Wing tip, wing tip forming mold and forming method

The composite wingtip molding is performed through the removable upper and lower molds, and the supporting ribs are glued on the mold, which solves the problems of difficulty and high mold cost of composite wingtip molding, and achieves efficient and accurate wingtip molding and assembly.

CN112873897BActive Publication Date: 2024-11-26科泰思创新技术(江苏)股份有限公司
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202110269337.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-11-26
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

The molding of composite wing tips is difficult, especially in male molding methods, because the shape of the wing tip is special and complex, it makes it difficult to demold.

Method used

The upper and lower molds that can be detachably connected are used to form the product cavity through the clamping of the upper and lower molds, and strips are laid at the opening for co-curing, ensuring the pneumatic surface accuracy and mechanical properties of the wingtip. After co-curing, the supporting ribs are directly bonded to the mold to reduce positioning errors and assemble the mold.

Benefits of technology

It reduces the difficulty of forming the wingtip, ensures the accuracy and mechanical properties of the pneumatic surface, reduces mold costs and production costs, and improves assembly efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112873897B_ABST
    Figure CN112873897B_ABST
Patent Text Reader

Abstract

The present invention provides a wing tip, a wing tip forming mold and a forming method, wherein the wing tip forming mold comprises an upper mold and a lower mold detachably connected to the upper mold; a first paving cavity is arranged in the upper mold, and a second paving cavity is arranged in the lower mold; a first groove is arranged on the upper mold, and a second groove is arranged on the lower mold; when the upper mold and the lower mold are molded together, the first paving cavity and the second paving cavity are enclosed to form a product cavity, and the first groove and the second groove are enclosed to form an opening. The wing tip forming mold provided by the present invention can lay the prepreg layers of the upper skin and the lower skin respectively through the detachably connected upper mold and the lower mold, which is easy to operate, solves the problem that the wing tip is difficult to lay due to the complex structure, and reduces the difficulty of forming the wing tip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite material molding, and in particular to a wing tip, a wing tip molding die and a molding method. Background Art

[0002] The wing tip is similar in shape to the wing and is installed at the edge of the wing at a certain angle to the plane where the wing is located. The wing tip can significantly change the flow field near the wing, weaken the wing tip vortex, and reduce the energy consumption directly related to drag. The wing tip can be used to improve the efficiency of the fixed-wing aircraft wing, and can also be used to improve the aircraft's handling characteristics.

[0003] With the advancement of science and technology, composite materials such as carbon fiber are playing an increasingly important role in the aerospace field with their excellent characteristics such as high strength, high modulus, designability, corrosion resistance, fatigue resistance, and easy overall molding. The use of composite materials on the wingtips can significantly reduce weight and improve flight efficiency.

[0004] At present, in the production process of composite wing tips, if the positive mold forming method is adopted, the wing tip has a special and complex shape and is difficult to demould, resulting in greater difficulty in forming the wing tip. Summary of the invention

[0005] The problem solved by the present invention is that it is currently difficult to form a composite material wing tip.

[0006] In order to solve the above problems, the present invention provides a wing tip forming mold, comprising an upper mold and a lower mold detachably connected to the upper mold; a first paving cavity is arranged in the upper mold, and a second paving cavity is arranged in the lower mold; a first groove is arranged on the upper mold, and a second groove is arranged on the lower mold; when the upper mold and the lower mold are closed, the first paving cavity and the second paving cavity are enclosed to form a product cavity, and the first groove and the second groove are enclosed to form an opening;

[0007] The wing tip forming method comprises the following steps:

[0008] S1: Laying out the prepreg layer of the upper skin in the first laying cavity of the upper mold, and laying out the prepreg layer of the lower skin in the second laying cavity of the lower mold;

[0009] S2: closing the upper mold and the lower mold;

[0010] S3: laying a strip through the opening at the junction of the prepreg ply of the upper skin and the prepreg ply of the lower skin;

[0011] S5: co-curing the prepreg plies of the upper skin and the prepreg plies of the lower skin to obtain a wing tip body;

[0012] S6: forming the supporting ribs;

[0013] S7: gluing the support rib to the wing tip body through the opening, and performing gluing and curing at room temperature;

[0014] S8: Demould and obtain the wing tip.

[0015] Optionally, at least one positioning card plate is further included; the positioning card plate includes a first connecting plate and a second connecting plate connected to each other, the first connecting plate is fixedly connected to the lower mold; the second connecting plate is connected to the supporting rib of the wing tip.

