Interconnected corrugated carbon-based network
Through infrared laser laser laser marking of graphite oxide film in optical disk drives, the problems of high cost and complex patterning in the prior art are solved, and the cost-effective production of interconnected corrugated carbon-based networks with high surface area and high conductivity are realized. The manufacturing of electronic devices is simplified and height adjustable control of electrochemical properties is provided.
Patent Information
- Application Number
- CN202011342273.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2011-12-21
- Filing Date
- 2012-12-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2032-12-21
AI Technical Summary
The prior art is difficult to effectively produce interconnected corrugated carbon-based networks with high surface area and high conductivity, and commonly used methods require expensive equipment and high annealing temperatures, and the patterning process is complex and difficult to implement on a large scale.
The graphite oxide film is laser-scored in a computer-controlled optical disk drive. By adjusting the laser power density and grayscale level, an interconnected corrugated carbon-based network is directly formed on the carbon-based oxide film to achieve electrical conductivity and Patterning control.
Achieve inexpensive, single-step production of interconnected corrugated carbon-based networks with high surface area and high conductivity, and can be manufactured simultaneously on various substrates, simplifying the development of lightweight electronic devices and providing electrical conductivity and electricity Height adjustable control of chemical properties.
Smart Images

Figure CN112661139B_ABST
Abstract
Description
[0001] This application is a divisional application of the following application: Application date: December 21, 2012; Application number: 201280070343.4 (PCT / US2012 / 071407); Invention name: "Interconnected corrugated carbon-based network".
[0002] This invention was made with government support under Grant No. HR0011-10-3-0002 awarded by the Defense Advanced Research Projects Agency of the U.S. Department of Defense. The government has certain rights in this invention. This research was supported in part by the Egyptian Ministry of Higher Education through the Graduate Research Fellowship-Assignment Program.
[0003] Related Applications
[0004] This application claims the benefit of U.S. Provisional Patent Application No. 61 / 578,431, filed December 21, 2011, the disclosure of which is incorporated herein by reference in its entirety.
[0005] FIELD OF THE DISCLOSURE
[0006] The present invention provides interconnected corrugated carbon-based networks and inexpensive processes for making, patterning, and tuning the electrical, physical, and electrochemical properties of the interconnected corrugated carbon-based networks.
[0007] background
[0008] In order to achieve the production of high-quality large quantities of carbon-based devices such as organic sensors, a variety of syntheses are now incorporated with graphite oxide (GO) as a precursor for the generation of large-scale carbon-based materials. A cheap method for producing a large amount of GO from the oxidation of graphite powder is now available. In addition, the water dispersibility of GO combined with the cheap production method makes GO an ideal raw material for the production of carbon-based devices. Specifically, GO has water-dispersible properties. Unfortunately, the same oxygen species that give GO its water-dispersible properties also produce defects in its electronic structure, and therefore GO is an electrically insulating material. Therefore, the formation of device-level carbon-based films with superior electronic properties requires the removal of these oxygen species, the reconstruction of the conjugated carbon network, and a method for controllably patterning carbon-based device features.
[0009] Methods for reducing graphite oxide include chemical reduction by hydrazine, hydrazine derivatives or other reducing agents, high temperature annealing under chemical reducing gas and / or inert atmosphere, solvent thermal reduction, a combination of chemical and thermal reduction methods, flash reduction, and recently laser reduction of GO. Although several of these methods have demonstrated relatively high-quality graphite redox, many methods are limited by expensive equipment, high annealing temperatures, and nitrogen impurities in the final product. Therefore, among these difficulties, the combination of properties including high surface area and high conductivity of the expanded interconnected carbon network remains elusive. In addition, large-scale film patterning by all-inclusive steps for GO reduction and patterning has proven to be difficult and generally depends on a photomask to provide the most basic pattern. Therefore, there is a need for an inexpensive process for making and patterning interconnected corrugated carbon-based networks with high surface areas with highly adjustable conductivity and electrochemical properties.
[0010] Overview
[0011] The present invention provides a method for producing an interconnected corrugated carbon-based network. The produced interconnected corrugated carbon-based network has a property combination of high surface area and high electrical conductivity of an expanded network including interconnected carbon layers.
[0012] In one embodiment, the method produces a patterned interconnected corrugated carbon-based network. In the specific embodiment, the initial step receives a substrate having a carbon-based oxide film. Once the substrate is received, the next step involves generating a light beam having a power density sufficient to reduce a portion of the carbon-based oxide film to an interconnected corrugated carbon-based network. Another step involves directing the light beam in a predetermined pattern on the carbon-based oxide film by a computer control system, while adjusting the power density of the light beam by a computer control system according to predetermined power density data associated with the predetermined pattern.
[0013] In one embodiment, the substrate is a disc-shaped, digital versatile disc (DVD)-sized plastic sheet that is removably adhered to a DVD-sized plate containing a DVD centering hole. The DVD-sized plate carrying the disc-shaped substrate can be loaded into a direct-to-disc labeling-enabled optical drive. A software program executed by a computer control system reads out data defining a predetermined pattern. The computer control system directs a laser beam generated by the optical drive onto the disc-shaped substrate, thereby partially reducing the carbon-based oxide film to an interconnected corrugated carbon-based network that is conductive, and the interconnected corrugated carbon-based network matches the shape, size, and conductivity level described by the data of the predetermined pattern.
[0014] Those skilled in the art will understand the scope of the disclosure and realize additional aspects thereof after reading the following detailed description in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate certain aspects of the disclosure and together with the description serve to explain the principles of the disclosure.
[0016] FIG. 1 depicts the label side of a prior art direct disc labeling type CD / DVD disc.
[0017] FIG. 2 is a schematic diagram of a prior art direct disc marking type optical disc drive.
[0018] Figure 3 is a flow chart of an exemplary process for providing a graphite oxide (GO) film on a substrate.
[0019] Figure 4 is a flow chart for laser scribing an interconnected corrugated carbon-based network and subsequently fabricating an electrical component from the interconnected corrugated carbon-based network.
[0020] Figure 5 is a line drawing of a sample of an interconnected corrugated carbon-based network of the present embodiment.
[0021] Fig. 6A It is an artwork image of a male head covered with circuits.
