Silicon carbide substrate
The metal catalyst and impurities on the silicon carbide substrate are removed through a multi-step cleaning process, which solves the problem of increased surface roughness of the epitaxial layer and achieves higher smoothness and epitaxial layer quality.
Patent Information
- Application Number
- CN202011131017.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2014-10-23
- Filing Date
- 2015-08-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2035-08-31
AI Technical Summary
In the process of manufacturing silicon carbide substrates, after using polishing agents containing metal catalysts, the silicon carbide epitaxial layer may grow abnormally, resulting in an increase in surface roughness, and the metal catalyst residue is difficult to completely remove, affecting the smoothness of the epitaxial layer.
A multi-step cleaning process is used, including the use of cleaning agents such as aqua regia, sulfuric acid-hydrogen peroxide, ammonia-hydrogen peroxide, hydrochloric acid-hydrogen peroxide and hydrofluoric acid, combined with different concentrations and treatment times, to remove the residue in the polish The metal catalyst and other metal impurities reduce the surface roughness of the epitaxial layer.
It effectively reduces the metal residue on the surface of the silicon carbide substrate, reduces the surface roughness of the epitaxial layer, and improves the smoothness of the substrate and the quality of the epitaxial layer.
Smart Images

Figure CN112531019B_ABST
Abstract
Description
[0001] This application is a divisional application of an invention patent application filed on August 31, 2015, whose applicant is "Sumitomo Electric Industries, Ltd.", whose invention name is "Silicon carbide substrate and method for manufacturing the silicon carbide substrate", and whose application number is 201580055161.3. Technical Field
[0002] The present disclosure relates to a silicon carbide substrate and a method for manufacturing the silicon carbide substrate. Background Art
[0003] In recent years, in order to achieve high breakdown voltage, low loss, etc. in semiconductor devices, silicon carbide (SiC) has begun to be adopted as a material constituting semiconductor devices.
[0004] In the process of manufacturing a silicon carbide substrate, a silicon carbide substrate sliced from a silicon carbide ingot is polished to make its surface smooth, and then the silicon carbide substrate is cleaned. For example, PTD1 (Japanese Patent Laid-Open No. 2010-4073) discloses a technology for cleaning a silicon carbide substrate using an aqueous solution containing sulfuric acid and hydrogen peroxide water.
[0005] Reference List
[0006] Patent Literature
[0007] PTD 1: Japanese Patent Publication No. 2010-4073 Summary of the invention
[0008] The silicon carbide substrate according to the present disclosure is a silicon carbide substrate having a main surface having a surface roughness (Ra) of less than or equal to 0.1 nm, and in the main surface, vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium each having a surface roughness of less than or equal to 1.0×10 12 Atom / cm 2 concentration.
[0009] The method for manufacturing a silicon carbide substrate according to the present disclosure includes the steps of preparing a silicon carbide substrate having a main surface, polishing the main surface of the silicon carbide using a polishing agent containing a metal catalyst, and cleaning the silicon carbide substrate after the polishing step. The cleaning step includes cleaning the silicon carbide substrate using aqua regia. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is a partial cross-sectional view showing a configuration of a silicon carbide substrate according to the first embodiment.
[0011] Figure 2 is a flowchart for schematically illustrating a method for manufacturing a silicon carbide substrate according to the first embodiment.
[0012] Figure 3 is a schematic view for illustrating a step in the method for manufacturing the silicon carbide substrate according to the first embodiment.
[0013] Figure 4 is a schematic configuration diagram of a polishing device used in the polishing step.
[0014] Figure 5 is a schematic view for illustrating a step in the method for manufacturing the silicon carbide substrate according to the first embodiment.
[0015] Figure 6 Schematic diagram of the cleaning equipment used in the cleaning step.
[0016] Figure 7 is a flowchart for schematically illustrating a cleaning method in the method for manufacturing a silicon carbide substrate according to the first embodiment.
[0017] Figure 8 is a flow chart for schematically illustrating a cleaning method according to a first variation.
[0018] Fig. 9 is a flow chart for schematically illustrating a cleaning method according to a second variation. DETAILED DESCRIPTION
[0019] [Description of Embodiments]
[0020] In order to polish the silicon carbide substrate, for example, a chemical mechanical polishing method called a CMP (chemical mechanical polishing) method is used. In the CMP method, for example, a polishing agent containing a metal catalyst that reforms the surface by a catalytic reaction to increase the oxidizing power of the oxidant is used so as to achieve good surface roughness at a high polishing rate. An oxide layer having a hardness lower than that of silicon carbide is formed on the surface of the silicon carbide substrate by the metal catalyst. Since polishing is promoted by removing the oxide layer by mechanical force, both a high polishing rate and good surface roughness can be achieved.