[0016] Optionally, it also includes a vacuum bag arranged in the product cavity, and a baffle arranged outside the opening; the upper mold and the lower mold are both detachably connected to the baffle.

[0017] Optionally, a first air filling hole and a first pressure measuring hole are provided on the baffle; a second air filling hole and a second pressure measuring hole are provided on the vacuum bag; the first air filling hole is communicated with the second air filling hole, and the first pressure measuring hole is communicated with the second pressure measuring hole.

[0018] Optionally, in step S1, laying the prepreg ply of the upper skin in the first laying cavity of the upper mold includes: at the junction of the upper skin and the lower skin, the first layer of prepreg ply of the upper skin extends outward by a first preset length relative to the boundary line of the upper mold to form a first overlapping layer; and laying the prepreg ply of the lower skin in the second laying cavity of the lower mold includes: at the junction of the upper skin and the lower skin, the outermost layer of prepreg ply of the lower skin extends outward by a second preset length relative to the boundary line of the lower mold to form a second overlapping layer.

[0019] Optionally, before gluing the support rib into the wing tip body in step S7, the method further includes: positioning the support rib by a positioning clamp.

[0020] Optionally, it also includes:

[0021] S4: placing a vacuum bag in the product cavity, inflating the vacuum bag, and connecting a baffle to the outside of the opening.

[0022] Optionally, it also includes:

[0023] S4: Place the vacuum bag in the product cavity, connect the baffle to the outside of the opening, and inflate the vacuum bag through the first inflation hole and the second inflation hole, and measure the pressure in the vacuum bag through the first pressure measuring hole and the second pressure measuring hole.

[0024] Another object of the present invention is to provide a wing tip, which is formed using the wing tip forming mold as described above.

[0025] Compared with the prior art, the wing tip forming mold provided by the present invention has the following advantages:

[0026] The wingtip forming mold provided by the present invention can respectively lay the prepreg layers of the upper skin and the lower skin through the detachably connected upper mold and the lower mold, which is easy to operate, solves the problem that the wingtip is difficult to lay due to the complex structure of the wingtip, reduces the molding difficulty of the wingtip, and at the same time, can ensure the accuracy of the aerodynamic shape surface of the wingtip; then, the upper mold and the lower mold are molded together and co-cured to obtain a wingtip with an integrated structure; through the opening in the wingtip forming mold, on the one hand, a strip can be laid at the connection between the upper skin and the lower skin, thereby improving the integrity of the wingtip skin and improving the mechanical properties of the wingtip; on the other hand, through the opening, after co-curing, the support rib can be directly glued to the wingtip forming mold without re-positioning the skin, thereby reducing the positioning error, improving the assembly efficiency, and reducing the assembly mold, thereby greatly reducing the mold cost and reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The structure of the wing tip forming mold in the present invention is shown in FIG. Figure 1 ;

[0028] Figure 2 The structure of the wing tip forming mold in the present invention is shown in FIG. Figure 2 ;

[0029] Figure 3 It is a schematic diagram of the structure of the prepreg layer in the present invention;

[0030] Figure 4 It is a simplified structural diagram of the wing tip in the present invention.

[0031] Description of reference numerals:

[0032] 1-upper mold; 11-first groove; 2-lower mold; 21-second groove; 3-lifting ring; 4-positioning card plate; 41-first connecting plate; 42-second connecting plate; 5-baffle; 51-first inflation hole; 52-first pressure measuring hole; 6-upper skin; 61-first overlapping layer; 7-lower skin; 71-second overlapping layer; 8-support rib; 81-first support plate; 82-second support plate; 83-third support plate; 9-strip. DETAILED DESCRIPTION

[0033] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but are not to be construed as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.

[0034] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "circumferential", "radial" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0035] In addition, the terms "first" and "second" are only used to simplify the description and cannot be understood as indicating or implying relative importance, or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0036] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" the first feature may include that the first feature is in direct contact with the second feature, or may include that the first feature and the second feature are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" the second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" the second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0038] The wing tip usually has an irregular curved surface structure and a complex shape. When a male mold is used to mold the composite wing tip, demolding is difficult, resulting in greater difficulty in molding the composite wing tip.

