Titanate@silicon dioxide core-shell nanocomposite particle electrorheological fluid and preparation method thereof
Through the combination of titanate@silica core-shell nanoparticles and dimethyl silicone oil, hydrothermal method and controlled hydrolysis method are used to synthesize one-dimensional nanocomposite particles, which solves the problem of insufficient changes in rheological properties of electrorheological fluids and stable anti-sedimentation. It solves the problem of insufficient sex, achieves efficient electrorheological effect and temperature stability, and expands its application prospects in the field of smart materials.
Patent Information
- Application Number
- CN202011142090.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-10-22
AI Technical Summary
Under the action of an external electric field, the rheological properties of existing electrorheological fluids do not change significantly, and their resistance to precipitation and temperature stability are insufficient, which limits their application prospects in clutches, shock absorbers and other fields.
Electrorheological fluid composed of titanate@silica core-shell nanoparticles and dimethyl silicone oil is used to synthesize one-dimensional nanocomposite particles through hydrothermal method and controlled hydrolysis method to form core-shell structure and hollow structure to enhance interfacial polarization. capacity and rheological properties.
It achieves extremely strong electrorheological effect, good anti-precipitation stability and temperature stability, significantly improves the performance of electrorheological fluid, and is suitable for the field of smart materials.
Smart Images

Figure HDA0002738580170000011 
Figure HDA0002738580170000012 
Figure HDA0002738580170000013
Abstract
Description
Technical Field
[0001] The invention relates to an electrorheological fluid and a preparation method thereof, and in particular to a titanate@silicon dioxide core-shell nanocomposite particle electrorheological fluid and a preparation method thereof. Background Art
[0002] Electrorheological fluid is a type of two-phase fluid mainly composed of polarizable particles dispersed in insulating oil. Its rheological properties can undergo instantaneous reversible changes under the action of an electric field. The effect of the electric field on the internal structure and rheological properties of the dispersed system is called the electrorheological effect. This effect comes from the mutual attraction of adjacent particles in the electrorheological fluid under the action of the electric field to form a chain structure arranged along the direction of the electric field. The dispersed system with electrorheological effect is called electrorheological fluid or electrorheological fluid, and is called electrorheological fluid. Under the action of an external field strength, the viscosity, shear stress and flow properties of the electrorheological fluid undergo tremendous changes. It exhibits the characteristics of a Newtonian fluid when there is no external electric field, but when a voltage is added, it exhibits the properties of a Bingham fluid.
[0003] As a new type of smart material, electrorheological materials have attracted widespread attention. Electrorheological materials are usually colloidal suspensions composed of dielectric particles dispersed in an insulating medium, and their mechanical and rheological properties change under the action of an applied electric field. Under the action of an applied electric field, the randomly dispersed particles form a chain structure along the direction of the electric field, thereby achieving a state transition from liquid to solid. In addition, the response of electrorheological fluids to electrical stimulation is reversible, controllable and rapid.
[0004] Electrorheological fluid is a smart material that responds quickly to electric fields. Electrorheological fluid is usually composed of an insulating carrier fluid (such as silicone oil and liquid paraffin) and polarizable particles. Without an external electric field, the polarized particles are randomly dispersed in a non-conductive continuous phase, and the fluid has a low viscosity. When an external electric field acts on the electrorheological fluid, it causes the liquid-like phase to transform into a solid-like phase. It can reversibly form a chain structure under the action of an external electric field. Since electrorheological fluid has the characteristics of rapid and reversible response to electrical signals, it has broad application prospects in the fields of clutches, shock absorbers, and brakes. So far, a variety of materials have been used in the field of electrorheology, including inorganic semiconductors and conductive polymers.
