Porous carbon-graphite composite material, preparation method thereof, silicon-carbon material and electrochemical device
By setting a porous carbon layer on the surface of graphite-based material, adjusting the relationship between oxygen element content and particle size, forming a conductive network and buffer structure, the problem of insufficient performance of graphite and silicon materials in electrochemical testing is solved, and the energy of the electrochemical device is improved Density and cycling performance.
Patent Information
- Application Number
- CN202411052373.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
AI Technical Summary
Existing graphite has insufficient rate performance and cyclic performance in electrochemical tests. Silicon materials have rapid capacity attenuation due to poor conductivity and volume expansion. Existing improvement methods such as porous carbon or graphite carriers limit lithium ion transmission or fail to effectively alleviate the expansion problem. .
By setting a porous carbon layer on the surface of the graphite-based material, the relationship between the oxygen content of the graphite-based material and the thickness of the porous carbon layer and the average particle size of the composite material is regulated, a good conductive network and buffer structure is formed, and the silicon deposition capacity is improved and expansion is suppressed. performance.
The energy density, rate performance and cycling performance of the electrochemical device are significantly improved, structural damage is reduced, and the transmission path of lithium ions and the stability of electrode materials are optimized.
Smart Images

Figure CN119008255A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of energy storage technology, and specifically relates to a porous carbon-graphite composite material and a preparation method thereof, a silicon-carbon material and an electrochemical device. Background Art
[0002] Although graphite has shown good rate performance and cycle performance in electrochemical tests, its theoretical capacity (372mAh / g) can no longer meet the current market requirements for battery capacity. In pursuit of higher energy density, silicon material is regarded as the most promising negative electrode material due to its extremely high theoretical gram capacity (3579mAh / g). However, silicon material has extremely poor conductivity (<0.01S / cm) and its volume expands by 400% during charge and discharge, which can easily cause rapid capacity decay during the cycle.
[0003] The existing improvement methods for the volume expansion of silicon materials during the cycle are as follows: 1) Using porous carbon as a carrier, depositing nano-silicon into it. However, the conductivity of porous carbon and nano-silicon limits the transmission speed of lithium ions, weakening the rate performance of the overall material. 2) Using porous graphite as a carrier, depositing silicon nanoparticles into the porous graphite, and using the reserved holes in the porous graphite to alleviate the volume expansion of silicon. However, the volume expansion of graphite itself during the lithium insertion process (10%) is not improved, which will also seriously affect the cycle performance of the overall material. Summary of the invention
[0004] In view of this, the present application provides a porous carbon-graphite composite material and a preparation method thereof, a silicon-carbon material and an electrochemical device. Through the composite of a graphite-based material and a porous carbon layer, the energy density can be improved while also improving the expansion suppression performance, rate performance and cycle performance of the electrochemical device.
[0005] In the first aspect, the present application provides a porous carbon-graphite composite material, including a graphite-based material and a porous carbon layer located on the surface of the graphite-based material; the mass content of oxygen in the graphite-based material is Y%, 0.05≤Y≤41; the average particle size of the porous carbon-graphite composite material is Lμm, the thickness of the porous carbon layer is Hμm, 4.3≤L / H≤29.3. The present application sets a porous carbon layer on the surface of the graphite-based material, and by controlling the oxygen content of the graphite-based material and regulating the relationship between the thickness of the porous carbon layer and the average particle size of the composite material, the silicon deposition capacity of the porous carbon-graphite composite material can be increased, thereby increasing the energy density of the electrochemical device, and the porous carbon and graphite form a good conductive network in the silicon-carbon material, and the composite material can provide structural support when the silicon material undergoes a volume change, reduce structural damage to the electrode material, and thus improve the expansion suppression performance, rate performance and cycle performance of the electrochemical device.
[0006] In some embodiments, the porous carbon-graphite composite material satisfies at least one of the following conditions:
[0007] (1) 1.5≤Y≤29.5; When the oxygen content in the graphite-based material is regulated to meet this condition, the interlayer spacing of the (002) crystal plane of the graphite-based material can be increased through the oxygen atoms in the structure, thereby increasing the deposition space of the silicon material and further improving the silicon deposition capacity. At the same time, after cooperating with the porous carbon layer, a more sufficient conductive network is formed on the surface of the silicon material, and the volume expansion of the silicon material is buffered together, thereby further improving the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0008] (2) 5.0≤L / H≤12.5; when the thickness of the porous carbon layer and the average particle size of the composite material are further adjusted to meet this range, the graphite-based material and the porous carbon layer can be better coordinated to form a conductive network and a buffer structure, thereby optimizing the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0009] (3) 1≤L≤40; regulating the average particle size of the porous carbon-graphite composite material within this range can optimize the conductive network structure and the silicon material buffer structure, and further improve the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0010] (4) 0.2 ≤ H ≤ 12. Controlling the thickness of the porous carbon layer within this range can provide better buffering for the expansion of the silicon material, while reducing the transmission path of lithium ions, so that the electrochemical device can achieve better rate performance, expansion suppression performance and cycle performance.
[0011] In some embodiments, in the spectrum of the graphite-based material analyzed by an X-ray diffraction device using CuKα1 rays, the diffraction angle 2θ of the (002) peak satisfies: 22.0°≤2θ≤23.0°. Regulating the diffraction angle 2θ of the (002) peak within this range is conducive to improving the silicon deposition capacity of the composite material, and can improve the conductivity and buffer the volume expansion of the silicon material after being combined with the porous carbon layer, further improving the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0012] In some embodiments, the average particle size of the graphite-based material is Ds μm, 0.2≤Ds≤20.
[0013] In some embodiments, in the spectrum of the porous carbon-graphite composite material analyzed by an X-ray diffraction device using CuKα1 rays, the diffraction angle 2θ of the (002) peak satisfies: 22.0°≤2θ≤23.0°. Regulating the diffraction angle 2θ of the (002) peak within this range is conducive to improving the silicon deposition capacity of the composite material, and can improve the conductivity and buffer the volume expansion of the silicon material after being matched with the porous carbon layer, further improving the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0014] In some embodiments, based on the mass of the porous carbon-graphite composite material, the mass content of the porous carbon layer is M1%, the mass content of the graphite-based material is M2%, and 0.2≤M2 / M1≤5.5. Controlling the mass content ratio of the graphite-based material and the porous carbon layer to meet the above range can promote the graphite-based material and the porous carbon layer to better cooperate to form a conductive network and a buffer structure, and optimize the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0015] In some embodiments, the porous carbon-graphite composite material is subjected to a pressure of 5000 kgf and a force-bearing area of 0.745 cm 2 The compacted density under the condition of Pd g / cm 3 , 0.68≤Pd≤2.00. Controlling the compaction density of the porous carbon-graphite composite material to meet the above range can further improve the rate performance, expansion suppression performance and cycle performance of the electrochemical device.