[0022] Figure 6B is Fig. 6A An artwork image of a photograph of a GO membrane after being patterned directly on the GO membrane using the laser scribing technique of the present invention.
[0023] Figure 7 By using various gray levels Fig. 6A Artwork is laser scribed to produce Figure 6B The patterned GO film makes Figure 6B Graph comparing the conductivity of GO membranes after reduction.
[0024] Fig. 8A is a scanning electron microscope (SEM) image showing the effect of infrared laser on a GO film after laser treatment on the right side of the image, in contrast to the aligned interconnected corrugated carbon-based network on the left side of the image.
[0025] Figure 8B is a SEM image showing that the thickness of the interconnected corrugated carbon-based network is approximately 10 times that of the untreated GO film.
[0026] Figure 8C is a SEM image showing a cross-sectional view of a single laser-converted interconnected corrugated carbon-based network.
[0027] Fig.8D It is shown Figure 8C Larger magnification SEM image of a selected area within the interconnected corrugated carbon-based network.
[0028] Fig. 9 The powder X-ray diffraction (XRD) pattern of the interconnected corrugated carbon-based network was compared with the diffraction patterns of graphite and graphite oxide.
[0029] Fig.10 is the log of the peak current 10 The log of the applied voltammetric scan rate 10 Graph of the curve.
[0030] FIG. 11A to FIG. 11E It is a graph related to Raman spectroscopy analysis.
[0031] Fig. 12A is a diagram showing the structure of a set of interdigitated electrodes made of an interconnected corrugated carbon-based network, measuring 6 mm x 6 mm and spaced approximately 500 μm apart, which are patterned directly onto a thin film of GO.
[0032] Fig. 12B is a diagram showing the structure of an interdigitated electrode combination transferred to another type of substrate.
[0033] Fig.13 Shown is the sensor response of a patterned flexible assembly of interdigitated electrodes made of an interconnected corrugated carbon-based network exposed to 20 ppm of nitrous oxide (NO2) in dry air.
[0034] FIG. 14A to FIG. 14D Shown are SEM images illustrating the growth of platinum (Pt) nanoparticles onto a scaffold made of an interconnected corrugated carbon-based network for electrodeposition times corresponding to 0 seconds, 15 seconds, 60 seconds, and 120 seconds.
[0035] Fig.15 The CV profiles of GO, graphite, and a carbon-based network made of interconnected corrugated carbon were compared in an equimolar mixture of 5 mM K3[Fe(CN)6] / K4[Fe(CN)6] dissolved in 1.0 M KCl solution at a scan rate of 50 mV / s.
[0036] Details
[0037] The embodiments set forth below represent necessary information to enable those skilled in the art to practice the present disclosure and illustrate the best mode for implementing the present disclosure. After reading the following description in view of the accompanying drawings, those skilled in the art will understand the concepts of the present disclosure and recognize the application of these concepts not specifically proposed herein. It should be understood that these concepts and applications are within the scope of the present disclosure and the appended claims.
[0038] The present invention provides an inexpensive process for making and patterning interconnected corrugated carbon-based networks, which have strict requirements for high surface areas with highly adjustable electrical conductivity and electrochemical properties. The embodiments described herein not only meet these strict requirements, but also provide direct control of the conductivity and patterning of the interconnected corrugated carbon-based networks, while forming flexible electronic devices in a single step process. In addition, the production of these interconnected corrugated carbon-based networks does not require reducing agents or expensive equipment. Therefore, the simple and direct manufacture of interconnected corrugated carbon-based networks on flexible substrates simplifies the development of lightweight electronic devices. Interconnected corrugated carbon-based networks can be synchronized on various substrates such as plastics, metals and glass. In this article, an all-organic NO2 gas sensor, a fast redox-active electrode and a support for the direct growth of platinum (Pt) nanoparticles are demonstrated.
[0039] In at least one embodiment, the interconnected corrugated carbon-based network is a conductive film produced using a common and inexpensive infrared laser that is coupled inside a compact disk / digital versatile disk (CD / DVD) optical drive unit that provides direct disc marking writing capabilities. LightScribe (a registered trademark of Hewlett-Packard Company) and LabelFlash (a registered trademark of Yamaha Corporation) are exemplary direct disc marking technologies that pattern text and graphics onto the surface of a CD / DVD disc. LightScribe DVD drives are commercially available for around $20 and the LightScribing process is controlled using a standard desktop computer.
[0040] 1 depicts the label side of a standard direct disc labeling type CD / DVD disc 10, which includes a labeling area 12 and a clamping area 14 surrounding a centering hole 16. A dye film 18 covers the labeling area 12 and is sensitive to laser energy typically directed onto the labeling area 12 to produce a permanent visible image that may include graphics 20 and text 22. Position tracking marks 24 may be used by an optical disc drive (not shown) to accurately locate the absolute angular position of the CD / DVD disc 10 within the optical disc drive so that the graphics 20 and / or text 22 may be rewritten to increase contrast. In addition, the position tracking marks 24 may be used by the optical disc drive to allow other graphics and / or text to be rewritten without undesirably overwriting the graphics 20 and / or text 22.
[0041] FIG. 2 is a schematic diagram of a prior art direct disc marking type optical disc drive system 26. In this exemplary case, a cross section of a CD / DVD disc 10 is depicted and loaded onto a spindle assembly 28 driven by a CD / DVD spindle motor 30. The marking area 12 is shown facing the laser assembly 32, which includes a label writer laser (LWL) 34, a lens 36, and a focus actuator 38. The LWL 34 is typically a laser diode. Exemplary specifications for the LWL 34 include a maximum pulsed optical power of 350 mW at 780 nm emission and a maximum pulsed output power of 300 mW at 660 nm emission. The laser beam 40 emitted by the LWL 34 is focused by the lens 36, which is alternately translated toward and away from the LWL 34 by the focus actuator 38 to maintain the focus of the laser beam 40 onto the marking area 12 of the CD / DVD disc 10. The laser beam 40 is typically focused to a diameter ranging from about 0.7 μm to about 1 μm.