[0005] The purpose of the present invention is to provide a titanate@silicon dioxide core-shell nanoparticle electrorheological fluid, wherein the dispersed phase is titanate@silicon dioxide core-shell nanoparticles and the continuous phase is dimethyl silicone oil. The titanate@silicon dioxide core-shell nanoparticles have a unique morphology. The results of scanning electron microscopy and transmission electron microscopy show that the obtained titanate@silicon dioxide nanocomposite particles are titanate nanotubes coated on the surface of silicon dioxide, which have both a core-shell structure and a hollow structure, and belong to the category of one-dimensional nanomaterials. The preparation process is a combination of a hydrothermal method and a controlled hydrolysis method, the synthesis is simple, and the product is a one-dimensional nano hollow core-shell structure. The process can also control the morphology, size, coating degree, etc. of the product by controlling the reaction time and the solvent ratio, and has strong adjustability.
[0006] The purpose of the present invention is also to provide a method for preparing titanate@silicon dioxide core-shell nanoparticles, which adopts a two-step method, firstly adopts a hydrothermal method to prepare hollow tubular titanate nanoparticles; and then adopts a controlled hydrolysis method to coat a layer of silicon dioxide film on the titanate nanotubes to form a titanate@silicon dioxide core-shell one-dimensional nanoparticle with both a core-shell structure and a hollow structure. It not only takes advantage of the hollow effect of the hollow nanotubes, but also utilizes the core-shell structure to improve the interface polarization ability, and also retains the one-dimensional anisotropic nanometer scale. The preparation process is simple, the raw materials are easy to obtain, and the component performance is easy to control. The electrorheological fluid prepared with the material and methyl silicone oil has some excellent properties, including extremely strong electrorheological effect, good anti-precipitation stability, good temperature stability, and good chemical stability.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] The electrorheological fluid prepared by the present invention has a dispersed phase of titanate@silicon dioxide core-shell nanoparticles and a continuous phase of dimethyl silicone oil.
[0009] The preparation process of the electrorheological fluid comprises the following steps:
[0010] (1) A mixture of 1.5 g TiO2 (P25) powder and 150 mL 10 M NaOH aqueous solution was stirred at room temperature for 30 min. The mixture was then homogenized in an ultrasonic generator for 1 h and transferred to a hydrothermal reactor and heated at 120 °C for 24 h. After cooling to room temperature, the product was centrifuged and washed with 1 M HCl solution and then rinsed with deionized water until the pH value reached 7. After centrifugation, the obtained titanate nanotube product was dried at 70 °C for 12 h.
[0011] (2) 0.5 g of the prepared titanate nanotube sample was uniformly dispersed in a mixed solution of 100 mL of ethanol, 40 mL of deionized water and 2 mL of ammonia solution (25-28 wt.%) and stirred for 6 h to ensure that the titanate nanotubes were fully dispersed. Then, a mixed solution of 60 ml of ethanol and 1.92 mL of TEOS (ethyl silicate) was uniformly and slowly added dropwise to the above solution, and the stirring reaction was continued for 6 hours. The product was then collected by centrifugation, thoroughly washed three times with deionized water and ethanol, and finally dried at 80 ° C for 24 hours.
[0012] (3) The sample was mixed with dimethyl silicone oil to prepare an electrorheological fluid at a weight ratio of 10 wt % of solid particles to silicone oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 SEM photo of titanate nanotubes
[0014] Figure 2 TEM image of titanate nanotubes
[0015] Figure 3 Titanate nanotubes, Titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis method in Example 1, and XRD curve of silicon dioxide
[0016] Figure 4 Titanate nanotubes, titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis in Example 1, and FTIR spectrum of silicon dioxide
[0017] Figure 5 Dielectric spectra of titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis in Examples 1 and 3
[0018] Figure 6 SEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 1.92 mL TEOS for 12 h
[0019] Figure 7 TEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 1.92 mL TEOS for 12 h
[0020] Figure 8 Electrorheological properties of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 1.92 mL TEOS for 12 h
[0021] Fig. 9 SEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 2.24 mL TEOS for 12 h
[0022] Fig.10 TEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 2.24 mL TEOS for 12 h
[0023] Fig.11 Electrorheological properties of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 2.24 mL TEOS for 12 h
[0024] Fig.12 SEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 3.2 mL TEOS for 12 h
[0025] Fig.13 Electrorheological properties of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 3.2 mL TEOS for 12 h
[0026] Fig.14 SEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 5.12 mL TEOS for 12 h
[0027] Fig.15 SEM image of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 5.8 mL TEOS for 4 h DETAILED DESCRIPTION
[0028] Example 1 (Preparation of titanate@silicon dioxide nanocomposite material by controlled hydrolysis):
[0029] A mixture of 1.5 g TiO2 (P25) powder and 150 mL 10 M NaOH aqueous solution was stirred at room temperature for 30 min. The mixture was then homogenized in an ultrasonic generator for 1 h and transferred to a hydrothermal reactor and heated at 120 ° C for 24 h. After cooling to room temperature, the product was centrifuged and washed with 1 M HCl solution and then with deionized water until the pH value reached 7. After centrifugation, the obtained titanate nanotube product was dried at 70 ° C for 12 h.