[0016] In some embodiments, the porous carbon-graphite composite material satisfies at least one of the following conditions:
[0017] (1) The pore volume of porous carbon-graphite composite material is Vt cm 3 / g, 0.2≤Vt≤0.8; regulating the pore volume of the porous carbon-graphite composite material to meet the above range can provide a suitable silane deposition space, while taking into account high mechanical strength, reducing structural damage due to expansion effect during the cycle, and further improving the expansion inhibition performance, rate performance and cycle performance of the electrochemical device.
[0018] (2) The specific surface area of the porous carbon graphite composite material is S m 2 / g, 300≤S≤1500; by regulating the specific surface area and pore volume of the porous carbon-graphite composite material, the diffusion of silane gas in the composite material and the formation of nano-silicon can be promoted, and the expansion inhibition performance and cycle performance of the electrochemical device can be further improved.
[0019] (3) The silicon deposition capacity of the porous carbon graphite composite material is Cs%, 5≤Cs≤50; by regulating the silicon deposition capacity of the porous carbon graphite composite material within this range, the electrochemical device can exhibit better expansion suppression performance, rate performance and cycle performance.
[0020] (4) The average particle size of the porous carbon graphite composite material is Dd μm, 1≤Dd≤40.
[0021] In the second aspect, the present application provides a method for preparing any one of the above-mentioned porous carbon-graphite composite materials, comprising the following steps: Step 1, providing a graphite-based material; the graphite-based material includes graphite and / or graphite oxide; Step 2, mixing the graphite-based material, an organic carbon source and a pore-forming agent and granulating the mixture to obtain a composite intermediate; the average particle size of the composite intermediate is Zμm, 1.25≤Z≤45.5; Step 3, carbonizing the composite intermediate to obtain a porous carbon-graphite composite material.
[0022] In some embodiments, the organic carbon source includes at least one of resin, glucose, fructose, sucrose, cellulose, and asphalt; and / or the pore-forming agent includes at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, sodium carbonate, sodium bicarbonate, zinc chloride, silica, phosphoric acid, diammonium phosphate, and poloxamer; and / or the carbonization treatment temperature is Te°C and the time is Ti h; 500≤Te≤2500, 1≤Ti≤12.
[0023] In a third aspect, the present application provides a silicon-carbon material, including the porous carbon-graphite composite material provided in the first aspect or the porous carbon-graphite composite material obtained by the preparation method provided in the second aspect.
[0024] In a fourth aspect, the present application provides an electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector; the negative electrode mixture layer comprises the silicon-carbon material provided in the third aspect.
[0025] Based on the porous carbon-graphite composite material and its preparation method, silicon-carbon material and electrochemical device provided in the present application, by arranging a porous carbon layer on the surface of the graphite-based material, controlling the oxygen content of the graphite-based material, and regulating the relationship between the thickness of the porous carbon layer and the average particle size of the composite material, a good conductive network can be formed in the silicon-carbon material, and structural support can be provided when the silicon material undergoes volume changes, thereby improving the expansion suppression performance, rate performance and cycle performance of the electrochemical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the XRD pattern of the modified graphite powder of Example 1 of the present application;
[0027] Figure 2 is the XRD pattern of the graphite of Example 1 of the present application;
[0028] Figure 3 This is a SEM image of a cut cross section of the porous carbon-graphite composite material of Example 1 of the present application;
[0029] Figure 4 This is a SEM image of the cut cross section of the porous carbon material of Comparative Example 1. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0031] In order to solve the problems existing in the prior art, the inventors proposed to use a porous carbon / graphite composite material as a carrier and then compound it with silicon nanoparticles. For example, nano-silicon, graphite and an organic carbon source are first mixed and dried to make powder, and then carbonized to prepare a silicon-carbon composite material, which can improve the first coulombic efficiency and cycle performance of the negative electrode to a certain extent.
[0032] In view of this, the present application provides a porous carbon-graphite composite material in the first aspect, including a graphite-based material and a porous carbon layer located on the surface of the graphite-based material; the mass content of oxygen in the graphite-based material is Y%, 0.05≤Y≤41; the average particle size of the porous carbon-graphite composite material is Lμm, the thickness of the porous carbon layer is Hμm, 4.3≤L / H≤29.3. The present application sets a porous carbon layer on the surface of the graphite-based material, and by controlling the oxygen content of the graphite-based material, the porous carbon layer is tightly combined with the graphite-based material. On this basis, the relationship between the thickness of the porous carbon layer and the average particle size of the composite material is regulated to promote the interaction between the porous carbon layer and the graphite-based material, wherein the porous carbon layer provides a higher specific surface area, provides a deposition space for silicon elements to form a silicon-carbon material, and utilizes the sliding, folding and deformation of the graphite layered structure after pressurization when preparing the negative electrode to fill the gap, so that the silicon-carbon material has a higher compaction density and improves the energy density of the electrochemical device. On the other hand, by regulating the thickness of the porous carbon layer and the particle size of the composite material to conform to the above relationship, the porous carbon and graphite can form a good conductive network in the subsequent silicon-carbon material, and the porous carbon layer can act as a buffer to provide structural support when the silicon material undergoes volume changes, absorb and release expansion stress, and reduce structural damage to the electrode material. At the same time, the porous carbon layer is also beneficial to the penetration of the electrolyte and promotes the rapid insertion and extraction of lithium ions, thereby improving the expansion inhibition performance and rate charge and discharge performance of the electrochemical device, and is beneficial to reducing its capacity attenuation during the cycle.