[0042] The laser assembly 32 is responsive to a control system 42 which provides control signals 44 via an optical drive interface (ODI) 46. The control system 42 further includes a central processing unit (CPU) 48 and a memory 50. Label image data (LID) having information required to realize a permanent image to be written to the label area 12 of the CD / DVD disc 10 is processed by the CPU 48 which in turn provides a LID stream signal 52 which turns the LWL 34 on or off in order to heat the dye film 18 to realize the image defined by the LID.
[0043] The CPU 48 also processes the LID through the ODI 46 to provide a position control signal 54 to a radial actuator 56 which causes the laser assembly 32 to translate relative to the label area 12 in response to the position information contained in the LID. In some versions of embodiments, the optical disc drive system 26 monitors the focus of the laser beam 40 via an optical receiver (not shown) so that the ODI 46 can generate a focus control signal 58 for the focus actuator 38. The ODI 46 also provides a motor control signal 60 for the CD / DVD spindle motor 30 which maintains the proper rotational speed of the CD / DVD disc 10 while the label writing process is in progress.
[0044] In some versions of the optical drive system 26, the LWL 34 is dedicated to mark writing directly to the label area 12 of the CD / DVD disc 10 and a separate laser diode (not shown) is used to write data to the data surface 62 of the CD / DVD disc 10 and / or read data from the data surface. In other versions of the optical drive system 26, the LWL 34 is used for mark writing and data reading and / or writing. When the LWL 34 is used for data reading and / or writing, the CD / DVD disc 10 is turned over to expose the data surface 62 of the CD / DVD disc 10 to the laser beam 40. In the version in which the LWL 34 is also used as a data reading / writing laser, the laser assembly 32 includes an optical pickup component (not shown), such as a beam diverging mirror and at least one optical receiver. During the data reading operation, the output power of the LWL 34 is typically around 3mW.
[0045] In order to achieve an inexpensive process for making and patterning a high surface area interconnected corrugated carbon-based network with highly tunable electrical conductivity and electrochemical properties using an optical drive system 26, the fuel membrane 18 (Figure 1) is replaced with a carbon-based membrane. In one embodiment, graphite oxide (GO) is synthesized from high purity graphite powder using a modified Hummer method. A dispersion of GO in water (3.7 mg / mL) is then used to form GO films on various substrates. Exemplary substrates include, but are not limited to, polyethylene terephthalate (PET), nitrocellulose membrane (pore size of 0.4 μm), aluminum foil, aluminum carbide, copper foil, and conventional copy paper.
[0046] Reference Figure 3, process 100 starts with providing graphite powder 64. Graphite powder 64 undergoes oxidation reaction using a modified Hummer method to become GO 66 (step 102). However, it should be understood that other oxidation methods for producing GO are also available and such methods are within the scope of the present invention. The stripping process produces stripped GO 68 (step 104). The stripping process can be completed by ultrasonic action. It should be understood that the stripped GO 68 is produced by partial stripping to a single GO layer rather than complete stripping. Partial stripping is used to form a high accessible surface area for achieving rapid redox reactions, which achieves a rapid sensor response. In addition, the partial stripping of GO 68 provides a high surface area for growing metal nanoparticles, which can then be used for catalysis. The substrate 70 carries a GO film 72, which is produced by a deposition process that deposits the stripped GO 68 onto the substrate 70 (step 106). In at least some embodiments, the GO film 72 is made by dripping or vacuum filtering a GO dispersion onto a substrate 70, and the substrate is the size of a CD / DVD disc. The GO film 72 is typically allowed to dry for 24 hours under ambient conditions. However, controlled exposure of the GO film 72 to relatively low humidity and relatively high temperature conditions will allow the GO film 72 to dry relatively quickly. The term GO herein refers to graphite oxide.
[0047] Reference Figure 4 , and then a single one of the GO films 72 is attached to a substrate carrier 74 having a size similar to that of the CD / DVD disc 10 ( FIG. 1 ) (step 108). The substrate carrier 74 carrying the substrate 70 with the GO film 72 is loaded into the optical disc drive system 26 ( FIG. 2 ) so that the GO film 72 faces the LWL 34 for laser processing (step 110). In this way, the present embodiment uses the GO film 72 to replace the dye film 18 ( FIG. 1 ). It should be understood that the substrate carrier 74 can be a hard or semi-hard optical disc on which the GO film 72 can be directly manufactured. In the case, the substrate carrier 74 replaces the function of the substrate 70.
[0048] The image 76 for realizing the electrical component 78 is patterned in a concentric circular manner, moving outward from the center of the substrate carrier 74 (step 112). The laser irradiation process results in the removal of oxygen species and sp 2This results in a change in the conductivity of the GO film 72, which has a typical resistance (>20MΩ / sq), to become a plurality of relatively highly conductive expanded and interconnected carbon layers, which constitute an interconnected corrugated carbon-based network 80. The laser treatment of the GO film 72 results in a significant and controllable change in the conductivity of the interconnected corrugated carbon-based network 80. The interconnected corrugated carbon-based network 80 has a combination of properties of high surface area and high conductivity of an expanded interconnected network of carbon layers. In one embodiment, the plurality of expanded and interconnected carbon layers has a surface area greater than 1400 m 2 In another embodiment, the plurality of expanded and interconnected carbon layers has a surface area greater than 1500 m 2 In yet another embodiment, the surface area is about 1520 m 2 / g or so. In one embodiment, the plurality of expanded and interconnected carbon layers produce a conductivity of greater than about 1500 S / m. In another embodiment, the plurality of expanded and interconnected carbon layers produce a conductivity of greater than about 1600 S / m. In yet another embodiment, the plurality of expanded and interconnected carbon layers produce a conductivity of greater than about 1650 S / m or so. In another embodiment, the plurality of expanded and interconnected carbon layers produce a conductivity of greater than about 1700 S / m or so. In yet another embodiment, the plurality of expanded and interconnected carbon layers produce a conductivity of greater than about 1738 S / m or so. Furthermore, in one embodiment, the plurality of expanded and interconnected carbon layers produce a conductivity of greater than about 1700 S / m and greater than about 1500 S / m. 2 In another embodiment, the plurality of expanded and interconnected carbon layers produces a conductivity of about 1650 S / m and a surface area of about 1520 m 2 / g of surface area.