[0030] 0.5g titanate nanotube sample was evenly dispersed in a mixed solution of 100mL ethanol, 40mL deionized water and 2mL ammonia solution (25-28wt.%) and stirred for 6h to ensure that the titanate nanotube sample was fully dispersed in the solution. Then a mixed solution of 60mL ethanol and 1.92mL TEOS was evenly and slowly added dropwise to the above solution, and the stirring reaction was continued for 6 hours. The product was then collected by centrifugation, and after being thoroughly washed three times with deionized water and ethanol, titanate@silicon dioxide nanoparticles were obtained, which were placed in an oven and dried at 80°C for 24 hours to obtain a solid powder; the sample was mixed with dimethyl silicone oil at a weight ratio of 10wt% of solid particles to silicone oil to prepare an electrorheological fluid.
[0031] Figure 1 This is a SEM photo of titanate nanotubes, with a diameter of about 10 nanometers and a length of 300-500 nanometers. Figure 2This is a TEM photo of titanate nanotubes. According to the transmission image, it can be seen that the particles are hollow tubes with a diameter of 10 nanometers. Figure 3 is the XRD curve of titanate nanotubes, compared with the standard titanate card PDF # 47-0124 comparison shows that the crystal plane index corresponding to 9.94° is (200), the crystal plane index corresponding to 24.10° is (110), the crystal plane index corresponding to 27.92° is (310), and the crystal plane index corresponding to 48.37° is (020). It can be seen from the figure that the diffraction peak is sharp, indicating good crystallinity. Example 1 The XRD curve of the titanate@silicon dioxide nanocomposite particles prepared by the controlled hydrolysis method is similar to the XRD curve of the titanate nanotubes, and the intensity is reduced. This is caused by the coating of amorphous silicon dioxide, showing that the core-shell structure of the two is formed. The XRD curve of pure silicon dioxide also shows that the pure silicon dioxide prepared by a similar method without adding titanate nanotubes is amorphous, with only a large dispersion peak between 20-30.
[0032] Figure 4 The FTIR spectra of titanate nanotubes, titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis in Example 1, and pure silicon dioxide, 3400 cm -1 The left and right sides correspond to the stretching vibration peak of OH on the silica surface, 500-800cm -1 O-Si stretching peak appears between 1000-1700cm -1 The corresponding ones are CH bonds and CO bonds. Figure 5 The dielectric spectrum of titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis method in Examples 1 and 3. In the dielectric curve, 10 2 -10 5 The larger the dielectric constant difference Δε′ corresponding to the Hz frequency range is, the stronger the polarization force at the interface between the dispersed phase and the silicone oil is, and the better the electrorheological performance is. Figure 6 and Figure 7 The SEM and TEM images of titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis of 1.92 mL TEOS for 12 hours show that the shape of the particles is similar to that of a rod, that is, a layer of film is coated on the outside of the tube, with a length of about 500 nanometers, and the surface diameter of the composite particles is about 50 nanometers; the coating layer thickness is about 20-30 nanometers. The transmission image shows that the coating is complete and a core-shell structure is formed.
