RRAM device and method of forming the same

By using high-binding energy dopants to form bonds with oxygen in RRAM devices and controlling the distribution of oxygen vacancies, the problem of conductive wire coarsening caused by the destruction of oxygen-oxygen bonds is solved, and the reset efficiency of the device and the stability of the read window are improved. sex.

CN112670407BActive Publication Date: 2024-10-29TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010639969.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-06
Publication Date
2024-10-29
Estimated Expiration
2040-07-06

AI Technical Summary

Technical Problem

As time goes by, during read and write cycles of RRAM devices, the destruction of oxygen-oxygen bonds leads to an increase in oxygen vacancies in the data storage structure and the thickening of conductive filaments, which reduces the ability of the device to switch from a low-resistance state to a high-resistance state. efficiency, thereby reducing reset efficiency and read window, leading to device failure.

Method used

Adopting a doped data storage structure, using high binding energy dopants (such as nitrogen, fluorine, carbon, phosphorus, etc.) to form bonds with oxygen to reduce the number of oxygen vacancies, and control the oxygen vacancy distribution through non-uniform doping profiles to maintain The fineness of the conductive filament and the stability of the read window.

Benefits of technology

It effectively reduces the number of oxygen vacancies, maintains the fineness of the conductive wire, improves the reset efficiency of the RRAM device and the stability of the read window, and extends the service life of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112670407B_ABST
    Figure CN112670407B_ABST
Patent Text Reader

Abstract

Embodiments of the present invention relate to a resistive random access memory (RRAM) device and a method for forming the same. In some embodiments, the method may be performed by forming a first electrode structure over a substrate. A doped data storage element is formed over the first electrode structure. The doped data storage element is formed by forming a first data storage layer over the first electrode structure and a second data storage layer over the first data storage layer. The first data storage layer is formed as a dopant having a first doping concentration, and the second data storage layer is formed as a dopant having a second doping concentration, the second doping concentration being less than the first doping concentration. A second electrode structure is formed over the doped data storage element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to RRAM devices and methods of forming the same. Background Art

[0002] Many modern electronic devices contain electronic memory configured to store data. Electronic memory can be either volatile memory or non-volatile memory. Volatile memory stores data when power is on, while non-volatile memory is able to store data when power is off. Resistive random access memory (RRAM) is a promising candidate for the next generation of non-volatile memory technology due to its simple structure and compatibility with CMOS logic manufacturing processes. Summary of the invention

[0003] An embodiment of the present invention provides a method for forming a resistive random access memory (RRAM) device, comprising: forming a first electrode structure above a substrate; forming a doped data storage element above the first electrode structure, wherein forming the doped data storage element comprises: forming a first data storage layer above the first electrode structure, wherein the first data storage layer is formed as a dopant having a first doping concentration; forming a second data storage layer above the first data storage layer, wherein the second data storage layer is formed as the dopant having a second doping concentration, the second doping concentration being less than the first doping concentration; and forming a second electrode structure above the doped data storage element.

[0004] Another embodiment of the present invention provides a method for forming a resistive random access memory (RRAM) device, comprising: forming a lower electrode structure above a conductive interconnect layer disposed above a substrate; forming a doped data storage element comprising a plurality of data storage layers above the lower electrode structure, wherein the plurality of data storage layers are formed to have different concentrations of dopants; and forming an upper electrode structure above the doped data storage element.

[0005] Yet another embodiment of the present invention provides a resistive random access memory (RRAM) device, comprising: a first electrode located above a conductive lower interconnect layer; a second electrode located above the first electrode; and a doped data storage structure disposed between the first electrode and the second electrode and having a variable resistance, wherein the doped data storage structure comprises a dopant having a doping concentration with a non-uniform doping profile along the height of the doped data storage structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Various aspects of the present invention will be best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be emphasized that, in accordance with standard practice in the industry, the various components are not drawn to scale and are for illustration purposes only. In fact, the dimensions of the various components may be arbitrarily increased or reduced for clarity of discussion.

[0007] Figure 1A Cross-sectional views of some embodiments of a resistive random access memory (RRAM) device having a doped data storage structure configured to provide good reliability to the RRAM device are shown.

[0008] Figure 1B to Figure 1C Cross-sectional views of some embodiments of a doped data storage structure having multiple data storage layers with different doping concentrations are shown.

[0009] Figure 2 Some embodiments are illustrated in diagrams showing the resistance of a high-resistance state and a low-resistance state of a RRAM device having a doped data storage structure.

[0010] FIG. 3A to FIG. 3B Graphs illustrating some embodiments of exemplary doping concentrations within doped data storage structures of the disclosed RRAM devices are shown.

[0011] FIG. 4A to FIG. 4B Some embodiments of the operation of a RRAM device having a doped data storage structure are shown.

[0012] Figure 5 Cross-sectional views of some embodiments of an integrated chip including a RRAM device having a doped data storage structure are shown.

[0013] Figure 6 Cross-sectional views of some alternative embodiments of integrated chips including RRAM devices having doped data storage structures are shown.

[0014] Figures 7 to 17 Some embodiments of cross-sectional views are shown illustrating a method of forming an integrated chip including a RRAM device having a doped data storage structure.

[0015] Fig.18 A flow chart illustrating some embodiments of a method of forming an integrated chip including a RRAM device having a doped data storage structure.

[0016] Figures 19 to 20 A block diagram is shown illustrating some embodiments of a processing tool configured to form a doped data storage structure of the disclosed RRAM device. DETAILED DESCRIPTION

[0017] The following disclosure provides many different embodiments or examples for implementing the different features of the provided subject matter. Specific embodiments or examples of components and arrangements are described below to simplify the present invention. Of course, these are only examples and are not intended to be limiting. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.

[0018] Additionally, for ease of description, spacing relation terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another element or component as shown in the figures. The spacing relation terms are intended to encompass different orientations of the device in use or in the process of operation in addition to the orientation shown in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spacing relation descriptors used herein may likewise be interpreted accordingly.

[0019] A resistive random access memory (RRAM) device is configured to store data by switching between a high resistance state corresponding to a first data state (e.g., "0") and a low resistance state corresponding to a second data state (e.g., "1"). To achieve this "resistive switching", the RRAM device has a lower electrode separated from an upper electrode by a data storage structure having a variable resistance. The data storage structure typically includes a high-k dielectric material (e.g., hafnium oxide) that is capable of changing its internal resistance in response to an applied bias voltage.

[0020] For example, the resistance of a data storage structure is generally determined by whether there is a conductive filament including a plurality of oxygen vacancies within the data storage structure. If the conductive filament is present, the data storage structure has a relatively low resistance associated with a low resistance state. If the conductive filament is not present, the data storage structure has a relatively high resistance associated with a high resistance state. To change between the low resistance state and the high resistance state, an applied bias voltage may move oxygen vacancies into or out of the data storage structure to form a conductive filament extending through the data storage structure or to destroy a conductive filament extending through the data storage structure.

[0021] It has been recognized that, over time (e.g., after a large number of read and / or write cycles), the current flowing through the data storage structure may break the oxygen-oxygen bonds within the data storage structure, thereby increasing the number of oxygen vacancies present within the data storage structure. Although oxygen vacancies near the upper electrode can be easily moved into and out of the data storage structure during operation, oxygen vacancies away from the upper electrode may be more difficult to remove, resulting in excess oxygen vacancies within the data storage structure. When the RRAM device is in a low resistance state, the excess oxygen vacancies will cause the conductive filament to become thicker (e.g., along the lower half of the data storage structure). The thicker filament makes it more difficult for the RRAM device to switch from a low resistance state to a high resistance state, reducing the reset efficiency of the RRAM device. Over time, this reduction may reduce the read window (e.g., the difference between the signals output from the RRAM device in the low resistance state and the high resistance state) and cause device failure.

[0022] In some embodiments, the present invention relates to a RRAM device having a doped data storage structure configured to mitigate degradation of a read window over time. The doped data storage structure is doped with one or more dopants having a high binding energy with oxygen. The high binding energy of the one or more dopants (e.g., greater than about 500 KJ / mol) prevents bond breakage within the doped data storage structure, thereby reducing the number of oxygen vacancies within the doped data storage structure. By reducing the number of oxygen vacancies within the doped data storage structure, the increase in thickness of the conductive filament after a large number of read and / or write cycles is mitigated, thereby maintaining good reset efficiency, which provides a stable read window and good data retention.