[0049] The electrical component 78 including the electrode 82 for manufacturing the device 84 is laser irradiated 6 times before reaching a relatively high conductivity of about 1738S / m. The laser irradiation process takes about 20 minutes per cycle. Afterwards, the substrate 70 carrying the interconnected corrugated carbon-based network 80 and any remaining GO film 72 is removed from the substrate carrier 74 (step 114). Next, the interconnected corrugated carbon-based network 80 is manufactured into the electrical component 78 constituting the device 84 (step 116). In this exemplary case, the portion of the interconnected corrugated carbon-based network 80 on the substrate 70 is cut into rectangular segments to form an electrical component 78, which includes an electrode 82 formed by the interconnected corrugated carbon-based network 80.
[0050] The interconnected corrugated carbon-based network 80 has a very low oxygen content of only 3.5%. In other embodiments, the oxygen content of the expanded and interconnected carbon layers ranges from about 1% to about 5%. Figure 5is a line drawing of a sample of an interconnected corrugated carbon-based network 80, the interconnected corrugated carbon-based network being composed of a plurality of expanded and interconnected carbon layers, the carbon layers including corrugated carbon layers such as a single corrugated carbon thin layer 86. In one embodiment, each of the expanded and interconnected carbon layers includes at least one corrugated carbon thin layer that is one atom thick. In another embodiment, each of the expanded and interconnected carbon layers includes a plurality of corrugated carbon thin layers that are each one atom thick. It has been found that the thickness of the interconnected corrugated carbon-based network 80 (as measured by cross-sectional scanning electron microscopy (SEM) and photometry) is about 7.6 μm. In one embodiment, the thickness of the plurality of expanded and interconnected carbon layers that make up the interconnected corrugated carbon-based network 80 ranges from about 7 μm to about 8 μm.
[0051] As an illustration of the variety possible in image patterning, Fig. 6A and Figure 6B The complex image formed by direct laser reduction of GO is shown in FIG. Fig. 6A It is an artwork image of a male head covered with circuits. Figure 6B is Fig. 6A A photograph of a GO film after being patterned directly on the GO film using the laser scribing technique of the present invention. In essence, any portion of the GP film that comes into direct contact with the 780nm infrared laser is effectively reduced to an interconnected corrugated carbon-based network, where the amount of reduction is controlled by the laser intensity; a factor determined by the power density of the laser beam impinging on the GO film. Figure 6B The resulting image is Fig. 6A However, in this case, Figure 6B The images are composed of various reductions of the GO film. As expected, the darkest black areas indicate exposure to the strongest laser intensity, while the lightest gray areas are only partially reduced. Since the different gray levels are directly related to the laser intensity, it is possible to tune the electrical properties of the generated interconnected corrugated carbon-based network over a range of five to seven orders of magnitude in sheet resistance (Ω / sq) simply by changing the gray levels used in the patterning process. Figure 7 As shown in , there is a clear relationship between sheet resistance, grayscale level and the number of times the GO film is irradiated. It is possible to control the conductivity of a completely insulating GO film (typical sheet resistance value > 20 MΩ / sq) to a conductive interconnected corrugated carbon-based network (indicating a sheet resistance of about 80 Ω / sq), which varies to a conductivity of about 1650 S / m. Figure 7The distinction between similar gray levels shown in the graph of is sensitive enough that only small changes in gray level can lead to significant changes in sheet resistance. In addition, the number of times the GO film is laser treated results in significant and controllable changes in sheet resistance. Each additional laser treatment reduces the sheet resistance (e.g. Figure 7 ), where the film was laser irradiated once (black squares), twice (circles), and three times (triangles) in terms of grayscale. Thus, the sheet resistance of the film can be adjusted by controlling the grayscale used and the number of times the film is reduced by the laser, a property that has been difficult to control by other methods until now.
[0052] Scanning electron microscopy (SEM) techniques can be used to understand the effects of low-energy infrared laser on the structural properties of GO membranes by comparing the morphological differences between the interconnected corrugated carbon-based networks and untreated graphite oxide GO membranes. Fig. 8A is a SEM image showing the effect of infrared laser on a GO film after laser treatment on the right side of the image, in contrast to the aligned interconnected corrugated carbon-based network on the left side of the image that appears after reduction using an infrared laser. The image not only gives a clear definition between the interconnected corrugated carbon-based network and the untreated GO area, but also demonstrates the level of precision possible when using this method as a way to pattern and reduce GO. The areas of the interconnected corrugated carbon-based network (which are created due to laser treatment) can be further analyzed by cross-sectional SEM.
[0053] Figure 8B is a SEM image showing a cross-sectional view of a free-standing film of laser treated and untreated GO membranes, the image showing a significant difference between the GO membrane thickness. Figure 8B As shown by the white bracket in the figure, the thickness of the interconnected corrugated carbon-based network increases by about 10 times compared to the thickness of the untreated GO film. In addition, the thickness of the multiple colliding and interconnected carbon layers ranges from about 7 μm to about 8 μm. In one embodiment, the average thickness of the multiple expanded and interconnected carbon layers is about 7.6 μm. The increased thickness originates from the rapid exhaust of the gases generated and released during the laser treatment (similar to thermal shock), which effectively causes the reduced GO to expand and peel off as these gases quickly pass through the GO film. Figure 8C is a SEM image showing a cross-sectional view of a single interconnected corrugated carbon-based network showing the expanded structure that is characteristic of the interconnected corrugated carbon-based network of the present invention.
[0054] Fig.8D It is shown Figure 8C Larger magnification SEM image of a selected area within the corrugated carbon-based network. Fig.8DThe SEM images allow the thickness of the multiple expanded and interconnected carbon layers to be calculated to be between 5-10 nm. However, the number of carbon layers in the multiple expanded and interconnected carbon layers that constitute the interconnected corrugated carbon-based network is greater than 100. In another embodiment, the number of carbon layers in the multiple expanded and interconnected carbon layers is greater than 1000. In yet another embodiment, the number of carbon layers in the multiple expanded and interconnected carbon layers is greater than 10,000. In another embodiment, the number of carbon layers in the multiple expanded and interconnected carbon layers is greater than 100,000. SEM analysis shows that although the infrared laser emission is only slightly absorbed by GO, sufficient power and focus (i.e., power density) can result in the generation of sufficient thermal energy to effectively reduce, deoxygenate, expand, and exfoliate the GO film. In addition, the surface area of the interconnected corrugated carbon-based network is greater than about 1500 m 2 / g.
