Positive electrode active material and lithium secondary battery including the same

By forming a charge transfer channel in the lithium composite oxide, the concentration gradient interval adjustment of nickel, cobalt and manganese is solved, and the battery life and electrochemistry are improved. performance.

CN112687850BActive Publication Date: 2024-11-22ECOPRO BM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011039521.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-18
Filing Date
2020-09-28
Publication Date
2024-11-22
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

The increase in resistance of high-nickel lithium composite oxides in lithium secondary batteries leads to a decrease in life, and the existing positive electrode active materials have problems of gelation and gas generation during charging and discharging, which affects the cycle stability of the battery.

Method used

By forming a charge transfer channel in the lithium composite oxide, different types of concentration gradient intervals exist on the outer peripheral surface of the secondary particles, the electrochemical characteristics of the positive electrode active material are improved. The specific methods include the concentration gradient intervals of nickel, cobalt and manganese. Adjustments are made to form a charge transfer channel.

Benefits of technology

It effectively reduces the resistance of the positive electrode active material, improves the life and efficiency characteristics, improves the electrochemical performance of lithium secondary batteries, and avoids problems of gelation and gas generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112687850B_ABST
    Figure CN112687850B_ABST
Patent Text Reader

Abstract

A positive electrode active material and a lithium secondary battery including the same. The present invention relates to a positive electrode active material and a lithium secondary battery using a positive electrode including the positive electrode active material. More specifically, the present invention relates to a positive electrode active material that can solve the problem of increased resistance due to increased nickel (Ni) content by forming a charge transfer channel in a lithium composite oxide and a lithium secondary battery using the positive electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material and a lithium secondary battery using a positive electrode including the positive electrode active material. Background Art

[0002] Batteries store electricity using substances that can undergo electrochemical reactions at positive and negative electrodes. A representative example of such batteries is a lithium secondary battery that stores electrical energy by changes in chemical potential during the insertion / extraction of lithium ions at the positive and negative electrodes.

[0003] The lithium secondary battery is manufactured by using a material that can reversibly intercalate or deintercalate lithium ions as a positive electrode active material and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.

[0004] As a positive electrode active material of a lithium secondary battery, a lithium composite oxide has been used, and for example, composite oxides of LiCoO 2 , LiMN 2 O 4 , LiNiO 2 , LiMnO 2 , and the like are being studied.

[0005] Among the above-mentioned positive electrode active materials, although LiCoO 2 having excellent life characteristics and charge and discharge efficiency is widely used, the above-mentioned material has limitations in price competitiveness due to the limited resources of cobalt used as a raw material and high price.

[0006] Although lithium manganese oxides such as LiMnO2 and LiMN2O4 have the advantages of good thermal stability and low price, they have problems such as small capacity and poor high temperature characteristics. In addition, although LiNiO2-based positive electrode active materials have battery characteristics of high discharge capacity, they are very difficult to synthesize due to the cation mixing problem between lithium and transition metals, and there are great problems in rate characteristics.

[0007] In addition, according to the degree of the above-mentioned cation mixing, a large amount of lithium by-products are generated, and since most of the lithium by-products are composed of LiOH and Li2CO3 compounds, there are problems of gelation when manufacturing positive electrode slurry and gas generation during charge and discharge after manufacturing electrodes. Residual Li2CO3 increases the expansion of the battery, not only reducing the cycle, but also causing the battery to expand.

[0008] On the other hand, recently, lithium-based composite oxides compounded with nickel (Ni), cobalt (Co) and manganese (Mn) and / or aluminum (Al) as positive electrode active materials have been developed. Generally, similar to LiNiO2-based positive electrode active materials, the above-mentioned lithium-based composite oxides have the advantages of increased energy density and improved output characteristics as the nickel content increases, but on the other hand, there is a problem of increased resistance characteristics. Therefore, in the lithium-based composite oxide compounded with nickel, cobalt and manganese and / or aluminum, it is necessary to develop a positive electrode active material that can maintain the excellent reversible capacity of LiNiO2 and prevent the resistance characteristics and life characteristics from deteriorating. Summary of the invention

[0009] Technical issues

[0010] In the lithium secondary battery market, the growth of lithium secondary batteries for electric vehicles plays a leading role in the market, and the demand for positive electrode materials used in lithium secondary batteries is also changing.

[0011] For example, conventionally, lithium secondary batteries using LFP have been mainly used from the viewpoint of ensuring safety, but recently, the use of nickel-based lithium composite oxides having a larger energy capacity per unit weight than LFP has been expanding.

[0012] According to this trend of positive electrode materials, the present invention aims to provide a high-nickel lithium composite oxide and / or a positive electrode active material containing the lithium composite oxide for realizing high capacity of a battery for a vehicle. However, in the case of the high-nickel lithium composite oxide known so far, as the nickel content increases, the resistance increases, so there is a problem of reduced life.

[0013] Therefore, an object of the present invention is to provide a lithium composite oxide and / or a positive electrode active material including the same which can solve the problem of resistance increase due to an increase in nickel content by forming a charge transfer path in the lithium composite oxide.

[0014] Furthermore, another object of the present invention is to provide a positive electrode slurry composition comprising the positive electrode active material defined herein.

[0015] In addition, another object of the present invention is to provide a lithium secondary battery comprising a positive electrode, wherein the positive electrode is formed by coating the positive electrode slurry composition defined herein on a current collector.

[0016] The purpose of the present invention is not limited to the purpose mentioned above, and other purposes and advantages of the present invention not mentioned can be understood through the following description, and can be more clearly understood through the embodiments of the present invention. In addition, it can be easily understood that the purpose and advantages of the present invention can be achieved by the means and combinations thereof in the claims.

[0017] Solutions to the problem

[0018] According to one aspect of the present invention, there is provided a positive electrode active material, the positive electrode active material comprising: primary particles capable of absorbing and releasing lithium; and secondary particles formed by agglomeration of the primary particles.

[0019] In which, the above-mentioned secondary particles may include a first concentration gradient interval and a second concentration gradient interval along the outer peripheral surface of the above-mentioned secondary particles, and the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned secondary particles increases in the above-mentioned first concentration gradient interval, and the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned secondary particles decreases in the above-mentioned second concentration gradient interval.

[0020] In one embodiment, the first concentration gradient region and the second concentration gradient region may selectively exist on the surface of the secondary particles.

[0021] Furthermore, the first concentration gradient section and the second concentration gradient section may exist repeatedly along the outer peripheral surface of the secondary particle.

[0022] According to another aspect of the present invention, there is provided a positive electrode slurry composition comprising a positive electrode active material as defined herein, a conductive material and a binder.

[0023] According to another aspect of the present invention, there is provided a lithium secondary battery comprising a positive electrode, wherein the positive electrode is formed by coating the positive electrode slurry composition defined herein on a current collector.

[0024] Effects of the Invention

[0025] The surface portion of the secondary particles of the positive electrode active material of various embodiments of the present invention includes a first concentration gradient interval in which the concentration of at least one selected from nickel, cobalt and manganese is increased and a second concentration gradient interval in which the concentration of at least one selected from nickel, cobalt and manganese is decreased, thereby forming a charge transfer channel in the positive electrode active material.