[0021] However, when a silicon carbide substrate is polished using a polishing agent containing a metal catalyst and thereafter a silicon carbide epitaxial layer (hereinafter also referred to as an epitaxial layer (epi layer)) is grown on the silicon carbide substrate, the silicon carbide epitaxial layer may grow abnormally locally and may have high surface roughness.
[0022] First, aspects of the present disclosure will be described in a list form.
[0023] (1) A silicon carbide substrate according to the present disclosure is a silicon carbide substrate having a main surface having a surface roughness (Ra) of less than or equal to 0.1 nm, and in the main surface, vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium each having a surface roughness of less than or equal to 1.0×1012 Atom / cm 2 Here, the main surface means a surface on which a device such as a transistor, a diode, etc. is to be formed.
[0024] By using a polishing agent containing a metal catalyst in a CMP method, the surface roughness (Ra) of the main surface of the silicon carbide substrate is easily set to be less than or equal to 0.1 nm.
[0025] For example, the metal catalyst includes at least one metal element selected from the group consisting of vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium. These metal elements have a catalytic effect of breaking the bonds between atoms arranged in the surface of silicon carbide, so that the surface is easily oxidized. Therefore, an oxide layer having a hardness lower than that of silicon carbide can be suitably formed on the main surface of the silicon carbide substrate. Therefore, the polishing of the silicon carbide substrate can be promoted.
[0026] However, even when the silicon carbide substrate is cleaned after polishing using a polishing agent containing the above-mentioned metal catalyst, the metal derived from the metal catalyst attached to the main surface of the silicon carbide substrate may remain on the main surface. When an epitaxial layer is grown on a silicon carbide substrate having a metal retained on the main surface, the material molecules of the epitaxial layer can selectively adhere to the portion where the metal is retained in the initial stage of epitaxial growth. As a result, the epitaxial layer grows abnormally. When the epitaxial layer grows abnormally locally, the epitaxial layer has a high surface roughness. Therefore, in order to reduce the surface roughness of the epitaxial layer, it is necessary to reduce the metal retained in the main surface of the silicon carbide substrate.
[0027] In the silicon carbide substrate described above, the surface roughness of the epitaxial layer grown on the main surface of the silicon carbide substrate can be reduced.
[0028] (2) Preferably, in the above-mentioned silicon carbide substrate, vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium each have an area less than or equal to 2.0×10 11 Atom / cm 2 .
[0029] (3) Preferably, in the silicon carbide substrate described in (1) or (2) above, potassium, sodium, calcium, iron, copper, aluminum, and tin each have an area less than or equal to 1.0×10 10 Atom / cm 2 concentration.
[0030] (4) Preferably, in the silicon carbide substrate described in any one of (1) to (3) above, the silicon carbide substrate has a diameter greater than or equal to 100 mm.
[0031] (5) A method for manufacturing a silicon carbide substrate according to the present disclosure includes the steps of preparing a silicon carbide substrate having a main surface, polishing the main surface of the silicon carbide using a polishing agent containing a metal catalyst, and cleaning the silicon carbide substrate after the polishing step. The cleaning step includes cleaning the silicon carbide substrate using aqua regia. By cleaning the silicon carbide substrate using aqua regia after polishing the silicon carbide substrate, the metal catalyst remaining in the main surface (which is the polished surface) of the silicon carbide can be removed. Therefore, the surface roughness of the epitaxial layer formed on the main surface can be reduced.
[0032] (6) Preferably, in the above-mentioned method for manufacturing a silicon carbide substrate, in the polishing step, the polishing agent contains at least one metal element selected from the group consisting of vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium as a metal catalyst.
[0033] (7) Preferably, in the method for manufacturing a silicon carbide substrate described in (5) or (6) above, the step of cleaning further includes the following steps: cleaning the silicon carbide substrate with a sulfuric acid-hydrogen peroxide aqueous mixture, and cleaning the silicon carbide substrate with an ammonia-hydrogen peroxide aqueous mixture after the step of cleaning with the sulfuric acid-hydrogen peroxide aqueous mixture. The step of cleaning with aqua regia is performed after the step of cleaning with the ammonia-hydrogen peroxide aqueous mixture. The step of cleaning further includes the following steps: cleaning the silicon carbide substrate with a hydrochloric acid-hydrogen peroxide aqueous mixture after the step of cleaning with the aqua regia, and cleaning the silicon carbide substrate with hydrofluoric acid after the step of cleaning with the hydrochloric acid-hydrogen peroxide aqueous mixture. Thus, the metal catalyst and the metal other than the metal catalyst remaining in the main surface of the silicon carbide can be reduced. "Metal other than the metal catalyst" includes, for example, at least one metal selected from the group consisting of, for example, potassium, sodium, calcium, iron, copper, aluminum and tin.