[0023] Figure 1A A cross-sectional view of some embodiments of an integrated chip 100 including a resistive random access memory (RRAM) device having a doped data storage structure configured to provide good reliability to the RRAM device is shown.

[0024] The integrated chip 100 includes a RRAM device 101 surrounded by an interlayer dielectric (ILD) structure 104 disposed above a substrate 102. The RRAM device 101 includes a doped data storage structure 110 disposed between a lower electrode 108 and an upper electrode 116. The lower electrode 108 is separated from the substrate 102 by one or more lower interconnect layers 106 (e.g., metal vias and / or metal lines). The upper electrode 116 is disposed between the doped data storage structure 110 and the upper interconnect layer 118 (e.g., metal vias and / or metal lines).

[0025] The doped data storage structure 110 is configured to store different data states by undergoing a reversible change between a high resistance state associated with a first data state (e.g., “0”) and a low resistance state associated with a second data state (e.g., “1”). For example, to achieve the low resistance state within the doped data storage structure 110, a first set of bias conditions may be applied to the lower electrode 108 and the upper electrode 116. The first set of bias conditions may drive oxygen from the doped data storage structure 110 to the upper electrode 116, thereby forming a conductive filament 112 of oxygen vacancies 114 on the doped data storage structure 110. Alternatively, to achieve the high resistance state within the doped data storage structure 110, a second set of bias conditions may be applied to the lower electrode 108 and the upper electrode 116. The second set of bias conditions may break the conductive filament 112 by driving oxygen from the upper electrode 116 to the doped data storage structure 110.

[0026] The doped data storage structure 110 is doped with one or more dopants configured to form a bond with oxygen, the bond having a binding energy greater than the binding energy of the oxygen-oxygen bond (e.g., about 498 kJ / mol). For example, in some embodiments, the dopant may bind to oxygen with a binding energy greater than about 500 kJ / mol. In other embodiments, the dopant may bind to oxygen with a binding energy greater than about 600 kJ / mol. In various embodiments, the doped data storage structure 110 may include hafnium oxide, zirconium oxide, aluminum oxide, tantalum oxide, hafnium aluminum oxide, hafnium zirconium oxide, and the like. In various embodiments, the dopant may include nitrogen, fluorine, carbon, phosphorus, and the like. In some embodiments, the dopant may cause the doped data storage structure 110 to include metal oxynitrides (e.g., hafnium oxynitride, tantalum oxynitride, and the like), metal oxyfluorides (e.g., hafnium oxyfluoride, zirconium oxyfluoride, and the like), metal oxycarbides (e.g., hafnium oxycarbide, aluminum oxycarbide, and the like), metal phosphorus oxides (e.g., hafnium oxyphosphorus, zirconium oxyphosphorus, and the like), and the like. In some such embodiments, a dopant comprising carbon may form a carbon-oxygen bond having a binding energy of about 1076 KJ / mol, and / or a dopant comprising nitrogen may form a nitrogen-oxygen bond having a binding energy of about 630 KJ / mol. The binding energy between the dopant and the oxygen molecule firmly bonds the oxygen molecule to the dopant within the doped data storage structure 110, thereby preventing bond breakage within the doped data storage structure 110 and mitigating an increase in the number of oxygen vacancies within the doped data storage structure 110 over time.

[0027] In some embodiments, the dopant has a non-uniform doping profile that varies relative to the thickness T of the doped data storage structure 110 (i.e., is non-uniform along the height of the doped data storage structure 110). For example, in some embodiments, the non-uniform doping profile can have a peak doping concentration that occurs at a location separated by a non-zero distance from the lower electrode 108 and the upper electrode 116. Because the binding energy of the dopant is greater than the binding energy of the oxygen-oxygen bond, the non-uniform doping profile of the dopant can be used to control the number of oxygen vacancies present at different locations within the doped data storage structure 110. For example, in some embodiments, the non-uniform doping profile can have a higher dopant concentration along the lower half of the doped data storage structure 110 than along the upper half. In such an embodiment, the doping profile provides sufficient oxygen vacancies within the upper half to form a conductive filament while limiting the number of oxygen vacancies along the lower half of the doped data storage structure 110 (and mitigating the increase in the width of the conductive filament 112). Controlling the number of oxygen vacancies present at different locations within the doped data storage structure 110 enables the RRAM device to maintain a low resistance state and a good read window between the high resistance state and the low resistance state.

[0028] Figure 1B to Figure 1C Cross-sectional views 120 and 122 of some embodiments of a doped data storage structure 110 are shown that includes multiple data storage layers having different doping concentrations of a dopant that combines with oxygen with a binding energy greater than about 500 kJ / m. Figure 1B to Figure 1C Embodiments of doped data storage structures having two and three data storage layers are shown, but it should be understood that the disclosed doped data storage structures (e.g., Figure 1A The doped data storage structure 110 is not limited to such an embodiment. Instead, the disclosed doped data storage structure can have any number of data storage layers.

[0029] like Figure 1BAs shown in the cross-sectional view 120 of , in some embodiments, the plurality of data storage layers 110a-110b may include a first data storage layer 110a having a first doping concentration and a second data storage layer 110b having a second doping concentration. In some embodiments, the first doping concentration may be greater than the second doping concentration. In some embodiments, the first doping concentration may be a non-zero doping concentration, and the second doping concentration may be substantially zero. In some embodiments, the first and second doping concentrations may be discrete (e.g., discontinuous) at the interface between the first data storage layer 110a and the second data storage layer 110b. For example, in some embodiments, the first data storage layer 110a may have a first doping concentration between about 7% and about 8%, and the second data storage layer 110b may contact the first data storage layer 110a and have a second doping concentration between about 2% and about 3%. In other embodiments, the first and second doping concentrations may be continuous at the interface.

[0030] like Figure 1C As shown in the cross-sectional view 122 of , in some embodiments, the plurality of data storage layers 110a-110b may include a first data storage layer 110a having a first doping concentration, a second data storage layer 110b having a second doping concentration, and a third data storage layer 110c having a third doping concentration. In some embodiments, the first doping concentration may be less than the second doping concentration, and the second doping concentration may be greater than the third doping concentration. In other embodiments, the first doping concentration may be greater than the second doping concentration, and the second doping concentration may be greater than the third doping concentration. In some embodiments, the first doping concentration and the second doping concentration may be non-zero doping concentrations, and the third doping concentration may be substantially zero. In some embodiments, the first, second, and third doping concentrations may be discrete (e.g., discontinuous) at the interface between adjacent data storage layers, while in other embodiments, the first, second, and third doping concentrations may be continuous at the interface.

[0031] Figure 2 Graph 200 shows some embodiments of resistance values ​​of a disclosed RRAM device (eg, RRAM device 101 of FIG. 1 ) in a low resistance state and a high resistance state. Graph 200 shows the resistance of the RRAM device along the y-axis and the number of read and / or write cycles along the x-axis.

[0032] As shown in graph 200, the resistance of the high resistance state 202 is greater than the resistance of the low resistance state 204. During a read operation, a signal applied to the RRAM device causes an output signal (e.g., a current) having a certain value, which depends on the resistance of the RRAM device. For example, a RRAM device in a low resistance state (e.g., indicating a first data state "1") will cause the output signal to have a different value than a RRAM device in a high resistance state (e.g., indicating a second data state "0"). The read window is the difference between the signal (e.g., current) read out from the RRAM device in the high resistance state and the low resistance state. During operation of a RRAM device (e.g., RRAM device 101 of FIG. 1), it is desirable to maintain a relatively large read window (e.g., defined by the difference 206 between the resistance of the high resistance state 202 and the resistance of the low resistance state 204, between 3-4 orders of magnitude), because a larger read window makes it easier to distinguish different data states during a read operation.