[0039] In order to solve the problem that the current composite material wing tip molding is difficult, the present invention provides a wing tip molding die, see Figure 1 As shown, the wing tip forming mold includes an upper mold 1 and a lower mold 2 detachably connected to the upper mold 1; the detachable connection method can be any common detachable connection method such as a snap connection, and the present application preferably uses a fastener to connect the detachable connection method, that is, the present application preferably uses a fastener to connect the upper mold 1 and the lower mold 2; a first paving cavity is provided in the upper mold 1, and a second paving cavity is provided in the lower mold 2; a first groove 11 is provided on the upper mold 1, and a second groove 21 is provided on the lower mold 2; wherein the first paving cavity is used to pave the upper skin 6 of the wing tip The first paving cavity is used for paving, and the second paving cavity is used for paving the lower skin 7 of the wing tip; the shapes of the first paving cavity and the second paving cavity are determined according to the outer shape of the wing tip to be formed, and the present application does not limit the specific structure and size of the first paving cavity and the second paving cavity; when the upper mold 1 and the lower mold 2 are closed, the upper mold 1 and the lower mold 2 are connected by fasteners, and the first paving cavity and the second paving cavity are enclosed to form a product cavity, and the shape and size of the product cavity are consistent with the wing tip to be formed; the first groove 11 and the second groove 21 are enclosed to form an opening.

[0040] Specifically, the present application preferably adopts a rectangular parallelepiped structure as the wing tip forming mold, wherein the upper mold 1 and the lower mold 2 are connected by two connecting surfaces with curved cross-sections, that is, the lower surface of the upper mold 1 matches the upper surface of the lower mold 2, wherein the first paving cavity is located at the lower surface of the upper mold 1, and the second paving cavity is located at the upper surface of the lower mold 2; when the wing tip is formed, the upper mold 1 and the lower mold 2 are disassembled, and then the prepreg ply of the upper skin 6 and the prepreg ply of the lower skin 7 are paved in the first paving cavity and the second paving cavity respectively; after the paving is completed, the upper mold 1 and the lower mold 2 are assembled. The molds are closed, and the lower surface of the upper mold 1 contacts the upper surface of the lower mold 2. At this time, the first paving cavity and the second paving cavity are combined to form a product cavity, and the prepreg ply in the first paving cavity contacts the prepreg ply in the second paving cavity; after the upper mold 1 and the lower mold 2 are connected and locked by fasteners, the prepreg plies in the upper mold 1 and the lower mold 2 are further co-cured, so that the upper skin 6 and the lower skin 7 are co-cured into an integrated structure, and the shape is consistent with the product cavity. The composite material structure after molding is recorded as the wingtip body in this application. The specific co-curing method can be selected from the existing composite material curing method that is compatible with the material of the prepreg ply, and this application does not specifically limit the co-curing method.

[0041] In order to reduce the difficulty of mold closing and improve the mold closing accuracy, a matching positioning structure can be provided on the upper mold 1 and the lower mold 2. The positioning structure can be a positioning pin and a positioning hole matching the positioning pin.

[0042] The wing tip forming mold provided in the present application also includes a lifting ring 3, so as to facilitate operations such as lifting the wing tip forming mold through the lifting ring 3; in the present application, preferably, both the upper mold 1 and the lower mold 2 are provided with a lifting ring 3.

[0043] In the present application, the position and shape of the first groove 11 and the second groove 21 are determined according to the position and shape of the opening part in the wing tip; when the upper mold 1 and the lower mold 2 are closed, since the first groove 11 and the second groove 21 enclose an opening part, at the opening part, the prepreg layers in the first laying cavity and the second laying cavity are not in contact, therefore, after co-curing, an opening structure is formed at a position corresponding to the opening part on the wing tip body.

[0044] In order to further improve the mechanical properties of the wing tip, after the prepreg plies in the first laying cavity and the second laying cavity are laid and the upper mold 1 and the lower mold 2 are closed, the strip 9 can be laid at the connection between the prepreg plies of the upper skin 6 and the prepreg plies of the lower skin 7 through the opening of the wing tip forming mold, and then the strip 9 and the prepreg plies of the upper skin 6 and the prepreg plies of the lower skin 7 are co-cured at the same time, and the prepreg plies are connected by the strip 9 to improve the integration of the upper skin 6 and the lower skin 7, thereby improving the connection strength between the upper skin 6 and the lower skin 7 in the wing tip.

[0045] In addition, the wingtip molding mold provided in the present application can also connect at least one supporting rib 8 in the molded wingtip body through the opening on the wingtip molding mold after co-curing molding, thereby obtaining a wingtip with supporting ribs 8 inside, so as to further improve the mechanical properties of the wingtip through the supporting ribs 8.