[0026] As described above, the charge transfer channels formed by the presence of different types of concentration gradient regions can solve the resistance problem of the positive electrode active material caused by the increase in nickel content, thereby helping to improve the electrochemical characteristics of the positive electrode active material, such as the life characteristics and efficiency characteristics.

[0027] Specific matters for implementing the invention will be described below, and specific effects of the present invention and the above-mentioned effects will be described. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The cathode active material according to one embodiment of the present invention and the concentration gradient of the metal elements in the cathode active material are schematically shown.

[0029] Figure 2 A cross-sectional SEM image of a portion (surface portion) of a positive electrode active material (secondary particle) according to an example of the present invention is shown.

[0030] Figures 3 to 5 Show Figure 2 A line sum spectrum of the content of metal elements (nickel, cobalt and manganese) present in a part (surface portion) of the positive electrode active material (secondary particle) shown in FIG. 1 along a direction (lateral) perpendicular to the direction (longitudinal) from the center portion of the secondary particle toward the surface portion of the secondary particle.

[0031] Figure 6 This is a cross-sectional SEM image of a portion (surface portion) of a positive electrode active material (secondary particle) according to another example of the present invention.

[0032] Figures 7 to 9 Show Figure 6 A line sum spectrum of the content of metal elements (nickel, cobalt and manganese) present in a part (surface portion) of the positive electrode active material (secondary particle) shown in FIG. 1 along a direction (lateral) perpendicular to the direction (longitudinal) from the center portion of the secondary particle toward the surface portion of the secondary particle.

[0033] Fig.10 This is a cross-sectional SEM image of a portion (surface portion) of a positive electrode active material (secondary particle) according to still another example of the present invention.

[0034] Figures 11 to 13 Show Fig.10 The distribution of metal elements (nickel, cobalt, and manganese) is measured by TEM / EDX mapping on a part (surface part) of the positive electrode active material (secondary particles) shown in FIG.

[0035] Fig.14 Show Fig.10 A cross-sectional SEM image of the central portion of the positive electrode active material (secondary particle) shown in FIG.

[0036] Figures 15 to 17 Show Fig.14 The distribution of metal elements (nickel, cobalt, and manganese) in the center of the positive electrode active material (secondary particle) shown in FIG. 5 is measured by TEM / EDX mapping.

[0037] Fig.18 A cross-sectional SEM image of a portion of commercial NCM 811 is shown.

[0038] Figures 19 to 21 Show Fig.18A line sum spectrum of the content of metal elements (nickel, cobalt and manganese) present in a portion of the positive electrode active material (secondary particles) along a direction (lateral) perpendicular to the direction (longitudinal) from the center of the secondary particles toward the surface of the secondary particles.

[0039] Fig. 22 A graph showing EIS measurement results of positive electrode active materials according to examples of the present invention and comparative examples. DETAILED DESCRIPTION

[0040] In order to easily understand the present invention, specific terms are appropriately defined in this application. Unless otherwise defined herein, the scientific terms and technical terms used in the present invention have the meanings commonly understood by those skilled in the art to which the present invention belongs. In addition, unless the context requires otherwise, the terms in the singular form shall include the plural form and the terms in the plural form shall include the singular form.

[0041] Hereinafter, the cathode active material according to the present invention and a lithium secondary battery using a cathode including the cathode active material will be described in further detail.

[0042] Positive electrode active material

[0043] According to one aspect of the present invention, there is provided a positive electrode active material, the positive electrode active material comprising: primary particles capable of absorbing and releasing lithium; and secondary particles formed by agglomeration of the primary particles.

[0044] Here, the primary particle refers to a crystal grain (grain or crystallite), and the secondary particle refers to an aggregate formed by agglomeration of a plurality of primary particles. There may be gaps and / or grain boundaries between the primary particles constituting the secondary particles.

[0045] In which, the above-mentioned secondary particles may include a first concentration gradient interval and a second concentration gradient interval along the outer peripheral surface of the above-mentioned secondary particles, and the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned secondary particles increases in the above-mentioned first concentration gradient interval, and the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned secondary particles decreases in the above-mentioned second concentration gradient interval.

[0046] The above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval as defined herein are terms used to distinguish between regions where the concentration of at least one selected from nickel, cobalt and manganese increases and regions where the concentration decreases, and the concentration gradient intervals need not be interpreted as limited to modified ordinal numbers.

[0047] As described above, the secondary particles contain a first concentration gradient interval and a second concentration gradient interval showing a concentration gradient in which the concentration of at least one selected from nickel, cobalt and manganese increases and decreases continuously or discontinuously, so that a charge transfer channel can be formed in the positive electrode active material. The charge transfer channel formed by making these different types of concentration gradient intervals exist in the secondary particles can solve the resistance problem of the positive electrode active material caused by the increase in nickel content. Thus, it can help to improve the electrochemical characteristics of the positive electrode active material, such as the life characteristics and efficiency characteristics.

[0048] The first concentration gradient interval and the second concentration gradient interval may present a concentration gradient in which the concentration of at least one selected from nickel, cobalt and manganese increases and decreases continuously or discontinuously.

[0049] Thus, the first concentration gradient interval may present a concentration gradient in which the concentration of at least one selected from nickel, cobalt and manganese increases continuously or discontinuously, and the second concentration gradient interval may present a concentration gradient in which the concentration of at least one selected from nickel, cobalt and manganese decreases continuously or discontinuously.

[0050] In the first concentration gradient interval, at least one selected from nickel, cobalt, and manganese may be increased to a concentration higher than an average content of the at least one selected from nickel, cobalt, and manganese in the secondary particles.

[0051] For example, refer to Figure 4 , when the metal element forming the concentration gradient in the first concentration gradient interval a is cobalt, the cobalt in the first concentration gradient interval a can be increased to a concentration higher than the average cobalt content Avg in the secondary particles. In other words, the maximum cobalt content in the first concentration gradient interval a is higher than the average cobalt content Avg in the secondary particles.

[0052] In one embodiment, the metal elements forming the concentration gradient in the first concentration gradient interval and the second concentration gradient interval may be cobalt, cobalt and manganese, or nickel, cobalt and manganese. In this case, nickel in the first concentration gradient interval and the second concentration gradient interval may present a concentration gradient with a tendency opposite to that of cobalt or cobalt and manganese.

[0053] That is, when the concentration gradient of cobalt or cobalt and manganese in the first concentration gradient interval increases continuously or discontinuously, the concentration of nickel in the second concentration gradient interval may decrease continuously or discontinuously. Conversely, when the concentration gradient of cobalt or cobalt and manganese in the second concentration gradient interval decreases continuously or discontinuously, the concentration of nickel in the second concentration gradient interval may increase continuously or discontinuously.