[0033] If the concentration of the dopant within the doped data storage structure 110 is too low (e.g., less than about 1%), the difference 206 between the resistances of the high resistance state 202 and the low resistance state 204 will shrink over time (represented by line 208) and eventually become too small to provide a large enough read window to accurately distinguish between different data states. However, if the concentration of the dopant within the doped data storage structure 110 is between about 1% and about 20%, the difference 206 between the resistances of the high resistance state 202 and the low resistance state 204 of the RRAM device remains substantially constant (e.g., within about 10 cycles) as the number of read and / or write cycles increases (e.g., to more than 10,000 cycles). 3 -10 5 ohms), so that the RRAM device maintains a large enough read window to operate reliably.

[0034] In various embodiments, the doping profiles of dopants within the doped data storage structure may have different profiles. FIG. 3A to FIG. 3B Graphs 300 and 304 are shown showing some exemplary doping profiles of doped data storage structures within the disclosed RRAM device. Graphs 300 and 304 show the position within the doped data storage structure 110 of the RRAM device along the y-axis and the concentration of the dopant within the doped data storage structure 110 along the x-axis. In various embodiments, the concentration of the dopant within the doped data storage structure 110 can be a percentage of oxygen ions that have been replaced by dopant ions, a weight percentage of the dopant, a mole (atomic) percentage of the dopant, etc.

[0035] like Figure 3A Graphics 300 and Figure 3BAs shown in the graph 304 of FIG. 3 , the doped data storage structure 110 has a thickness T. In some embodiments, the thickness T may be in a range between about 1 nm and about 20 nm. In other embodiments, the thickness T may be in a range between about 2 nm and about 20 nm. In other embodiments, the thickness T may be in a range between about 5 nm and about 10 nm.

[0036] In some embodiments, Figure 3A As shown in the graph 300 of FIG. 3 , the doping profile 302 has a non-zero doping concentration that extends continuously over the thickness T. In such an embodiment, the doping profile 302 has a non-zero doping concentration that extends continuously between the top surface and the bottom surface of the doped data storage structure 110. The non-zero doping concentration results from introducing a dopant (e.g., nitrogen, fluorine, carbon, phosphorus, etc.) into a metal oxide (e.g., hafnium oxide, tantalum oxide, zirconium oxide, aluminum oxide, hafnium aluminum oxide, hafnium zirconium oxide, etc.) to form a doped data storage structure 110 having a metal oxynitride, a metal oxyfluoride, a metal oxyphosphorus, etc.

[0037] In some such embodiments, the doped data storage structure 110 may include the same material having a gradient doping concentration extending continuously between the top and bottom surfaces of the doped data storage structure 110. For example, in some embodiments, the doped data storage structure 110 may include hafnium oxynitride, tantalum oxynitride, hafnium oxyfluoride, hafnium oxycarbide, hafnium oxyphosphide, etc. In other embodiments (not shown), the doped data storage structure 110 may include different materials stacked on top of each other to extend between the top and bottom surfaces of the doped data storage structure 110. The different materials together have a gradient doping concentration extending continuously between the top and bottom surfaces of the doped data storage structure 110. For example, the doped data storage structure may include a first doped data storage layer and a second doped data storage layer thereon, the first doped data storage layer being a first material having a first doping concentration (e.g., hafnium oxynitride), and the second doped data storage layer being a second material having a second doping concentration (e.g., tantalum oxynitride).

[0038] In other embodiments, Figure 3BAs shown in the graph 304 of , the doping profile 306 has a non-zero doping concentration extending over a distance less than the thickness T. For example, the doped data storage structure 110 may have a non-zero doping concentration that is separated from the top of the doped data storage structure 110 having a substantially zero doping concentration by a non-zero distance d1. In some such embodiments, the doped data storage structure 110 may include layers having different materials. For example, the doped data storage structure 110 may include a first data storage layer 110a and a second data storage layer 110b, the first data storage layer 110a including a first material (e.g., hafnium oxynitride, tantalum oxynitride, zirconium oxynitride, aluminum oxynitride, hafnium aluminum oxynitride, hafnium zirconium oxynitride, etc.), and the second data storage layer 110b including a second material (e.g., hafnium oxide, tantalum oxide, zirconium oxide, aluminum oxide, hafnium aluminum oxide, hafnium zirconium oxide, etc.).

[0039] like Figure 3A Graphics 300 and Figure 3B As shown in the graph 304, the doping profile 302 of the dopant in the doped data storage structure 110 has a peak dopant concentration C at a position P1 vertically spaced apart from the lower electrode 108 by a second non-zero distance d2. P . In some embodiments, the second non-zero distance d2 is in a range between about 5% and about 40% of the thickness T. For example, in some embodiments, the position P1 is between about 1 angstrom and about 80 angstroms above the bottom of the doped data storage structure 110. Although oxygen vacancies near the upper electrode 116 can be easily moved out of the doped data storage structure 110, oxygen vacancies far from the upper electrode 116 may be more difficult to remove, resulting in excess oxygen vacancies within the data storage structure. Having a peak doping concentration at a position between about 5% and about 40% of the thickness T prevents oxygen vacancies from accumulating at distances that are difficult to remove (e.g., moving to the upper electrode 116), thereby preventing the accumulation of oxygen vacancies within the doped data storage structure 110. In some embodiments, the doped data storage structure 110 has a doping profile that is asymmetric along the thickness of the doped data storage structure 110.

[0040] In some embodiments, the doping profile 302 has a peak doping concentration C in a range between about 1% and about 20%. P (eg, molar percentage of a dopant). In some additional embodiments, the doping concentration has a peak doping concentration C in a range between about 1% and about 10%. PHaving a doping concentration greater than about 20% may reduce the number of oxygen vacancies present in the doped data storage structure 110, thereby making it difficult to form a conductive filament within the doped data storage structure 110. Alternatively, a doping concentration less than about 1% may not sufficiently mitigate the increase of excess oxygen vacancies within the doped data storage structure 110, thereby failing to mitigate degradation of the read window of the RRAM device.

[0041] FIG. 4A to FIG. 4B Cross-sectional views 400 and 402 of some embodiments of RRAM devices during various stages of operation are shown.

[0042] like Figure 4A As shown in the cross-sectional view 400 of FIG. 1 , the RRAM device 101 includes a doped data storage structure 110 disposed between a lower electrode 108 and an upper electrode 116. In a low resistance state (e.g., storing a first data state "1"), a conductive filament 402 extends through the doped data storage structure 110 of the RRAM device 101 by a distance d L , the distance d L The conductive filament 402 includes a plurality of oxygen vacancies 404 that collectively define the conductive filament 402. As shown in graph 406, the conductive filament 402 extends vertically through the peak doping concentration C of the doped data storage structure 110. P In some embodiments, the width of the conductive filament 402 decreases between the upper electrode 116 and the lower electrode 108 .

[0043] Figure 4B The cross-sectional view 408 shows the RRAM device 101 in a high resistance state. In the high resistance state (eg, storing the second data state "0"), the portion of the conductive filament 410 extends within the doped data storage structure 110 by a distance d H (d H <d L ≈T). As shown in graph 412, the portion of the conductive filament 410 extends through the doped data storage structure 110 to a position vertically located between the upper electrode 116 and the peak doping concentration C P In other words, the portion of the conductive filament 410 does not vertically extend through the peak doping concentration C of the doped data storage structure 110. P This is because the peak doping concentration C P The result is that a large number of oxygen-dopant bonds have relatively high binding energies (eg, greater than the binding energy of oxygen-oxygen bonds). The relatively high binding energy mitigates the number of excess oxygen vacancies within the lower portion of the doped data storage structure 110 .

[0044] Figure 5Some additional embodiments of an integrated chip 500 having a RRAM device (with a doped data storage structure) are shown.

[0045] The integrated chip 500 includes a RRAM device 501 disposed within an interlayer dielectric (ILD) structure 104 disposed above a substrate 102. In some embodiments, the ILD structure 104 includes a plurality of stacked interlayer dielectric (ILD) layers 504a-504e. The plurality of stacked ILD layers 504a-504e include one or more lower ILD layers 504a-504d, the one or more lower ILD layers 504a-504d laterally surrounding one or more lower interconnect layers 503, the lower interconnect layers 503 including conductive contacts 506, interconnect lines 508, and interconnect vias 510. In some embodiments, the plurality of stacked ILD layers 504a-504e may include one or more of silicon dioxide, SiCOH, fluorosilicate glass, phosphate glass (e.g., borophosphosilicate glass), and the like. In some embodiments, the one or more lower interconnect layers 503 may include a conductive metal, such as copper, aluminum, and / or tungsten, for example. In some embodiments, two or more adjacent layers of the plurality of stacked ILD layers 504 a - 504 e may be separated by an etch stop layer (not shown) including nitride, carbide, or the like.