[0033] In some embodiments, 0.05≤Y≤41, preferably 1.5≤Y≤29.5; for example, Y is selected from 0.05, 1.5, 2.1, 3.2, 5.0, 6.2, 7.9, 9.9, 10.6, 12.8, 13.3, 15.5, 17.3, 17.9, 19.8, 22.0, 22.3, 24.5, 25.7, 27.6, 29.2, 29.5, 35.5, 38.3, 41 or a value in the range formed by any two of these values. When the oxygen content in the graphite-based material is regulated to meet the above range, the interlayer spacing of the (002) crystal plane of the graphite-based material can be increased through the oxygen atoms in the structure, forming a deposition space for the silicon material, further improving the silicon deposition capacity, and obtaining an extremely high energy density. At the same time, the graphite-based material and the porous carbon layer can cooperate on the surface of the silicon material to form a more complex conductive network and jointly buffer the volume expansion of the silicon material. The appropriate oxygen content is also beneficial to improving the bonding effect between the graphite-based material and the porous carbon layer, further improving the structural stability of the composite material, and improving the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0034] The present application does not impose any particular restrictions on the method for regulating the oxygen content of the graphite-based material, and methods known in the art may be used, such as oxidative modification of graphite to obtain graphite-based materials with different oxygen contents. The graphite may be selected from natural graphite and / or artificial graphite.
[0035] In some embodiments, 4.3≤L / H≤29.3, preferably 5.0≤L / H≤12.5; illustratively, the value of L / H is 4.3, 5.1, 6.2, 7.0, 8.3, 10.6, 11.1, 12.3, 14.5, 15.8, 16.8, 17.8, 20.0, 20.2, 22.3, 23.2, 25.0, 25.7, 26.7, 28.9, 29.3 or a value in the range of any two of these values. When the thickness of the porous carbon layer and the average particle size of the composite material are further regulated to meet the above range, the graphite-based material and the porous carbon layer can be promoted to better cooperate to form a conductive network and a buffer structure, and optimize the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0036] In some embodiments, 1≤L≤40; for example, L is 1, 2, 4, 5, 8, 9, 13, 15, 16, 18, 21, 22, 24, 28, 30, 31, 33, 35, 37, 39, 40 or a value within the range formed by any two of these values. Regulating the average particle size of the porous carbon-graphite composite material within the above range can optimize the conductive network structure and the silicon material buffer structure, and further improve the rate performance, expansion inhibition performance and cycle performance of the electrochemical device. The present application does not impose any particular restrictions on the test method for the average particle size of the porous carbon-graphite composite material, and can be carried out by methods known in the art, such as taking a scanning electron microscope photo of the porous carbon-graphite composite material to be tested, and then randomly selecting 10 particles of the porous carbon-graphite composite material from the scanning electron microscope photo as samples, and calculating the area of each of these samples. Then, assuming that the sample is circular, the diameter R0 of each of these samples is calculated by the following formula: R0 = 2×(S / π) 1 / 2 ; Where S is the area of the sample. The particle sizes of the 10 samples were arithmetic averaged to obtain the average particle size of the porous carbon graphite composite material.
[0037] In some embodiments, 0.2≤H≤12, for example, H is 0.2, 0.4, 0.6, 0.8, 1.0, 1.8, 2.6, 2.7, 3.9, 4.3, 5.1, 5.7, 6.2, 6.5, 7.1, 8.0, 8.4, 9.0, 9.8, 10.7, 11.2, 11.6, 12 or a value in the range formed by any two of these values. Controlling the thickness of the porous carbon layer within the above range can provide better buffering for the expansion of the silicon material, while reducing the transmission path of lithium ions, so that the electrochemical device can achieve better rate performance, expansion suppression performance and cycle performance.
[0038] The present application does not impose any particular limitation on the testing method for the thickness of the porous carbon layer, and the method can be performed using methods known in the art. For example, the porous carbon-graphite composite material can be cut using argon ion polishing technology, and then a SEM image of the cut cross section can be taken using an electron scanning microscope. The thickness of the porous carbon layer in the test sample coated with multiple porous carbon-graphite composite materials can then be observed and measured, and the arithmetic mean value can be calculated, which is the thickness of the porous carbon layer.
[0039] In some embodiments, in the spectrum of the graphite-based material analyzed by an X-ray diffraction device using CuKα1 rays, the diffraction angle 2θ of the (002) peak satisfies: 22.0°≤2θ≤23.0°. For example, 2θ is 22.0°, 22.1°, 22.2°, 22.3°, 22.4°, 22.5°, 22.6°, 22.7°, 22.8°, 22.9°, 23.0°, or a value within the range of any two thereof. The interlayer spacing of the graphite (002) crystal plane is inversely proportional to the diffraction angle corresponding thereto. Therefore, based on the oxygen content of the graphite-based material, regulating the diffraction angle 2θ of the (002) peak within the above range is beneficial to ensure a suitable interlayer spacing to improve the silicon deposition capacity of the composite material, and can improve the conductivity and buffer the volume expansion of the silicon material after being combined with the porous carbon layer, which is beneficial to further improve the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0040] In some embodiments, the average particle size of the graphite-based material is Ds μm, 0.2 ≤ Ds ≤ 20. For example, Ds is 0.2, 1.0, 2.0, 2.5, 3.5, 4.8, 5.9, 6.7, 7.9, 8.7, 9.9, 11.4, 12.4, 13.0, 14.0, 15.2, 16.8, 17.2, 18.6, 19.4, 20 or a value in the range of any two of these values. Regulating the average particle size of the graphite-based material to conform to the above range is beneficial to further improve the expansion suppression performance, rate performance and cycle performance of the electrochemical device.
