A composite board of CSP ceramic substrate and preparation method thereof

By arranging annular loop strips and metal strips on the CSP ceramic substrate composite board and covering them with a sealed insulating layer, electrolytic plating and multi-layer co-fired ceramic processes are used to solve the problem of poor flatness of the ceramic substrate composite board and the high cost of precious metal plating. problem, achieving high mechanical strength and air tightness, reducing costs and improving packaging reliability.

CN112778002BActive Publication Date: 2024-10-25JIAXING GLEAD ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110211804.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-10-25
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

During the manufacturing process of existing CSP ceramic substrate combination boards, there are problems such as poor flatness caused by multiple metal conductor circuit layers, high cost of precious metal plating, and easy chipping of metal strips, which affects packaging reliability and cost.

Method used

It uses a combination of ceramic substrates arranged vertically and horizontally, with annular loop belts and metal belts, and covers its surface with a closed insulating layer. The metal is evenly plated through electrolytic plating technology, and is prepared using a multi-layer co-fired ceramic process to form high mechanical strength. and airtight CSP ceramic substrate combination board.

Benefits of technology

It improves the mechanical strength and airtightness of the ceramic substrate, reduces the amount of precious metals, reduces the cost, and solves the problem of edge chipping of the metal strips during slitting, improving the economy and packaging reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112778002B_ABST
    Figure CN112778002B_ABST
Patent Text Reader

Abstract

The present invention relates to a composite board of CSP ceramic substrates and a preparation method thereof, comprising a composite board formed by a plurality of ceramic substrates arranged in parallel vertically and horizontally; an annular loop belt arranged on the periphery of the composite board; a first metal belt for connecting adjacent ceramic substrates; a second metal belt for connecting the ceramic substrate and the annular loop belt; and a closed insulating layer covering the surface of the first metal belt and the second metal belt. The composite board of CSP ceramic substrates provided by the present invention has the characteristics of high mechanical strength, good air tightness, and high metal-ceramic bonding strength; and because the closed insulating layer is densely bonded, the bonding firmness of the first and second metal belts with the ceramic matrix is ​​improved, and the problem of "collapse of the edge" of the second metal belt caused by the ceramic substrate composite board when it is cut is effectively solved. In addition, because the closed insulating layer covers the first and second metal belts, the amount of precious metal plated on the surface is reduced, the cost is reduced, and the economy of the product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic component packaging substrates, and in particular to a combined plate of a CSP ceramic substrate and a preparation method thereof. Background Art

[0002] The Japan Electronics Industry Association defines CSP as a package with a chip area to package area ratio greater than 80%; the J-STK-012 standard of the U.S. Department of Defense Component Supply Center defines CSP as a package with an area of ​​LSI packaged products less than or equal to 120% of the LSI chip area. CSP packaged memory is not only small in size, but also thinner, which improves the reliability of memory chips after long-term operation, significantly reduces line impedance, and greatly improves chip speed.

[0003] CSP package ceramic substrate is the carrier of the chip. CSP package ceramic substrate should not only have physical properties such as high mechanical strength, good heat dissipation, good air tightness, high insulation resistance, but also have processing requirements such as high dimensional accuracy and good flatness, and also involve surface metallization process, especially surface plating of precious metals such as gold / silver. Therefore, how to improve the reliability of CSP package ceramic substrate and how to further reduce costs on the basis of meeting basic performance are urgent needs for product technology development.

[0004] The patent document with application publication number CN 110098170A discloses a ceramic packaging substrate combination board, including a ceramic substrate combination board and an annular loop belt; the ceramic substrate has a base metal, the annular loop belt includes at least two inner and outer annular loop belts, the inner and outer annular loop belts are connected by a branch connection belt, and the inner annular loop belt is electrically connected to the substrate metal.

[0005] The non-welding functional areas of the above technical solution (such as the inner and outer two annular loop belts, and the branch connection belts) are all exposed, which brings the following technical problems: First, the ceramic substrate composite board is manufactured in a stacking manner, and the metal conductor line layer is 3 or more layers. The amount of metal conductor material is large, which increases the proportion of metal / ceramic heterogeneous materials, resulting in poor flatness of the co-fired ceramic substrate, affecting the reliability of subsequent chip packaging; Second, when gold is plated on the surface of the substrate, precious metals such as gold are not only plated on the functional pads of the ceramic substrate, but also on the metal belts connecting the pads and non-functional areas such as the annular loop belts, resulting in an increase in material costs; Third, when the ceramic substrate composite board is cut, the directly exposed metal belt is prone to "edge collapse", reducing the yield of the finished device. Summary of the invention

[0006] In order to solve the above technical problems, the first object of the present invention is to provide a CSP ceramic substrate assembly board with reasonable structural design and capable of ensuring packaging reliability and economy. The second object of the present invention is to provide a method for preparing a CSP ceramic substrate assembly board.