[0033] Figure 8This is the relationship between shear strength and shear rate of the electrorheological fluid based on titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis of 1.92mL TEOS for 12h under different field strengths. As can be seen from the figure, the voltage was added to 2.5kV, and its current density was small, indicating that the electrorheological fluid of this system has good anti-breakdown performance. As can be seen from the figure, in the absence of an electric field, the shear stress increases linearly with the increase of the shear rate, and the fluid exhibits Newtonian fluid behavior; after the electric field is applied, the particles are rapidly polarized in the electric field, the dipoles attract each other, and the particles are arranged in a chain structure. With the increase of the electric field strength, the shear stress continues to rise, and a platform area is shown in the high-frequency region, which is characterized by a Bingham fluid with an electrorheological efficiency of 21.
[0034] Embodiment 2:
[0035] 0.5g titanate nanotube sample was evenly dispersed in a mixed solution of 100mL ethanol, 40mL deionized water and 2mL ammonia solution (25-28wt.%) and stirred for 6h to ensure that the titanate nanotubes were fully dispersed in the solution. Then a mixed solution of 60ml ethanol and 2.24mL TEOS was evenly and slowly added dropwise to the above solution, and the stirring reaction was continued for 6 hours. The product was then collected by centrifugation, and after being thoroughly washed three times with deionized water and ethanol, titanate@silicon dioxide nanoparticles were obtained, which were placed in an oven and dried at 80°C for 24 hours to obtain a solid powder. The sample was mixed with dimethyl silicone oil at a weight ratio of 10wt% of solid particles to silicone oil to prepare an electrorheological fluid.
[0036] Fig. 9 and Fig.10 They are SEM and TEM images of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 2.24 mL TEOS for 12 h. Fig. 9 Compared with the embodiment 1 Figure 6 , it can be seen that the coating layer is thicker, with a length of about 300-500 nanometers, and the surface diameter of the composite particles is about 80 nanometers; the coating layer thickness is about 30-40 nanometers. The transmission photo shows that the coating is complete and the core-shell structure is formed.
[0037] Fig.11This is the relationship between shear strength and shear rate of the electrorheological fluid based on titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis of 2.24mL TEOS for 12h under different field strengths. As can be seen from the figure, the voltage was added to 3.0kV, and its current density was small, indicating that the electrorheological fluid of this system has good anti-breakdown performance. As can be seen from the figure, in the absence of an electric field, the shear stress increases linearly with the increase of the shear rate, and the fluid exhibits Newtonian fluid behavior; after the electric field is applied, the particles are rapidly polarized in the electric field, the dipoles attract each other, and the particles are arranged in a chain structure. With the increase of the electric field strength, the shear stress continues to rise, and a platform area is shown in the high-frequency region, which is characterized by a Bingham fluid, and the electrorheological efficiency is 151, reflecting a very strong electrorheological effect.
[0038] Embodiment three:
[0039] 0.5g titanate nanotube sample was evenly dispersed in a mixed solution of 100mL ethanol, 40mL deionized water and 2mL ammonia solution (25-28wt.%) and stirred for 6h to ensure that the titanate nanotubes were fully dispersed in the solution. Then a mixed solution of 60ml ethanol and 3.2mL TEOS was evenly and slowly added dropwise to the above solution, and the stirring reaction was continued for 6 hours. The product was then collected by centrifugation, thoroughly washed three times with deionized water and ethanol to obtain titanate@silicon dioxide nanoparticles, which were placed in an oven and dried at 80°C for 24 hours to obtain a solid powder. The sample was mixed with dimethyl silicone oil at a weight ratio of 10wt% of solid particles to silicone oil to prepare an electrorheological fluid.
[0040] Fig.12 and Fig.13 The SEM images and electrorheological performance diagrams of titanate@silicon dioxide nanocomposite particles prepared by controlled hydrolysis of 3.2 mL TEOS for 12 h are shown respectively. Fig.12 It can be seen that the coating is thicker, with a length of about 200-300 nanometers, and the surface diameter of the composite particles is about 100 nanometers; Fig.13 It can be seen that the voltage was increased to 2.5 kV, and the current density was small, indicating that the electrorheological fluid of this system has good anti-breakdown performance. The electrorheological efficiency is 60.