[0054] Furthermore, the concentration increase rate of at least one selected from nickel, cobalt and manganese in the first concentration gradient interval may be equal to or greater than 5 wt% per 0.1 μm, but the present invention is not limited thereto. That is, as long as the concentration selected from at least one selected from nickel, cobalt and manganese (hereinafter referred to as the specific metal element) in the first concentration gradient interval increases toward the average content of the specific metal element in the secondary particles or increases to a concentration higher than the average content.

[0055] Herein, the average content direction may refer to the slope (vector) direction when the concentration of the specific metal element in the secondary particles on the line sum spectrum representing the concentration change of the specific metal element in the secondary particles increases or decreases toward the average content in the secondary particles.

[0056] On the other hand, at least one selected from nickel, cobalt and manganese in the second concentration gradient range may be reduced to a concentration lower than an average content of the at least one selected from nickel, cobalt and manganese in the secondary particles.

[0057] For example, refer to Figure 4 When the metal element forming the concentration gradient in the second concentration gradient interval b is cobalt, the cobalt in the second concentration gradient interval b can decrease toward the average content Avg of cobalt in the secondary particles.

[0058] Among them, the decrease of cobalt in the direction of the average cobalt content Avg in the above-mentioned secondary particles in the above-mentioned second concentration gradient interval b means that when the cobalt content at any point in the above-mentioned second concentration gradient interval b is greater than the average cobalt content Avg in the above-mentioned secondary particles, the cobalt content at any point in the above-mentioned second concentration gradient interval b is reduced to the level of the average cobalt content Avg in the above-mentioned secondary particles.

[0059] Furthermore, the concentration reduction rate of at least one selected from nickel, cobalt and manganese in the first concentration gradient interval may be equal to or greater than 5 wt% per 0.1 μm, but the present invention is not limited thereto. That is, as long as the concentration in the second concentration gradient interval is selected from at least one selected from nickel, cobalt and manganese (hereinafter referred to as the specific metal element) and decreases in the direction of the average content of the specific metal element in the secondary particles, it is sufficient.

[0060] On the other hand, the existence of the first concentration gradient interval and the second concentration gradient interval along the outer peripheral surface of the secondary particle should be understood as a concept different from the existence of a concentration gradient along the direction from the center of the secondary particle to the surface of the secondary particle.

[0061] For example, when the secondary particle is spherical or nearly spherical, the first concentration gradient interval and the second concentration gradient interval may exist along the circumferential direction of the secondary particle.

[0062] Thus, the concentration of at least one selected from nickel, cobalt and manganese in the first concentration gradient interval increases along the direction of the outer peripheral surface of the secondary particles, while the concentration of at least one selected from nickel, cobalt and manganese in the second concentration gradient interval decreases along the direction of the outer peripheral surface of the secondary particles.

[0063] In one embodiment, the secondary particle may include: a central portion, which accounts for 1 volume % to 90 volume % of the total volume of the secondary particle from the center of the secondary particle; and a surface portion surrounding the outside of the central portion.

[0064] At this time, the first concentration gradient region and the second concentration gradient region may selectively exist in the surface portion, or may exist in both the central portion and the surface portion at the same time.

[0065] Since the first concentration gradient interval and the second concentration gradient interval selectively exist in the surface portion, the first concentration gradient interval and the second concentration gradient interval may exist in a manner that reaches a predetermined depth from the surface portion of the secondary particle toward the center portion of the secondary particle.

[0066] That is, the concentration gradient of at least one selected from nickel, cobalt and manganese continuously or discontinuously increasing or decreasing along the peripheral surface of the secondary particle may appear restrictively on the surface of the secondary particle, while the concentration gradient of at least one selected from nickel, cobalt and manganese continuously or discontinuously increasing or decreasing may not appear in the central part of the secondary particle. The charge transfer channel can be effectively formed in the positive electrode active material by restrictively forming the concentration gradient interval as described above.

[0067] Among them, in the secondary particles, the central part and the surface part are terms introduced to explain the existence and position of the first concentration gradient interval and the second concentration gradient interval in the secondary particles, and do not mean that there is a boundary that distinguishes the central part and the surface part in the secondary particles. In other words, the central part and the surface part in the secondary particles can be continuous areas without boundaries.

[0068] In one embodiment, the first concentration gradient zone and the second concentration gradient zone may exist repeatedly along the outer peripheral surface of the secondary particle.

[0069] According to the above embodiment, while the first concentration gradient section and the second concentration gradient section are repeatedly present along the outer peripheral surface of the secondary particle, the first concentration gradient section and the second concentration gradient section may be alternately formed.

[0070] Therefore, the concentration of at least one selected from nickel, cobalt, and manganese may repeatedly increase and decrease along the outer peripheral surface of the secondary particle.

[0071] In the first concentration gradient interval and the second concentration gradient interval, the concentration of at least one selected from nickel, cobalt, and manganese may present a concentration gradient that changes continuously or discontinuously.

[0072] Thus, the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned first concentration gradient interval can present a continuously or discontinuously increasing concentration gradient, and the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned second concentration gradient interval can present a continuously or discontinuously decreasing concentration gradient.

[0073] Furthermore, the concentration gradient slope values ​​of at least one selected from nickel, cobalt, and manganese in the plurality of first concentration gradient intervals existing along the outer peripheral surface of the secondary particle may be independent of each other.

[0074] For example, assuming that there are a first concentration gradient interval A, a second concentration gradient interval B, a first concentration gradient interval A', a second concentration gradient interval B'..., in which the concentration of cobalt repeatedly increases and decreases along the peripheral surface of the above-mentioned secondary particles, the concentration gradient slope value of cobalt in the first concentration gradient interval A and the concentration gradient slope value of cobalt in the first concentration gradient interval A' can be independent of each other.

[0075] Similarly, the concentration gradient slope values ​​of at least one selected from nickel, cobalt, and manganese in the plurality of second concentration gradient sections existing along the outer peripheral surface of the secondary particle may be independent of each other.

[0076] For example, assuming that there are a first concentration gradient interval A, a second concentration gradient interval B, a first concentration gradient interval A', a second concentration gradient interval B'..., in which the concentration of cobalt repeatedly increases and decreases along the peripheral surface of the above-mentioned secondary particles, the concentration gradient slope value of cobalt in the second concentration gradient interval B and the concentration gradient slope value of cobalt in the second concentration gradient interval B' can be independent of each other.

[0077] The above example is used to illustrate that the multiple first concentration gradient intervals and the multiple second concentration gradient intervals existing along the outer peripheral surface of the above-mentioned secondary particles have mutually independent concentration gradient slope values. In the above-mentioned first concentration gradient intervals and the above-mentioned second concentration gradient intervals, the concentration of nickel and / or manganese can have a concentration gradient to replace cobalt.

[0078] Furthermore, as described above, when the secondary particle is spherical or nearly spherical, the first concentration gradient interval and the second concentration gradient interval may exist along the circumferential direction of the secondary particle.

[0079] At this time, in a portion of the secondary particles, the circumferential direction may be the same as a direction (defined herein as a lateral direction) perpendicular to a direction from the center of the secondary particles toward the surface of the secondary particles (defined herein as a longitudinal direction).