[0007] In order to achieve the first object of the above invention, the present invention adopts the following technical solutions:

[0008] A CSP ceramic substrate combination board includes a combination board formed by a plurality of ceramic substrates arranged in parallel vertically and horizontally; an annular loop belt arranged on the periphery of the combination board; a first metal belt used to connect adjacent ceramic substrates; a second metal belt used to connect the ceramic substrate and the annular loop belt; and a closed insulating layer is coated on the surfaces of the first metal belt and the second metal belt.

[0009] The ceramic substrate can be a ceramic made of aluminum oxide, aluminum nitride, silicon nitride or beryllium oxide. The annular loop belt is arranged on the periphery of the combined plate, and is used to connect the cathode of the power supply during electrolytic plating, and evenly distribute the current so that the combined plate of the ceramic substrate is evenly plated with a metal coating; the first metal belt is used to electrically connect the ceramic substrates adjacent to each other, and form a two-dimensional network circuit during electrolytic plating. The second metal belt is used to electrically connect the annular loop belt with the ceramic substrate at the edge, and to guide the current of the annular loop belt to the ceramic substrates arranged in an array during electrolytic plating. The enclosed insulating layer is tightly bonded to the outer surfaces of the first metal belt and the second metal belt, and is in an electrically insulating state.

[0010] As a preferred solution, the ceramic substrate includes a ceramic base and a pad, and two pads are arranged in parallel on the ceramic base.

[0011] As a preferred solution, the material of the sealed insulating layer is an insulating mineral or insulating plastic. The insulating mineral can be at least one or more of sealing glass with good insulation properties and low-temperature sintered ceramics. The insulating plastic can be at least one or more of polyethylene, polytetrafluoroethylene, polyvinyl chloride, and polyimide.

[0012] As a preferred solution, the material of the insulating mineral is the same as the material of the ceramic matrix of the ceramic substrate.

[0013] As a preferred solution, the annular loop belt is in a square shape, and dicing mark blocks are arranged at equal intervals on each side. When dicing after chip packaging, the dicing mark on the annular loop belt can be used for dicing machine capture and positioning.

[0014] As a preferred solution, the thickness of the sealed insulating layer is 1 to 50 um. The sealed insulating layer can be coated, masked, screen printed, etc., and after appropriate heat treatment or rapid curing, the sealed insulating layer is coated on the surface of the first metal belt and the second metal belt, so that the metal belts are tightly fixed and insulated.

[0015] As a preferred solution, the composite plate is prepared by a multi-layer co-fired ceramic process.

[0016] The multilayer co-fired ceramic process is low-temperature co-fired ceramic technology (LTCC) or high-temperature co-fired ceramic technology (HTCC). Specifically, the process includes: powder preparation, ceramic slurry preparation, tape casting, green ceramic tape slitting, drilling, hole filling, screen printing, green body cutting, low-temperature (850-900 degrees) or high-temperature (1400-1650 degrees) conductor ceramic co-sintering, leveling and other processes.

[0017] In order to achieve the second purpose of the above invention, the present invention adopts the following technical solutions:

[0018] A method for preparing a composite plate of a CSP ceramic substrate as described above comprises the following steps:

[0019] Step 1) adding micron-sized alumina powder to xylene and ethanol organic solvents, and adding dispersant, PVB resin and plasticizer, mixing the mixture thoroughly, removing bubbles by vacuum, and then tape casting to form a green porcelain tape;

[0020] Step 2) drilling and filling holes in the green porcelain tape, and then screen printing electrodes on the upper and lower surfaces of the green body with tungsten slurry, and then cutting and high-temperature co-firing in a high-temperature reducing kiln at 1500-1600 degrees to form a first semi-finished product;

[0021] Step 3) making a mask plate, the mask plate is printed at positions corresponding to the first metal belt and the second metal belt, transferring the fast volatilizing and curing acrylic concentrated solution to the mask plate, aligning the positions, and scraping and printing on the surfaces of the first metal belt and the second metal belt of the first semi-finished product, after the solvent of the acrylic concentrated solution evaporates, it solidifies to form a closed insulating layer, the closed insulating layer is made of acrylic and has a thickness of 35-50um, forming a second semi-finished product;

[0022] Step 4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt is energized. The nickel ions and gold ions are sequentially plated onto the pad surface of the ceramic substrate under the action of the electric field, forming a composite board of the CSP ceramic substrate.