[0046] The support rib 8 can be manufactured by a positive mold forming method, and the mold material of the support rib 8 is preferably aluminum alloy. When designing the mold, the thermal expansion coefficient is considered and the mold is scaled proportionally to ensure that the final size of the support rib 8 meets the requirements; after the support rib 8 is cured, the temperature is lowered and the mold shrinks to facilitate demoulding of the support rib 8; the present application further prefers that the support rib 8 is connected to the wing tip body by gluing; the specific structural form and number of the support rib 8 can be selected according to actual needs, and the present application prefers that the number of the support rib 8 is three.

[0047] Furthermore, to facilitate gluing of the support ribs 8, the present application preferably comprises at least one positioning card plate 4, wherein the specific number of the positioning card plates 4 is determined according to the number of the support ribs 8. For the present application, the preferred number of the positioning card plates 4 is three; specifically, the present application preferably comprises a first connecting plate 41 and a second connecting plate 42 connected to each other, the first connecting plate 41 is fixedly connected to the lower mold 2; the second connecting plate 42 is connected to the support ribs 8 of the wing tip, so that when the support ribs 8 are glued, the support ribs 8 are positioned and fixed by the positioning card plates 4, which can improve the connection accuracy of the support ribs 8 while ensuring the connection strength of the support ribs 8.

[0048] For further information, see Figure 2 As shown, the present application preferably comprises the wing tip forming mold further comprising a vacuum bag arranged in the product cavity, and a baffle 5 arranged outside the opening; the upper mold 1 and the lower mold 2 are both detachably connected to the baffle 5 .

[0049] When the wingtip is formed by the wingtip forming mold, the upper mold 1 and the lower mold 2 are closed, and after the strip 9 is laid, a vacuum bag suitable for the product cavity is placed in the product cavity, and the vacuum bag is inflated, and the baffle 5 is further connected to the outside of the opening so that the inflated vacuum bag can support the internal space of the product cavity to ensure the shape and quality of the wingtip skin; the present application further prefers that the baffle 5 is detachably connected to the upper mold 1 and the lower mold 2 by fasteners.

[0050] After the curing and molding is completed, the baffle 5 is disassembled, the gas in the vacuum bag is exhausted, and then the exhausted vacuum bag is taken out from the inside of the molded wing tip body, which is convenient, fast and easy to operate.

[0051] The vacuum bag may be made of common materials such as plastic. In the present application, the vacuum bag is preferably made of silicone rubber to avoid damage to the vacuum bag during use, extend the service life of the vacuum bag, and reduce loss.

[0052] Furthermore, to facilitate operation, the present application preferably provides a first inflation hole 51 and a first pressure measuring hole 52 on the baffle 5; a second inflation hole and a second pressure measuring hole are provided on the vacuum bag; the first inflation hole 51 is communicated with the second inflation hole, and the first pressure measuring hole 52 is communicated with the second pressure measuring hole, so that during use, after the vacuum bag is placed in the product cavity, the vacuum bag is inflated through the first inflation hole 51 and the second inflation hole, and the pressure in the vacuum bag is measured through the first pressure measuring hole 52 and the second pressure measuring hole, so as to reduce the difficulty of inflation while improving the accuracy of pressure control in the vacuum bag, thereby ensuring the quality of the formed wingtip while improving safety, and improving the consistency and stability of the wingtip quality.

[0053] The wingtip forming mold provided by the present invention can lay the prepreg layers of the upper skin 6 and the lower skin 7 respectively during the forming process through the detachably connected upper mold 1 and the lower mold 2, which is easy to operate, solves the problem that the wingtip is difficult to lay due to the complex structure, reduces the difficulty of forming the wingtip, and at the same time, can ensure the accuracy of the aerodynamic shape surface of the wingtip; then, the upper mold 1 and the lower mold 2 are molded together and co-cured to obtain a wingtip with an integrated structure; through the opening in the wingtip forming mold, on the one hand, the strip 9 can be laid at the connection between the upper skin 6 and the lower skin 7, thereby improving the integrity of the wingtip skin and the mechanical properties of the wingtip; on the other hand, through the opening, the support rib 8 can be directly glued to the wingtip forming mold after co-curing, without the need to re-position the skin, thereby reducing the positioning error, improving the assembly efficiency, and reducing the assembly mold, thereby greatly reducing the mold cost and reducing the production cost.