[0080] That is, the first concentration gradient section and the second concentration gradient section may exist along a lateral direction perpendicular to a longitudinal direction from the center portion of the secondary particle toward the surface portion of the secondary particle.

[0081] Thus, in the first concentration gradient interval, the concentration of at least one selected from nickel, cobalt and manganese may increase continuously or discontinuously along the transverse direction perpendicular to the longitudinal direction from the center of the secondary particle toward the surface of the secondary particle. And, in the second concentration gradient interval, the concentration of at least one selected from nickel, cobalt and manganese may decrease continuously or discontinuously along the transverse direction perpendicular to the longitudinal direction from the center of the secondary particle toward the surface of the secondary particle.

[0082] In another embodiment, the secondary particle may include a concentration increasing / decreasing portion and a concentration maintaining portion along the outer peripheral surface of the secondary particle, the concentration increasing / decreasing portion includes the first concentration gradient interval and the second concentration gradient interval, and the concentration maintaining portion maintains the concentration of at least one selected from nickel, cobalt and manganese in the secondary particle. Figure 4 The above-mentioned concentration increase and decrease portion can be defined as a region including the above-mentioned first concentration gradient interval a and the above-mentioned second concentration gradient interval b, and the above-mentioned concentration maintaining portion can be defined as a region c located between adjacent concentration increase and decrease portions and maintaining the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned secondary particles.

[0083] The definitions of the first concentration gradient interval and the second concentration gradient interval in the concentration increasing and decreasing section are as described above.

[0084] Unlike the above-mentioned concentration increasing and decreasing portion, in the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned concentration maintaining portion, the concentration change amplitude along the lateral direction perpendicular to the longitudinal direction from the center portion of the above-mentioned secondary particle to the surface portion of the above-mentioned secondary particle may not be large. The concentration change rate of at least one selected from nickel, cobalt and manganese in the above-mentioned concentration maintaining portion may be equal to or less than 5 weight% per 0.1 μm, but the present invention is not limited thereto.

[0085] That is, it is sufficient that the concentration change rate of at least one selected from nickel, cobalt and manganese (hereinafter referred to as specific metal element) in the concentration holding portion is small enough to distinguish the first concentration gradient interval from the second concentration gradient interval.

[0086] As described above, the above-mentioned secondary particles have the above-mentioned concentration increase and decrease portion showing a concentration gradient in which the concentration of at least one selected from nickel, cobalt and manganese increases and decreases continuously or discontinuously (that is, the concentration change of at least one selected from nickel, cobalt and manganese is large) and the above-mentioned concentration maintaining portion in which the concentration change of at least one selected from nickel, cobalt and manganese is small, thereby more effectively forming a charge transfer channel in the positive electrode active material.

[0087] Furthermore, while the concentration increasing / decreasing portion and the concentration maintaining portion are repeatedly present along the outer peripheral surface of the secondary particle, the concentration increasing / decreasing portion and the concentration maintaining portion may be formed alternately.

[0088] The primary particles forming the secondary particles may be defined as a lithium composite oxide represented by Chemical Formula 1 below.

[0089] [Chemical formula 1]

[0090] Li w Ni 1-(x+y+z) Co x M1 y M2 z O2

[0091] (wherein, M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, B, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0.01≤x≤0.40, 0.01≤y≤0.40, 0.001≤z≤0.30)

[0092] The average diameter of the primary particles may be 0.1 μm to 3.0 μm, and the average diameter of the secondary particles may be 3.0 μm to 20.0 μm. At this time, the primary particles may form a surface existing inside the secondary particles by contacting with internal voids, without forming a grain boundary by contacting with adjacent primary particles. On the other hand, the surface of the primary particles existing on the outermost surface of the secondary particles exposed to the external air forms the surface of the secondary particles.

[0093] Furthermore, the M3 present on the surface of the secondary particle may have a concentration gradient that decreases toward the center of the secondary particle. That is, the concentration gradient direction of M3 may be from the surface of the secondary particle toward the center of the secondary particle.

[0094] At this time, the secondary particle may include a first region and a second region having different concentrations of M3.

[0095] The first region may be a region where the M3 has a concentration gradient that decreases toward the center of the secondary particle.

[0096] For example, when the distance from the outermost surface of the secondary particle forming the above-mentioned lithium composite oxide to the center of the above-mentioned secondary particle is defined as R, if the region where the distance R' from the outermost surface of the above-mentioned secondary particle is 0 to 0.02R is defined as the first region, the M3 present in the above-mentioned first region can present a concentration gradient decreasing toward the center of the above-mentioned secondary particle.

[0097] On the other hand, the nickel present in the first region may present a concentration gradient that increases toward the center of the secondary particle in the opposite direction to M3, wherein the center of the secondary particle may refer to the exact center of the secondary particle.

[0098] At this time, the concentration change rate of M3 in the first region may be equal to or greater than 50%, preferably, equal to or greater than 60%, but the present invention is not limited thereto.

[0099] And, the remaining area except the above-mentioned first area may be defined as a second area.

[0100] For example, when a region where the distance R' from the outermost surface of the secondary particle is 0 to 0.02R is defined as the first region, a region where the distance R' from the outermost surface of the secondary particle is 0.02R to 1.0R may be defined as the second region. The M3 present in the second region may not have a concentration gradient in the form of increasing or decreasing concentration in a certain direction in the primary particle.

[0101] Furthermore, even if the M3 in the second region has a certain level of concentration gradient, the slope of the concentration gradient in the second region may be smaller than the slope of the concentration gradient of the M3 in the first region.

[0102] In another embodiment, the concentration change rate of M3 in the second region may be equal to or less than 49%, preferably, equal to or less than 30%, and more preferably, equal to or less than 15%.

[0103] Also, in another embodiment, the positive electrode active material may include a coating layer covering at least a portion of the surface of the primary particles (eg, interfaces between the primary particles) and / or secondary particles formed by agglomerating the primary particles.

[0104] For example, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle. In particular, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle at the outermost periphery of the secondary particle.

[0105] Thus, the coating layer may exist as a layer that continuously or discontinuously coats the surface of the primary particles and / or the secondary particles formed by agglomerating the primary particles. When the coating layer exists discontinuously, it may exist in the form of islands.

[0106] The presence of the coating as above can help improve the physical and electrochemical characteristics of the positive electrode active material.

[0107] Furthermore, the coating layer may exist in the form of a solid solution without forming a boundary with the primary particles and / or the secondary particles formed by agglomerating the primary particles.

[0108] The coating layer may include at least one oxide represented by the following Chemical Formula 2. That is, the coating layer may be defined as a region where the oxide represented by the following Chemical Formula 2 exists.

[0109] [Chemical formula 2]

[0110] Li a A b O c

[0111] (wherein A is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd and Nd, 0≤a≤6, 0≤b≤4, 2≤c≤8)

[0112] Also, the coating layer may have a form in which different types of oxides exist simultaneously in one layer or may have a form in which different types of oxides represented by the above Chemical Formula 2 exist in different layers, respectively.