[0055] Since each of the carbon layers has 2630m 2 / g theoretical surface area, so greater than 1500m 2 / g surface indicates that almost all the surface of the carbon layer is accessible. The interconnected corrugated carbon-based network has a conductivity greater than 17S / cm. The interconnected corrugated carbon-based network is formed when light of a certain wavelength hits the surface of GO, and is subsequently absorbed and converted into heat almost immediately, which releases carbon dioxide (CO2). Exemplary light sources include but are not limited to 780nm lasers, green lasers, and flash lamps. The light beam emission of the light source may range from near-red wavelengths to ultraviolet wavelengths. The typical carbon content of the interconnected corrugated carbon-based network is greater than 97%, with less than 3% oxygen remaining. Some samples of the interconnected corrugated carbon-based network are greater than 99% carbon, even when the laser reduction process is carried out in air.
[0056] Fig. 9 The powder X-ray diffraction (XRD) pattern of the corrugated carbon-based network is compared with the diffraction patterns of graphite and graphite oxide. A typical XRD pattern of graphite (in Fig. 9 As shown in FIG. 1 , trace A) shows a characteristic peak at 2θ = 27.8°, d - spacing is 3.20 Å. On the other hand, the XRD pattern of GO ( Fig. 9 , trace B) shows a single peak at 2θ = 10.76°, which corresponds to an interlayer distance of 8.22 Å. d - Spacing. GO's increase d - spacing is due to the oxygen-containing functional groups in the graphite oxide thin layers, which tend to trap water molecules between the bottom surfaces, causing the thin layers to expand and separate. XRD pattern of the corrugated carbon-based network ( Fig. 9 , trace C) shows the presence of GO (10.76° 2θ) and a d- spacing related to the broad graphite peak of 25.97 ° 2θ. It is expected that GO is present in the corrugated carbon-based network because the laser has an expected penetration depth, which results in only the top portion of the film being reduced, while the bottom layer is not affected by the laser. The small presence of GO is more prominent in thicker films, but begins to weaken in thinner films. In addition, a partially blocked peak of 26.66 ° 2θ can also be observed, which shows an intensity similar to the broad 25.97 ° 2θ peak. Both peaks are considered to be graphite peaks, which are related to the two different lattice spacings between the bottom plates.
[0057] It has been previously shown that the immobilization of carbon nanotubes (CNTs) on glassy carbon electrodes will result in the production of thin CNT films, which directly affects the voltammetric performance of CNT modified electrodes. In the iron / ferrocyanide redox couple, the voltammetric current measured at the CNT modified electrode may have two types of supply. The thin layer effect is an important factor in the voltammetric current. The thin layer effect originates from the oxidation of ferrocyanide ions, which are trapped between nanotubes. Other factors are caused by the semi-infinite diffusion of ferrocyanide toward the planar electrode surface. Unfortunately, mechanical information is not easy to deconvolute and requires knowledge of film thickness.
[0058] In contrast, no thin layer effects were observed in connection with the interconnected corrugated carbon-based networks of the present invention. Fig.10 is the log of the peak current 10 The log of the applied voltammetric scan rate 10 In this case, no thin layer effect is observed as the plot has a consistent slope of 0.53 and is linear. The slope of 0.53 is relatively close to the theoretical value calculated using a semi-infinite diffusion model governed by the Randles-Sevcik equation, which is shown below:
[0059]
[0060] Raman spectroscopy was used to characterize and compare the structural changes induced by laser treatment of GO films. FIG. 11A to FIG. 11E This is a graph related to Raman spectroscopy analysis. Fig.11A It can be seen that characteristic D, G, 2D and S3 peaks are observed in GO as well as in the interconnected corrugated carbon-based network. The presence of the D band in both spectra indicates that the carbon sp 3 The centers still exist after reduction. Interestingly, the spectrum of the interconnected corrugated carbon-based network shows a peak at about 1350 cm -1 The results are consistent with the SEM analysis, in which the exfoliated folded graphite domains ( Figure 5 ) form a large number of edges. However, the D band also shows a significant overall peak narrowing, which indicates a reduction in defect types in the interconnected corrugated carbon-based network. The G band undergoes a narrowing and a decrease in peak intensity as well as a peak intensity from 1585 to 1579 cm -1 These results are consistent with the peak shift of sp 2 The reconstruction of carbon is consistent with the reduction of structural defects in the base plate. The overall change in the G band indicates a transition from an amorphous carbon state to a higher quality carbon state. In addition, a shift from about 2730 cm -1 From left to right to approximately 2688cm -1 The prominent and shifted 2D peaks at about 2700 cm-1 and 2700 cm-2 indicate considerable reduction of the GO film and largely point to the presence of several layers of interconnected graphitic structures. In one embodiment, after the interconnected corrugated carbon-based network is reduced by the carbon-based oxide, the 2D Raman peak of the interconnected corrugated carbon-based network shifts from about 2700 cm-1 to about 2700 cm-1. -1 The left and right change is about 2600cm -1 In addition, due to the disordered lattice, the combination of DG generates the S3 second-order peak (the S3 second-order peak is shown at about 2927cm -1 ) and (as expected) after infrared laser treatment, decreases with reduced disorder. In some embodiments, the plurality of expanded and interconnected carbon layers have a range of about 2920 cm -1 About 2930cm -1 Raman spectroscopy of the S3 second order peak range. Raman analysis demonstrates the effect of infrared laser treatment of GO as a way to efficiently and controllably produce interconnected corrugated carbon-based networks.
[0061] X-ray photoelectron spectroscopy (XPS) was used to correlate the effect of laser irradiation on oxygen functional groups and to monitor structural changes on GO films. Comparison of the carbon-oxygen (C / O) ratio between GO and the interconnected corrugated carbon-based network provides an effective measure of the degree of reduction achieved using a simple low-energy infrared laser. Fig. 11B A significant difference between the C / O ratio before and after laser treatment of the GO film is shown. Before laser reduction, a typical GO film has a C / O ratio of about 2.6:1, which corresponds to a carbon / oxygen content of about 72% and 38%. On the other hand, the interconnected corrugated carbon-based network has an enhanced carbon content of 96.5% and a reduced oxygen content of 3.5%, giving an overall C / O ratio of 27.8:1. Since the laser reduction process occurs under ambient conditions, it is speculated that some of the oxygen present in the interconnected corrugated carbon-based network film is a result of the film having static interactions with the oxygen found in the environment.