[0054] Another object of the present invention is to provide a wing tip forming method, which uses the wing tip forming mold as described above for forming; specifically, the wing tip forming method comprises the following steps:

[0055] S1: Laying the prepreg layer of the upper skin 6 in the first laying cavity of the upper mold 1, and laying the prepreg layer of the lower skin 7 in the second laying cavity of the lower mold 2;

[0056] S2: closing the upper mold 1 and the lower mold 2, and connecting the upper mold 1 and the lower mold 2 through a fastener;

[0057] S: through the opening, laying the strip 9 at the junction of the prepreg ply of the upper skin 6 and the prepreg ply of the lower skin 7;

[0058] S5: co-curing the prepreg plies of the upper skin 6 and the prepreg plies of the lower skin 7 to obtain a wing tip body;

[0059] S6: forming the support rib 8;

[0060] S7: gluing the support rib 8 to the wing tip body through the opening, and performing gluing and curing at room temperature;

[0061] S8: Demould and obtain the wing tip.

[0062] The wingtip forming method provided by the present application is that the upper and lower skins of the wingtip are separately laid on the upper mold 1 and the lower mold 2 of the mold, respectively, so there is enough space and the laying is convenient; after the prepreg ply is laid, the upper mold 1 and the lower mold 2 are closed; during the closing process, the position of the upper mold 1 and the lower mold 2 can be adjusted by the positioning structure, and then the upper mold 1 and the lower mold 2 are connected and locked by fasteners, so that the prepreg ply of the upper skin 6 is in contact with the prepreg ply of the lower skin 7; through the opening, at the junction of the prepreg ply of the upper skin 6 and the prepreg ply of the lower skin 7, the strip 9 is laid, and then co-curing is carried out to achieve the connection between the upper skin 6 and the lower skin 7, thereby ensuring the integrity of the wingtip skin.

[0063] During the laying process of the strip 9, in order to prevent bridging, nylon wedges are used to press and flatten the strip 9, and then the strip 9 is co-cured with the upper skin 6 and the lower skin 7 to obtain the wingtip body.

[0064] When the support rib 8 is formed, a positive mold can be used, and the mold is simple.

[0065] When installing the support rib 8, the present application can directly glue the support rib 8 on the wingtip forming mold after the wingtip skin is cured without removing the wingtip body, which can save the assembly tooling for gluing and reduce the tooling cost; since the steps of disassembling the wingtip body from the wingtip forming mold and then assembling the wingtip body on a new tooling for repositioning are reduced, the molding process is simplified and the efficiency of wingtip molding is improved; in addition, since there is no need to reposition the wingtip body when gluing the support rib 8, the gluing assembly accuracy of the support rib 8 is high and the consistency of the wingtip product quality is good.

[0066] Among them, in step S1, laying the prepreg ply of the upper skin 6 in the first laying cavity of the upper mold 1 includes: at the junction of the prepreg ply of the upper skin 6 and the prepreg ply of the lower skin 7, the first layer of prepreg ply of the upper skin 6 extends outward by a first preset length relative to the boundary line of the upper mold 1 to form a first overlapping layer 61; laying the prepreg ply of the lower skin 7 in the second laying cavity of the lower mold 2 includes: at the junction of the prepreg ply of the upper skin 6 and the prepreg ply of the lower skin 7, the outermost layer of prepreg ply of the lower skin 7 extends outward by a second preset length relative to the boundary line of the lower mold 2 to form a second overlapping layer 71.

[0067] The number of prepreg plies of the upper skin 6 and the number of prepreg plies of the lower skin 7 can be set according to demand. In the present application, it is preferred that the number of prepreg plies of the upper skin 6 is the same as the number of prepreg plies of the lower skin 7, and it is further preferred that the number of plies of both is four.

