A steel grain size etchant and its application

By using a steel grain size etchant composed of an aromatic nitro compound and a surfactant, the problems of environmental pollution and poor corrosion effects in the existing technology are solved, the steel grain size is clearly displayed, the operation is simplified and the cost is saved. cost.

CN112082912BActive Publication Date: 2024-10-11CRRC QISHUYAN INSTITUTE CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202010947818.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-10
Publication Date
2024-10-11
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

The existing steel grain size assessment method uses reagents such as nitric ethanol solution and picric acid, which has problems of environmental pollution and poor erosion effects. The high-temperature oxidation treatment process is complex and cannot effectively display grain boundaries.

Method used

Steel grain size etching agent composed of aromatic nitro compounds and surfactants (such as p-nitrobenzoic acid and sodium dodecyl sulfate) and diluents (water and glycerol), with a component ratio of 1:1~ 1:2, used for direct chemical attack of steel materials to reveal grain boundaries.

Benefits of technology

This etchant avoids the toxicity of picric acid and environmental pollution. It can clearly display large and small grains and mixed grain boundaries under the microscope. The effect is good at 100 times, simplifying the operation, saving time and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112082912B_ABST
    Figure CN112082912B_ABST
Patent Text Reader

Abstract

The present invention provides a steel grain size etchant and its application. The etchant of the present invention adopts an aromatic nitro compound, a surfactant and a diluent, wherein the component ratio of the aromatic nitro compound and the surfactant is 1:1 to 1:2 by mass. The aromatic nitro compound is p-nitrobenzoic acid and / or 2-nitrobenzoic acid. The surfactant is any one or a combination of sodium dodecyl sulfate, sodium sulfate of fatty alcohol polyoxyethylene ether, dodecylbenzene sulfonic acid, dodecyl alcohol amide, and nonylphenol polyoxyethylene ether. The diluent is water and glycerol. The etchant of the present invention does not contain picric acid with toxicity and explosiveness, avoids pollution to the environment and affects public safety, and meets environmental protection requirements. In addition, the etchant provided by the present invention can clearly display the grain boundaries of large grains, small grains and large and small mixed crystal grains of the sample, and the grain size is clear and complete at 100 times, and it is easy to grade the grain size, with good effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the application field of etchants, and in particular to a steel grain size etchant and application thereof. Background Art

[0002] The actual grain size of steel has a great influence on the mechanical properties, physical properties and chemical properties. Therefore, the assessment of the actual grain size is of great significance for judging the quality of steel, testing the correctness of the hot working process, and studying the influence of grain size on related properties.

[0003] The grain size of steel materials is generally displayed by etching with reagents such as nitric acid ethanol solution (usually high-temperature oxidation method), saturated picric acid, and mixed solution of picric acid and sodium dodecylbenzene sulfonate. However, when the above methods are used to erode grain boundaries, on the one hand, picric acid has been listed as an environmental pollutant due to its poor biodegradability, explosiveness, toxicity and acidity, and is restricted from large-scale use to avoid polluting the environment and affecting public safety; on the other hand, the oxidation method requires the use of a heat treatment furnace to perform high-temperature oxidation treatment on the sample. The high-temperature oxidation treatment process and subsequent sample preparation process are complicated, and the detection area is small, which cannot reflect the overall grain size distribution of the sample, and is prone to missed detection of mixed crystals. Summary of the invention

[0004] The main purpose of the present invention is to provide a steel grain size etchant to solve the problem that reagents such as nitric acid ethanol solution and picric acid in the prior art pollute the environment or have poor etch effects.

[0005] In order to achieve the above object, according to one aspect of the present invention, a steel grain size etchant is provided, comprising: an aromatic nitro compound, a surfactant and a diluent, wherein the component ratio of the aromatic nitro compound to the surfactant is 1:1 to 1:2 by mass, and the remainder is the diluent.

[0006] Furthermore, the component ratio of the aromatic nitro compound to the surfactant is 1:1.3 to 1:1.7.

[0007] Furthermore, the aromatic nitro compound is p-nitrobenzoic acid and / or 2-nitrobenzoic acid.

[0008] Furthermore, the surfactant is any one or a combination of sodium dodecyl sulfate, sodium fatty alcohol polyoxyethylene ether sulfate, dodecylbenzene sulfonic acid, dodecyl alcohol amide, and nonylphenol polyoxyethylene ether.

[0009] Furthermore, the ratio of the sum of the components of the aromatic nitro compound and the surfactant to the components of the diluent is 0.6:100 to 1.3:100 by mass.

[0010] Furthermore, the ratio of the sum of the components of the aromatic nitro compound and the surfactant to the components of the diluent is 0.7:100 to 1:100 by mass.

[0011] Furthermore, the diluent is water and glycerol, wherein the ratio of water to glycerol components is 5.5:1 to 10:1 by mass.