[0034] (8) Preferably, in the method for manufacturing a silicon carbide substrate described in (7) above, in each of the following cleaning steps, the processing time is set to be greater than or equal to 15 minutes: cleaning with a sulfuric acid-hydrogen peroxide aqueous mixture, cleaning with an ammonia-hydrogen peroxide aqueous mixture, cleaning with aqua regia, cleaning with a hydrochloric acid-hydrogen peroxide aqueous mixture, and cleaning with hydrofluoric acid.
[0035] (9) Preferably, in the method for manufacturing a silicon carbide substrate described in (5) or (6) above, the step of cleaning further includes: a step of cleaning the silicon carbide substrate with an ammonia-hydrogen peroxide aqueous mixture. The step of cleaning the silicon carbide substrate with aqua regia is performed after the step of cleaning with the ammonia-hydrogen peroxide aqueous mixture. Thus, organic substances adhering to the main surface of the silicon carbide substrate can be reduced, and metal catalysts and metals other than metal catalysts remaining in the main surface of the silicon carbide substrate can be reduced.
[0036] (10) Preferably, in the method for manufacturing a silicon carbide substrate described in (9) above, the processing time is set to be greater than or equal to 15 minutes in each of the following steps: cleaning with an ammonia-hydrogen peroxide aqueous mixture and cleaning with aqua regia.
[0037] (11) Preferably, in the method for manufacturing a silicon carbide substrate described in (5) or (6) above, the cleaning step further includes: cleaning the silicon carbide substrate with a sulfuric acid-hydrogen peroxide aqueous mixture. The cleaning step with aqua regia is performed after the cleaning step with the sulfuric acid-hydrogen peroxide aqueous mixture. The cleaning step further includes, after the cleaning step with aqua regia, cleaning the silicon carbide substrate with hydrofluoric acid.
[0038] (12) In the method for manufacturing a silicon carbide substrate described in (11) above, the processing time is set to be greater than or equal to 15 minutes in each of the following steps: cleaning with a sulfuric acid-hydrogen peroxide aqueous mixture, cleaning with aqua regia, and cleaning with hydrofluoric acid.
[0039] (13) Preferably, in the method for manufacturing a silicon carbide substrate described in any one of (5) to (12) above, in the step of cleaning with aqua regia, the aqua regia in the mixed solution prepared by mixing aqua regia and ultrapure water has a volume concentration greater than or equal to 50% and less than or equal to 100%.
[0040] (14) Preferably, in the method for manufacturing a silicon carbide substrate described in any one of (7), (8), (11) and (12) above, in the step of cleaning with a sulfuric acid-hydrogen peroxide aqueous mixture, the volume of sulfuric acid contained in the sulfuric acid-hydrogen peroxide aqueous mixture is greater than or equal to one times the volume of ultrapure water contained in the sulfuric acid-hydrogen peroxide aqueous mixture and less than or equal to five times the volume of the ultrapure water contained in the sulfuric acid-hydrogen peroxide aqueous mixture, and the volume of hydrogen peroxide aqueous solution contained in the sulfuric acid-hydrogen peroxide aqueous mixture is greater than or equal to one times the volume of the ultrapure water contained in the sulfuric acid-hydrogen peroxide aqueous mixture and less than or equal to three times the volume of the ultrapure water contained in the sulfuric acid-hydrogen peroxide aqueous mixture.
[0041] (15) Preferably, in the method for manufacturing a silicon carbide substrate described in any one of (7) to (10) above, in the step of cleaning with an ammonia-hydrogen peroxide aqueous mixture, the volume of the ammonia aqueous solution contained in the ammonia-hydrogen peroxide aqueous mixture is greater than or equal to one tenth of the volume of ultrapure water contained in the ammonia-hydrogen peroxide aqueous mixture and less than or equal to one times the volume of the ultrapure water contained in the ammonia-hydrogen peroxide aqueous mixture, and the volume of the hydrogen peroxide aqueous solution contained in the ammonia-hydrogen peroxide aqueous mixture is greater than or equal to one tenth of the volume of the ultrapure water contained in the ammonia-hydrogen peroxide aqueous mixture and less than or equal to one times the volume of the ultrapure water contained in the ammonia-hydrogen peroxide aqueous mixture.
[0042] (16) Preferably, in the method for manufacturing a silicon carbide substrate described in any one of (5) to (15) above, in the cleaning step, the silicon carbide substrate is set to have a temperature of 40° C. or less.
[0043] [Details of implementation]
[0044] Hereinafter, specific examples of embodiments of the present disclosure will be described with reference to the accompanying drawings. It should be noted that the same or corresponding parts in the following drawings will be referred to by the same reference numerals, and their description will not be repeated. In addition, in this specification, an independent plane is represented by (), and a group of planes is represented by {}. In addition, negative indices should be indicated crystallographically by placing a "-" (bar) above the number, but in this specification it is indicated by placing a minus sign before the number.