[0046] The one or more lower interconnect layers 503 are configured to connect the RRAM device 501 to an access device 502 disposed within the substrate 102. In some embodiments, the access device 502 may include a MOSFET device having a gate structure 502c disposed laterally between a source region 502a and a drain region 502b. In some embodiments, the gate structure 502c may include a gate electrode separated from the substrate 102 by a gate dielectric. In some such embodiments, the source region 502a is connected to a source line SL, and the gate structure 502c is connected to a word line WL. In other embodiments, the access device 502 may include a HEMT, a BJT, a JFET, etc.

[0047] The lower insulating layer 512 is over the one or more lower ILD layers 504a-504d and includes sidewalls defining an opening extending through the lower insulating layer 512. In various embodiments, the lower insulating layer 512 may include silicon nitride, silicon dioxide, silicon carbide, or the like.

[0048] The RRAM device 501 is disposed between sidewalls of the lower insulating layer 512 and over the lower insulating layer 512. In some embodiments, the RRAM device 501 includes a lower electrode 108 separated from an upper electrode 116 by a doped data storage structure 110. In some embodiments, the lower electrode 108 and the upper electrode 116 may include a metal such as tantalum, titanium, tantalum nitride, titanium nitride, platinum, nickel, hafnium, zirconium, ruthenium, iridium, etc. In some embodiments, the lower electrode 108 may include a diffusion barrier layer (e.g., tantalum nitride) and an overlying metal (e.g., titanium).

[0049] In some embodiments, the doped data storage structure 110 may include a first data storage layer 110a having a non-zero doping concentration and a second data storage layer 110b having a substantially zero doping concentration. In some embodiments, the first data storage layer 110a may have an upper surface that is completely covered by the second data storage layer 110b. In some additional embodiments, the second data storage layer 110b may have a smaller thickness laterally outside the upper electrode 116 than directly below the upper electrode 116.

[0050] In some embodiments, the capping layer 514 is disposed between the doped data storage structure 110 and the upper electrode 116. The capping layer 514 is configured to store oxygen, which can promote resistance changes within the doped data storage structure 110. In some embodiments, the capping layer 514 can include a metal such as titanium, tantalum, hafnium, platinum, aluminum, etc. In other embodiments, the capping layer 514 can include a metal nitride such as titanium nitride, tantalum nitride, etc. In other embodiments, the capping layer 514 can include a metal oxide such as titanium oxide, hafnium oxide, zirconium oxide, germanium oxide, cesium oxide, etc. In some optional embodiments, the capping layer 514 can be disposed between the lower electrode 108 and the doped data storage structure 110. In such embodiments, the doped data storage structure 110 can have a peak doping concentration that is closer to the top of the doped data storage structure 110 than to the bottom of the doped data storage structure 110.

[0051] In some embodiments, a masking layer 516 may be disposed over the upper electrode 116. In some embodiments, the masking layer 516 may include silicon oxynitride, silicon dioxide, plasma-enhanced silicon nitride, and the like. In some embodiments, a sidewall spacer 518 may be disposed along the sidewalls of the capping layer 514 and the upper electrode 116. In some embodiments, the sidewall spacer 518 may include an oxide (e.g., a silicon-rich oxide), a nitride (e.g., silicon nitride), a carbide (e.g., silicon carbide), and the like. In some embodiments, the sidewall spacer 518 may be the same material as the masking layer 516, such that the same material continuously extends along the sidewalls and upper surface of the upper electrode 116. The sidewall spacer 518 and the masking layer 516 are disposed between the RRAM device 501 and the upper ILD layer 504e of the plurality of stacked ILD layers 504a-504e.

[0052] In some embodiments, the upper interconnect structure 519 is connected to the upper electrode 116. In some embodiments, the upper interconnect structure 519 may include a top electrode via 520 and an upper interconnect line 522 located above the top electrode via 520. The top electrode via 520 extends through the masking layer 516 to contact the upper electrode 116. In some embodiments, the top electrode via 520 and / or the upper interconnect line 522 may include aluminum, copper, tungsten, etc. In some embodiments, the upper interconnect line 522 is further connected to the bit line BL.

[0053] Figure 6 Some alternative embodiments of an integrated chip 600 having a RRAM device (with a doped data storage structure) are shown.

[0054] The integrated chip 600 includes a RRAM device 601 having a lower electrode 108 separated from an upper electrode 116 by a doped data storage structure 110 and a capping layer 514. The lower electrode 108, the doped data storage structure 110, the capping layer 514, and the upper electrode 116 each have an inner region 602 laterally surrounded by an outer region 604. The layers within the inner region 602 each have a recessed upper surface that is laterally disposed between upper surfaces of corresponding layers within the outer region 604 and vertically below upper surfaces of corresponding layers within the outer region 604. For example, the doped data storage structure 110 has an upper surface within the inner region 602 that is laterally disposed between upper surfaces of doped data storage structures 110 within the outer region 604 and vertically below upper surfaces of doped data storage structures 110 within the outer region 604. In some embodiments, when viewed in a top view of the RRAM device 601 , the outer region 604 may extend continuously around the inner region 602 in an uninterrupted ring.

[0055] In some embodiments, the lower electrode 108, the doped data storage structure 110, the capping layer 514, and the upper electrode 116 can each have substantially equal thicknesses between the outermost walls. In some alternative embodiments, the inner region 602 of the doped data storage structure 110 can have a first thickness, and the outer region 604 of the doped data storage structure 110 can have a second thickness that is less than the first thickness.

[0056] Figures 7 to 17 Some embodiments of cross-sectional views 700-1700 are shown, illustrating a method of forming an integrated chip including an RRAM device having a doped data storage structure. Figures 7 to 17 , but it should be understood that Figures 7 to 17 The structure disclosed in is not limited to this method, but can be independently used as a structure independent of this method.

[0057] like Figure 7 As shown in the cross-sectional view 700 of , an access device 502 is formed in the substrate 102. In various embodiments, the substrate 102 can be any type of semiconductor body (e.g., silicon, SiGe, SOI, etc.), such as a semiconductor wafer and / or one or more dies located on the wafer and any other type of semiconductor and / or epitaxial layer associated therewith. In some embodiments, the access device 502 may include a transistor formed by depositing a gate dielectric film and a gate electrode film over the substrate 102. The gate dielectric film and the gate electrode film are then patterned to form a gate structure 502c having a gate dielectric 502d and a gate electrode 502e. The substrate 102 may then be implanted to form a source region 502a and a drain region 502b in the substrate 102 on opposite sides of the gate structure 502c.

[0058] like Figure 8 As shown in the cross-sectional view 800 of FIG. 1 , one or more lower interconnect layers 503 are formed in one or more lower interlayer dielectric (ILD) layers 504a-504b above the substrate 102. In some embodiments, the one or more lower interconnect layers 503 may include conductive contacts 506 and interconnect lines 508. The one or more lower interconnect layers 503 may be formed by forming one of the one or more lower ILD layers 504a-504b above the substrate 102, selectively etching the ILD layer (e.g., oxide, low-k dielectric, or ultra-low-k dielectric) to define vias and / or trenches in the ILD layer, forming a conductive material (e.g., copper, aluminum, etc.) in the vias and / or trenches, and performing a planarization process (e.g., a chemical mechanical planarization process).

[0059] like Fig. 9As shown in the cross-sectional view 900 of FIG. 1 , a lower insulating layer 902 is formed on one or more lower interconnect layers 503 and one or more lower ILD layers 504a-504b. In some embodiments, the lower insulating layer 902 may include silicon nitride, silicon carbide, or a similar composite dielectric film. In some embodiments, the lower insulating layer 902 may be formed by a deposition technique (e.g., physical vapor deposition (PVD), chemical vapor deposition (CVD), PE-CVD, atomic layer deposition (ALD), etc.) to a thickness in the range of about 200 angstroms to about 300 angstroms.