[0113] The oxide represented by the above Chemical Formula 2 may be physically and / or chemically bonded to the primary particles represented by the above Chemical Formula 1. Also, the oxide may exist in a state of forming a solid solution with the primary particles represented by the above Chemical Formula 1.

[0114] The positive electrode active material according to the present embodiment includes a coating, and the coating covers at least a portion of the surface of the primary particles (e.g., the interface between the primary particles) and / or the secondary particles formed by agglomerating the primary particles, thereby improving the structural stability. Moreover, when the positive electrode active material is used in a lithium secondary battery, the high temperature storage stability and life characteristics of the positive electrode active material can be improved. Moreover, the oxide reduces the residual lithium in the positive electrode active material and serves as a path for the movement of lithium ions, thereby affecting the improvement of the efficiency characteristics of the lithium secondary battery.

[0115] Furthermore, depending on circumstances, the oxide may exist not only at the interface between the primary particles and at least a portion of the surface of the secondary particles, but also in internal voids formed in the secondary particles.

[0116] The oxide is an oxide obtained by combining lithium and an element represented by A or an oxide of A. Examples of the oxide are Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a B b O c , W b O c 、Zr b O c 、Ti b O c or B b O c However, the above examples are only described for ease of understanding, and the oxides defined in this article are not limited to the above examples.

[0117] In another embodiment, the oxide may be an oxide formed by compounding lithium and at least two elements represented by A or further includes an oxide formed by compounding lithium and at least two elements represented by A. Examples of the oxide formed by compounding lithium and at least two elements represented by A may be Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr)b O c , Li a (W / Ti / B) b O c Etc., but the present invention is not limited thereto.

[0118] The oxide may present a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle. Thus, the concentration of the oxide may decrease from the outermost surface of the secondary particle toward the center of the secondary particle.

[0119] As described above, the oxide presents a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle, thereby effectively reducing the residual lithium present on the surface of the positive electrode active material to prevent side reactions caused by unreacted residual lithium. In addition, the oxide can also prevent the crystallinity of the inner region of the surface of the positive electrode active material from decreasing. In addition, the oxide can prevent the overall structure of the positive electrode active material from collapsing during the electrochemical reaction.

[0120] Furthermore, the coating layer may include a first oxide layer and a second oxide layer, the first oxide layer including at least one oxide represented by the chemical formula 2, and the second oxide layer including at least one oxide represented by the chemical formula 2 different from the oxide included in the first oxide layer.

[0121] For example, the first oxide layer may exist in a manner that covers at least a portion of the exposed surface of the primary particle at the outermost periphery of the secondary particle, and the second oxide layer may exist in a manner that covers the exposed surface of the primary particle not covered by the first oxide layer and at least a portion of the surface of the first oxide layer.

[0122] Lithium secondary battery

[0123] According to another aspect of the present invention, a positive electrode including a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector may be provided. The positive electrode active material layer may include a positive electrode active material according to various embodiments of the present invention. Therefore, the positive electrode active material is the same as the positive electrode active material described above, so a detailed description will be omitted for convenience, and only the remaining composition will be specifically described below.

[0124] The positive electrode collector is not particularly limited as long as it has conductivity without causing chemical changes in the battery, and examples thereof may include: stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode collector may generally have a thickness of 3 μm to 500 μm, or the adhesion of the positive electrode active material may be increased by forming micro-concave and convex on the surface of the collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.

[0125] The positive electrode active material layer may be prepared by coating a positive electrode slurry composition on the positive electrode current collector. The positive electrode slurry composition includes the positive electrode active material and a conductive material, and optionally includes a binder as required.

[0126] The content of the positive electrode active material may be 80 wt % to 99 wt %, more specifically 85 wt % to 98.5 wt %, relative to the total weight of the positive electrode active material layer. When the content of the positive electrode active material is within the above range, the positive electrode active material may have excellent capacity characteristics, but the present invention is not necessarily limited thereto.

[0127] The above-mentioned conductive material is used to provide conductivity to the electrode, and can be used without limitation, as long as it has electronic conductivity and does not cause chemical changes in the assembled battery. Specific examples thereof may include: graphite such as natural graphite or artificial graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, etc., and these substances can be used as a single one or as a mixture of two or more. The content of the above-mentioned conductive material can be 0.1 wt% to 15 wt% relative to the total weight of the positive electrode active material layer.

[0128] The above-mentioned binder serves to adhere the positive electrode active material particles to each other and improve the adhesion of the positive electrode active material and the collector. Specific examples thereof may include: polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile (polyacrylonitrile), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, etc., and these substances can be used as a single or as a mixture of two or more. Relative to the total weight of the positive electrode active material layer, the content of the above-mentioned binder can be 0.1% by weight to 15% by weight.

[0129] In addition to using the above-mentioned positive electrode active material, the above-mentioned positive electrode can be prepared using a common positive electrode preparation method. Specifically, the above-mentioned positive electrode can be prepared by coating a positive electrode slurry composition prepared by dissolving or dispersing the above-mentioned positive electrode active material and a selective binder and a conductive material in a solvent onto a positive electrode collector, and then drying and rolling the obtained product.

[0130] The above-mentioned solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and these substances may be used alone as a substance, or as a mixture of two or more. Considering the coating thickness and preparation yield of the slurry, as long as the above-mentioned solvent can dissolve or disperse the above-mentioned positive electrode active material, conductive material and binder and has a viscosity sufficient to obtain excellent thickness uniformity when it is used to prepare the positive electrode coating thereafter, the amount of the solvent used is sufficient.

[0131] Furthermore, in another embodiment, the positive electrode may be prepared by casting the positive electrode slurry composition on a separate support, and then laminating a film obtained by peeling off the support on a positive electrode collector.

[0132] In addition, according to another aspect of the present invention, an electrochemical device including the positive electrode may be provided. The electrochemical device may be specifically a battery, a capacitor, etc., and more specifically, may be a lithium secondary battery.

[0133] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, and a separator and an electrolyte between the positive electrode and the negative electrode. Since the positive electrode is the same as the positive electrode described above, a detailed description will be omitted for convenience, and only the remaining components will be described in detail below.

[0134] The lithium secondary battery may further include a battery container for accommodating an electrode assembly including the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.

[0135] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0136] The above-mentioned negative electrode collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and examples thereof may include: copper, stainless steel, aluminum, nickel, titanium, sintered carbon, or copper or stainless steel, aluminum-cadmium alloy, etc., whose surface is treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode collector may generally have a thickness of 3 μm to 500 μm, or, like the positive electrode collector, may increase the adhesion of the negative electrode active material by forming tiny concave-convex shapes on the surface of the above-mentioned collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.

[0137] The negative electrode active material layer may be prepared by coating a negative electrode slurry composition on the negative electrode current collector. The negative electrode slurry composition includes the negative electrode active material and a conductive material, and optionally includes a binder as required.