[0045] (First embodiment)
[0046] <Structure of Silicon Carbide Substrate>
[0047] First, the configuration of a silicon carbide substrate according to a first embodiment will be described. Figure 1 FIG. 1 is a partial cross-sectional view showing the configuration of silicon carbide substrate 10 according to the first embodiment.
[0048] like Figure 1 As shown, silicon carbide substrate 10 has main surface 10A. For example, silicon carbide substrate 10 is made of hexagonal silicon carbide single crystal having a polytype of 4H. For example, silicon carbide substrate 10 contains n-type impurities such as nitrogen. The impurities of silicon carbide substrate 10 have, for example, greater than or equal to 5.0×10 18 cm -3 and less than or equal to 2.0×10 19 cm -3 Silicon carbide substrate 10 has a diameter of, for example, greater than or equal to 100 mm (greater than or equal to 4 inches), and may have a diameter of greater than or equal to 150 mm (6 inches).
[0049] Main surface 10A has a surface roughness (Ra) of less than or equal to 0.1 nm. “Surface roughness (Ra)” is a value measured in accordance with JIS B 0601. For example, surface roughness (Ra) can be measured using an atomic force microscope (AFM).
[0050] As the AFM, for example, "Dimension 300" manufactured by Veeco can be used. In addition, as the cantilever (probe) of the above AFM, for example, the model "NCHV-10V" manufactured by Bruker can be used. As an example, as a condition for measuring using AFM, the measurement mode is set to the tapping mode, the measurement area in the tapping mode is set to a square with each side length of 10μm, the spacing is set to 40nm, and the measurement depth is set to 1.0μm. In addition, sampling in the tapping mode is performed under the conditions that the scanning speed in the above measurement range is 5 seconds per cycle, the number of data for each scanning line is 512 points, and the number of scanning lines is 512. In addition, the displacement control for the cantilever is set to 15.50nm.
[0051] Main surface 10A may be, for example, a {0001} plane, or a surface having a predetermined off-angle (for example, an off-angle of less than or equal to 10°) with respect to the {0001} plane.
[0052] Vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium each have an area greater than or equal to 1.0×10 6 Atom / cm 2 and less than or equal to 1.0×10 12 Atom / cm 2 More preferably, potassium, sodium, calcium, iron, copper, aluminum, and tin each have a concentration of less than or equal to 1.0×10 10 Atom / cm 2 The concentration of the metal impurities in main surface 10A can be measured by ICP-MS (Inductively Coupled Plasma Mass Spectrometry). Specifically, for example, ICP-MS7500 manufactured by Agillent can be used.
[0053] <Method for Manufacturing Silicon Carbide Substrate>
[0054] A method for manufacturing silicon carbide substrate 10 according to the first embodiment will be described. Figure 2 As shown, the method for manufacturing silicon carbide substrate 10 according to the present embodiment includes a preparing step ( S10 ), a polishing step ( S20 ), and a cleaning step ( S30 ).
[0055] In the preparation step (S10), silicon carbide substrate 10 cut out from a single-crystal silicon carbide ingot is prepared. Figure 3 As shown, silicon carbide substrate 10 according to the present embodiment is made of hexagonal silicon carbide single crystal having a polytype of, for example, 4H, and has main surface 11A.
[0056] In the grinding step (S20), for example, Figure 4 1. For example, a CMP apparatus is used as the polishing apparatus 100. In the polishing step (S20), as shown in FIG. Figure 5 As shown in FIG. 1 , a new main surface 10A is formed by polishing the main surface 11A. Figure 4 As shown, the polishing apparatus 100 used in the first embodiment includes a substrate holding portion 101, a turntable portion 104, a polishing cloth 102, and a polishing agent supply portion 108. The substrate holding portion 101 includes a pressure head that rotates about a rotation axis C2 through a transmission shaft not shown. The turntable portion 104 includes a disc-shaped portion that rotates about a rotation axis C1 through a rotation shaft 106. The polishing cloth 102 is fixed to the upper surface of the turntable portion 104. The polishing agent supply portion 108 for supplying a polishing agent 110 is provided above the turntable portion 104.
[0057] When the polishing step (S20) is performed, silicon carbide substrate 10 is attached to the lower surface of the pressure head of substrate holding portion 101 and arranged so that main surface 11A faces polishing cloth 102. Then, the pressure head is lowered to apply a predetermined pressure to silicon carbide substrate 10. Next, while polishing agent 110 is supplied from polishing agent supply portion 108 to polishing cloth 102, the polishing agent 110 is supplied to polishing cloth 102 in the same direction (by Figure 4 The substrate holding portion 101 and the turntable portion 104 are rotated in the direction indicated by the arrow in FIG. 1 . It should be noted that the substrate holding portion 101 and the turntable portion 104 may be rotated in opposite directions, or one of them may be rotated while the other is fixed.