[0023] A method for preparing a composite plate of a CSP ceramic substrate as described above, characterized in that it comprises the following steps:

[0024] Step 1) adding micron-level low-temperature sintered ceramic powder to xylene and ethanol organic solvents, and adding dispersant, PVB resin and plasticizer, fully mixing, vacuum removing bubbles, and then performing tape casting to form a green ceramic tape;

[0025] Step 2) drilling and filling holes in the green porcelain tape, and then screen printing electrodes on the upper and lower surfaces of the green body with silver paste, and then cutting and low-temperature co-firing in an air atmosphere at 850 to 900 degrees to form a first semi-finished product;

[0026] Step 3) making a mask plate, the mask plate is printed at positions corresponding to the first metal belt and the second metal belt, transferring a fast volatilizing and curing polyimide concentrated solution to the mask plate, aligning the positions, and scraping and printing on the surfaces of the first metal belt and the second metal belt of the first semi-finished product, after the solvent of the concentrated polyimide solution evaporates, it solidifies to form a closed insulating layer, the closed insulating layer is made of polyimide and has a thickness of 20-40 um, to form a second semi-finished product;

[0027] Step 4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt is energized. The nickel ions and gold ions are sequentially plated onto the pad surface of the ceramic substrate under the action of the electric field, forming a composite board of the CSP ceramic substrate.

[0028] As a preferred solution, the low-temperature sintered ceramic powder contains 40-60% of aluminum oxide crystal particles and 40-60% of Ca-Al-Si amorphous glass, and the sum of the two components is 100%.

[0029] The technical solution disclosed in the present invention has the following beneficial effects:

[0030] 1. The combined board of CSP ceramic substrate provided has the characteristics of high mechanical strength, good air tightness, and high bonding strength between metal and ceramic.

[0031] 2. Due to the dense bonding of the closed insulating layer, the bonding strength between the first and second metal strips and the ceramic substrate is improved, and the problem of "collapse of the edge" of the second metal strip caused by cutting the ceramic substrate composite plate is effectively solved.

[0032] 3. Since the closed insulating layer covers the first and second metal strips, the amount of precious metal plated on the surface is reduced, the cost is reduced, and the economy of the product is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The drawings in the specification, which constitute a part of the present application, are used to provide a further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute a limitation on the present application.

[0034] Figure 1 Schematic diagram of the combined plate of the CSP ceramic substrate in Examples 1 to 4;

[0035] Figure 2 is a three-dimensional diagram of the ceramic substrate in Examples 1 to 4;

[0036] Figure 3 Schematic diagram of the ceramic substrate in Examples 1 to 4;

[0037] Figure 4 Schematic diagram of the ceramic substrate in Comparative Examples 1 to 4;

[0038] Figure 5 is a cross-sectional view of the CSP ceramic substrate assembly plate in Example 4 when being cut;

[0039] Figure 6 This is a cross-sectional view of the CSP ceramic substrate assembly board in Comparative Example 4 when it is cut.

[0040] The reference numerals in the figure are: 100, ceramic substrate; 101, ceramic base; 102, pad; 200, annular loop belt; 301, first metal belt; 302, second metal belt; 400, closed insulating layer. DETAILED DESCRIPTION

[0041] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0042] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0043] In addition, in the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0044] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more, unless otherwise clearly specified.

[0045] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0046] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0047] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0048] Example 1

[0049] The combined plate of the CSP ceramic substrate of this embodiment is prepared by the following method.

[0050] (1) Add micron-sized alumina powder to xylene and ethanol organic solvents, and add appropriate amounts of dispersant, PVB resin and plasticizer to fully mix the slurry. After vacuum removal of bubbles, tape casting is performed to form a green porcelain tape.