[0138] The above-mentioned negative electrode active material can use a compound that can reversibly intercalate and deintercalate lithium. Specific examples thereof may include: carbon materials such as artificial graphite, natural graphite, graphitized carbon fiber and amorphous carbon; metal compounds that can be alloyed with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy or Al alloy; metal oxides that can be doped and dedoped with lithium such as SiO β (0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite comprising a metal compound and a carbon material such as a Si-C composite or a Sn-C composite, and any one of these substances or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, the carbon material can use both low-crystalline carbon and high-crystalline carbon. Low-crystalline carbon generally includes soft carbon and hard carbon, and high-crystalline carbon generally includes: amorphous, plate-like, scaly, spherical or fibrous natural graphite or artificial graphite, and high-temperature sintered carbon such as floating graphite (Kish graphite), pyrolytic carbon (pyrolytic carbon), mesophase pitch carbon fiber (mesophase pitch based carbon fiber), mesophase carbon microbeads (meso-carbon microbeads), mesophase pitch (Mesophase pitches) and petroleum or coal tar pitch derived coke (petroleum or coal tar pitch derived cokes).

[0139] The negative electrode active material may be included in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode active material layer.

[0140] The binder is a component that helps to bind the conductive material, the active material and the current collector, and its content is generally 0.1 wt % to 10 wt % based on the total weight of the negative electrode active material layer. Examples of the binder may include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber and various copolymers thereof.

[0141] The above conductive material is a component for further improving the conductivity of the negative electrode active material, and the content of the conductive material can be 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. The above conductive material is not subject to any restrictions as long as it has conductivity and does not cause chemical changes in the battery, and conductive materials such as graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black can be used; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbons, aluminum or nickel powders; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.

[0142] In one embodiment, the negative electrode active material layer can be prepared by: coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector and drying the obtained product; or by casting the negative electrode slurry composition on a separate carrier and then laminating a film obtained by peeling off the carrier on the negative electrode collector.

[0143] Furthermore, in another embodiment, the negative electrode active material layer can be prepared by: coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector and drying the obtained product; or by casting the negative electrode slurry composition on a separate carrier and then laminating the film obtained by peeling off the carrier on the negative electrode collector.

[0144] On the other hand, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode, and provides a migration channel for lithium ions, and there is no particular limitation, as long as it is generally used as a separator in a lithium secondary battery. In particular, a separator with low resistance to electrolyte ion migration and excellent ability to contain electrolyte liquid moisture is preferred. Specifically, it is possible to use: a porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure of more than two layers thereof. In addition, commonly used porous non-woven fabrics such as non-woven fabrics made of high melting point glass fibers or polyethylene terephthalate fibers can be used. In addition, in order to ensure heat resistance and mechanical strength, a coated separator comprising a ceramic component or a polymer material can also be used, and can be selectively used in a single-layer or multilayer structure.

[0145] In addition, the electrolyte used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc. that can be used in the preparation of lithium secondary batteries, but the present invention is not limited thereto.

[0146] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0147] The above-mentioned organic solvent can be used without particular limitation as long as it can function as a medium through which ions participating in the electrochemical reaction of the battery can migrate. Specific examples of the above-mentioned organic solvents may include: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene or fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methylethyl carbonate (MEC), ethylmethyl carbonate (EMC), ethylene carbonate (EC) or propylene carbonate (PC); alcohol solvents such as ethanol or isopropanol; nitrile solvents such as R-CN (R is C2~C 20Straight chain, branched or cyclic hydrocarbon group, and may contain double bond aromatic ring or ether bond); amide such as dimethylformamide; dioxolane such as 1,3-dioxolane; sulfolane, etc. Among them, carbonate solvents are preferred, and a mixture of cyclic carbonates (such as ethylene carbonate, propylene carbonate, etc.) with high ion conductivity and high dielectric constant that can enhance the charging and discharging performance of the battery and low viscosity linear carbonate compounds (such as ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, mixing cyclic carbonates and chain carbonates in a volume ratio of about 1:1 to 1:9 can produce excellent electrolyte performance.

[0148] The above-mentioned lithium salt can be used without particular limitation, as long as it is a compound capable of providing lithium ions in a lithium secondary battery. Specific examples of the above-mentioned lithium salts may include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The lithium salt can be advantageously used in a concentration range of 0.1M to 2.0M. When the lithium salt concentration is included in the above range, the electrolyte has appropriate conductivity and viscosity, thereby being able to exhibit excellent electrolyte performance, and lithium ions can be effectively migrated.

[0149] In the above electrolyte, in order to increase the battery life property, inhibit the decline of battery capacity, improve the battery discharge capacity, etc., in addition to the above electrolyte forming components, one or more additives may be further included, including, for example: halogenated alkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N, N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum chloride. Wherein, relative to the total weight of the electrolyte, the content of the above additives can be 0.1% by weight to 5% by weight.

[0150] The lithium secondary battery containing the positive electrode active material according to the present invention as described above stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore used in the following fields: the field of portable devices such as mobile phones, laptop computers and digital cameras; and the field of electric vehicles such as hybrid electric vehicles (HEV) and the like.

[0151] The shape of the lithium secondary battery according to the present invention is not particularly limited, but may have a cylindrical, angular, pouch or coin shape using a can. And, preferably, the lithium secondary battery can be used as a battery cell for a power source of a small device, and can also be used as a unit battery of a medium and large battery module including a plurality of battery cells.

[0152] According to another aspect of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit battery and / or a battery pack including the same may be provided.

[0153] The battery module or the battery pack may be used in power tools (Power Tool); electric vehicles including electric vehicles (EV), hybrid vehicles and plug-in hybrid electric vehicles (PHEV); or as a power source for one or more medium and large devices in a system for storing electricity.

[0154] Hereinafter, the present invention will be described in more detail with reference to Examples. However, it should be understood that these Examples are for illustrative purposes only and should not be construed as limiting the scope of the present invention.

[0155] Experimental example 1.

[0156] (1) Preparation of positive electrode active materials

[0157] Example 1

[0158] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a hydroxide precursor is synthesized by coprecipitation reaction, LiOH is added to the synthesized precursor, and then calcined to prepare a lithium composite oxide. Specifically, LiOH is mixed with the precursor, an O2 atmosphere is maintained in a sintering furnace, the temperature is increased at 2°C per minute, a heat treatment is performed at 690°C for 10 hours, and quenching is performed at 10°C / minute or more to obtain a lithium composite oxide.

[0159] Next, distilled water was added to the above lithium composite oxide, and then washed with water for 1 hour, and the washed lithium composite oxide was filtered and dried. Drying was performed by maintaining an O2 atmosphere in the same sintering furnace, heating at 2°C per minute, heat-treating at 300°C for 8 hours, and then naturally cooling to obtain a lithium composite oxide. A cross-sectional SEM image of the above positive electrode active material is shown in Figure 2 middle.

[0160] Example 2

[0161] The lithium composite oxide was prepared in the same manner as in Example 1 except that the lithium composite oxide of Example 1 was mixed with Al2O3, TiO2 and ZrO2 and further heat treated so that the final lithium composite oxide contained aluminum, titanium and zirconium. A cross-sectional SEM image of the above positive electrode active material is shown in FIG. Figure 6 middle.