[0058] The polishing agent 110 used in the polishing step (S20) contains abrasive grains, an oxidizing agent, and a metal catalyst. The abrasive grains are materials softer than silicon carbide to reduce surface roughness and process damage layers. For example, colloidal silica, silica powder, aluminum oxide, diamond, or the like are used as abrasive grains. The oxidizing agent forms an oxide film on the main surface 11A. For example, hydrogen peroxide water, sodium hypochlorite, barium percarbonate, etc. are used as oxidizing agents.
[0059] The metal catalyst includes at least one metal element selected from the group consisting of vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium. For example, sodium tungstate, sodium vanadate, sodium molybdate, etc. are used as the metal catalyst.
[0060] The polishing agent 110 has a pH of preferably less than or equal to 6 or greater than or equal to 9.5, and more preferably less than or equal to 4 or greater than or equal to 10.5 to increase the chemical reaction. The pH of the polishing agent 110 can be controlled by adding an inorganic acid such as hydrochloric acid, nitric acid, sulfuric acid, or phosphoric acid; an organic acid such as formic acid, acetic acid, oxalic acid, citric acid, malic acid, tartaric acid, succinic acid, phthalic acid, or fumaric acid; an inorganic base such as KOH, NaOH, or NH4OH; an organic base such as choline, ammonia, or TMAH (sodium tetramethylammonium hydroxide); or a salt thereof.
[0061] The main surface 10A subjected to the polishing step (S20) has a surface roughness (Ra) less than or equal to 0.1 nm. Foreign matter such as dust, a polishing agent used in the polishing step (S20), etc. may adhere to the main surface 10A. Specifically, abrasive grains, organic substances, metals, etc. may adhere to the main surface 10A. The metal adhered to the main surface 10A originates from, for example, a metal catalyst contained in the polishing agent, or the surrounding environment.
[0062] Next, perform a wash step ( Figure 2 :S30). Figure 6 As shown, the cleaning device 120 used in the first embodiment includes a cleaning treatment tank 122, a pump 124, a filter 126, and a heater 128. By immersing the silicon carbide substrate 10 in the cleaning treatment tank 122 filled with a cleaning solution 130 for a certain period of time, the cleaning treatment is performed. At least part of the impurities (such as dust, organic matter, and metal) adhering to the immersed main surface 10A are dissolved in the cleaning solution 130 and removed. The cleaning solution 130 is always circulated by the pump 124 and filtered by the filter 126. In addition, by temperature control performed using the heater 128, the cleaning solution 130 is maintained at a desired temperature.
[0063] like Figure 7 As shown, the cleaning step (S30) includes a plurality of steps performed in order: for example, cleaning with a sulfuric acid-hydrogen peroxide water mixture (S31), cleaning with an ammonia-hydrogen peroxide water mixture (S32), cleaning with aqua regia (S33), cleaning with a hydrochloric acid-hydrogen peroxide water mixture (S34), and cleaning with hydrofluoric acid (S35). A step of cleaning with ultrapure water may be performed after completing each cleaning step to rinse the cleaning solution on the main surface 10A, etc. For example, water having a resistivity greater than or equal to 15 MΩ·cm, a total organic carbon (TOC) less than 100 ppb, and residual silicon dioxide less than 10 ppb can be used as ultrapure water. The same applies to ultrapure water used in subsequent steps.
[0064] It should be noted that, before the step of cleaning with sulfuric acid-hydrogen peroxide water mixture, an alkaline cleaning step may be performed. In the alkaline cleaning step, abrasive grains (such as colloidal silica) adhering to main surface 10A in the polishing step (S20) are removed, for example, by TMAH and a surfactant.
[0065] In the step of cleaning with sulfuric acid-hydrogen peroxide mixture (S31), organic substances adhering to the main surface 10A are removed by sulfuric acid-hydrogen peroxide mixture. The sulfuric acid-hydrogen peroxide mixture is a solution prepared by mixing sulfuric acid, hydrogen peroxide and ultrapure water. For example, concentrated sulfuric acid with a mass percentage concentration of 98% can be used as sulfuric acid. For example, hydrogen peroxide with a mass percentage concentration of 30% can be used as hydrogen peroxide. The same applies to the hydrogen peroxide used in subsequent steps.