[0012] According to another aspect of the present invention, there is provided a use of a steel grain size etchant in the corrosion of steel materials.

[0013] Furthermore, the steel material is one of 18CrNiMo7-6, GCr15 bearing steel, 52CrMoV spring steel, 42CrMo quenched and tempered steel, and carbon structural steel.

[0014] The beneficial effects of the present invention are:

[0015] 1. The etchant provided by the present invention does not contain picric acid which is toxic and explosive, thus avoiding the use of environmental pollutants to pollute the environment and affect public safety, thus meeting environmental protection requirements;

[0016] 2. In the prior art, nitric acid ethanol solution can only reflect the structure morphology after corroding the steel material, but cannot show the grain boundary, and cannot distinguish between large and small grains; while the etchant provided by the present invention can clearly show the grain boundary of large grains, small grains and large and small mixed grains of the sample, and the grain size is clear and complete at 100 times, and it is easy to grade the grain size, and the effect is good. Therefore, the etchant provided by the present invention has a better corrosion effect than nitric acid ethanol solution;

[0017] 3. In the prior art, when nitric acid ethanol solution is used to erode steel materials, it is usually necessary to use a heat treatment furnace to perform high-temperature oxidation treatment on the steel materials; however, when the etchant of the present invention is used to erode steel materials, there is no need to use a high-temperature oxidation treatment process, and the grain boundaries can be directly chemically etched, which is simple to operate and can save time and cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0019] Figure 1 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the scheme of Example 1 of the present invention is shown;

[0020] Figure 2 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the solution of Example 2 of the present invention is shown; and

[0021] Figure 3 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the solution of Example 3 of the present invention is shown; and

[0022] Figure 4 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the scheme of Example 4 of the present invention is shown; and

[0023] Figure 5 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the scheme of Example 5 of the present invention is shown; and

[0024] Figure 6 A schematic diagram of the metallographic structure of 42CrMo quenched and tempered steel (quenched + high temperature tempered state) obtained after etching using the scheme of Example 6 of the present invention is shown; and

[0025] Figure 7 A schematic diagram of the metallographic structure of GCr15 bearing steel (quenched + low temperature tempered state) obtained after etching using the scheme of Example 7 is shown; and

[0026] Figure 8 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the comparative example 1 is shown; and

[0027] Fig. 9 A schematic diagram of the metallographic structure of GCr15 bearing steel (quenched + low-temperature tempered state) obtained after etching using the comparative example 2 is shown.

[0028] Fig.10 A schematic diagram of the metallographic structure of the gear steel (18CrNiMo7-6) obtained after etching using the comparative example 3 is shown. DETAILED DESCRIPTION

[0029] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0030] The present application is further described in detail below in conjunction with specific embodiments. These embodiments are representative embodiments of the present application and should not be construed as limiting the scope of protection claimed in the present application.

[0031] Embodiment 1:

[0032] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is 2-nitrobenzoic acid, the surfactant is sodium dodecyl sulfate, and the diluent is water and glycerol. In terms of mass, the component ratio of 2-nitrobenzoic acid to sodium dodecyl sulfate is 1:1.10, the ratio of the total component of 2-nitrobenzoic acid and sodium dodecyl sulfate to the component of the diluent is 1.25:100, and the component ratio of water to glycerol is 8:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0033] The gear steel (18CrNiMo7-6) was etched by the etchant of this embodiment and observed by metallographic microscope. The metallographic structure results are as follows: Figure 1 As shown. Figure 1 It can be seen that the erosion effect of this embodiment is good, the organizational structure and grain boundaries (black thin lines) of the gear steel (18CrNiMo7-6) are clear, the grains are complete, and the large and small grains and mixed grains are clearly distinguished.

[0034] Embodiment 2:

[0035] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is 2-nitrobenzoic acid, the surfactant is sodium dodecyl sulfate, and the diluent is water and glycerol. In terms of mass, the component ratio of 2-nitrobenzoic acid to sodium dodecyl sulfate is 1:1.30, the ratio of the total component of 2-nitrobenzoic acid and sodium dodecyl sulfate to the component of the diluent is 1.25:100, and the component ratio of water to glycerol is 8:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0036] The gear steel (18CrNiMo7-6) was etched by the etchant of this embodiment and observed by metallographic microscope. The metallographic structure results are as follows: Figure 2 As shown. Figure 2 It can be seen that the erosion effect of this embodiment is good, the organizational structure and grain boundaries (black thin lines) of the gear steel (18CrNiMo7-6) are clear, the grains are complete, and the large and small grains and mixed grains are clearly distinguished.