[0068] See also Figure 3As shown, when the prepreg plies of the upper skin 6 are laid, at the joint with the prepreg plies of the lower skin 7, the first layer of prepreg plies of the upper skin 6, that is, the prepreg plies in the prepreg plies of the upper skin 6 close to the inner wall of the first laying cavity, forms a first overlap layer 6; when the prepreg plies of the lower skin 7 are laid, at the joint with the prepreg plies of the upper skin 6, the outermost layer of prepreg plies of the lower skin 7, that is, the prepreg plies away from the inner wall of the second laying cavity, forms a second overlap layer 71; wherein the widths of the first overlap layer 61 and the second overlap layer 71, that is, the values ​​of the first preset length and the second preset length, may be the same or different; the present application preferably has the first preset length being the same as the second preset length, and In one step, the first preset length and the second preset length are preferably both 25 mm; among the prepreg plies of the upper skin 6, except for the first layer of prepreg plies, the other prepreg plies are aligned with the boundary line of the upper mold 1; similarly, among the prepreg plies of the lower skin 7, except for the outermost layer of prepreg plies, the other prepreg plies are aligned with the boundary line of the lower mold 2, and, to facilitate mold closing, during the paving process of the prepreg plies of the lower skin 7, at the docking position of the upper skin 6 and the lower skin 7, all the prepreg plies of the lower skin 7 are folded into the second paving cavity by a second preset length, and for this application, folded 25 mm into the second paving cavity; and an isolation film is placed at the folded position to prevent the folded prepreg plies from sticking to each other.

[0069] The present application prefers that the prepreg plies of the upper skin 6 and the lower skin 7 have the same laying direction, both of which are [±45° / (0 / 90°) / (0 / 90°) / ±45°]; and preferably, the prepreg plies are carbon fiber prepreg plies, the thickness of a single-layer prepreg ply is 0.25mm, and the total thickness of the prepreg plies of the upper skin 6 and the total thickness of the prepreg plies of the lower skin 7 are both 1mm.

[0070] After the prepreg plies of the upper skin 6 and the lower skin 7 are laid, during the mold closing process, the first overlap layer 61 is laid in the second laying cavity of the lower mold 2, and then the 25mm prepreg folded in the prepreg ply of the lower skin 7 is overlapped on the first overlap layer 61. At the same time, the second overlap layer 71 is overlapped on the prepreg ply of the upper skin 6, thereby realizing the overlap of the prepreg plies between the upper skin 6 and the lower skin 7, ensuring the connection strength and surface quality of the upper skin 6 and the lower skin 7.

[0071] After the prepreg plies of the upper skin 6 and the lower skin 7 are overlapped, the prepreg plies of the strip 9 are laid at the connection between the upper skin 6 and the lower skin 7; the present application prefers that the prepreg plies of the strip 9 are carbon fiber prepreg plies, and the number and thickness of the prepreg plies of the strip 9 are consistent with the prepreg plies of the upper skin 6 and the lower skin 7, which are also four layers, and the total thickness of the prepreg plies of the strip 9 is 1 mm.

[0072] In the wing tip forming method provided in the present application, before gluing the support rib 8 into the wing tip body in step S7, the method further includes: positioning the support rib 8 by means of a positioning clamp plate 4 so as to improve the connection strength and positioning accuracy of the support rib.

[0073] The number and shape of the support ribs 8 can be set according to needs. In the present application, the preferred number of the support ribs 8 is three; the number of the positioning clamps 4 is the same as the support ribs 8, which is also three.

[0074] Specifically, after the wingtip body is formed, the corresponding positioning clamp 4 is connected to the lower mold 2 according to the installation position of the support rib 8; the present application preferably connects the positioning clamp 4 to the lower mold 2 through fasteners; after the positioning clamp 4 is installed in place, the spanwise and chordwise positions of the support rib 8 can be guaranteed; then, the support rib 8 and the wingtip skin, that is, the gluing assembly gap between the inner wall of the wingtip body, is adjusted using gaskets, and the present application preferably adjusts the assembly gap to 0.6mm~1.0mm; then, the positioning clamp 4 is used to drill the support rib 8, and two process holes are punched to facilitate the subsequent rapid positioning of the gluing of the support rib 8.

[0075] After positioning is completed, draw a line on the bonding area of ​​the wing tip skin, and apply paper tape to the non-bonding area of ​​the wing tip skin. The width of the paper tape preferably ranges from 25 to 50 mm in this application to prevent overflow of glue from contaminating the wing tip.

[0076] After the lines are drawn, clean up impurities, dust and other debris in the bonding area and protect the bonding area.

[0077] Furthermore, at the center line of the bonding area of ​​the wing tip skin, the adhesive is continuously squeezed out using a glue gun. To ensure the connection strength, bubbles are not allowed to be wrapped in the adhesive. Then, glue is applied to the bonding surface of the support rib 8. During the gluing process, a serrated scraper with a width equal to that of the bonding surface is used to scrape the adhesive into a thin serrated layer of adhesive. Bubbles are not allowed to be wrapped in the adhesive.