[0041] In some embodiments, in the spectrum of the porous carbon graphite composite material analyzed by an X-ray diffraction device using CuKα1 rays, the diffraction angle 2θ of the (002) peak satisfies: 22.0°≤2θ≤23.0°. For example, 2θ is 22.0°, 22.1°, 22.2°, 22.3°, 22.4°, 22.5°, 22.6°, 22.7°, 22.8°, 22.9°, 23.0°, or a value in the range composed of any two thereof. Regulating the diffraction angle 2θ of the (002) peak within the above range is conducive to ensuring a suitable interlayer spacing to improve the silicon deposition capacity of the composite material. After being combined with the porous carbon layer, it can improve the conductivity and buffer the volume expansion of the silicon material, which is conducive to further improving the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0042] The average particle size in the present application can be determined by a method known in the art, for example, the following steps may be included: after ultrasonic dispersion of the particles to be measured, the particle size analyzer is used to obtain the particle size of the material. V50, repeat the test, and calculate the average value of the seven sets of data after removing the abnormal points. In addition, when the above average particle size test method requires separation of the particles to be tested from the mixed component sample, and the separation of the particles to be tested is difficult to perform, the mixed component sample can also be observed through a scanning electron microscope photo, and multiple particles to be tested in the mixed component can be selected in combination with the morphological characteristics of the particles to be tested, and their particle sizes can be averaged to obtain the average particle size of the material.
[0043] In some embodiments, based on the mass of the porous carbon-graphite composite material, the mass content of the porous carbon layer is M1%, the mass content of the graphite-based material is M2%, and 0.2≤M2 / M1≤5.5. For example, the value of M2 / M1 is 0.2, 0.5, 0.7, 0.8, 1.1, 1.6, 1.7, 1.9, 2.2, 2.7, 2.9, 3.1, 3.4, 3.8, 4.0, 4.3, 4.4, 4.7, 5.0, 5.5 or a value in the range composed of any two of these values. Controlling the mass content ratio of the graphite-based material and the porous carbon layer to meet the above range can promote the graphite-based material and the porous carbon layer to better cooperate to form a conductive network and a buffer structure, and optimize the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0044] The mass content ratio of the graphite-based material and the porous carbon layer in the present application can be tested by methods known in the art, for example, 1g of the porous carbon-graphite composite material is put into a crucible, and sintered at a temperature of 20°C to 1000°C in an air atmosphere to obtain a mass-to-time curve, i.e., a thermogravimetric curve. According to the different weight loss temperatures of the porous carbon and graphite in the thermogravimetric curve, the mass ratio of the porous carbon layer and the graphite-based material is obtained.
[0045] In some embodiments, the porous carbon-graphite composite material is subjected to a pressure of 5000 kgf and a force-bearing area of 0.745 cm 2 The compacted density under the condition of Pd g / cm 3 , 0.68≤Pd≤2.00, preferably 1.16≤Pd≤1.69, and more preferably 1.47≤Pd≤1.52. For example, Pd is 0.68, 0.69, 0.78, 0.84, 0.96, 1.00, 1.04, 1.16, 1.18, 1.25, 1.31, 1.39, 1.47, 1.50, 1.52, 1.60, 1.69, 1.73, 1.79, 1.93, 1.96, 2.00 or a value within the range of any two of these values. Controlling the compaction density of the porous carbon-graphite composite material to meet the above range can further improve the energy density of the electrochemical device and increase the ion transmission path, while also helping to enhance structural support, improve the rate performance, suppress expansion performance and cycle performance of the electrochemical device.
[0046] In some embodiments, the pore volume of the porous carbon-graphite composite is Vt cm 3 / g, 0.2≤Vt≤0.8; for example, Vt is 0.2, 0.21, 0.25, 0.29, 0.32, 0.35, 0.38, 0.40, 0.42, 0.46, 0.51, 0.55, 0.55, 0.60, 0.62, 0.67, 0.70, 0.71, 0.76, 0.78, 0.8 or a value in the range formed by any two of these values. Regulating the pore volume of the porous carbon-graphite composite material to meet the above range can provide a suitable silane deposition space, while accommodating more silicon material to increase energy density, it can also ensure the mechanical strength of the composite material, reduce structural damage caused by expansion effect during the cycle, and further improve the expansion inhibition performance, rate performance and cycle performance of the electrochemical device.
[0047] In some embodiments, the specific surface area of the porous carbon-graphite composite is S m 2 / g, 300≤S≤1500; for example, S is 300, 360, 390, 460, 550, 590, 620, 700, 770, 850, 910, 970, 1010, 1100, 1130, 1220, 1270, 1340, 1430, 1490, 1500 or a value in the range formed by any two of these values. On the basis of regulating the pore volume of the porous carbon-graphite composite material, the specific surface area is controlled to meet the above range, which can increase the proportion of micropores in the composite material, promote the diffusion of silane gas in the composite material and the formation of nano-silicon, reduce or avoid the formation of macropores to form micron silicon, thereby alleviating the volume expansion of the silicon material and improving the expansion inhibition performance and cycle performance of the electrochemical device.
[0048] The method for specific surface area and pore volume in the present application can be carried out by methods known in the art. For example, a physical adsorption instrument (model: ipore 620) can be used to test the porous carbon-graphite composite material. The process includes: taking the porous carbon-graphite composite material as a sample to be tested and placing it in a sample tube, first degassing at 200°C for 6 hours, and then testing the adsorption amount of argon by the sample at different pressures, thereby drawing the isothermal adsorption curve of the sample, and then using BET fitting to calculate the specific surface area of the sample, and using non-localized density functional theory (NLDFT) fitting to calculate the pore volume of the sample.
[0049] In some embodiments, the silicon deposition capacity of the porous carbon graphite composite material is Cs%, 5≤Cs≤50; for example, Cs is 5, 6, 8, 11, 14, 15, 19, 20, 23, 26, 28, 30, 33, 34, 36, 39, 41, 44, 46, 50 or a value within the range formed by any two of these values. In the present application, the silicon deposition capacity refers to the mass proportion of the silicon element based on the mass of the silicon-carbon material after the porous carbon graphite composite material is subjected to silane vapor deposition to prepare the silicon-carbon material. By regulating the silicon deposition capacity of the porous carbon graphite composite material to meet the above range, a higher energy density can be achieved. When combined with the porous carbon graphite composite material, the electrochemical device can exhibit better expansion inhibition performance, rate performance and cycle performance.
[0050] In the present application, the silicon deposition capacity can be tested by a method including the following steps: chemical vapor deposition is performed on the porous carbon graphite composite material by introducing a silicon-containing gas source, and nitrogen is introduced to purge the furnace for 0.2 hours after the introduction for 0.3 hours, and then 0.7% of the silicon source gas is introduced again, and the chemical vapor deposition and purge are repeated 3 times in this manner to obtain a silicon-carbon material. The silicon-carbon material is acid-digested with HF and HNO3 to obtain a solution, and then an ICP test is performed to calculate the silicon content according to the standard curve. The mass content of silicon in the silicon-carbon material is the silicon deposition capacity of the porous carbon graphite composite material of the present application.