[0037] Embodiment 3:

[0038] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is 2-nitrobenzoic acid, the surfactant is sodium dodecyl sulfate, and the diluent is water and glycerol. In terms of mass, the component ratio of 2-nitrobenzoic acid to sodium dodecyl sulfate is 1:1.70, the ratio of the total component of 2-nitrobenzoic acid and sodium dodecyl sulfate to the component of the diluent is 1.25:100, and the component ratio of water to glycerol is 8:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0039] The gear steel (18CrNiMo7-6) was etched by the etchant of this embodiment and observed by metallographic microscope. The metallographic structure results are as follows: Figure 3 As shown. Figure 3 It can be seen that the erosion effect of this embodiment is good, the organizational structure and grain boundaries (black thin lines) of the gear steel (18CrNiMo7-6) are clear, the grains are complete, and the large and small grains and mixed grains are clearly distinguished.

[0040] Embodiment 4:

[0041] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is 2-nitrobenzoic acid, the surfactant is sodium dodecyl sulfate, and the diluent is water and glycerol. In terms of mass, the component ratio of 2-nitrobenzoic acid to sodium dodecyl sulfate is 1:20, the ratio of the total component of 2-nitrobenzoic acid and sodium dodecyl sulfate to the component of the diluent is 1.25:100, and the component ratio of water to glycerol is 8:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0042] The gear steel (18CrNiMo7-6) was etched by the etchant of this embodiment and observed by metallographic microscope. The metallographic structure results are as follows: Figure 4 As shown. Figure 4 It can be seen that the erosion effect of this embodiment is good, the organizational structure and grain boundaries (black thin lines) of the gear steel (18CrNiMo7-6) are clear, the grains are relatively complete, and the large and small grains and mixed grains are clearly distinguished.

[0043] Embodiment 5:

[0044] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is p-nitrobenzoic acid, the surfactant is dodecylbenzenesulfonic acid, and the diluent is water and glycerol. In terms of mass, the component ratio of nitrobenzoic acid to dodecylbenzenesulfonic acid is 1:1.52, the ratio of the total components of nitrobenzoic acid and dodecylbenzenesulfonic acid to the components of the diluent is 0.70:100, and the component ratio of water to glycerol is 6:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0045] The gear steel (18CrNiMo7-6) was etched by the etchant of this embodiment and observed by metallographic microscope. The metallographic structure results are as follows: Figure 5 As shown. Figure 5 It can be seen that the erosion effect of this embodiment is better, the organizational structure and grain boundaries (black thin lines) of the gear steel (18CrNiMo7-6) are clear, the grains are relatively complete, and the distinction between large and small grains and mixed grains is more obvious.

[0046] Embodiment 6:

[0047] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is 2-nitrobenzoic acid, the surfactant is dodecylbenzenesulfonic acid, and the diluent is water and glycerol. In terms of mass, the component ratio of nitrobenzoic acid to dodecylbenzenesulfonic acid is 1:1.79, the ratio of the total components of nitrobenzoic acid and dodecylbenzenesulfonic acid to the components of the diluent is 0.75:100, and the component ratio of water to glycerol is 6:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0048] The etchant of this embodiment was used to erode 42CrMo quenched and tempered steel (quenched + high temperature tempered state), and the metallographic structure obtained by metallographic microscope was as follows: Figure 6 As shown. Figure 6 It can be seen that the erosion effect of this embodiment is good, the organizational structure and grain boundaries (black thin lines) of 42CrMo quenched and tempered steel (quenched + high temperature tempered state) are clear, the grains are relatively complete, and the large and small grains and mixed grains are clearly distinguished.

[0049] Embodiment 7:

[0050] A steel grain size etchant includes an aromatic nitro compound, a surfactant and a diluent. The aromatic nitro compound is p-nitrobenzoic acid, the surfactant is sodium dodecyl sulfate, and the diluent is water and glycerol. In terms of mass, the component ratio of p-nitrobenzoic acid to sodium dodecyl sulfate is 1:1.65, the ratio of the sum of the components of p-nitrobenzoic acid and sodium dodecyl sulfate to the component of the diluent is 0.85:100, and the component ratio of water to glycerol is 10:1. The steel grain size etchant of this embodiment is obtained by uniformly mixing the above raw materials.

[0051] The etchant of this embodiment was used to erode GCr15 bearing steel (quenched + low temperature tempered state) and observed with a metallographic microscope. The metallographic structure obtained is as follows: Figure 7 As shown. Figure 7 It can be seen that the erosion effect of this embodiment is good, the organizational structure and grain boundaries (black thin lines) of GCr15 bearing steel (quenched + low-temperature tempered state) are clear, the grains are relatively complete, and the large and small grains and mixed grains are clearly distinguished.

[0052] Embodiment 8-20:

[0053] The specific implementation is shown in Table 1.