[0051] (2) drilling and filling holes in the green porcelain tape, and then screen printing electrodes on the upper and lower surfaces of the green body with tungsten slurry, and then cutting and high-temperature co-firing in a high-temperature reducing kiln at 1500-1600 degrees to form a first semi-finished product;

[0052] The first semi-finished product includes: a ceramic substrate 100; an annular loop belt 200 arranged on the periphery of the combined plate; a first metal belt 301 for connecting adjacent ceramic substrates 100; a second metal belt 302 for connecting the ceramic substrate 100 and the annular loop belt 200; the annular loop belt 200, the first metal belt 301 and the second metal belt 302 are all made of tungsten alloy.

[0053] (3) A mask plate is prepared, and the mask plate can be omitted at the corresponding positions of the first metal strip 301 and the second metal strip 302. The fast-evaporating and solidifying acrylic thick solution is transferred to the above-mentioned mask plate, and the position is aligned. The surface of the first metal strip 301 and the second metal strip 302 of the above-mentioned first semi-finished product is scraped and printed. After the solvent of the acrylic thick solution evaporates, it solidifies to form a closed insulating layer 400. The material of the above-mentioned closed insulating layer 400 is acrylic and the thickness is 45um, forming a second semi-finished product.

[0054] (4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt 200 is energized. The nickel ions and gold ions are sequentially plated onto the surface of the pad 102 of the ceramic substrate under the action of the electric field, thereby forming a composite board of the CSP ceramic substrate.

[0055] like Figures 1 to 3 As shown, the combined board structure of the CSP ceramic substrate of this embodiment includes: a ceramic substrate 100, wherein the ceramic base 101 of the ceramic substrate 100 is a 96% alumina ceramic substrate, and the materials of the pad 102 are gold, nickel, and tungsten alloy from the surface layer downward; an annular loop belt 200 arranged on the periphery of the combined board, and the materials are gold, nickel, and tungsten alloy from the surface layer downward; a first metal belt 301 for connecting adjacent ceramic substrates 100, and the material is metal tungsten; a second metal belt 302 for connecting the ceramic substrate 100 with the annular loop belt 200, and the material is metal tungsten; a closed insulating layer 400 is covered on the surface of the first metal belt 301 and the second metal belt 302, and the material is acrylic with a thickness of 45um.

[0056] Example 2

[0057] The combined plate of the CSP ceramic substrate of this embodiment is prepared by the following method.

[0058] (1) A micron-level low-temperature sintered ceramic powder, comprising 40-60% alumina crystal particles and 60-40% Ca-Al-Si amorphous glass, is added to an organic solvent such as xylene and ethanol, and an appropriate amount of dispersant, PVB resin and plasticizer are added to fully mix the slurry. After vacuum removal of bubbles, the slurry is tape-casted to form a green ceramic tape.

[0059] (2) drilling and filling holes in the green porcelain tape, and then screen-printing electrodes on the upper and lower surfaces of the green body with silver paste, and then slitting and low-temperature co-firing in an air atmosphere at 850 to 900 degrees to form a first semi-finished product;

[0060] The first semi-finished product includes: a ceramic substrate 100; an annular loop belt 200 arranged on the periphery of the combined plate; a first metal belt 301 for connecting adjacent ceramic substrates 100; a second metal belt 302 for connecting the ceramic substrate 100 and the annular loop belt 200; the annular loop belt 200, the first metal belt 301 and the second metal belt 302 are all made of metallic silver.

[0061] (3) A mask plate is prepared, and the mask plate can be omitted at the corresponding positions of the first metal strip 301 and the second metal strip 302. A fast volatilizing and curing polyimide concentrated solution is transferred to the mask plate, and the positions are aligned. The surface of the first metal strip 301 and the second metal strip 302 of the first semi-finished product is scraped and printed. After the solvent of the polyimide concentrated solution evaporates, it solidifies to form a closed insulating layer 400. The closed insulating layer 400 is made of polyimide and has a thickness of 30 um, forming a second semi-finished product.

[0062] (4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt 200 is energized. The nickel ions and gold ions are sequentially plated onto the surface of the pad 102 of the ceramic substrate under the action of the electric field, thereby forming a composite board of the CSP ceramic substrate.

