing a graphite phase carbonized nitrogen / graphite composite material with a peapod structure for use in a negative electrode of a sodium ion battery, characterized in that The following steps are involved: Step 1: high-energy ball milling of flake graphite and g-C3N4 in an inert atmosphere, the ball size is 3-6 mm, the ball milling time is 18-24 hours, the rotation speed is 300-600 r / min, the ball-to-material mass ratio is 20:1 or 40:1, the energy generated by the appropriate amount of flake graphite and ball milling drives the graphite phase carbonitride to curl to form a tubular structure, and the graphite is coated in the tubular structure to form a pod-like structure, the mass ratio of the graphite to g-C3N4 is: 2-4:1, and the graphite particle size is: 300-600 mesh; Step 2: Screen the ball-milled material to obtain graphite phase carbonized nitrogen coated flake graphite material (g-C3N4 / graphite).
2. A preparation method according to claim 1, characterized in that: The inert atmosphere in step 1 is selected from one of nitrogen, argon and helium inert gases.
3. A composite material prepared by the preparation method according to any one of claims 1 to 2 for use as a negative electrode of a sodium ion battery.