[0062] Fig. 11CIt was shown that, in addition to a small π to π* peak at 290.4 eV, the C1s XPS spectrum of GO also shows two broad peaks that can be decomposed into three different carbon components corresponding to the functional groups commonly found on the GO surface. These functional groups include carboxyl, sp in the form of epoxy and hydroxyl groups. 3 carbon, and sp 2 For carbon, the above are associated with the following binding energies: approximately 288.1, 286.8, and 284.6 eV, respectively.
[0063] Fig.11D The results are expected because the large degree of oxidation in GO leads to the generation of various oxygen components in the C1s XPS spectrum. These results are in contrast to the interconnected corrugated carbon-based network, which shows a significant reduction in oxygen-containing functional groups and CC sp 2 There is an overall increase in the carbon peak. This indicates an effective deoxygenation process and the reconstruction of C=C bonds in the interconnected corrugated carbon-based network. These results are consistent with the Raman analysis. Therefore, an infrared laser such as LWL 34 (Figure 2) is powerful enough to remove most of the oxygen functional groups, as clearly seen in the XPS spectrum of the interconnected corrugated carbon-based network, which shows only a small disorder peak and a peak at 287.6 eV. The latter case corresponds to the sp 3 The presence of type carbon indicates that a small amount of carbonyl groups remain in the final product. In addition, the presence of the π to π* companion peak at about 290.7 eV indicates that the delocalized π conjugation is significantly stronger in the interconnected corrugated carbon-based network, as this peak is extremely small in the GO XPS spectrum. The appearance of the delocalized π peak clearly indicates that the conjugation in the GO film is restored during the laser reduction process and increases the contribution to the reconstruction of sp 2 The increased intensity of oxygen-containing functional groups, the presence of major C=C bond peaks, and delocalized π-conjugation all indicate that low-energy infrared lasers are an effective tool for generating interconnected corrugated carbon-based networks.
[0064] Fig.11E Depicted is the UV visible light absorbance spectrum of GO shown in black. The inset shows a magnification of the boxed area showing the absorbance of GO in the 650 to 850 nm region with respect to a 780 nm infrared laser.
[0065] The future development of multifunctional flexible electronic devices such as roll-up displays, photovoltaic cells, and even wearable devices poses new challenges in the design and manufacture of lightweight, flexible energy storage devices.
[0066] Embodiments of the present invention also include other types of electrical and electronic devices. For example, Fig. 12AA set of interdigitated electrodes measuring 6mm x 6mm and spaced approximately 500μm apart are shown, which are patterned directly onto a thin film of GO. Prior to patterning, the GO film was deposited on a thin flexible substrate (polyethylene terephthalate (PET)) in order to create a mechanically flexible set of electrodes. The top arrow points to the area of the interconnected corrugated carbon-based network that constitutes the black interdigitated electrodes, while the bottom arrow points to the unreduced gold GO film. Since the electrodes are patterned directly onto the GO film on the flexible substrate, the need for post-processing such as transferring the film to a new substrate is unnecessary. Although if desired, a peel-and-stick method can be used to selectively lift the black interdigitated electrodes made of the interconnected corrugated carbon-based network and (for example) polydimethylsiloxane (PDMS) and transfer them to other types of substrates ( Fig. 12B ). The simplicity of the present method allows substantial control over the pattern size, substrate selectivity, and electrical properties of the interconnected corrugated carbon-based networks by controlling the laser intensity and, thereby, the amount of reduction in each film.
[0067] These interdigitated electrodes can then be used as an all-organic flexible gas sensor for detecting NO2. Fig.13 The sensor response of a patterned flexible combination of interdigitated electrodes made of interconnected corrugated carbon-based networks exposed to 20ppm of NO2 in dry air is shown. This sensor is made by patterning the interconnected corrugated carbon-based network to make active electrodes and reducing the area between the electrodes by a small amount to have a consistent sheet resistance of about 7775ohm / sq. In this way, it is possible to omit the use of metal electrodes and pattern electrodes and sensing materials simultaneously on a flexible substrate. The graph relates to NO2 gas exposed to R / R0, where R0 is the sheet resistance in the initial state and R is the resistance of the interconnected corrugated carbon-based network film after exposure to the gas. The film is exposed to NO2 gas for 10 minutes and then immediately purged with air for another 10 minutes. This process is then repeated nine more times in a total of 200 minutes. Even at a slightly lower sensitivity than more complex and optimized sensors, the unoptimized sensor consisting of the interconnected corrugated carbon-based network still shows good reversible sensing for NO2 and its ease of manufacture makes this quite advantageous for these systems. Sensors composed of interconnected corrugated carbon-based networks for NO2 hold promise for improving the fabrication of all-organic flexible sensor devices at low cost by using inexpensive raw materials that are directly patterned with inexpensive lasers.
[0068] The high conductivity and increased surface area due to multiple expanded and interconnected carbon layers make the interconnected corrugated carbon-based network a viable candidate for heterogeneous catalyst supports of metal nanoparticles. Specifically, the direct growth of Pt nanoparticles on the interconnected corrugated carbon-based network can help improve methanol-based fuel cells, which have shown enhanced device performance from large surface area and conductive carbon-based supports. The present invention shows that the interconnected corrugated carbon-based network is a viable support for the controllable growth of Pt nanoparticles. By using 0.5M H2SO4 at -0.25V in different time periods to electrochemically reduce 1mM K2PtCl4, it is possible to actively control the Pt particle size electrodeposited on the interconnected corrugated carbon-based network film. FIG. 14A to FIG. 14D Scanning electron microscopy images illustrating the growth of Pt nanoparticles for electrodeposition times corresponding to 0 seconds, 15 seconds, 60 seconds, and 120 seconds are shown. As expected, at 0 seconds of electrodeposition ( Fig.14A ) when no Pt particles were present, but in just 15 seconds ( Fig. 14B ) Small Pt nanoparticles are clearly visible, with the size of the nanoparticles ranging from 10-50 nm ( Fig. 14B , inset). After 60 s of electrodeposition, larger Pt nanoparticles grew with an average particle size of 100 to 150 nm ( Fig. 14C Finally, after 120 seconds, particles ranging from 200 to 300 nm were found to be evenly distributed on the surface of the interconnected corrugated carbon-based network ( Fig.14D ). The active growth of Pt nanoparticles at controlled diameters on interconnected corrugated carbon-based networks can make potentially useful hybrid materials for applications that require metal nanoparticles, such as methanol fuel cells and gas-phase catalysts. In addition, if palladium (Pd) is deposited, sensors made from interconnected corrugated carbon-based networks can be used as sensors to detect hydrogen or for catalysis such as Suzuki coupling or Heck coupling.