[0063] like Figures 1 to 3 As shown, the combined board of the CSP ceramic substrate of the present embodiment comprises: a ceramic substrate 100, wherein the ceramic base 101 of the ceramic substrate 100 is made of a low-temperature sintered ceramic substrate, and the materials of the pad 102 are gold, nickel, and silver in order from the surface layer downward; an annular loop belt 200 arranged on the periphery of the combined board, and the materials are gold, nickel, and silver in order from the surface layer downward; a first metal belt 301 for connecting adjacent ceramic substrates 100, and the material is metallic silver; a second metal belt 302 for connecting the ceramic substrate 100 with the annular loop belt 200, and the material is metallic silver; a closed insulating layer 400 is covered on the surface of the first metal belt 301 and the second metal belt 302, and the material is polyimide with a thickness of 30um.

[0064] Example 3

[0065] The combined plate of the CSP ceramic substrate of this embodiment is prepared by the following method.

[0066] (1) Add micron-sized alumina powder to an organic solvent such as xylene or ethanol, and add appropriate amounts of dispersant, PVB resin and plasticizer to fully mix the mixture. After removing air bubbles by vacuum, the mixture is tape-casted to form a green porcelain tape.

[0067] (2) drilling and filling holes in the green porcelain tape, and then screen printing electrodes on the upper and lower surfaces of the green body with tungsten-molybdenum slurry, and then cutting and high-temperature co-firing in a high-temperature reducing kiln at 1500-1600 degrees to form a first semi-finished product;

[0068] The first semi-finished product includes: a ceramic substrate 100; an annular loop belt 200 arranged on the periphery of the combined plate; a first metal belt 301 for connecting adjacent ceramic substrates 100; a second metal belt 302 for connecting the ceramic substrate 100 and the annular loop belt 200; the annular loop belt 200, the first metal belt 301 and the second metal belt 302 are all made of tungsten-molybdenum alloy.

[0069] (3) A mask plate is prepared, and the mask plate can be omitted at the corresponding positions of the first metal strip 301 and the second metal strip 302. The ceramic slurry with the same solid component as in step (1) is transferred to the above-mentioned mask plate, and the positions are aligned. The surface of the first metal strip 301 and the second metal strip 302 of the above-mentioned first semi-finished product is scraped and printed. After the solvent of the ceramic slurry evaporates, it is solidified to form a closed insulating layer 400. The material of the above-mentioned closed insulating layer 400 is exactly the same as that of the ceramic substrate, and the thickness is 10um, forming a second semi-finished product.

[0070] (4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt 200 is energized. The nickel ions and gold ions are sequentially plated onto the surface of the pad 102 of the ceramic substrate under the action of the electric field, thereby forming a composite board of the CSP ceramic substrate.

[0071] like Figures 1 to 3 As shown, the combined plate structure of the CSP ceramic substrate of this embodiment includes: a ceramic substrate 100, wherein the ceramic base 101 of the ceramic substrate 100 is alumina ceramic, and the materials of the pad 102 are gold, nickel, and tungsten-molybdenum alloy from the surface layer downward; an annular loop belt 200 arranged on the periphery of the combined plate, and the materials are gold, nickel, and tungsten-molybdenum alloy from the surface layer downward; a first metal belt 301 for connecting adjacent ceramic substrates 100, and the material is metal tungsten-molybdenum; a second metal belt 302 for connecting the ceramic substrate 100 with the annular loop belt 200, and the material is metal tungsten-molybdenum; a closed insulating layer 400 is covered on the surface of the first metal belt 301 and the second metal belt 302, and the material is alumina ceramic, which is exactly the same as the ceramic base, and the thickness is 10um.

[0072] The application of the composite plate of the CSP ceramic substrate of this embodiment is as follows.

[0073] The above-mentioned CSP ceramic substrate assembly board is used in the field of quartz crystal packaging. The above-mentioned quartz crystal chip is welded to the above-mentioned array-distributed ceramic substrate through a flip chip process. After the chip is packaged and tested, the ceramic substrate assembly board is sliced ​​and cut to form a single quartz crystal oscillator.

[0074] Example 4

[0075] The combined plate of the CSP ceramic substrate of this embodiment is prepared by the following method.

[0076] (1) A micron-level low-temperature sintered ceramic powder, comprising 40-60% alumina crystal particles and 60-40% Ca-Al-Si amorphous glass, is added to an organic solvent such as xylene and ethanol, and an appropriate amount of dispersant, PVB resin and plasticizer are added to fully mix the slurry. After vacuum removal of bubbles, the slurry is tape-casted to form a green ceramic tape.