[0078] Use the positioning card plate 4 and the process holes on the support rib 8 to quickly position and install the support rib 8. Once the assembly and positioning are completed, unauthorized disassembly or re-positioning is not allowed. Use a clean shaping scraper or scraper to round the corners of the glue joints, tear off the paper tape, and leave it at room temperature for 24 hours to complete the bonding and curing.

[0079] After curing is completed, the positioning clamps 4 are removed respectively, and the fasteners connecting the upper mold 1 and the lower mold 2 are removed to complete the mold separation of the upper mold 1 and the lower mold 2 to obtain the wing tip.

[0080] The wing tip forming method provided by the present invention can respectively lay the prepreg layers of the upper skin 6 and the lower skin 7 through the detachably connected upper mold 1 and the lower mold 2. The operation is convenient and the operation space is large, which solves the problem that the wing tip is difficult to lay due to the complex structure, reduces the difficulty of forming the wing tip, and at the same time, can ensure the accuracy of the aerodynamic shape surface of the wing tip; then the upper mold 1 and the lower mold 2 are molded together and co-cured to obtain a wing tip with an integrated structure; through the opening portion in the wing tip forming mold, on the one hand, the strip 9 can be laid at the connection between the upper skin 6 and the lower skin 7, thereby improving the integrity of the wing tip skin and improving the mechanical properties of the wing tip; on the other hand, through the opening portion, the support rib 8 can be directly glued to the wing tip forming mold after co-curing, without the need to re-position the skin, thereby reducing the positioning error, improving the assembly efficiency, and reducing the assembly mold, thereby greatly reducing the mold cost and reducing the production cost.

[0081] Furthermore, in order to improve the quality of the wing tip, the wing tip forming method provided in the present application also includes:

[0082] S4: placing the vacuum bag in the product cavity, inflating the vacuum bag, and connecting the baffle 5 to the outside of the opening.

[0083] The present application preferably connects the baffle 5 to the upper mold 1 and the lower mold 2 via fasteners; by placing a vacuum bag in the product cavity and inflating the vacuum bag, the quality of the wingtip skin can be ensured through the vacuum bag pressing process.

[0084] In order to further reduce the difficulty of inflating the vacuum bag, the wing tip forming method provided in the present application can also realize the pressurization of the vacuum bag through the following steps. Specifically, the wing tip forming method provided in the present application also includes:

[0085] S4: Place the vacuum bag in the product cavity, connect the baffle 5 to the outside of the opening, and inflate the vacuum bag through the first inflation hole 51 and the second inflation hole. At the same time, measure the pressure in the vacuum bag through the first pressure measuring hole 52 and the second pressure measuring hole, so as to reduce the difficulty of inflation while improving the accuracy of pressure control in the vacuum bag, thereby ensuring the quality of the molded wing tip while improving the consistency and stability of the wing tip quality while improving safety.

[0086] Another object of the present invention is to provide a wing tip, which is formed by using the wing tip forming mold as described above; Figure 4As shown, the wingtip includes an upper skin 6 and a lower skin 7, and the upper skin 6 and the lower skin 7 are an integrated structure, and the upper skin 6 and the lower skin 7 together enclose a wingtip body; a strip 9 is provided in the wingtip body, and the strip 9 is provided at the connection between the upper skin 6 and the lower skin 7; further, at least one supporting rib 8 is also provided in the wingtip body; the present application preferably has three supporting ribs 8; the supporting ribs 8 are used to support the wingtip body to ensure the rigidity and strength of the wingtip.

[0087] In the present application, it is preferred that the materials of the upper skin 6, the lower skin 7, the support ribs 8 and the strips 9 are all carbon fiber composite materials.

[0088] The shape of the support rib 8 can be determined according to actual needs. In the present application, the shape of the support rib 8 is preferably a channel-like steel structure, that is, the support rib 8 includes a first support plate 81, and a second support plate 82 and a third support plate 83 respectively vertically connected to the two sides of the first support plate 81, and the second support plate 82 and the third support plate 83 extend to the same side of the first support plate 81, so as to reduce the weight of the wingtip while ensuring the connection strength between the support rib 8 and the wingtip body through the channel-like steel structure.

[0089] When the support ribs 8 are connected to the wingtip body, the extension directions of the second support plates 82 and the third support plates 83 in all the support ribs 8 may be the same or different. To further ensure the mechanical properties of the wingtip, the present application preferably has the second support plates 82 and the third support plates 82 in opposite extension directions in adjacent support ribs 8, that is, the installation directions of adjacent support ribs 8 are opposite.