[0069] For various electrochemical applications, carbon electrodes have attracted great interest due to their wide potential window and good electrocatalytic activity for many redox reactions. Considering the high surface area and flexibility of the carbon electrodes and the fact that the carbon electrodes are all-carbon electrodes, the interconnected corrugated carbon-based networks can revolutionize electrochemical systems by making miniaturized and fully flexible devices. Herein, understanding the electrochemical properties of the interconnected corrugated carbon-based networks is highly beneficial for determining their potential for electrochemical applications. Recently, the electrocatalytic properties of monolayer graphite have been shown to originate largely from the efficient electron transfer at its edges rather than at the base. In fact, it has been reported that monolayer graphite exhibits electrocatalytic activity similar to that of edge-planed highly ordered pyrolytic graphite in certain systems. In addition to having a highly expanded network, the interconnected corrugated carbon-based network also shows a large number of edge planing (return to reference Figure 5 ), making the network an ideal system to study the role of edge planing in the electrochemistry of nanomaterials based on monolayer graphene.
[0070] In this regard, the electrochemical properties related to electron transfer of flexible electrodes made of interconnected corrugated carbon-based networks are characterized using [Fe(CN)6] 3- / 4- As a redox probe. For example, Fig.15 Comparison of CV profiles of GO, graphite, and an electrode made of interconnected corrugated carbon-based networks in an equimolar mixture of 5 mM K3[Fe(CN)6] / K4[Fe(CN)6] dissolved in 1.0 M KCl solution at a scan rate of 50 mV / s. Unlike GO and graphite, the electrode made of the interconnected corrugated carbon-based network approaches the performance of a fully reversible system with a low ΔE ranging from 59.5 mV at a scan rate of 10 mV / s to 97.6 mV at a scan rate of 400 mV / s. p (Peak potential separation). Low ΔE p The value is close to the calculated theoretical value of 59 mV. Considering ΔE p and the electron transfer rate constant (k 0 obs ) is directly related to ΔE p The low experimental value of indicates a very fast electron transfer rate. The calculated k 0 obs The value for graphite ranges from 1.266x 10 -4 cm s -1 changes and increases to 1.333 x 10 -2 cm s -1 .
[0071] The redox system used to evaluate the electron transfer kinetics was 5 mM K3[Fe(CN)6] / K4[Fe(CN)6] (1:1 molar ratio) dissolved in 1.0 M KCl solution. To ensure a stable electrochemical response, the electrode was first cycled at least 5 times before collecting experimental data. The inhomogeneous electron transfer rate constant (k) was determined using the method developed by Nicholson. 0 obs ), which allows peak separation (ΔE p ) is related to the dimensionless kinetic parameter ψ and is therefore related to k according to the following equation 0 obs Related:
[0072]
[0073] Where DO and D R are the diffusion coefficients of the redox species, respectively. Other variables include v - applied scan rate, n - number of electrons transferred in the reaction, F - Faraday constant, R - gas constant, T - absolute temperature, and α - transfer coefficient. The diffusion coefficients of the redox species are usually similar; hence the term (D R / D O ) α / 2 is about 1.726 x 10 -6 cm 2 s -1 The diffusion coefficient (D O ) for [[Fe(CN)6] in 1.0 M KCl 3- / 4- .
[0074] In addition to the relatively large increase in the electron transfer rate at the electrode made of the interconnected corrugated carbon-based network (about two orders of magnitude faster than the graphite electrode), there is also substantial electrochemical activity in the electrode made of the interconnected corrugated carbon-based network, as seen by an increase of about 268% in the voltammetric peak current. These substantial improvements can be attributed to the expanded architecture of the interconnected corrugated carbon-based network film, which provides a large open area for the efficient diffusion of electroactive species and allows better interfacial interactions with the interconnected corrugated carbon-based network surface. In addition, it can be speculated that the amount of edge-like surface per unit mass is therefore much larger than that of graphite, and therefore contributes to a higher electron transfer rate, as seen herein. Considering the large number of exposed edge sites in the interconnected corrugated carbon-based network, it is found that the interconnected corrugated carbon-based network not only has a higher k than graphite, but also has a higher k than graphite. 0 obs value, and exceeds the k value of carbon nanotube-based electrodes 0 obs and k of stacked monolayer graphene nanofibers 0 obs The value is not surprising.
[0075] Note that the electrode made of the interconnected corrugated carbon-based network is made on a flexible PET substrate covered with GO, which, when subjected to laser reduction, serves as an electrode and current collector, making this particular electrode not only lightweight and flexible, but also inexpensive. In addition, the low oxygen content (about 3.5%) in the interconnected corrugated carbon-based network (as shown by XPS analysis) is quite favorable for the electrochemical activity seen herein, as higher oxygen content at the edge planing sites has been shown to limit and slow electron transfer of the iron / ferrocyanide redox couple. Thus, embodiments of the present invention provide methods for making highly electroactive electrodes for potential applications in vapor sensing, biosensing, electrocatalysis, and energy storage.