[0162] Example 3

[0163] The lithium composite oxide was prepared in the same manner as in Example 1 except that the lithium composite oxide of Example 1 was mixed with H3BO3 as a boron-containing raw material and further heat-treated so that the finally produced lithium composite oxide contained boron. A cross-sectional SEM image of the above positive electrode active material is shown in FIG. Fig.10 middle.

[0164] Example 4

[0165] A lithium composite oxide was prepared in the same manner as in Example 1 except that the lithium composite oxide of Example 1 was mixed with Al2O3, TiO2, ZrO2 and H3BO3 and further heat treated so that the final lithium composite oxide contained aluminum, titanium, zirconium and boron.

[0166] Comparative Example 1

[0167] The lithium composite oxide was prepared in the same manner as in Example 1 except that LiOH was mixed with the precursor and then heat-treated in a sintering furnace and then naturally cooled without separate quenching. A cross-sectional SEM image of the above positive electrode active material is shown in Fig.14 middle.

[0168] Comparative Example 2

[0169] The lithium composite oxide of Comparative Example 1 was mixed with a cobalt-containing raw material (Co3O4) using a mixer so that the content of the cobalt-containing raw material (Co3O4) was 30 mol % relative to the total content of the positive electrode active material. The lithium composite oxide was prepared in the same manner as Comparative Example 1 except that it was coated with cobalt.

[0170] (2) TEM / EDX (Energy-dispersive X-ray spectroscopy) analysis of positive electrode active materials

[0171] The positive electrode active materials (secondary particles) according to the examples and comparative examples were subjected to cross-sectional processing using FIB (gallium ion source) to obtain TEM images (see Figure 2 , Figure 6 , Fig.10 and Fig.14 ).

[0172] Figures 3 to 5 for Figure 2 The figure shows a line sum spectrum of the content of metal elements (nickel, cobalt and manganese) in a part (surface part) of the positive electrode active material (secondary particle) according to Example 1 along a direction (lateral) perpendicular to the direction (longitudinal) from the center part of the secondary particle toward the surface part of the secondary particle. Figures 3 to 5 The concentration gradient of the metal elements (nickel, cobalt and manganese) shown in Figure 1 The direction corresponding to the line data (Line Data) shown in .

[0173] Reference Figure 3 It can be confirmed that the concentration of cobalt changes along the direction of the outer peripheral surface of the above-mentioned secondary particles, that is, along the direction (lateral) perpendicular to the direction (longitudinal) from the center of the above-mentioned secondary particles toward the surface of the above-mentioned secondary particles, and changes along the first concentration gradient interval a and the second concentration gradient interval b. The concentration in the above-mentioned first concentration gradient interval a increases in the direction of the average content of cobalt in the above-mentioned secondary particles (Avg) or in the direction of a concentration higher than the average content (Avg), and the concentration in the second concentration gradient interval b decreases in the direction of the average content of cobalt in the above-mentioned secondary particles (Avg) or in the direction of a concentration lower than the average content (Avg).

[0174] And, refer to Figure 4 When the first concentration gradient interval a and the second concentration gradient interval b connected to the highest point of the first concentration gradient interval a are defined as concentration increasing and decreasing sections, it can be confirmed that there is a concentration maintaining section c that maintains the concentration of the cobalt between adjacent concentration increasing and decreasing sections. In other words, the concentration of the cobalt presents a concentration gradient tendency defined by the concentration increasing and decreasing section and the concentration maintaining section, so that a charge transfer channel can be formed in the secondary particles.

[0175] Reference Figure 5 , it can be confirmed that the concentration of manganese also has a first concentration gradient interval and a second concentration gradient interval at a position corresponding to the above-mentioned cobalt concentration. Figure 4 , it can be confirmed that nickel presents the same Figure 4 and Figure 5 In other words, the concentration of nickel decreases in the direction of the average nickel content in the secondary particles or a concentration lower than the average nickel content in the first concentration gradient interval of cobalt, and increases in the direction of the average nickel content in the secondary particles or a concentration higher than the average nickel content in the second concentration gradient interval of cobalt.

[0176] Figures 7 to 9 for Figure 6 The figure shows a line sum spectrum of the content of metal elements (nickel, cobalt and manganese) in a part (surface part) of the positive electrode active material (secondary particle) according to Example 2 along a direction (lateral) perpendicular to the direction (longitudinal) from the center part of the secondary particle toward the surface part of the secondary particle. Figures 7 to 9 The concentration gradient of the metal elements (nickel, cobalt and manganese) shown in Figure 5 The direction of the line data (Line Data) shown in the figure can be confirmed. Figures 7 to 9 The concentration gradient of the metal elements (nickel, cobalt and manganese) shown in Figures 3 to 5 Similar to Example 1 shown in .

[0177] And, reference is made to the Fig.10 The distribution of metal elements (nickel, cobalt and manganese) measured by TEM / EDX mapping (mapping) of a part (surface part) of the positive electrode active material (secondary particles) according to Example 3 is shown. Figures 11 to 13 It can be confirmed that the concentration gradients of nickel, cobalt and manganese in the secondary particles exist along the peripheral surface of the secondary particles. In addition, the concentration gradients of nickel, cobalt and manganese have different directions. In particular, it can be confirmed that although the concentration gradients of cobalt and manganese have the same direction, the concentration gradients of cobalt and manganese have different directions from that of nickel.

[0178] Refer to Fig.10 The TEM image of the center portion of the positive electrode active material (secondary particle) according to Example 3 is shown. Fig.14 and show that Fig.14 The distribution of metal elements (nickel, cobalt and manganese) in the center of the positive electrode active material (secondary particle) according to Example 3 is measured by TEM / EDX mapping. Figures 15 to 17 It can be confirmed that unlike the surface portion of the secondary particle, the concentration gradient of nickel, cobalt and manganese in the secondary particle does not exist in the central portion of the secondary particle.

[0179] On the other hand, referring to the example Fig.18 The line sum spectrum of the content of metal elements (nickel, cobalt and manganese) in a part (surface part) of the commercial NCM 811 shown in FIG. 1 is a graph showing the content of metal elements (nickel, cobalt and manganese) in a direction (lateral) perpendicular to the direction (longitudinal) from the center part of the secondary particle toward the surface part of the secondary particle. Figures 19 to 21 , there is no tendency that the positive electrode active materials according to Examples 1 to 3 have.

[0180] (3) XPS analysis of positive electrode active materials

[0181] XPS analysis was performed on each positive electrode active material according to each embodiment and comparative example to confirm whether there was a coating in the positive electrode active material. XPS analysis was performed using K-Alpha+ (Thermo Fisher Scientific) (accelerating voltage: 0.5-2keV, energy resolution: about 0.5eV, minimum analysis area: 30micro, monatomic and gas cluster ion source).