[0051] In some embodiments, the average particle size of the porous carbon graphite composite material is Dd μm, 1≤Dd≤40. For example, Dd is 1, 2, 4, 6, 9, 11, 12, 15, 17, 18, 20, 22, 25, 26, 29, 31, 32, 35, 38, 40 or a value in the range of any two of these values. Regulating the average particle size of the porous carbon graphite composite material within the above range can further improve the rate performance, expansion suppression performance and cycle performance of the electrochemical device.
[0052] In the second aspect, the present application provides a method for preparing any of the above-mentioned porous carbon-graphite composite materials, comprising the following steps: step 1, providing a graphite-based material; the graphite-based material includes graphite and / or graphite oxide; step 2, mixing the graphite-based material, an organic carbon source and a pore-forming agent and granulating the mixture to obtain a composite intermediate; the average particle size of the composite intermediate is Zμm, 1.25≤Z≤45.5; step 3, carbonizing the composite intermediate to obtain a porous carbon-graphite composite material. The present application granulates the graphite-based material, the organic carbon source and the pore-forming agent, so that the organic carbon source and the pore-forming agent are carbonized on the surface of the graphite-based material to prepare a porous carbon layer in situ, and on this basis, the average particle size of the composite intermediate is regulated within the scope of the present application, and the ratio of the average particle size of the composite material to the thickness of the porous carbon layer can be indirectly controlled within a suitable range, and the combination of the two is conducive to improving the conductivity and structural stability of the silicon-carbon material, and improving the rate performance, expansion inhibition performance and cycle performance of the electrochemical device.
[0053] In some embodiments, Z is 1.25, 1.6, 5.1, 7.2, 9.3, 11.3, 13.4, 16.0, 18.3, 21.1, 23.3, 25.1, 27.8, 29.4, 31.6, 35.5, 36.5, 38.9, 41.2, 43.8, 45.5, or a range consisting of any two of these values.
[0054] In some embodiments, the organic carbon source includes at least one of resin, glucose, fructose, sucrose, cellulose, and asphalt. Exemplarily, the resin includes at least one of phenolic resin, polypropylene resin, amine-formaldehyde resin, and epoxy resin.
[0055] In some embodiments, the pore-forming agent includes at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, sodium carbonate, sodium bicarbonate, zinc chloride, silicon dioxide, phosphoric acid, ammonium dihydrogen phosphate, and poloxamer. The pore-forming agent chemically corrodes the organic carbon source at high temperature to form pores, or it can leave pores after volatilization, thereby forming a porous carbon layer on the surface of the graphite-based material.
[0056] In some embodiments, the carbonization temperature is Te °C, the time is Ti h; 500≤Te≤2500, 1≤Ti≤12. For example, Te is 500, 550, 690, 800, 900, 990, 1110, 1140, 1330, 1370, 1500, 1650, 1660, 1810, 1890, 2040, 2110, 2250, 2310, 2490, 2500 or a value in the range formed by any two of these values, and Ti is 1, 1.4, 2.0, 3.4, 3.6, 5.0, 5.5, 6.8, 7.1, 8.5, 9.1, 10.3, 10.7, 11.5, 12 or a value in the range formed by any two of these values. Under the above temperature and time conditions, the pyrolysis of the organic carbon source and the pore-forming effect of the pore-forming agent can be promoted, thereby improving the pore volume and specific surface area of the porous carbon-graphite composite material.
[0057] In some embodiments, in step 3, the atmosphere of the carbonization treatment is one or more of water vapor, air, carbon dioxide, oxygen, and inert gas, which is conducive to further pore formation and pore expansion of the organic carbon source, improves the pore volume and specific surface area of the porous carbon graphite composite material, and increases the silicon deposition capacity.
[0058] In some embodiments, in step 2, the mixing further includes adding a dispersant, which is at least one of water, ethanol, methanol, propanol, ethylene glycol, etc. The dispersant can disperse the organic carbon source, and promote the organic carbon source to pass through the capillary better and enter the atomizer for granulation treatment.
[0059] In some embodiments, the granulation process can be carried out by spray drying. The inlet air temperature of the spray drying process is 80°C to 200°C, the outlet air temperature is 50°C to 150°C, the feed rate is 0.05mL / s to 100mL / s, and the atmosphere in the chamber is air or inert gas. The above parameters can promote the average particle size of the composite intermediate to reach a suitable range.
[0060] In some embodiments, graphite oxide can be prepared by a method comprising the following steps: stirring, washing and drying graphite powder, an oxidant and a dispersant to obtain modified graphite, namely the graphite oxide of the present application.
[0061] In some embodiments, the oxidant is one or more of concentrated sulfuric acid, concentrated nitric acid, potassium permanganate, potassium chlorate, hydrogen peroxide, fluorine, chlorine, etc. These oxidants have sufficient oxidizing power to complete the modification of graphite. In some embodiments, two oxidants are required, specifically, such as concentrated sulfuric acid / hydrogen peroxide, concentrated nitric acid / hydrogen peroxide, potassium permanganate / hydrogen peroxide, and the use of an oxidant without heteroatoms in the two oxidants for dilution can prevent the introduction of excessive heteroatoms on the surface. In some embodiments, the dispersant is at least one of water, ethanol, methanol, propanol, ethylene glycol, etc. In some embodiments, the mass concentration ratio of graphite powder to oxidant is 0.01g / mL to 0.2g / mL, such as 0.01g / mL, 0.05g / mL, 0.10g / mL, 0.15g / mL, 0.2g / mL or a value within the range of any two of them.
[0062] In a third aspect, the present application provides a silicon-carbon material, including the porous carbon-graphite composite material provided in the first aspect or the porous carbon-graphite composite material obtained by the preparation method provided in the second aspect.
[0063] In a fourth aspect, the present application provides an electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector; the negative electrode mixture layer comprises the silicon-carbon material provided in the third aspect.