[0076] The present invention relates to a convenient, solid-state and environmentally safe method for generating, patterning and electrically regulating graphite-based materials at low cost. It has been confirmed that interconnected corrugated carbon-based networks are successfully produced and selectively patterned by direct laser irradiation of GO films under ambient conditions. Circuits and complex designs are directly patterned on various flexible substrates without masks, templates, post-processing, transfer techniques or metal catalysts. In addition, by changing the laser intensity and laser irradiation treatment, the electrical properties of the interconnected corrugated carbon-based networks are accurately adjusted within five orders of magnitude, which is a feature that has been confirmed to be difficult to adjust by other methods. This new mode of generating interconnected corrugated carbon-based networks provides a new location for manufacturing all-organic devices such as gas sensors and other electronic devices. The relatively inexpensive method of generating interconnected corrugated carbon-based networks on thin flexible organic substrates makes it a relatively ideal heterogeneous scaffold for the selective growth of metal nanoparticles. In addition, the selective growth of metal nanoparticles has potential in the electrocatalysis of methanol fuel cells. Furthermore, films made of interconnected corrugated carbon-based networks show exceptional electrochemical activity in electronic charge transfer of iron / ferrocyanide redox couples over other carbon-based electrodes. The simultaneous reduction and patterning of GO by using inexpensive lasers is a new technology that offers significant versatility in fabricating electronic devices, all-organic devices, asymmetric membranes, microfluidic devices, integrated dielectric layers, batteries, gas sensors, and electronic circuits.
[0077] Compared to other photolithography techniques, this process uses a low-cost infrared laser in combination with the LightScribe technology in an unmodified, commercially available CD / DVD optical drive to pattern complex images on GO and has the added benefit of simultaneously producing a laser-converted corrugated carbon network. The LightScribe technology laser is typically operated at a wavelength of 780nm at a power output ranging from about 5mW to about 350mW. However, it should be understood that the process can be implemented at any wavelength at a given power output as long as the carbon-based oxide absorbs within the spectrum of the laser emission. The present method is a simple, single-step, low-cost, and mask-free solid-state method for generating interconnected corrugated carbon-based networks that can be performed without any post-processing of a variety of thin films. Unlike other reduction methods for generating graphite-based materials, the present method is a chemical-free and relatively simple and environmentally friendly process that is not limited by chemical reducing agents.
[0078] The techniques described herein are inexpensive, do not require bulky equipment, show direct control over film conductivity and image patterning, and can be used as a single step in the manufacture of flexible electronic devices, all without the need for complex alignment or the production of expensive masks. Moreover, due to the conductive properties of the materials used, it is possible to control the resulting conductivity simply at different laser intensities and powers, a property that has not yet been demonstrated by other methods. Working circuit boards, electrodes, capacitors and / or wires are precisely patterned by a computer program. The technology allows control of various parameters and therefore provides a location for simplifying device manufacturing and has the potential for scaling, which is different from other technologies that are controlled by cost or equipment. The present method can be used for any photothermally active material, including but not limited to GO, conductive polymers and other photothermally active chemicals such as carbon nanotubes.
[0079] As described above, a method for producing graphite-based materials has been proposed, which is not only convenient, cheap and versatile, but also a single-step environmentally safe process for reducing and patterning graphite films in a solid state. Simple, low-energy, inexpensive infrared lasers are used as powerful tools for the effective reduction, subsequent expansion, and detachment and fine patterning of GO. In addition to the ability to directly pattern and effectively produce large-area highly reduced laser-converted graphite films, the present method can also be applied to a variety of other thin substrates and has the potential to simplify the manufacturing process of devices made entirely of organic materials. Flexible all-organic gas sensors have been directly made by laser patterning of GO deposited on thin flexible PET. Interconnected corrugated carbon-based networks are also shown to be effective scaffolds for the successful growth and size control of Pt nanoparticles through simple electrochemical processes. Finally, flexible electrodes made of interconnected corrugated carbon-based networks are manufactured, and the interconnected corrugated carbon-based networks show textbook reversibility, with electrochemical activity increasing by about 238% compared to graphite-oriented electron transfer between iron / ferrocyanide redox couples. This proof-of-concept process has the potential to effectively advance applications that benefit from the high electrochemical activity demonstrated here, including batteries, sensors, and electrocatalysis.
[0080] Those skilled in the art will appreciate modifications and variations of the embodiments of the present disclosure. All such modifications and variations are considered to be within the scope of the concepts disclosed herein and the following claims.
Claims
1. A hybrid material comprising an interconnected corrugated carbon-based network and platinum nanoparticles electrodeposited on the interconnected corrugated carbon-based network, wherein the interconnected corrugated carbon-based network comprises a plurality of expanded and interconnected graphene layers, comprising a plurality of corrugated, stacked, expanded and interconnected reduced graphene oxide thin layers, wherein the interconnected corrugated carbon-based network is a graphene-based network, and wherein after the interconnected corrugated carbon-based network is patterned and reduced by a carbon-based oxide, the second-order disorder Raman peak of the interconnected corrugated carbon-based network increases from 2730 cm to 40 cm. -1 Change to 2688cm -1 And wherein each of the expanded and interconnected graphene layers has an oxygen content of 1% to 5%, wherein each of the expanded and interconnected graphene layers includes a plurality of corrugated carbon thin layers each being one atom thick.
2. The interconnected corrugated carbon-based network of claim 1, wherein each of the expanded and interconnected graphene layers has an oxygen content of 3.5% as measured by X-ray photoelectron spectroscopy.
3. The interconnected corrugated carbon-based network of claim 1, wherein the plurality of expanded and interconnected graphene layers yields a conductivity of 1650 S / m.
4. The interconnected corrugated carbon-based network of claim 1, wherein the plurality of expanded and interconnected graphene layers has a carbon to oxygen ratio of 27.8:1 as measured by X-ray photoelectron spectroscopy.
5. The interconnected corrugated carbon-based network of claim 1, wherein the plurality of expanded and interconnected graphene layers has a sheet resistance of 80 ohms / square.
6. The interconnected corrugated carbon-based network of claim 1, wherein the plurality of expanded and interconnected graphene layers have a carbon content of 2927 cm -1 Raman spectroscopy S3 second-order peak.
7. The interconnected corrugated carbon-based network of claim 1, wherein the interconnected corrugated carbon-based network is formed using an infrared laser.
8. The interconnected corrugated carbon-based network of claim 1, wherein the platinum nanoparticles have a size of 10 nm to 50 nm, 100 nm to 150 nm, or 200 nm to 300 nm.
9. The interconnected corrugated carbon-based network of claim 1, wherein the interconnected corrugated carbon-based network is patterned to form interdigitated electrodes.