[0060] like Fig.10 As shown in the cross-sectional view 1000, in the lower insulating layer ( Fig. 9 A first masking layer 1002 is formed on the top of 902. Then, a lower insulating layer ( Fig. 9 The first etchant 1004 defines an opening 1006 in the lower insulating layer 512 , and the opening 1006 extends through the lower insulating layer 512 to the one or more lower interconnect layers 503 .

[0061] like Fig.11 As shown in the cross-sectional view 1100 of FIG. 1100 , a lower electrode structure 1102 is formed over one or more lower interconnect layers 503 and a lower insulating layer 512. In some embodiments, the lower electrode structure 1102 is formed by depositing one or more lower electrode films 1104-1106. For example, the lower electrode structure 1102 can be formed by depositing a first lower electrode film 1104 and then depositing a second lower electrode film 1106 over the first lower electrode film 1104. The first lower electrode film 1104 extends from within the opening 1006 to a position above the lower insulating layer 512. In some embodiments, the first lower electrode film 1104 can include tantalum nitride, titanium nitride, etc. A planarization process (e.g., a chemical mechanical planarization process) can then be performed. In some embodiments, the planarization process produces a first lower electrode film 1104 having a thickness in a range between about 100 angstroms and about 300 angstroms over the lower insulating layer 512. The second lower electrode film 1106 is formed over the first lower electrode 1104. In some embodiments, the second lower electrode film 1106 may include tantalum, titanium, etc. In some embodiments, the second lower electrode film 1106 may be formed to a thickness in a range between about 100 angstroms and about 200 angstroms.

[0062] FIG. 12A to FIG. 12D A cross-sectional view is shown illustrating some embodiments of forming a doped data storage element 1220 . FIG. 12A to FIG. 12D The doped data storage element 1220 is formed by a deposition process followed by a separate doping process. FIG. 12A to FIG. 12DThe formation of a doped data storage element 1220 including two data storage layers is shown, but it should be understood that a greater number of data storage layers (e.g., 10, 100, 1000, etc.) may be formed within the doped data storage element 1220. For example, in some embodiments, the doped data storage element 1220 may be repeated. FIG. 12A to FIG. 12B to form a plurality of doped data storage layers (eg, a first doped data storage layer having a first doping concentration and a second doped data storage layer having a second doping concentration greater than the first doping concentration), followed by Fig. 12C and / or Fig.12D to form one or more undoped data storage layers and / or one or more doped data storage layers (eg, having a third doping concentration less than the second doping concentration).

[0063] like Fig. 12A As shown in the cross-sectional view 1200 of , a first undoped data storage layer 1202 is formed above the lower electrode structure 1102. In some embodiments, the first undoped data storage layer 1202 can be formed by a first ALD cycle, which sequentially alternates pulses of gaseous chemical precursors. For example, during the first ALD cycle, a precursor (e.g., tetrakis(ethylmethylamino)hafnium (TEMAHf), hafnium dioxide, hafnium tetrachloride, zirconium tetrachloride, tantalum-based precursors, etc.) is provided to the processing chamber under vacuum. Subsequently, the processing chamber is purged with an inert carrier gas (e.g., nitrogen, argon, etc.) to remove any unreacted precursors or reaction byproducts. A relative reactant precursor (e.g., oxygen, water, etc.) is then introduced into the processing chamber to form the first undoped data storage layer 1202. Subsequently, the processing chamber is purged with an inert carrier gas (e.g., nitrogen, argon, etc.).

[0064] like Fig. 12B As shown in the cross-sectional view 1204 of FIG. 1 , the first undoped data storage layer (eg, Fig. 12A 1202) to form a first doped data storage layer 1208 having a first dopant concentration. In some embodiments, the first undoped data storage layer 1202 may be doped by a plasma treatment. For example, the first undoped data storage layer 1202 may be exposed to a nitrogen-containing plasma (e.g., N2 plasma). In other embodiments, the first undoped data storage layer 1202 may be doped by a diffusion doping process. For example, the first undoped data storage layer 1202 may be exposed to nitrogen at an elevated temperature (e.g., greater than 100°C). In other embodiments, the first undoped data storage layer 1202 may be doped by an optional method such as an implantation process.

[0065] In some embodiments, the first undoped data storage layer 1202 may be formed and doped in situ (e.g., without breaking vacuum between the formation and doping of the first undoped data storage layer 1202). In some such embodiments, the first undoped data storage layer 1202 may be formed and doped within the same processing chamber. In other such embodiments, the first undoped data storage layer 1202 may be formed within a first processing chamber and doped within a second processing chamber. In other embodiments, the first undoped data storage layer 1202 may be formed and doped ex situ (e.g., with breaking vacuum between the formation and doping of the first undoped data storage layer 1202).

[0066] like Fig. 12C As shown in the cross-sectional view 1210 of FIG. 1 , a second undoped data storage layer 1212 is formed above the first doped data storage layer 1208. The second undoped data storage layer 1212 can be formed by a second ALD cycle that sequentially alternates pulses of gaseous chemical precursors. In some embodiments, the second ALD cycle can be performed by the same process as the first ALD cycle (with respect to FIG. 1 ). Fig. 12A In some embodiments, the second undoped data storage layer 1212 can be formed in-situ with the first doped data storage layer 1208 .

[0067] like Fig.12D As shown in the cross-sectional view 1214 of FIG. 1 , in some embodiments, the second undoped data storage layer ( FIG. 1 ) is doped by exposing the second undoped data storage layer to a dopant 1216. Fig. 12C 1212) to form a second data storage layer 1218 having a non-zero doping concentration and define a doped data storage element 1220. In various embodiments, the second undoped data storage layer 1212 may be doped by a plasma treatment, a thermal annealing process, an implantation process, or the like. In some embodiments, the second undoped data storage layer 1212 is doped to a second doping concentration that is different from (e.g., greater than or less than) the first doping concentration. In some embodiments, the first and second doping concentrations may be discrete (e.g., discontinuous) at the interface between the first doped data storage layer 1208 and the second data storage layer 1218, while in other embodiments, the first and second doping concentrations may be continuous at the interface. In some embodiments, the second undoped data storage layer 1212 may be formed and doped in situ. In some embodiments, due to the doping of the second undoped data storage layer, the doping concentration of the first doped data storage layer 1208 along the upper surface may be greater than the doping concentration along the lower surface.

[0068] In other embodiments, the second undoped data storage layer ( Fig. 12C1212) doping (for example, so that the capping film is directly formed on Fig. 12C In such an embodiment, the doped data storage element 1220 may have a doping profile having a substantially zero doping concentration that extends continuously from the top of the doped data storage element 1220 to the top surface of the first doped data storage layer 1208.

[0069] FIG. 13A to FIG. 13D Cross-sectional views are shown illustrating some alternative embodiments for forming a doped data storage element 1220 . FIG. 13A to FIG. 13D The doped data storage element 1220 is formed by an atomic layer deposition (ALD) process including a dopant. FIG. 13A to FIG. 13D The formation of two data storage layers is shown, but it should be understood that a greater number of data storage layers (e.g., 10, 100, 1000, etc.) may be formed within the doped data storage element 1220. FIG. 13A to FIG. 13D The doped data storage element 1220 is described as being formed using an ALD process, but in other embodiments, the doped data storage element 1220 may be formed using an alternative deposition process (eg, CVD, PVD, etc.).

[0070] like Fig.13A As shown in the cross-sectional view 1300 of FIG. 1 , a first monolayer 1302 is formed over the lower electrode structure 1102. In some embodiments, the first monolayer 1302 can be formed by introducing a precursor gas 1301 into a vacuum processing chamber. In some embodiments, the precursor gas 1301 can include tetrakis(ethylmethylamino)hafnium (TEMAHf), hafnium dioxide, hafnium tetrachloride, zirconium tetrachloride, tantalum-based precursors, etc. Subsequently, the processing chamber is purged with an inert carrier gas (e.g., nitrogen, argon, etc.) to remove any byproducts of the precursor gas 1301.