[0090] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A wing tip forming mold, characterized in that: The invention comprises an upper mold (1) and a lower mold (2) detachably connected to the upper mold (1); a first paving cavity is arranged in the upper mold (1), and a second paving cavity is arranged in the lower mold (2); a first groove (11) is arranged on the upper mold (1), and a second groove (21) is arranged on the lower mold (2); when the upper mold (1) and the lower mold (2) are molded together, the first paving cavity and the second paving cavity are enclosed to form a product cavity, and the first groove (11) and the second groove (21) are enclosed to form an opening; The wing tip forming method comprises the following steps: S1: laying out the prepreg layer of the upper skin (6) in the first laying cavity of the upper mold (1), and laying out the prepreg layer of the lower skin (7) in the second laying cavity of the lower mold (2); S2: closing the upper mold (1) and the lower mold (2); S3: Laying a strip (9) through the opening at the junction of the prepreg ply of the upper skin (6) and the prepreg ply of the lower skin (7); S5: co-curing the prepreg plies of the upper skin (6) and the prepreg plies of the lower skin (7) to obtain a wing tip body; S6: forming the support rib (8); S7: gluing the support rib (8) into the wing tip body through the opening, and performing gluing and curing at room temperature; S8: Demould and obtain the wing tip.

2. The wing tip forming mold according to claim 1, characterized in that: It also includes at least one positioning card plate (4); the positioning card plate (4) includes a first connecting plate (41) and a second connecting plate (42) connected to each other, the first connecting plate (41) is fixedly connected to the lower mold (2); the second connecting plate (42) is connected to the supporting rib (8) of the wing tip.

3. The wing tip forming mold according to claim 1 or 2, characterized in that: It also includes a vacuum bag arranged in the product cavity, and a baffle (5) arranged outside the opening; the upper mold (1) and the lower mold (2) are both detachably connected to the baffle (5).

4. The wing tip forming mold according to claim 3, characterized in that: The baffle (5) is provided with a first air-filling hole (51) and a first pressure-measuring hole (52); the vacuum bag is provided with a second air-filling hole and a second pressure-measuring hole; the first air-filling hole (51) is in communication with the second air-filling hole, and the first pressure-measuring hole (52) is in communication with the second pressure-measuring hole.

5. The wing tip forming mold according to claim 1, characterized in that: In step S1, laying the prepreg ply of the upper skin (6) in the first laying cavity of the upper mold (1) includes: at the junction of the upper skin (6) and the lower skin (7), the first layer of prepreg ply of the upper skin (6) extends outwardly by a first preset length relative to the boundary line of the upper mold (1), forming a first overlapping layer (61); laying the prepreg ply of the lower skin (7) in the second laying cavity of the lower mold (2) includes: at the junction of the upper skin (6) and the lower skin (7), the outermost layer of prepreg ply of the lower skin (7) extends outwardly by a second preset length relative to the boundary line of the lower mold (2), forming a second overlapping layer (71).

6. The wing tip forming mold according to claim 5, characterized in that: Before gluing the support rib (8) into the wing tip body in step S7, the method further includes: positioning the support rib (8) by means of a positioning card plate (4).

7. The wing tip forming mold according to claim 1, characterized in that: Also includes: S4: placing a vacuum bag in the product cavity, inflating the vacuum bag, and connecting a baffle (5) to the outside of the opening.

8. The wing tip forming mold according to claim 1, characterized in that: Also includes: S4: Place the vacuum bag in the product cavity, connect the baffle (5) to the outside of the opening, and inflate the vacuum bag through the first inflation hole (51) and the second inflation hole, and measure the pressure in the vacuum bag through the first pressure measuring hole (52) and the second pressure measuring hole.

9. A wing tip, characterized in that: The wing tip molding die according to any one of claims 1 to 4 is used for molding.

Citation Information

Patent Citations

  • Integrally-forming method of wing made of fiber reinforced resin matrix composites

    CN103407173A

  • Composite material wing integral molding technological method and composite material wing integral molding tool

    CN104626605A

  • Preparation method for winglet

    CN109016562A

  • Forming technological method of composite aileron of small unmanned aerial vehicle

    CN110193957A

  • Unmanned aerial vehicle composite material horizontal tail silicon rubber thermal expansion compression molding method

    CN111391362A