[0064] The electrochemical device of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction, such as a secondary battery. The present application is described below using a secondary battery as an example in combination with the embodiments of the present application. The secondary battery of the present application is not particularly limited, and may include, but is not limited to, a lithium-ion secondary battery (also known as a lithium-ion battery) or a sodium-ion secondary battery.
[0065] In the present application, the negative electrode includes a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode mixture layer disposed on at least one surface of the negative electrode current collector" means that the negative electrode mixture layer can be disposed on the surface of one side in the thickness direction of the negative electrode current collector, or on the surfaces of both sides in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of the negative electrode current collector, or it can be a partial area of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the thickness of the negative electrode mixture layer, as long as the purpose of this application can be achieved. For example, the thickness of a single-sided negative electrode mixture layer can be 30μm to 160μm.
[0066] In the present application, the silicon-carbon material is located in the negative electrode mixture layer. In some embodiments, the negative electrode mixture layer may further include natural graphite and / or artificial graphite.
[0067] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, composite current collector (such as carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector), polymer substrate coated with conductive metal or any combination thereof. The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 10μm.
[0068] In the present application, the negative electrode mixture layer may also include a negative electrode binder, which may include but is not limited to at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyacrylic acid (PAA), styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin or nylon.
[0069] In the present application, the negative electrode mixture layer may also include a conductive agent. The present application has no particular restrictions on the type of conductive agent in the negative electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to carbon-based materials, metal-based materials, conductive polymers and mixtures thereof. In some embodiments, the carbon-based material is selected from carbon black, acetylene black, Ketjen black, carbon fiber or any combination thereof. In some embodiments, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum or silver. In some embodiments, the conductive polymer is a polyphenylene derivative. The present application has no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent and the negative electrode binder in the negative electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the loading amount of the negative electrode material in the negative electrode sheet is 1.0 mg / cm 2 Up to 1.5 mg / cm 2 .
[0070] In the present application, there is no special restriction on the positive electrode, as long as the purpose of the present application can be achieved. For example, the positive electrode includes a positive electrode current collector and a positive electrode mixture layer arranged on at least one surface of the positive electrode current collector. The above-mentioned "positive electrode mixture layer arranged on at least one surface of the positive electrode current collector" means that the positive electrode mixture layer can be arranged on one surface of the positive electrode current collector along its own thickness direction, or it can be arranged on two surfaces of the positive electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the surface of the positive electrode current collector, or it can be a partial area of the surface of the positive electrode current collector. There is no special restriction in the present application, as long as the purpose of the present application can be achieved.
[0071] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate.
[0072] The positive electrode mixture layer of the present application includes a positive electrode active material. The present application has no particular restrictions on the type of the positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include lithium nickel cobalt manganese oxide (LiNi 0.90 Co 0.05 Mn 0.05 O2 (NCM955), NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide and lithium titanate. In the present application, the positive active material may also contain non-metallic elements, for example, the non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur. In the present application, there is no particular restriction on the thickness of the positive current collector and the positive electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive current collector is 5μm to 20μm, and the thickness of the single-sided positive electrode mixture layer is 30μm to 120μm.
[0073] In the present application, the positive electrode mixture layer may further include a positive electrode binder and a conductive agent. The present application does not particularly limit the type of positive electrode binder in the positive electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the positive electrode binder may include but is not limited to polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified styrene-butadiene rubber (SBR) or at least one of polyurethane. In some embodiments, the polyolefin binder includes at least one of polyethylene, polypropylene, polyolefin ester, polyolefin alcohol or polyacrylic acid.
[0074] The present application has no particular restrictions on the type of conductive agent in the positive electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the conductive agent can be the same type as the conductive agent in the above-mentioned negative electrode mixture layer. In some embodiments, the conductive agent includes carbon-based materials, such as carbon black, acetylene black, Ketjen black or carbon fiber; metal-based materials, such as metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof. The present application has no particular restrictions on the mass ratio of the positive electrode active material, the conductive agent, and the positive electrode binder in the positive electrode mixture layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, the loading amount of the positive electrode active material in the positive electrode sheet is 4.0 mg / cm 2 Up to 10.0mg / cm 2 .
[0075] According to some embodiments of the present application, the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide {LiN(CF3SO2)2, LiTFSI)}, lithium bis(fluorosulfonyl)imide {Li(N(SO2F)2), LiFSI}, lithium bis(oxalate borate) {LiB(C2O4)2, LiBOB}, lithium difluorooxalate borate {LiBF2(C2O4), LiDFOB}, LiNO3, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiC(SO2CF3)3, Li2SiF6, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or at least one of lithium difluoroborate. The present application does not limit the content of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. The application has no particular restrictions on non-aqueous solvents, as long as the purpose of the application can be achieved. For example, non-aqueous solvents may include but are not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of linear carbonate compounds, cyclic carbonate compounds or fluorocarbonate compounds. The above-mentioned linear carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or ethyl methyl carbonate (EMC). The above-mentioned cyclic carbonate may include but are not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate or vinyl ethylene carbonate. The fluorinated carbonate compound may include, but is not limited to, at least one of fluorinated ethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of 1,3-dioxolane (DOL), ethylene glycol dimethyl ether (1,2-dimethoxyethane, DME), dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran.The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.
[0076] The secondary battery of the present application also includes a separator. The material and shape of the separator used in the secondary battery of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application.
[0077] For example, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be selected.
[0078] A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polyvinylidene fluoride and poly (vinylidene fluoride-hexafluoropropylene).
[0079] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.
[0080] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and the present application has no special restrictions. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.
[0081] The present application also provides an electronic device, comprising the secondary battery provided in the fourth aspect of the present application.
[0082] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.
[0083] The following uses lithium-ion batteries as an example to illustrate the solution of the present application in combination with specific embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all from common commercial products, and the devices or equipment used are all purchased from conventional market sales channels.
[0084] Performance testing method:
[0085] Gram Capacity Test
[0086] At a test temperature of 25°C, the button cell was discharged to 0.01 V at a current density of 50 mA / g, and charged to 2.0 V at a current density of 50 mA / g, and the charging capacity of the button cell was recorded. Gram capacity = charging capacity / mass of negative electrode active material.