[0066] For example, the volume ratio between sulfuric acid, hydrogen peroxide and ultrapure water contained in the sulfuric acid-hydrogen peroxide mixture is 1 (sulfuric acid): 1 (hydrogen peroxide): 1 (ultrapure water). Preferably, the volume ratio between sulfuric acid, hydrogen peroxide and ultrapure water is 1 (sulfuric acid): 1 (hydrogen peroxide): 1 (ultrapure water) to 5 (sulfuric acid): 3 (hydrogen peroxide): 1 (ultrapure water). In other words, the volume of sulfuric acid is greater than or equal to one time and less than or equal to five times the volume of ultrapure water, and the volume of hydrogen peroxide is greater than or equal to one time and less than or equal to three times the volume of ultrapure water.
[0067] Next, in the step of cleaning with an ammonia-hydrogen peroxide aqueous solution (S32), organic substances adhering to the main surface 10A are removed by the ammonia-hydrogen peroxide aqueous solution. The ammonia-hydrogen peroxide aqueous solution is a solution prepared by mixing an ammonia aqueous solution, hydrogen peroxide aqueous solution, and ultrapure water. For example, an ammonia aqueous solution having a mass percentage concentration of 28% can be used as the ammonia aqueous solution.
[0068] The volume ratio between the aqueous ammonia solution, aqueous hydrogen peroxide and ultrapure water contained in the ammonia-hydrogen peroxide mixture is, for example, 1 (aqueous ammonia solution): 1 (aqueous hydrogen peroxide): 10 (ultrapure water). Preferably, the volume ratio between the aqueous ammonia solution, aqueous hydrogen peroxide and ultrapure water is 1 (aqueous ammonia solution): 1 (aqueous hydrogen peroxide): 10 (ultrapure water) to 1 (aqueous ammonia solution): 1 (aqueous hydrogen peroxide): 1 (ultrapure water). In other words, the volume of the aqueous ammonia solution is greater than or equal to one-tenth the volume of the ultrapure water and less than or equal to one times the volume of the ultrapure water, and the volume of the aqueous hydrogen peroxide is greater than or equal to one-tenth the volume of the ultrapure water and less than or equal to one times the volume of the ultrapure water.
[0069] Next, in the step of cleaning with aqua regia (S33), at least part of the metal originating from the metal catalyst remaining in the main surface 10A is removed by aqua regia. That is, the metal remaining in the main surface 10A is reduced. Aqua regia is a solution prepared by mixing hydrochloric acid and nitric acid. In this specification, "aqua regia" refers not only to a solution prepared by mixing hydrochloric acid and nitric acid, but also to a mixed solution of the solution and ultrapure water. In the first embodiment, the volume ratio between the hydrochloric acid, nitric acid and ultrapure water contained in the aqua regia is, for example, 3 (hydrochloric acid): 1 (nitric acid): 0 (ultrapure water). Preferably, the volume ratio between hydrochloric acid, nitric acid and ultrapure water is 3 (hydrochloric acid): 1 (nitric acid): 0 (ultrapure water) to 3 (hydrochloric acid): 1 (nitric acid): 2 (ultrapure water). Preferably, in a mixed solution prepared by mixing aqua regia (a mixed solution of hydrochloric acid and nitric acid) and ultrapure water, the aqua regia has a volume concentration greater than or equal to 50% and less than or equal to 100%.
[0070] Next, in the step of cleaning with a hydrochloric acid-hydrogen peroxide aqueous solution (S34), at least part of the metal remaining in the main surface 10A (except the metal derived from the metal catalyst) is removed by the hydrochloric acid-hydrogen peroxide aqueous solution. The hydrochloric acid-hydrogen peroxide aqueous solution is a solution prepared by mixing hydrochloric acid, hydrogen peroxide aqueous solution and ultrapure water. For example, concentrated hydrochloric acid with a mass percentage concentration of 98% can be used as the hydrochloric acid.
[0071] The volume ratio between the hydrochloric acid, hydrogen peroxide and ultrapure water contained in the hydrochloric acid-hydrogen peroxide mixture is, for example, 1 (hydrochloric acid): 1 (hydrogen peroxide): 10 (ultrapure water). Preferably, the volume ratio between the hydrochloric acid, hydrogen peroxide and ultrapure water is 1 (hydrochloric acid): 1 (hydrogen peroxide): 10 (ultrapure water) to 1 (hydrochloric acid): 1 (hydrogen peroxide): 5 (ultrapure water). In other words, the volume of the hydrochloric acid is greater than or equal to one-tenth of the volume of the ultrapure water and less than or equal to one-fifth of the volume of the ultrapure water, and the volume of the hydrogen peroxide is greater than or equal to one-tenth of the volume of the ultrapure water and less than or equal to one-fifth of the volume of the ultrapure water.
[0072] Next, in the step of cleaning with hydrofluoric acid (S35), the silicon oxide film is removed by hydrofluoric acid. For example, the hydrofluoric acid in the mixed solution prepared by mixing hydrofluoric acid and ultrapure water has a concentration of 30%. Preferably, the hydrofluoric acid in the mixed solution has a concentration greater than or equal to 20% and less than or equal to 50%.