[0071] like Fig. 13B As shown in the cross-sectional view 1304 of FIG. 1 , a second monolayer 1306 is formed over the first monolayer 1302 to form a first doped data storage layer 1208. In some embodiments, the second monolayer 1306 may be formed by introducing a relative reactant precursor gas 1305 containing a dopant into the process chamber. In some embodiments, the relative reactant precursor gas 1305 containing a dopant may contain ammonium (NH4), ammonium nitride dissolved in water, ammonium hydroxide, etc. Molecules of the relative reactant precursor gas 1305 containing a dopant interact with the first monolayer 1302 to form a first doped data storage layer 1208 having a first dopant concentration.

[0072] like Fig. 13CAs shown in the cross-sectional view 1308 of FIG. 1 , a third monolayer 1310 is formed over the first doped data storage layer 1208. The third monolayer 1310 may be formed by introducing a precursor gas 1301 into a vacuum processing chamber. In some embodiments, the precursor gas 1301 may include tetrakis(ethylmethylamino)hafnium (TEMAHf), hafnium dioxide, hafnium tetrachloride, a tantalum-based precursor, and the like. Subsequently, the processing chamber is purged with an inert carrier gas (e.g., nitrogen, argon, etc.) to remove any unreacted precursors or reaction byproducts.

[0073] like Fig.13D As shown in the cross-sectional view 1312 of FIG. 1314 , in some embodiments, a fourth monolayer 1314 is formed over the third monolayer 1310. The molecules of the fourth monolayer 1314 interact with the third monolayer 1310 to form the second data storage layer 1218 and define the doped data storage element 1220. In some embodiments, the fourth monolayer 1314 can be formed by introducing a relative reactant precursor gas 1313 containing a dopant into the processing chamber so that the second data storage layer 1218 has a non-zero doping concentration. In some such embodiments, the relative reactant precursor gas 1305 containing a dopant can include ammonium (NH4), ammonium nitride dissolved in water, ammonium hydroxide, and the like. In other embodiments, the fourth monolayer 1314 can be formed by introducing a relative reactant precursor gas without a dopant into the processing chamber so that the second data storage layer 1218 has a doping concentration that is substantially zero. In some such embodiments, the relative reactant precursor gas can include oxygen, water, and the like.

[0074] like Fig.14 As shown in the cross-sectional view 1400 of FIG. 1400 , in some embodiments, a capping film 1402 may be formed over the doped data storage element 1220. In various embodiments, the capping film 1402 may include titanium, tantalum, titanium nitride, tantalum nitride, hafnium, aluminum, or a similar material. In some optional embodiments, the capping film 1402 may be formed before forming the doped data storage element 1220, so that the capping film 1402 is located between the lower electrode structure 1102 and the doped data storage element 1220. In some embodiments, the capping film 1402 may be formed by a deposition technique (e.g., PVD, CVD, PE-CVD, sputtering, ALD, etc.).

[0075] An upper electrode structure 1404 is then formed over the capping film 1402. In some embodiments, the upper electrode structure 1404 may include a metal such as titanium, tantalum, etc. In some embodiments, the upper electrode structure 1404 may be formed by a deposition technique (e.g., PVD, CVD, PE-CVD, sputtering, ALD, etc.).

[0076] like FIG. 15A to FIG. 15EAs shown, one or more patterning processes are performed to define the RRAM device 501 .

[0077] like Fig.15A As shown in the cross-sectional view 1500 of , a masking layer 516 is formed over the upper electrode structure 1404. In some embodiments, the masking layer 516 may include nitride, carbide, etc. In some embodiments, the masking layer 516 may be formed by a deposition process (e.g., CVD, PVD, PE-CVD, ALD, etc.) and a subsequent photolithography patterning process.

[0078] like Fig. 15B As shown in the cross-sectional view 1502, the upper electrode structure ( Fig.15A 1404) and covering film ( Fig.15A 1402) is exposed to one or more etchants 1504. The one or more etchants 1504 are configured to selectively remove the upper electrode structure ( Fig.15A The upper electrode 116 is defined by the unmasked portion of the 1404) and by selectively removing the cover film ( Fig.15A 1402) to further define the capping layer 514. In some embodiments, one or more etchants 1504 may also remove doped data storage elements ( Fig.14 1220) and / or the lower electrode structure ( Fig.14 In various embodiments, the one or more etchants 1504 may include a dry etchant having an etching chemistry and / or a wet etchant including hydrofluoric acid (HF), KOH, etc., wherein the etching chemistry includes chlorine and / or fluorine species (e.g., CF4, CHF3, C4F8, etc.).

[0079] like Fig. 15C As shown in the cross-sectional view 1506 of FIG. 1 , a spacer layer 1508 is formed over the substrate 102. In some embodiments, the spacer layer 1508 covers the upper surfaces of the data storage element 1220 and the masking layer 516. In some such embodiments, the spacer layer 1508 may further cover the sidewalls of the capping layer 514, the upper electrode 116, and the masking layer 516. In some embodiments, the spacer layer 1508 may include an oxide, a nitride, a carbide, etc. In some embodiments, the spacer layer 1508 may include the same material as the masking layer 516. In some embodiments, the spacer layer 1508 may be formed by a deposition process (e.g., CVD, PVD, PE-CVD, etc.).

[0080] like Fig.15D As shown in the cross-sectional view 1510, the spacer layer ( Fig. 15C 1508) is exposed to one or more etchants 1512. The one or more etchants 1512 remove the spacer layer ( Fig. 15C 1508), leaving a spacer layer ( Fig. 15C 1508) as sidewall spacers 518. In various embodiments, the one or more etchants 1512 may include a dry etchant and / or a wet etchant.

[0081] like Fig.15E As shown in the cross-sectional view 1514, the data storage structure ( Fig.15D 1220) and / or the lower electrode structure ( Fig.15D 1102) is selectively exposed to one or more etchants 1516. The one or more etchants are configured to define the data storage structure 110 and / or the lower electrode 108 of the RRAM device 501. In some embodiments, the data storage structure ( Fig.15D 1220) and / or the lower electrode structure ( Fig.15D 1102). In various embodiments, the one or more etchants 1516 may include a dry etchant and / or a wet etchant.

[0082] like Fig.16 As shown in the cross-sectional view 1600 of FIG. 1 , an encapsulation layer 1602 may be formed over the RRAM device 501 and the lower insulating layer 512. An upper interlayer dielectric (ILD) layer 1604 is then formed over the encapsulation layer 1602. The encapsulation layer 1602 has a first side adjacent to the lower electrode 108, the doped data storage structure 110, and the sidewall spacer 518, and a second side adjacent to the upper ILD layer 1604. In some embodiments, the encapsulation layer 1602 may include nitride, carbide, oxide, etc.

[0083] like Fig.17 As shown in the cross-sectional view 1700 of FIG. 17 , an upper interconnect structure 519 is formed in the upper ILD layer 504e. The upper interconnect structure 519 extends through the upper ILD layer 504d to a position adjacent to the upper electrode 116. In some embodiments, the upper interconnect structure 519 includes a top electrode via 520 and an upper interconnect line 522. In some embodiments, the upper interconnect structure 519 can be formed by etching the upper ILD layer 504e to form an opening extending through the encapsulation layer 1602 and the masking layer 516 to the upper electrode 116. The opening is then filled with a metal (e.g., copper and / or aluminum) to form a top electrode via 520 and an upper interconnect line 522.

[0084] Fig.18 A flow chart of some embodiments of a method 1800 of forming an integrated chip including a RRAM device having a doped data storage structure is shown.

[0085] Although method 1800 is shown and described as a series of steps or events below, it should be understood that the order of showing such steps or events should not be interpreted in a restrictive sense. For example, some steps can occur in different orders and / or occur simultaneously with other steps or events except those steps or events illustrated and / or described herein. In addition, all the steps shown may not be required to realize one or more aspects or embodiments described herein. In addition, one or more steps described herein can be performed in one or more separate steps and / or stages.

[0086] In step 1802, access devices are formed within a substrate. Figure 7 Some embodiments of the cross-sectional view 700 corresponding to step 1802 are shown.

[0087] In step 1804, one or more lower interconnect layers 503 are formed within one or more lower inter-layer dielectric (ILD) layers. Figure 8 Some embodiments of the cross-sectional view 800 corresponding to step 1804 are shown.