[0054]

[0055]

[0056]

[0057] Table 1

[0058] Comparative Example 1:

[0059] The gear steel (18CrNiMo7-6) material was etched with nitric acid ethanol solution. The nitric acid ethanol solution was obtained by mixing nitric acid and ethanol evenly, and the volume ratio of nitric acid to ethanol was 4:96. The gear steel (18CrNiMo7-6) sample etched with the nitric acid ethanol solution of this comparative example was observed under a metallographic microscope, and the metallographic structure obtained was as follows: Figure 8 As shown. Figure 8 It can be seen that the grain boundaries between the grains of the gear steel (18CrNiMo7-6) are not clearly displayed, and it is impossible to distinguish between large and small grains and mixed grains.

[0060] Comparative Example 2:

[0061] The GCr15 bearing steel (quenched + low temperature tempered state) material was etched with nitric acid ethanol solution. The nitric acid ethanol solution was obtained by mixing nitric acid and ethanol evenly, and the component ratio of nitric acid to ethanol was 4:96 by volume. The GCr15 bearing steel (quenched + low temperature tempered state) sample etched with nitric acid ethanol in this comparative example was observed under a metallographic microscope, and the metallographic structure obtained was as follows Fig. 9 As shown. Fig. 9 It can be seen that the grain boundaries between the grains of GCr15 bearing steel (quenching + low-temperature tempering state) are not clearly displayed, and it is impossible to distinguish between large and small grains and mixed grains.

[0062] Comparative Example 3:

[0063] The gear steel (18CrNiMo7-6) material is etched by using an etchant containing picric acid. The etchant containing picric acid includes picric acid, sodium dodecylbenzene sulfonate, alkyl alcohol amide and distilled water. The ratio of picric acid, sodium dodecylbenzene sulfonate and alkyl alcohol amide is 1:(1-2):(0.1-0.2) by mass, and the balance is distilled water. The above components are mixed evenly to obtain the etchant containing picric acid of this comparative example.

[0064] The gear steel (18CrNiMo7-6) was etched by the etchant of this comparative example and observed by metallographic microscope. The metallographic structure was as follows: Fig.10 As shown. Figure 1-5 and Fig.10 It can be seen that the corrosion effect of this comparative example on gear steel (18CrNiMo7-6) is basically consistent with the corrosion effect of the steel grain size etchant of the present invention on gear steel (18CrNiMo7-6), but due to the toxicity, explosiveness and poor biodegradability of picric acid, the use of this comparative example not only pollutes the environment but also affects public safety.

[0065] Through the above embodiments and the comparison with the corresponding comparative examples, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0066] 1. The steel grain size etchant of the present invention does not use picric acid, but can achieve the erosion effect of an etchant containing picric acid, and avoids polluting the environment and affecting public safety;

[0067] 2. The above embodiments of the present invention have better etching effect than nitric acid. Specifically, the etching agent provided by the present invention can clearly show the grain boundaries of large grains, small grains and large and small mixed grains of the sample, and the grain size is clear and complete at 100 times, and it is easy to grade the grain size, and the etching effect is good.

[0068] 3. The etchant of the present invention does not require high-temperature oxidation treatment when corroding steel materials, and is easy to operate, saving time and cost.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A steel grain size etchant, characterized in that: include: An aromatic nitro compound, a surfactant and a diluent, wherein, by mass, the component ratio of the aromatic nitro compound to the surfactant is 1:1.3 to 1:1.7, the aromatic nitro compound is p-nitrobenzoic acid and / or 2-nitrobenzoic acid, the diluent is water and glycerol, the ratio of the sum of the components of the aromatic nitro compound and the surfactant to the components of the diluent is 0.7:100 to 1:100, and the component ratio of water to glycerol in the diluent is 5.5:1 to 10:

1.

2. A steel grain size etchant according to claim 1, characterized in that: The surfactant is any one or a combination of sodium dodecyl sulfate, sodium fatty alcohol polyoxyethylene ether sulfate, dodecylbenzene sulfonic acid, dodecyl alcohol amide, and nonylphenol polyoxyethylene ether.

3. Application of a steel grain size etchant in the corrosion of steel materials, characterized in that: The steel grain size etchant as claimed in claim 1 or 2 is used.

4. The use of a steel grain size etchant in steel material corrosion according to claim 3, characterized in that: The steel material is one of 18CrNiMo7-6, GCr15 bearing steel, 52CrMoV spring steel, 42CrMo quenched and tempered steel, and carbon structural steel.

Citation Information

Patent Citations

  • Original crystalline grain displaying agent of high-alloy and low-carbon martensite steel and displaying method

    CN103018141A

  • 9% Ni steel crystal-boundary etching agent applied to QT (Quenching and Tempering) heat treatment state and use method thereof

    CN103320795A

  • Metallographic corrosive for showing grain boundaries of steels

    CN103628062A

  • Detection and display method of austenite grains of quenched and tempered steel for gears at room temperature

    CN104729963A

  • Corrosive for displaying grain boundary of original austenite of tempered martensite and corroding method

    CN105628480A