[0073] For example, the treatment time in each of the above steps (S31) to (S35) is, for example, 30 minutes. Preferably, the treatment time is greater than or equal to 15 minutes, and more preferably greater than or equal to 30 minutes.
[0074] For example, in each of the above steps (S31) to (S35), silicon carbide substrate 10 is at room temperature. Preferably, in each step, silicon carbide substrate 10 is set to have a temperature of 40°C or less.
[0075] As described above, silicon carbide substrate 10 ( Figure 1 ).
[0076] The cleaning step ( S30 ) in the method for manufacturing silicon carbide 10 according to the present embodiment is not limited to the one described above. A modification of the cleaning step ( S30 ) will be described below.
[0077] (First variant)
[0078] For example, Figure 8 As shown, the cleaning step includes a plurality of steps performed in order: cleaning with an ammonia-hydrogen peroxide aqueous mixture (S32) and cleaning with aqua regia (S33). The step of cleaning with aqua regia can be performed after each cleaning step is completed. It should be noted that the alkaline cleaning step can be performed before the step of cleaning with a sulfuric acid-hydrogen peroxide aqueous mixture.
[0079] (Second variant)
[0080] For example, Fig. 9 The cleaning step includes a plurality of steps performed in order: cleaning with a sulfuric acid-hydrogen peroxide mixture (S31), cleaning with an ammonia-hydrogen peroxide mixture (S32), cleaning with aqua regia (S33), and cleaning with hydrofluoric acid (S35). The step of cleaning with aqua regia may be performed after completing each cleaning step. It should be noted that the alkaline cleaning step may be performed before the step of cleaning with a sulfuric acid-hydrogen peroxide mixture.
[0081] [Example]
[0082] Table 1 shows the relationship between the concentration of metal present at main surface 10A and the method of cleaning silicon carbide substrate 10 .
[0083] [Table 1]
[0084]
[0085] Silicon carbide substrate 10 of each of Sample 1 to Sample 3 was manufactured by the manufacturing method according to the first embodiment.
[0086] The details of the cleaning step (S30) for each of Samples 1 to 3 will be described below. First, a cleaning step (S31) using a sulfuric acid-hydrogen peroxide aqueous mixture is performed. The volume ratio between sulfuric acid, hydrogen peroxide aqueous solution, and ultrapure water contained in the sulfuric acid-hydrogen peroxide aqueous mixture is 1 (sulfuric acid): 1 (hydrogen peroxide aqueous solution): 1 (ultrapure water). In the cleaning step (S31) using the sulfuric acid-hydrogen peroxide aqueous mixture, the treatment time is 30 minutes, and the sulfuric acid-hydrogen peroxide aqueous mixture is at room temperature.
[0087] Next, a step of cleaning with an ammonia-hydrogen peroxide aqueous mixture (S31) is performed. The volume ratio between the ammonia aqueous solution, hydrogen peroxide aqueous solution and ultrapure water contained in the ammonia-hydrogen peroxide aqueous mixture is 1 (ammonia aqueous solution): 1 (hydrogen peroxide aqueous solution): 10 (ultrapure water). In the step of cleaning with an ammonia-hydrogen peroxide aqueous mixture (S32), the treatment time is 30 minutes, and the ammonia-hydrogen peroxide aqueous mixture is at room temperature.
[0088] Next, a step of washing with aqua regia (S33) is performed. The volume ratio between hydrochloric acid, nitric acid and ultrapure water contained in the aqua regia is 3 (hydrochloric acid): 1 (nitric acid): 0 (ultrapure water). In the step of washing with aqua regia (S33), the treatment time is 30 minutes, and the aqua regia is at room temperature.
[0089] Next, a step (S34) of washing with a hydrochloric acid-hydrogen peroxide mixture is performed. The volume ratio between hydrochloric acid, hydrogen peroxide and ultrapure water contained in the hydrochloric acid-hydrogen peroxide mixture is 1 (hydrochloric acid): 1 (hydrogen peroxide): 10 (ultrapure water). In the step (S34) of washing with a hydrochloric acid-hydrogen peroxide mixture, the treatment time is 30 minutes, and the aqua regia is at room temperature.