[0087] Rate performance test
[0088] Take the lithium ion battery of the embodiment / comparative example to be tested and place it at a test temperature of 25°C for 5 minutes, then charge the lithium ion battery to 4.45V at a constant current of 0.7C, and then charge it to 0.05C at a constant voltage of 4.45V; let it stand for 5 minutes, then discharge it to 3.0V at a constant current of 0.2C, and record the 0.2C discharge capacity; then let it stand for 5 minutes, repeat the above charging process, and then discharge it at a constant current of 2C, and record the 2C discharge capacity. Rate capacity retention rate = 2C discharge capacity / 0.2C discharge capacity × 100%.
[0089] Cyclic performance test
[0090] At a test temperature of 25°C, let the lithium-ion battery to be tested stand for 5 minutes, and record the initial thickness MMC0 of the lithium-ion battery. Perform 3.4C step charging on the lithium-ion battery. The 3.4C step charging includes: charging the lithium-ion battery to 4.25V with a current of 3.4C, then charging to 4.4V with a constant current of 2C, then charging to 4.50V with a constant current of 1C, and then charging to 0.05C with a constant voltage of 4.50V. Then let it stand for 5 minutes, and then discharge to 3.0V with a constant current of 0.5C, let it stand for 5 minutes, and record the discharge capacity C1 of the lithium-ion battery. After the above 3.4C step charging / 0.5C discharge charge and discharge cycle process is cycled 400 times, record the thickness MMC1 and discharge capacity C2 of the lithium-ion battery. Cycle capacity retention rate (%) = C2 / C1×100%, record the number of cycles when the cycle capacity retention rate is 90%. Cycle thickness expansion ratio (%) = (MMC1-MMC0) / MMC0×100%.
[0091] Example 1
[0092] Preparation of modified graphite
[0093] 10 g of graphite powder, 200 ml of concentrated sulfuric acid with a mass concentration of 98% and 20 ml of hydrogen peroxide were mixed and stirred at room temperature for 30 minutes, then washed with deionized water and then dried in an oven at 80° C. to obtain modified graphite (i.e., graphite oxide).
[0094] Preparation of porous carbon-graphite composites
[0095] Step 1: Use the modified graphite as graphite-based material.
[0096] Step 2: Take 10g of the modified graphite, 50g of phenolic resin (organic carbon source), 50g of potassium hydroxide (pore-forming agent) and 1000ml of ethanol solution, mix them by ultrasonic dispersion to obtain a suspension, and then perform granulation. The granulation process includes: using a spray dryer to spray the suspension at an inlet temperature of 180°C, an outlet temperature of 80°C, a feed rate of 3mL / s, and a nitrogen atmosphere in the chamber to obtain a composite intermediate. The average particle size Zμm of the composite intermediate is 5.4μm.
[0097] Step 3: Place the composite intermediate in a crucible and put it into a rotary furnace. Then, in a nitrogen atmosphere, heat it to 900° C. at a heating rate of 5° C. / min and keep it at 900° C. for 6 hours for carbonization treatment to obtain a porous carbon-graphite composite material.
[0098] Preparation of negative electrode
[0099] The negative electrode active material porous carbon graphite composite material, conductive carbon black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are fully stirred and mixed in a solvent deionized water at a weight ratio of 95.7:1.5:1.8:1 to obtain a negative electrode slurry. The negative electrode slurry is coated on the negative electrode current collector copper foil, and then dried and cold pressed to form a negative electrode mixture layer, and then cut into pieces and welded to the pole ears to obtain a negative electrode sheet.
[0100] Preparation of positive electrode
[0101] Lithium cobalt oxide, carbon black and polyvinylidene fluoride (PVDF) were fully stirred and mixed in an N-methylpyrrolidone solvent system at a weight ratio of 95:2.5:2.5 to prepare a positive electrode slurry. The prepared positive electrode slurry was coated on a positive electrode current collector aluminum foil, dried, and cold pressed to obtain a positive electrode.
[0102] Preparation of electrolyte
[0103] In a dry argon environment, LiPF6 and fluoroethylene carbonate are added to a solvent mixed with propylene carbonate, ethylene carbonate, propyl propionate and ethyl propionate (weight ratio of 2:1:1:2) and mixed evenly to obtain an electrolyte, wherein the mass percentage of LiPF6 is 12.5% and the mass percentage of fluoroethylene carbonate is 3.5% based on the mass of the electrolyte.
[0104] Preparation of diaphragm
[0105] A polyethylene / polypropylene composite porous polymer film is used as the separator.
[0106] Preparation of electrochemical device
[0107] Button battery
[0108] Using a metal lithium sheet as a counter electrode, a metal lithium sheet with a diameter of 18 mm and a thickness of 0.6 mm, a separator, and the negative electrode sheets (cut into a diameter of 18 mm) in each embodiment and comparative example are assembled and stacked in sequence, and an electrolyte is added. The positive and negative electrodes are packaged in a button-type stainless steel shell to obtain a button-type battery.
[0109] Preparation of lithium-ion batteries
[0110] The positive electrode sheet and the negative electrode sheet prepared as above are connected to the pole ears. They are stacked via a separator to obtain a laminate. Then, the laminate is stored in an aluminum laminate housing together with an electrolyte. The opening of the housing is heat-sealed, and a lithium-ion battery is manufactured through steps such as formation and degassing.
[0111] The porous carbon materials of the embodiments and comparative examples in Table 1 are different from those of Example 1 mainly in that the preparation method of the porous carbon materials is adjusted according to the parameters in Table 1. The graphite oxides used have different oxidation degrees, and Comparative Example 1 is a porous carbon material, and Comparative Example 2 is a graphite oxide material.
[0112] Table 1
[0113]
[0114] The porous carbon materials of the embodiments and comparative examples were tested according to the above test method. The test results are shown in Table 2.
[0115]
[0116] As can be seen from Table 2, the present application sets a porous carbon layer on the surface of the graphite-based material, controls the value of Y in the oxygen content Y% of the graphite-based material to meet 0.05≤Y≤41, and regulates the relationship between the thickness Hμm of the porous carbon layer and the average particle size Lμm of the composite material to meet 4.3≤L / H≤29.3, which can promote the interaction between the porous carbon layer and the graphite-based material, and improve the rate performance, cycle performance and expansion inhibition performance of the lithium-ion battery. In particular, when the value of Y is regulated to meet 1.5≤Y≤29.5, or when 5.0≤L / H≤12.5 is met, the rate performance, expansion inhibition performance and cycle performance of the lithium-ion battery can be further improved. Further, when 13.7≤Y≤19.3 and / or 5.0≤L / H≤12.5 are met, the rate performance, expansion inhibition performance and cycle performance of the lithium-ion battery can be more significantly improved.