[0182] Tables 1 and 2 below show XPS analysis results of positive electrode active materials according to Examples and Comparative Examples, respectively.

[0183] Table 1

[0184] Classification Al2P B1s Co2p Li1s Mn2p Ni2p O1s Ti2p ZlUT Example 1 0 0 2.03 22.37 6.23 17.68 51.68 0 0 Example 2 6.12 0 1.32 21.64 3.99 8.81 54.44 3.42 0.25 Example 3 0 14.98 0.67 20.23 2.00 4.29 57.84 0 0 Example 4 4.87 9.54 0.81 20.30 2.53 5.57 54.07 2.10 0.20

[0185] Table 2

[0186] Classification Al2P B1s Co2p Li1s Mn2p Ni2p O1s Ti2p ZlUT Comparative Example 1 0 0 0.38 38.47 0.68 1.64 58.83 0 0 Comparative Example 2 0 0 9.88 17.81 9.45 23.26 39.60 0 0

[0187] Referring to the results of Table 1 above, in the case of the positive electrode active material according to Example 1, the XPS analysis results do not show Al2p, B1s, Ti2p or Zr3d peaks, in Example 2, Al2p, Ti2p and Zr3d peaks are shown, in Example 3, B1s peak is shown, and in Example 4, Al2p, B1s, Ti2p and Zr3d peaks are shown. It can be seen that the positive electrode active materials according to Examples 2 to 4 respectively form oxide coatings corresponding to the peaks shown in the XPS analysis results on the surface of the lithium composite oxide.

[0188] On the other hand, referring to the results of Table 2 showing the XPS analysis results according to Comparative Example 1 and Comparative Example 2, the size of the Co2p peak of the positive electrode active material according to Comparative Example 2 is larger than that of Comparative Example 1, from which it can be seen that the positive electrode active material according to Comparative Example 2 forms a cobalt oxide coating on the surface of the lithium composite oxide.

[0189] However, not only in Comparative Example 1, but also in Comparative Example 2 in which a coating containing a cobalt oxide is formed on the surface of the lithium composite oxide, there is no concentration gradient zone caused by cobalt or manganese, etc. shown in Examples 1 to 4. These results confirm that the concentration gradient of the metal element existing along the peripheral surface of the secondary particle found in the positive electrode active material of various embodiments of the present invention is not caused by the coating existing on the surface of the lithium composite oxide.

[0190] Experimental example 2.

[0191] (1) Preparation of lithium secondary batteries

[0192] A positive electrode slurry was prepared by dispersing 94 wt % of each positive electrode active material prepared according to Example 1, Comparative Example 1 and Comparative Example 2, 3 wt % of carbon black and 3 wt % of PVDF binder in 3.5 g of N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was coated on an aluminum (Al) film as a positive electrode collector having a thickness of 20 μm, dried and roll pressed to prepare a positive electrode. The loading level of the positive electrode was 7 mg / cm 2 , the electrode density is 3.2g / cm 3 .

[0193] A button cell was prepared by a known preparation method using a lithium foil as a counter electrode for the positive electrode, a porous polyethylene film (Celgard 2300, thickness: 25 μm) as an isolation film, and a liquid electrolyte containing LiPF6 dissolved at a concentration of 1.15 M in a solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7.

[0194] (2) Evaluation of the impedance characteristics of lithium secondary batteries (EIS; Electrochemical Impedance Spectroscopy)

[0195] The resistance of the lithium secondary battery (button battery) prepared above was measured using electrochemical impedance spectroscopy (EIS) within a frequency range (10 kHz to 0.01 Hz).

[0196] Referring to the table showing the resistance measurement results measured by the above-mentioned resistance spectroscopy method Fig. 22 It can be confirmed that in the case of the lithium secondary battery including the positive electrode active materials prepared according to Comparative Examples 1 and 2, the R ct (charge transfer resistance) value.

[0197] That is to say, the above results confirm that the resistance characteristics of the lithium secondary battery can be improved by using a positive electrode active material including a first concentration gradient interval and a second concentration gradient interval along the outer peripheral surface of the above secondary particles, the concentration of at least one selected from nickel, cobalt and manganese in the above secondary particles in the above first concentration gradient interval increases, and the concentration of at least one selected from nickel, cobalt and manganese in the above secondary particles in the above second concentration gradient interval decreases.

[0198] Although the embodiments of the present invention are described above, those skilled in the art will understand that various modifications and changes can be made to the present invention by adding, modifying, deleting, increasing, etc., without departing from the scope of the idea of ​​the present invention as described in the claims, and these also fall within the scope of the rights of the present invention.

Claims

1. A positive electrode active material, characterized in that: include: Primary particles, capable of occluding and releasing lithium; Secondary particles formed by agglomeration of the primary particles; and coating, The coating layer covers at least a portion of the interface between the primary particles and / or the surface of the secondary particles. There are a first concentration gradient interval and a second concentration gradient interval along the outer peripheral surface of the secondary particle, the concentration of at least one selected from nickel, cobalt and manganese in the secondary particle increases in the first concentration gradient interval, and the concentration of at least one selected from nickel, cobalt and manganese in the secondary particle decreases in the second concentration gradient interval, The first concentration gradient interval and the second concentration gradient interval exist along a direction perpendicular to a direction from a center portion of the secondary particle toward a surface portion of the secondary particle. The concentration gradient in the first concentration gradient interval and the concentration gradient in the second concentration gradient interval are not caused by the coating.

2. The positive electrode active material according to claim 1, characterized in that The first concentration gradient region and the second concentration gradient region exist on the surface of the secondary particle.

3. The positive electrode active material according to claim 1, characterized in that The first concentration gradient section and the second concentration gradient section are repeatedly present along the outer peripheral surface of the secondary particle.

4. The positive electrode active material according to claim 1, characterized in that The cobalt in the first concentration gradient region increases to a concentration higher than the average content of cobalt in the secondary particles.

5. The positive electrode active material according to claim 1, characterized in that The cobalt in the second concentration gradient region decreases toward the average content of cobalt in the secondary particles.

6. The positive electrode active material according to claim 1, characterized in that There are concentration increasing and decreasing parts and concentration maintaining parts along the outer peripheral surface of the above-mentioned secondary particles. The above-mentioned concentration increasing and decreasing parts include the above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval. The above-mentioned concentration maintaining part maintains the concentration of at least one selected from nickel, cobalt and manganese in the above-mentioned secondary particles.

7. The positive electrode active material according to claim 6, characterized in that The concentration change rate of at least one selected from nickel, cobalt and manganese in the concentration maintaining portion is equal to or less than 5 weight % per 0.1 μm.

8. The positive electrode active material according to claim 1, characterized in that The coating comprises at least one oxide represented by the following chemical formula: [Chemical formula] Li a A b O c Among them, A is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, V, Ba, Ta, Sn, Hf, Ce, Gd and Nd, 0≤a≤6, 0≤b≤4, 2≤c≤8.

9. A cathode slurry composition, characterized in that: The invention comprises the positive electrode active material according to any one of claims 1 to 8, a conductive material and a binder.