[0090] Next, a step (S35) of cleaning with hydrofluoric acid is performed. The hydrofluoric acid in the mixed solution prepared by mixing hydrofluoric acid and ultrapure water has a concentration of 30%. In the step (S35) of cleaning with hydrofluoric acid, the processing time is 30 minutes, and the hydrofluoric acid is at room temperature. That is, in the cleaning step (S30) for each of samples 1 to 3, the silicon carbide substrate 10 is set to have a temperature less than or equal to 40°C during cleaning. This cleaning step is performed at room temperature for the following reasons. Since silicon carbide is chemically inert, it takes a long time to oxidize its surface and perform lift-off. In conventional cleaning such as so-called RCA cleaning, a sulfuric acid-hydrogen peroxide water mixture and a hydrochloric acid-hydrogen peroxide water mixture at high temperature are used. However, when a sulfuric acid-hydrogen peroxide water mixture and a hydrochloric acid-hydrogen peroxide water mixture at high temperature are used to clean silicon carbide at high temperature, the sulfuric acid-hydrogen peroxide water mixture and the hydrochloric acid-hydrogen peroxide water mixture evaporate during the cleaning process, and thus reduce the cleaning effect. Therefore, silicon carbide is preferably cleaned at room temperature.
[0091] (Measurement method)
[0092] For each of samples 1 to 3, the concentration of the metal present in the main surface 10A is measured. For sample 1, the concentration of vanadium (V), tungsten (W), molybdenum (Mo), platinum (Pt), nickel (Ni), titanium (Ti), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), aluminum (Al), sodium (Na), calcium (Ca), potassium (K), and tin (Sn) is measured. For sample 2 and sample 3, the concentration of vanadium (V) and zinc (Zn) is measured. The concentration of the metal is measured by ICP-MS. Tables 2 and 3 show the measurement results of the concentration of the metal in the main surface 10A of sample 1. Table 2 shows the measurement results of the concentration of the metal catalyst present in the main surface 10A.
[0093] [Table 2]
[0094]
[0095] As shown in Table 2, for each of vanadium (V), tungsten (W), molybdenum (Mo), platinum (Pt), nickel (Ni), titanium (Ti), and chromium (Cr), in main surface 10A of sample 1, the metal concentration indicated a value less than or equal to 1.0×10 12 Atom / cm 2 The concentrations of vanadium (V) present in the main surface 10A of the sample 2 and the main surface 10A of the sample 3 are 72×10 9 Atom / cm 2 and 16×10 9 Atom / cm 2 .
[0096] Table 3 shows the measurement results of the concentration of metals present in main surface 10A other than the metal catalyst. It should be noted that "ND" in Table 3 indicates that the concentration is not detectable because it is lower than the detection lower limit value (1×10 7 Atom / cm 2 ).
[0097] [Table 3]
[0098]
[0099] As shown in Table 3, in the main surface 10A of the sample 1, iron (Fe), copper (Cu), zinc (Zn), aluminum (Al), sodium (Na), calcium (Ca), potassium (K), and tin (Sn) were determined as metals other than the metal catalyst. However, it was determined that each of these metals had a concentration of less than ×10 11 Atom / cm 2 The concentration of zinc (Zn) present in the main surface 10A of sample 2 and the main surface 10A of sample 3 are 16×10 9 Atom / cm 2 and 21×10 9 Atom / cm 2 .
[0100] It should be understood that the embodiments disclosed herein are illustrative and non-restrictive in every aspect. The scope of the present invention is defined by the scope of the claims, rather than by the embodiments described above, and is intended to include any modifications within the scope of the claims and within the meaning equivalent to the claims.
[0101] Reference Symbols List
[0102] 10: silicon carbide substrate; 10A: main surface; 11A: main surface; 20: epitaxial layer; 30: metal impurities; 100: polishing equipment; 101: substrate holding part; 102: polishing cloth; 104: turntable part; 106: transmission shaft; 108: polishing agent supply part; 110: polishing agent; 120: cleaning equipment; 122: cleaning treatment tank; 124: pump; 126: filter; 128: heater.
Claims
1. A silicon carbide substrate having a main surface, The major surface has a surface roughness (Ra) less than or equal to 0.1 nm, and The main surface includes vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium and chromium, wherein the vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium and chromium each have a relative humidity less than or equal to 1.0×10 12 Atom / cm 2 The concentration of in, Each of vanadium, tungsten, molybdenum, platinum and zirconium in the main surface has a value greater than or equal to 1.0×10 6 Atom / cm 2 The concentration of Among them, vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium, and chromium are derived from a metal catalyst contained in a polishing agent used for manufacturing the silicon carbide substrate.
2. The silicon carbide substrate according to claim 1, wherein In the main surface, vanadium, tungsten, molybdenum, platinum, nickel, titanium, zirconium and chromium each have a value less than or equal to 2.0×10 11 Atom / cm 2 concentration.
3. The silicon carbide substrate according to claim 1 or 2, wherein: In the main surface, potassium, sodium, calcium, iron, copper, aluminum and tin each have a value less than or equal to 1.0×10 10 Atom / cm 2 concentration. 4 . The silicon carbide substrate according to claim 1 , having a diameter greater than or equal to 100 mm.