[0088] In step 1806 , a lower insulating structure is formed over the one or more lower interconnect layers and the one or more lower ILD layers. Figures 9 and 10 Some embodiments of cross-sectional views 900 - 1000 corresponding to step 1806 are shown.

[0089] In step 1808, a lower electrode structure is formed over the one or more lower interconnect layers and the lower insulating structure. Fig.11 Some embodiments of the cross-sectional view 1100 corresponding to step 1808 are shown.

[0090] In step 1810, a doped data storage element is formed over the lower electrode structure. The doped data storage element may be formed by a multi-step process to include multiple data storage layers each having a different concentration of a dopant, so that the doped data storage element has a dopant concentration that varies with distance from the lower electrode structure. FIG. 12A to FIG. 12D Some embodiments of cross-sectional views corresponding to step 1810 are shown. FIG. 13A to FIG. 13D Some alternative embodiments corresponding to cross-sectional views of step 1810 are shown.

[0091] At step 1812, in some embodiments, a capping film is formed over the doped data storage element. Fig.14 Some embodiments of the cross-sectional view 1400 corresponding to step 1812 are shown.

[0092] In step 1814, an upper electrode structure is formed over the capping film. Fig.14 Some embodiments of the cross-sectional view 1400 corresponding to step 1814 are shown.

[0093] In step 1816 , one or more patterning processes are performed to define the RRAM device. FIG. 15 illustrates some embodiments of a cross-sectional view 1500 corresponding to step 1818 .

[0094] In step 1818 , an upper ILD layer is formed over the RRAM device. Fig.16 Some embodiments of cross-sectional view 1600 corresponding to step 1818 are shown.

[0095] In step 1820, an upper interconnect structure is formed on the RRAM device. Fig.17 Some embodiments of the cross-sectional view 1700 corresponding to step 1820 are shown.

[0096] Fig.19 A block diagram illustrating some embodiments of a processing tool 1900 configured to form a doped data storage structure of a disclosed RRAM device is shown.

[0097] The processing tool 1900 includes a transfer chamber 1902 connected to a first process chamber 1906, a second process chamber 1914, and a load port 1920. In some embodiments, the transfer chamber 1902 may be connected to the first process chamber 1906 through a first door 1912a, to the second process chamber 1914 through a second door 1912b, and to the load port 1920 through a third door 1912c. The transfer chamber 1902 includes a wafer transfer robot 1904. In some embodiments, the wafer transfer robot 1904 may include a robot arm 1904a connected to a wafer blade 1904b configured to hold a wafer.

[0098] The first wafer chuck 1908 is disposed in the first process chamber 1906. In some embodiments, the first wafer chuck 1908 may include a vacuum chuck. An ALD gas source 1910 is connected to the first process chamber 1906. The ALD gas source 1910 is configured to provide a precursor gas and a relative reactant precursor to the first process chamber 1906. In some embodiments, the ALD gas source 1910 may include a first gas source 1910a and a second gas source 1910c, the first gas source 1910a being selectively connected to the first process chamber 1906 through a first valve 1910b, and the second gas source 1910c being selectively connected to the first process chamber 1906 through a second valve 1910d. In some embodiments, the first gas source 1910a may include a first temperature controlled bath, and the second gas source 1910c may include a second temperature controlled bath. In some embodiments, the ALD gas source 1910 may also include a plasma source (not shown) configured to enhance the speed of the ALD process deposition.

[0099] The second wafer chuck 1916 is disposed within the second process chamber 1914. A dopant source 1918 is connected to the second process chamber 1914 and is configured to provide dopants to the substrate on the second wafer chuck 1916. In some embodiments, the dopant source 1918 may include an ion implantation tool, a vapor deposition tool, a plasma generator, or the like.

[0100] The load port 1920 is configured to receive a carrier 1922 holding one or more substrates. In various embodiments, the carrier 1922 may include a FOUP (front opening unit pod), a wafer box, etc. In some embodiments, the one or more substrates may include semiconductor wafers (e.g., 200 mm wafers, 300 mm wafers, 450 mm wafers, etc.).

[0101] One or more vacuum pumps 1924 are connected to the transfer chamber 1902, the first processing chamber 1906, and / or the second processing chamber 1914. In some embodiments, the one or more vacuum pumps 1924 are configured to maintain a vacuum within the transfer chamber 1902, the first processing chamber 1906, and / or the second processing chamber 1914.

[0102] During operation, the wafer transfer robot 1904 is configured to provide a substrate from the carrier 1922 to the first processing chamber 1906 (along line 1926), wherein a first undoped data storage layer (e.g., Fig. 12A The wafer transfer robot 1904 is then configured to transfer the substrate from the first processing chamber 1906 to the second processing chamber 1914 (along line 1928), wherein the first undoped data storage layer is doped to form a first doped data storage layer (e.g., Fig. 12B The wafer transfer robot 1904 may then transfer the substrate between the first processing chamber 1906 and the second processing chamber 1914 to form a defined doped data storage element (e.g., Fig.12D doped data storage element 1220) of an additional doped data storage layer (e.g., Fig.12D Once formation of the doped data storage element is complete, the wafer transfer robot 1904 transfers the substrate to a carrier 1922 within the transfer chamber 1902 (along line 1930).

[0103] Fig. 20 A block diagram illustrating some alternative embodiments of a processing tool 2000 configured to form a doped data storage structure of the disclosed RRAM device is shown.

[0104] The processing tool 2000 includes a transfer chamber 1902 connected to a first process chamber 1906 and a load port 1920. In some embodiments, the transfer chamber 1902 may be connected to the first process chamber 1906 through a first door 1912a and to the load port 1920 through a second door 1912b. The transfer chamber 1902 includes a wafer transfer robot 1904.

[0105] The first wafer chuck 1908 is disposed in the first process chamber 1906. An ALD gas source 1910 is connected to the first process chamber 1906. The ALD gas source 1910 is configured to provide a precursor gas and a relative reactant precursor to the first process chamber 1906. In some embodiments, the ALD gas source 1910 may include a first gas source 1910a selectively connected to the first process chamber 1906 through a first valve 1910b and a second gas source 1910c selectively connected to the first process chamber 1906 through a second valve 1910d.

[0106] In some embodiments, the second gas source 1910c can be configured to provide a doping gas (e.g., a gas including nitrogen, fluorine, carbon, phosphorus, etc.) to the first processing chamber to form a doped data storage layer above the substrate. In such an embodiment, during operation, the wafer transfer robot 1904 is configured to provide a substrate from the carrier 1922 to the first processing chamber 1906 (along line 2002), wherein a first doped data storage layer (e.g., Fig. 13B The first doped data storage layer 1208) and the additional data storage layer (eg, Fig.13D The second data storage layer 1218) is provided to define a doped data storage element (eg, Fig.13D Once formation of the doped data storage element is complete, the wafer transfer robot 1904 transfers the substrate to a carrier 1922 within the transfer chamber 1902 (along line 2004).

[0107] In some optional embodiments, dopant source 1918 is coupled to first process chamber 1906 and configured to provide dopant to a substrate on first wafer chuck 1908. In such embodiments, during operation, wafer transfer robot 1904 is configured to provide a substrate from carrier 1922 to first process chamber 1906 (along line 2002), wherein a first undoped data storage layer (e.g., Fig. 12A The dopant source 1918 is configured to subsequently dope the first undoped data storage layer to form a first doped data storage layer (eg, Fig. 12B Subsequently, one or more additional data storage layers (e.g., Fig.12DThe second data storage layer 1218) is provided to define a doped data storage element (e.g., Fig.12D doped data storage element 1220).

[0108] Accordingly, the present invention relates to a resistive random access memory (RRAM) device having a doped data storage structure configured to provide good endurance (ie, reliability) to the RRAM device and associated methods of formation.