[0117] In particular, when the mass content M1% of the porous carbon layer and the mass content M2% of the graphite-based material are regulated to satisfy: 0.2≤M2 / M1≤5.5, the rate performance, expansion suppression and cycle performance of the lithium-ion battery can be further optimized. In particular, when the compaction density Pd g / cm3 When 0.68≤Pd≤2.00, preferably 1.02≤Pd≤1.78, is satisfied, the lithium-ion battery can exhibit better expansion suppression performance, rate performance and cycle performance. In particular, when the pore volume Vt cm of the porous carbon-graphite composite material is regulated, 3 When the ratio of Vt to g satisfies 0.2≤Vt≤0.8, preferably 0.3≤Vt≤0.68, the rate performance, expansion inhibition and cycle performance of the lithium-ion battery can be improved more significantly. 2 / g satisfies 300≤S≤1500, preferably 1010≤S≤1343, which can further improve the rate performance, expansion inhibition performance and cycle performance of the lithium ion battery.
[0118] In particular, Figure 1 and Figure 2 The XRD patterns of the modified graphite powder and graphite of Example 1 are shown, and the diffraction angles corresponding to the (002) crystal plane are 23.0° and 22.1°, respectively, indicating that the modification of the graphite powder can reduce the diffraction angle 2θ of the (002) peak and increase the (002) crystal plane spacing.
[0119] Further, Figure 3 and Figure 4 SEM images of the cut cross sections of the porous carbon-coated modified graphite material of Example 1 and the porous carbon material of Comparative Example 3 are shown. It can be clearly observed by comparison that the porous carbon-graphite composite material structure of Example 1 includes a graphite-based material and a porous carbon layer located on the surface of the graphite-based material.
[0120] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the principles of the present application should be included in the protection scope of the present application.
Claims
1. A porous carbon-graphite composite material, characterized in that: It comprises a graphite-based material and a porous carbon layer located on the surface of the graphite-based material; the mass content of oxygen in the graphite-based material is Y%, and 0.05≤Y≤41; The average particle size of the porous carbon-graphite composite material is L μm, the thickness of the porous carbon layer is H μm, and 4.3≤L / H≤29.
3.
2. The porous carbon-graphite composite material according to claim 1, characterized in that: The porous carbon-graphite composite material satisfies at least one of the following conditions: (1)1.5≤Y≤29.5; (2) 5.0 ≤ L / H ≤ 12.5; (3)1≤L≤40; (4)0.2≤H≤12。 3. The porous carbon-graphite composite material according to claim 1 or 2, characterized in that: In the spectrum of the graphite-based material analyzed by an X-ray diffraction device using CuKα1 rays, the diffraction angle 2θ of the (002) peak satisfies: 22.0°≤2θ≤23.0°; and / or, The average particle size of the graphite-based material is Ds μm, 0.2≤Ds≤20.
4. The porous carbon-graphite composite material according to claim 1 or 2, characterized in that: In a spectrum of the porous carbon-graphite composite material analyzed by an X-ray diffraction apparatus using CuKα1 rays, a diffraction angle 2θ of a (002) peak satisfies: 22.0°≤2θ≤23.0°.
5. The porous carbon-graphite composite material according to claim 1 or 2, characterized in that: Based on the mass of the porous carbon-graphite composite material, the mass content of the porous carbon layer is M1%, the mass content of the graphite-based material is M2%, and 0.2≤M2 / M1≤5.
5.
6. The porous carbon-graphite composite material according to claim 1 or 2, characterized in that: The porous carbon graphite composite material is subjected to a pressure of 5000 kgf and a force-bearing area of 0.745 cm 2 The compacted density under the condition of Pd g / cm 3 , 0.68≤Pd≤2.
00.
7. The porous carbon-graphite composite material according to claim 1 or 2, characterized in that: The porous carbon-graphite composite material satisfies at least one of the following conditions: (1) The pore volume of the porous carbon-graphite composite material is Vt cm 3 / g, 0.2≤Vt≤0.8; (2) The specific surface area of the porous carbon graphite composite material is Sm 2 / g, 300≤S≤1500; (3) The silicon deposition capacity of the porous carbon graphite composite material is Cs%, 5≤Cs≤50; (4) The average particle size of the porous carbon-graphite composite material is Dd μm, 1≤Dd≤40.
8. The method for preparing a porous carbon-graphite composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: providing a graphite-based material; the graphite-based material includes graphite and / or graphite oxide; Step 2, mixing the graphite-based material, the organic carbon source and the pore-forming agent and then granulating the mixture to obtain a composite intermediate; the average particle size of the composite intermediate is Z μm, 1.25≤Z≤45.5; Step 3: Carbonizing the composite intermediate to obtain the porous carbon-graphite composite material.
9. The preparation method according to claim 8, characterized in that: The organic carbon source comprises at least one of resin, glucose, fructose, sucrose, cellulose and asphalt; and / or, The pore-forming agent includes at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, sodium carbonate, sodium bicarbonate, zinc chloride, silicon dioxide, phosphoric acid, ammonium dihydrogen phosphate, and poloxamer; and / or, The temperature of the carbonization treatment is Te°C, and the time is Ti h; 500≤Te≤2500, 1≤Ti≤12.
10. A silicon-carbon material, characterized in that: The porous carbon-graphite composite material comprises the porous carbon-graphite composite material according to any one of claims 1 to 7 or the porous carbon-graphite composite material obtained by the preparation method according to claim 8 or 9.
11. An electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, characterized in that: The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector; The negative electrode mixture layer includes the silicon-carbon material according to claim 10 .
Citation Information
Cited By
Silicon-carbon composite negative electrode material and preparation method thereof
CN119517973A
Silicon-carbon composite material as well as preparation method and application thereof
CN120878791A
Solid-state battery cell, battery device, electric device, and preparation method for porous carbon
WO2026138979A1