A high modulus copper foil production process
By adding tungsten, molybdenum, potassium and other alloying elements and additives such as gelatin and ascorbic acid in the copper foil production process, the shear modulus of the copper foil is increased, the problem of insufficient modulus of the copper foil is solved, and the performance of the PCB board at high temperatures is significantly improved. Rigidity and reliability.
Patent Information
- Application Number
- CN202011422027.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-12-08
AI Technical Summary
The modulus of existing copper foil is low, which results in insufficient rigidity of the PCB board at high temperatures and prone to board bending and warping, affecting the reliability of IC assembly.
A high-modulus copper foil production process is adopted, by dissolving copper rods and copper wires with sulfuric acid into a high-purity copper sulfate aqueous solution as the main electrolyte, adding alloying elements such as tungsten, molybdenum, and potassium, and adding gelatin, Ascorbic acid and chloride ions are used as additives, and electrolysis is performed to obtain a rough foil, which is then surface treated to increase the shear modulus of the copper foil.
It improves the production quality of copper foil, ensures that the modulus retention rate of PCB sheets at high temperatures reaches more than 80%, and significantly improves the flatness and reliability of the sheets.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal materials, and in particular to a production process of a high modulus copper foil. Background Art
[0002] Copper foil is used as a conductive material for printed circuit boards (PCBs). With the development of technology, electronic products tend to be multifunctional, light, thin and integrated. As PCBs become thinner, it is particularly important to maintain a certain rigidity of the material at high temperature to ensure the reliability of IC assembly. Once the board bends or warps, the original device cannot be assembled.
[0003] Modulus is a physical quantity that describes the ability of solid materials to resist deformation. Materials with high modulus are rigid and difficult to bend or stretch. The present invention develops a high modulus copper foil based on shear modulus. Shear modulus refers to the ratio of shear stress to shear strain. The elastic modulus of ordinary electrolytic copper foil at 20°C is 105GPa, and the shear modulus is 38GPa. It is generally related to the composition of the material and has little to do with the organizational structure.
[0004] By using high modulus copper foil, the modulus retention rate of PCB board at high temperature reaches more than 80%, and the flatness and reliability of the board are greatly improved in subsequent processing. The modulus retention rate of PCB pressed by ordinary copper foil at high temperature is only 25%. Summary of the invention
[0005] In view of the problems in the related art, the present invention proposes a high modulus copper foil production process to solve the problem of low modulus of copper foil produced by the existing production process.
[0006] In order to achieve the above technical objectives, the technical solution of the present invention is as follows:
[0007] A high modulus copper foil production process is used, comprising the following steps:
[0008] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0009] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0010] Step S3: filtering the main electrolyte to which the alloy element is added;
[0011] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0012] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0013] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0014] Furthermore, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 35-50 g / L and 60-90 g / L, respectively.
[0015] Furthermore, in step S2, the alloying elements include at least one of the following: sodium tungstate, ammonium tungstate, sodium molybdate, and potassium sodium tartrate, and the concentrations are 1.5-25 g / l, 1.0-20 g / l, 2.5-25 g / l, and 20-40 g / l, respectively.
[0016] Furthermore, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 3-15 ppm, 35-125 ppm and 10-30 ppm respectively.
[0017] Furthermore, in step S5, the electrolysis temperature of the main electrolyte is 45-60°C and the current density is 800-3000A / m 2 .
[0018] Furthermore, in step S6, the content of tungsten and molybdenum in the high modulus copper foil is 0.01%-0.05%.
[0019] Furthermore, in step S6, the electrodeposition thickness of the copper foil is 9-105 um.
[0020] Beneficial effects of the present invention: The copper foil production process can produce high-modulus copper foil, thereby improving the production quality of the copper foil. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0022] Embodiment 1:
[0023] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0024] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0025] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0026] Step S3: filtering the main electrolyte to which the alloy element is added;
[0027] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0028] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0029] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0030] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 50 g / L and 90 g / L, respectively.
[0031] In this embodiment, in step S2, the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations are 21.3 g / l and 40 g / l respectively.
[0032] In this embodiment, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 15 ppm, 75 ppm and 15 ppm respectively.
[0033] In this embodiment, in step S5, the main electrolyte electrolysis temperature is 60°C and the current density is 1500A / m 2 .
[0034] In this embodiment, in step S6, the electrodeposition thickness of the copper foil is 35 um.
[0035] Embodiment 2:
[0036] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0037] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0038] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0039] Step S3: filtering the main electrolyte to which the alloy element is added;
[0040] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0041] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0042] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0043] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 50 g / L and 90 g / L, respectively.
[0044] In this embodiment, in step S2, the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations are 10.65 g / l and 30 g / l respectively.
[0045] In this embodiment, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 15 ppm, 50 ppm and 15 ppm respectively.
[0046] In this embodiment, in step S5, the main electrolyte electrolysis temperature is 60°C and the current density is 1500A / m 2 .
[0047] In this embodiment, in step S6, the electrodeposition thickness of the copper foil is 35 um.
[0048] Embodiment three:
[0049] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0050] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0051] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0052] Step S3: filtering the main electrolyte to which the alloy element is added;
[0053] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0054] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0055] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0056] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 50 g / L and 90 g / L, respectively.
[0057] In this embodiment, in step S2, the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations are 4.25 g / l and 25 g / l respectively.
[0058] In this embodiment, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 15 ppm, 30 ppm and 15 ppm respectively.