[0077] (2) drilling and filling holes in the green porcelain tape, and then screen-printing electrodes on the upper and lower surfaces of the green body with silver paste, and then slitting and low-temperature co-firing in an air atmosphere at 850 to 900 degrees to form a first semi-finished product;

[0078] The first semi-finished product includes: a ceramic substrate 100; an annular loop belt 200 arranged on the periphery of the combined plate; a first metal belt 301 for connecting adjacent ceramic substrates 100; a second metal belt 302 for connecting the ceramic substrate 100 and the annular loop belt 200; the annular loop belt 200, the first metal belt 301 and the second metal belt 302 are all made of metallic silver.

[0079] (3) A mask plate is prepared, and the mask plate can be omitted at the corresponding positions of the first metal strip 301 and the second metal strip 302. The low-temperature sintered ceramic powder slurry that evaporates and solidifies quickly is transferred to the above-mentioned mask plate, and the position is aligned. The surface of the first metal strip 301 and the second metal strip 302 of the above-mentioned first semi-finished product is scraped and printed. After the solvent of the low-temperature sintered ceramic powder slurry evaporates through a heating oven, it is solidified to form a closed insulating layer 400. The material of the above-mentioned closed insulating layer 400 is low-temperature sintered ceramic with a thickness of 1um, forming a second semi-finished product.

[0080] (4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt 200 is energized. The nickel ions and gold ions are sequentially plated onto the surface of the pad 102 of the ceramic substrate under the action of the electric field, thereby forming a composite board of the CSP ceramic substrate.

[0081] like Figures 1 to 3 As shown, the combined board of CSP ceramic substrates of this embodiment comprises: a ceramic substrate 100, wherein the ceramic base 101 of the ceramic substrate 100 is made of a low-temperature sintered ceramic substrate, and the materials of the pad 102 are gold, nickel and silver in order from the surface layer downward; an annular loop belt 200 arranged on the periphery of the combined board, and the materials are gold, nickel and silver in order from the surface layer downward; a first metal belt 301 for connecting adjacent ceramic substrates 100, and the material is metallic silver; a second metal belt 302 for connecting the ceramic substrate 100 with the annular loop belt 200, and the material is metallic silver; a closed insulating layer 400 is covered on the surface of the first metal belt 301 and the second metal belt 302, and the material is a low-temperature sintered ceramic body same as the ceramic base, and the thickness is 1 um.

[0082] Comparative Examples 1 to 4

[0083] Comparative Examples 1 to 4 correspond to Examples 1 to 4 in sequence, and correspond to the composite plate structure of the CSP ceramic substrate, but do not contain the enclosed insulating layer 400, and the rest of the structures are the same, such as Figure 4 shown.

[0084] The electrode fabrication area and the surface area after gold plating of the above-mentioned embodiments 1 to 4 and comparative examples 1 to 4 were measured by an image measuring instrument, and the coplanar flatness of the pads on the surface of the ceramic substrate was measured by a surface profilometer. The specific parameters are shown in Table 1.

[0085] Table 1

[0086]

[0087] The combined plates of the CSP ceramic substrates of Example 4 and Comparative Example 4 were mechanically cut, and the cross-sections were observed using a SEM scanning electron microscope to observe the bonding degree between the second metal band 302 and the ceramic body, respectively. Figure 5 and Figure 6 As can be seen from the figure, after mechanical slitting, the second metal belt 302 of the combined plate of the CSP ceramic substrate of Example 4 is well bonded to the ceramic substrate; while after mechanical slitting, the second metal belt 302 on the surface of the combined plate of the CSP ceramic substrate of Comparative Example 4 has obvious cracks with the ceramic substrate, and such a ratio is relatively high in mass production.