[0041] Embodiment 4:
[0042] 0.5g titanate nanotube sample was evenly dispersed in a mixed solution of 100mL ethanol, 40mL deionized water and 2mL ammonia solution (25-28wt.%) and stirred for 6h to ensure that the titanate nanotubes were fully dispersed in the solution. Then a mixed solution of 60ml ethanol and 5.12mL TEOS was evenly and slowly added dropwise to the above solution, and the stirring reaction was continued for 6 hours. The product was then collected by centrifugation, and after being thoroughly washed three times with deionized water and ethanol, titanate@silicon dioxide nanoparticles were obtained, which were placed in an oven and dried at 80°C for 24 hours to obtain a solid powder. The sample was mixed with dimethyl silicone oil at a weight ratio of 10wt% of solid particles to silicone oil to prepare an electrorheological fluid.
[0043] Fig.14 This is a SEM photo of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 5.12 mL TEOS for 12 h. As can be seen from the figure, when the amount of TEOS is 5.12 mL, the titanate@silica nanocomposite particles obtained are close to spherical.
[0044] Embodiment five:
[0045] Disperse 0.55g titanate nanotube sample evenly in 158mL ethanol and stir for 30min to ensure that it is fully dispersed in the solution. Add 1.4mL deionized water and 2mL ammonia water and continue stirring, slowly add 5.8mL of tetraethyl orthosilicate (TEOS) and continue stirring the reaction for 4h. Then collect the product by centrifugation, wash it thoroughly with deionized water and ethanol three times to obtain titanate@silicon dioxide nanoparticles, put it in an oven and dry it at 80℃ for 24 hours to obtain solid powder. The sample and dimethyl silicone oil are formulated into an electrorheological fluid at a weight ratio of 10wt% of solid particles to silicone oil. Fig.15 This is a SEM photo of titanate@silica nanocomposite particles prepared by controlled hydrolysis of 5.8 mL TEOS for 4 hours. It can be seen from the figure that the shape of the particles is more like a rod.
Claims
1. An electrorheological fluid, characterized in that The dispersed phase of the electrorheological fluid is a titanate@silicon dioxide nanocomposite material, and the continuous phase is dimethyl silicone oil; the dispersed phase is a titanate@silicon dioxide nanotube composite material prepared by a two-step method, firstly a hydrothermal method is used to prepare titanate nanotubes, and then a controlled hydrolysis method is used to coat silicon dioxide on the surface of the titanate nanotubes to form a titanate@silicon dioxide one-dimensional nanocomposite material having both a core-shell structure and a hollow structure; The preparation process is simple, the raw materials are easily available, and the component properties are easily controlled. The electrorheological fluid prepared by the composite material and dimethyl silicone oil has some excellent properties, including good anti-precipitation stability, good temperature stability, and good chemical stability. The preparation process of the electrorheological fluid includes the following steps: (1) A mixture of 1.5 g P25 TiO2 powder and 150 mL 10 M NaOH aqueous solution was stirred at room temperature for 30 min. The mixture was then homogenized in an ultrasonic generator for 1 h and transferred to a hydrothermal reactor and heated at 120 °C for 24 h. After cooling to room temperature, the centrifuged product was first washed with 1 M HCl solution and then rinsed with deionized water until the pH value reached 7. After centrifugation, the obtained titanate nanotube product was dried at 70 °C for 12 h. (2) 0.5 g of the prepared titanate nanotube sample was uniformly dispersed in a mixed solution of 100 mL of ethanol, 40 mL of deionized water and 2 mL of 25-28 wt.% ammonia solution and stirred for 6 h to ensure that the titanate nanotubes were fully dispersed; then a mixed solution of 60 mL of ethanol and 2.24 mL of TEOS was uniformly and slowly added dropwise to the above solution, and the stirring reaction was continued for 6 hours; then the product was collected by centrifugation, thoroughly washed with deionized water and ethanol three times, and dried in an oven at 80°C for 24 hours to obtain a solid powder; (3) The solid powder and dimethyl silicone oil are mixed into an electrorheological fluid at a weight ratio of 10 wt % of the solid powder to the dimethyl silicone oil.