[0059] In this embodiment, in step S5, the main electrolyte electrolysis temperature is 60°C and the current density is 1750A / m 2 .
[0060] In this embodiment, in step S6, the electrodeposition thickness of the copper foil is 35 um.
[0061] Embodiment 4:
[0062] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0063] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0064] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0065] Step S3: filtering the main electrolyte to which the alloy element is added;
[0066] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0067] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0068] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0069] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 50 g / L and 90 g / L, respectively.
[0070] In this embodiment, in step S2, the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations are 10.5 g / l and 40 g / l respectively.
[0071] In this embodiment, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 15 ppm, 50 ppm and 15 ppm respectively.
[0072] In this embodiment, in step S5, the main electrolyte electrolysis temperature is 55°C and the current density is 1200A / m 2 .
[0073] In this embodiment, in step S6, the electrodeposition thickness of the copper foil is 18 um.
[0074] Embodiment five:
[0075] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0076] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0077] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0078] Step S3: filtering the main electrolyte to which the alloy element is added;
[0079] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0080] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0081] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0082] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 50 g / L and 90 g / L, respectively.
[0083] In this embodiment, in step S2, the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations are 15 g / l and 20 g / l respectively.
[0084] In this embodiment, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 12 ppm, 24 ppm and 18 ppm respectively.
[0085] In this embodiment, in step S5, the main electrolyte electrolysis temperature is 55°C and the current density is 1000A / m 2 .
[0086] In this embodiment, in step S6, the electrodeposition thickness of the copper foil is 18 um.
[0087] Embodiment six:
[0088] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0089] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0090] Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements contain at least one of tungsten, molybdenum and potassium;
[0091] Step S3: filtering the main electrolyte to which the alloy element is added;
[0092] Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions;
[0093] Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0094] Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
[0095] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 50 g / L and 90 g / L, respectively.
[0096] In this embodiment, in step S2, the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations are 5 g / l and 20 g / l respectively.
[0097] In this embodiment, in step S4, the concentrations of gelatin, ascorbic acid and chloride ions are 15 ppm, 30 ppm and 15 ppm respectively.
[0098] In this embodiment, in step S5, the main electrolyte electrolysis temperature is 55°C and the current density is 800A / m 2 .
[0099] In this embodiment, in step S6, the electrodeposition thickness of the copper foil is 18 um.
[0100] Embodiment 7 (comparative sample):
[0101] A high modulus copper foil production process according to an embodiment of the present invention comprises the following steps:
[0102] Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte;
[0103] Step S2: filtering the main electrolyte;
[0104] Step S3: adding additives to the filtered main electrolyte; the additives include gelatin and chloride ions;
[0105] Step S4: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil;
[0106] Step S5: Surface treatment is performed on the rough foil to obtain copper foil.
[0107] In this embodiment, in step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 80 g / L and 90 g / L, respectively.
[0108] In this embodiment, in step S3, the concentrations of gelatin and chloride ions are 15 ppm and 25 ppm respectively.
[0109] In this embodiment, in step S4, the main electrolyte electrolysis temperature is 55°C and the current density is 2500A / m 2 .
[0110] In this embodiment, in step S5, the electrodeposition thickness of the copper foil is 18 um.
[0111] The shear modulus under different production conditions in the above embodiment is measured as follows:
[0112] Test No. Product thicknessum Shear modulus E Gpa Example 1 35 42.3 Example 2 35 43.2 Example 3 18 42.8 Example 4 18 43.1 Example 5 18 44.1 Example 6 18 42.4 Example 7 (comparative sample) 18 38.2
[0113] In summary, the high modulus copper foil manufactured in the embodiment can be made into a high modulus electronic circuit copper foil by adopting any known peel strength enhancement and anti-oxidation surface treatment process.
[0114] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0115] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high modulus copper foil production process, characterized in that: The following steps are involved: Step S1: dissolving the copper rod and the copper wire with sulfuric acid to form a high-purity copper sulfate aqueous solution as the main electrolyte; Step S2: adding alloy elements to the main electrolyte, wherein the alloy elements include sodium tungstate and potassium sodium tartrate, and the concentrations thereof are 1.5-25 g / l and 20-40 g / l, respectively; Step S3: filtering the main electrolyte to which the alloy element is added; Step S4: adding additives to the filtered main electrolyte; the additives include gelatin, ascorbic acid and chloride ions; In step S4, the concentrations of gelatin, ascorbic acid and chloride ion are 3-15 ppm, 35-125 ppm and 10-30 ppm respectively; Step S5: feeding the main electrolyte with additives into the electrolytic cell for electrolysis to obtain a rough foil; Step S6: Surface treatment is performed on the rough foil to obtain a high modulus copper foil.
2. A high modulus copper foil production process according to claim 1, characterized in that: In step S1, the concentrations of copper and sulfuric acid in the main electrolyte are 35-50 g / L and 60-90 g / L, respectively.
3. A high modulus copper foil production process according to claim 1, characterized in that: In step S5, the electrolysis temperature of the main electrolyte is 45-60°C and the current density is 800-3000A / m 2 .
Citation Information
Patent Citations
High strength, high heat-resistance electrolytic copper foil, and manufacturing method for same
CN103827358A
Electrolytic copper foil and method for producing same
CN104903495A
Electrodeposited foil with controlled properties for printed circuit board applications and procedures and electrolyte bath solutions for preparing same
CN1053818A
Production of electrolytic copper foil
JP1997067693A