[0088] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0089] Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. Ordinary technicians in the field can change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite board of CSP ceramic substrates, the composite board comprising a composite board formed by a plurality of ceramic substrates (100) arranged in parallel vertically and horizontally; an annular loop belt (200) arranged at the periphery of the composite board; a first metal belt (301) for connecting adjacent ceramic substrates (100); and a second metal belt (302) for connecting the ceramic substrate (100) and the annular loop belt (200); characterized in that: A sealed insulating layer (400) is coated on the surfaces of the first metal strip (301) and the second metal strip (302); The ceramic substrate (100) comprises a ceramic base (101) and a soldering pad (102), wherein two soldering pads (102) are arranged in parallel on the ceramic base (101); The material of the sealed insulating layer (400) is insulating mineral or insulating plastic; The material of the insulating mineral is the same as the material of the ceramic matrix (101) of the ceramic substrate (100); The preparation method comprises the following steps: Step 1) adding micron-sized alumina powder to xylene and ethanol organic solvents, and adding dispersant, PVB resin and plasticizer, mixing the mixture thoroughly, removing bubbles by vacuum, and then tape casting to form a green porcelain tape; Step 2) drilling and filling holes in the green porcelain tape, and then screen printing electrodes on the upper and lower surfaces of the green body with tungsten slurry, and then cutting and high-temperature co-firing in a high-temperature reducing kiln at 1500-1600 degrees to form a first semi-finished product; Step 3) preparing a mask plate, which is printed at corresponding positions of the first metal strip (301) and the second metal strip (302), transferring a fast-evaporating and solidifying acrylic concentrated solution onto the mask plate, aligning the positions, and scraping and printing on the surfaces of the first metal strip (301) and the second metal strip (302) of the first semi-finished product, after the solvent of the acrylic concentrated solution evaporates, solidifies to form a closed insulating layer (400), the closed insulating layer (400) is made of acrylic and has a thickness of 35-50 um, to form a second semi-finished product; Step 4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt (200) is energized, so that the nickel ions and gold ions are sequentially plated onto the surface of the pad (102) of the ceramic substrate (100) under the action of the electric field, thereby forming a composite board of the CSP ceramic substrate.

2. The method for preparing a composite board of a CSP ceramic substrate according to claim 1, characterized in that: The annular loop belt (200) is in the shape of a square, and dicing marking blocks are arranged at equal intervals on each side.

3. The method for preparing a composite board of a CSP ceramic substrate according to claim 1, characterized in that: The sealed insulating layer (400) has a thickness of 1-50 um.

4. The method for preparing a composite board of a CSP ceramic substrate according to claim 1, characterized in that: The combined plate is prepared by a multi-layer co-fired ceramic process.

5. A method for preparing a composite board of CSP ceramic substrates, the composite board comprising a composite board formed by a plurality of ceramic substrates (100) arranged in parallel vertically and horizontally; an annular loop belt (200) arranged on the periphery of the composite board; a first metal belt (301) for connecting adjacent ceramic substrates (100); and a second metal belt (302) for connecting the ceramic substrate (100) and the annular loop belt (200); characterized in that: A sealed insulating layer (400) is coated on the surfaces of the first metal strip (301) and the second metal strip (302); The ceramic substrate (100) comprises a ceramic base (101) and a soldering pad (102), wherein two soldering pads (102) are arranged in parallel on the ceramic base (101); The material of the sealed insulating layer (400) is insulating mineral or insulating plastic; The material of the insulating mineral is the same as the material of the ceramic matrix (101) of the ceramic substrate (100); The preparation method comprises the following steps: Step 1) adding micron-level low-temperature sintered ceramic powder to xylene and ethanol organic solvents, and adding dispersant, PVB resin and plasticizer, fully mixing, vacuuming to remove bubbles, and then casting to form a green ceramic tape; Step 2) drilling and filling holes in the green porcelain tape, and then screen-printing electrodes on the upper and lower surfaces of the green body with silver paste, and then slitting and low-temperature co-firing in an air atmosphere at 850-900 degrees to form a first semi-finished product; Step 3) preparing a mask plate, which is printed at corresponding positions of the first metal strip (301) and the second metal strip (302), transferring a fast volatilizing and curing polyimide concentrated solution onto the mask plate, aligning the positions, and scraping and printing on the surfaces of the first metal strip (301) and the second metal strip (302) of the first semi-finished product. After the solvent of the concentrated polyimide solution evaporates, it is cured to form a closed insulating layer (400), the closed insulating layer (400) is made of polyimide and has a thickness of 20-40 um, thereby forming a second semi-finished product; Step 4) The second semi-finished product is sequentially immersed in a plating bath containing nickel ions and gold ions, and the annular loop belt (200) is energized, so that the nickel ions and gold ions are sequentially plated onto the surface of the pad (102) of the ceramic substrate (100) under the action of the electric field, thereby forming a composite board of the CSP ceramic substrate.

6. A CSP ceramic substrate assembly board according to claim 5, characterized in that: The low-temperature sintered ceramic powder contains 40-60% of aluminum oxide crystal particles and 40-60% of Ca-Al-Si amorphous glass, and the sum of the two components is 100%.