[0109] In some embodiments, the present invention relates to a method for forming a resistive random access memory (RRAM) device. The method includes forming a first electrode structure above a substrate; forming a doped data storage element above the first electrode structure by forming a first data storage layer above the first electrode structure, and forming a second data storage layer above the first data storage layer; forming a second electrode structure above the doped data storage element; the first data storage layer is formed as a dopant having a first doping concentration, and the second data storage layer is formed as a dopant having a second doping concentration, the second doping concentration being less than the first doping concentration. In some embodiments, the first data storage layer and the second data storage layer are formed by an atomic layer deposition process. In some embodiments, forming the first data storage layer includes forming a first undoped data storage layer above the first electrode structure; and doping the first undoped data storage layer with a dopant to form a first data storage layer having the first doping concentration. In some embodiments, forming the doped data storage element also includes forming a second undoped data storage layer above the first data storage layer; doping the second undoped data storage layer to form a second data storage layer having a second doping concentration; and forming a third data storage layer above the second data storage layer, the third doping concentration of the third data storage layer being less than the second doping concentration. In some embodiments, the second data storage layer has a non-zero doping concentration. In some embodiments, the second data storage layer is formed in situ with the first data storage layer. In some embodiments, the second data storage layer is formed to have a doping concentration that is substantially zero. In some embodiments, the dopant includes nitrogen, fluorine, carbon, or phosphorus. In some embodiments, the doped data storage element is formed to a certain thickness; and the doped data storage element has a peak dopant concentration at a distance in a range between about 5% and about 40% of the thickness separated from the first electrode structure. In some embodiments, the doped data storage element has a peak dopant concentration between about 1% and about 20%.

[0110] In other embodiments, the present invention relates to a method of forming a resistive random access memory (RRAM) device. The method includes forming a lower electrode structure above a conductive interconnect layer disposed above a substrate; forming a doped data storage element having a plurality of data storage layers above the lower electrode structure, the plurality of data storage layers being formed to have different concentrations of dopants; and forming an upper electrode structure above the doped data storage element. In some embodiments, the dopant is configured to form a bond with oxygen with a binding energy greater than about 500 kJ / mol. In some embodiments, the doped data storage element has a thickness; and the dopant has a peak dopant concentration at a distance in a range between about 5% and about 40% of the thickness separated from the lower electrode structure. In some embodiments, the doped data storage element has a doping profile having a non-zero doping concentration extending continuously from a bottom surface of the doped data storage element to a top surface of the doped data storage element. In some embodiments, the doped data storage element has a doping profile having a substantially zero doping concentration extending continuously from a top surface of the doped data storage element to a position separated from a bottom surface of the doped data storage element by a non-zero distance. In some embodiments, the doped data storage element has a doping profile that is asymmetric along the thickness of the doped data storage element.

[0111] In other embodiments, the present invention relates to a resistive random access memory (RRAM) device. The RRAM device includes: a first electrode located above a conductive lower interconnect layer; a second electrode located above the first electrode; and a doped data storage structure disposed between the first electrode and the second electrode and having a variable resistance, the doped data storage structure having a dopant having a doping concentration with a non-uniform doping profile along the height of the doped data storage structure. In some embodiments, the dopant includes nitrogen, fluorine, carbon, or phosphorus. In some embodiments, the dopant has a peak dopant concentration at a distance in the range between about 5% and about 40% of the height of the doped data storage structure separated from the first electrode. In some embodiments, the doped data storage structure has a peak dopant concentration between about 1% and about 10%.

[0112] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that this equivalent configuration does not deviate from the spirit and scope of the present invention, and that they can make multiple changes, substitutions and changes herein without deviating from the spirit and scope of the present invention.

Claims

1. A method of forming a resistive random access memory (RRAM) device, comprising: forming a first electrode structure over the substrate; Forming a doped data storage element above the first electrode structure, wherein forming the doped data storage element comprises: forming a first data storage layer over the first electrode structure, wherein the first data storage layer is formed with a dopant having a first doping concentration; forming a second data storage layer over the first data storage layer, wherein the second data storage layer is formed to have a second doping concentration of the dopant, the second doping concentration being less than the first doping concentration, wherein the first doping concentration continuously increases and then continuously decreases from a top surface of the first electrode structure to a bottom surface of the second data storage layer; and A second electrode structure is formed over the doped data storage element.

2. The method according to claim 1, wherein: The first data storage layer and the second data storage layer are formed by an atomic layer deposition process.

3. The method according to claim 1, wherein: Forming the first data storage layer includes: forming a first undoped data storage layer over the first electrode structure; and The first undoped data storage layer is doped with the dopant to form the first data storage layer having the first doping concentration.

4. The method according to claim 3, wherein: Forming the doped data storage element further comprises: forming a second undoped data storage layer above the first data storage layer; doping the second undoped data storage layer to form the second data storage layer having the second doping concentration; and A third data storage layer is formed above the second data storage layer, wherein a third doping concentration of the third data storage layer is less than the second doping concentration.

5. The method according to claim 1, wherein: The second data storage layer has a non-zero doping concentration.

6. The method according to claim 1, wherein: The second data storage layer is formed in-situ with the first data storage layer.

7. The method according to claim 1, wherein: The second data storage layer is formed to have a doping concentration of zero.

8. The method according to claim 1, wherein: The dopant includes nitrogen, fluorine, carbon or phosphorus.

9. The method according to claim 1, in, The doped data storage element is formed to a certain thickness; and Wherein the doped data storage element has a peak dopant concentration at a distance from the first electrode structure in a range between 5% and 40% of the thickness.

10. The method according to claim 1, wherein: The doped data storage element includes a peak dopant concentration between 1% and 20%.

11. A method of forming a resistive random access memory (RRAM) device, comprising: forming a lower electrode structure over a conductive interconnect layer disposed over a substrate; forming a doped data storage element above the lower electrode structure, wherein the doped data storage element comprises a doped region having a dopant and a non-doped region located on the doped region and having a dopant concentration of zero, the concentration of the dopant comprises turning points at non-zero distances from the top and the bottom of the doped data storage element, the concentration of the dopant varies between a continuous increase and a continuous decrease at the turning points, the bottom surface of the doped region is in direct contact with the top surface of the lower electrode structure, and the doped region is in direct contact with the non-doped region; as well as An upper electrode structure is formed over the doped data storage element.

12. The method according to claim 11, wherein: The dopant is configured to form a bond with oxygen with a binding energy greater than 500 kJ / mol.

13. The method according to claim 11, in, The doped data storage element has a thickness; and The dopant has a peak dopant concentration at a distance from the lower electrode structure that is within a range between 5% and 40% of the thickness.

14. The method according to claim 11, wherein: The doped data storage element has a doping profile having a non-zero doping concentration extending continuously from a bottom surface of the doped data storage element to a top surface of the doped data storage element.

15. The method according to claim 11, wherein: The doped data storage element has a doping profile having a doping concentration of zero extending continuously from a top surface of the doped data storage element to a location spaced apart a non-zero distance from a bottom surface of the doped data storage element.

16. The method according to claim 11, wherein: The doped data storage element has a doping profile that is asymmetric along a thickness of the doped data storage element.

17. A resistive random access memory (RRAM) device comprising: a first electrode disposed over the conductive lower interconnect layer; a second electrode, located above the first electrode; as well as A doped data storage structure is disposed between the first electrode and the second electrode and has a variable resistance, wherein the doped data storage structure comprises: a first data storage layer, the first data storage layer comprising a first dopant having a first doping concentration, the first dopant having a doping concentration of a non-uniform doping profile along a height of the first data storage layer, wherein the doping concentration of the non-uniform doping profile continuously increases and then continuously decreases, a bottom surface of the first data storage layer being in direct contact with a top surface of the first electrode; A second data storage layer is disposed on the first data storage layer and directly contacts the first data storage layer, the second data storage layer having a second dopant with a second doping concentration less than the first doping concentration.

18. The resistance random access memory according to claim 17, wherein: The dopant includes nitrogen, fluorine, carbon or phosphorus.

19. The resistance random access memory according to claim 17, wherein: The dopant has a peak dopant concentration at a distance separated from the first electrode in a range between 5% and 40% of the height of the doped data storage structure.

20. The resistance random access memory according to claim 17, wherein: The doped data storage structure includes a peak dopant concentration between 1% and 10%.

Citation Information

Patent Citations

  • Oxide film scheme for rram structure

    CN106159083A

  • Fabrication of correlated electron material films with varying atomic or molecular concentrations of dopant species

    CN109564969A

  • Shaping ReRAM conductive filaments by controlling grain-boundary density

    US9246085B1