Engine valve and preparation method thereof, engine, and vehicle

By hot-forged heat-resistant steel at 1150°C to 1250°C, combined with aging, hollow treatment and nitriding heating treatment, the nitride layer is removed, and the problem of insufficient durability of the engine valve at high temperatures is solved, and the strength and fatigue life are improved and creep life, suitable for exhaust valves of high-power engines.

CN112921162BActive Publication Date: 2024-12-03HYUNDAI MOTOR CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202010191940.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-06
Filing Date
2020-03-18
Publication Date
2024-12-03
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

Existing engine valves lack durability at high temperatures, especially the neck durability of exhaust valves, and improvement methods usually increase material cost and valve weight, affecting system performance.

Method used

The heat-forged heat-resistant steel at 1150°C to 1250°C is used for aging and hollowing treatment, and the nitride layer is removed by nitriding heating to improve the durability and physical properties of the valve.

Benefits of technology

The strength and fatigue life of the valve at high temperatures are achieved, the durability deterioration is reduced, and the creep life is improved. It is suitable for exhaust valves for high-power engines without increasing material cost and weight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112921162B_ABST
    Figure CN112921162B_ABST
Patent Text Reader

Abstract

An engine valve and a method for manufacturing the same, an engine, and a vehicle, the method comprising hot forging heat-resistant steel at a temperature of 1,150°C to 1,250°C to form a valve, aging the formed valve, and hollowing the aged valve. In addition, the method comprises nitriding heating the hollow valve and grinding the surface of the neck of the nitriding heated valve to remove a nitride layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2019-0161997, filed on Dec. 6, 2019, which is hereby incorporated by reference in its entirety. Technical Field

[0003] The present disclosure relates to a method of making an engine valve having improved physical properties, such as strength and fatigue life at high temperatures and improved creep life. Background Art

[0004] Referring to the prior art Figure 1 , a hollow engine valve "A" for a vehicle generally includes three components, namely, a valve head "1", a hollow shaft "2" and a shaft end sealant "3". In a hollow engine valve, specifically an exhaust hollow engine valve exposed to high temperature, a material having excellent heat resistance (such as manganese-based heat-resistant steel or nickel-based heat-resistant steel) is applied to the valve head exposed to the highest temperature, and ordinary steel or heat-resistant steel is applied to the hollow shaft and the shaft end sealant.

[0005] Meanwhile, recently developed high-power engines have higher exhaust temperatures than existing engines, and therefore the durability of the neck of the exhaust valve is insufficient. Methods for improving the durability of the neck of the exhaust valve have been proposed, including changing to a material having excellent heat resistance, and methods for ensuring durability by reinforcing the neck shape of the exhaust valve. When changing the material, the material cost increases. In addition, the reinforcement of the neck shape increases the weight of the exhaust valve, thereby increasing the friction and degradation characteristics of the valve system.

[0006] Another developed technology includes a method for manufacturing an engine exhaust valve, in which heat-resistant steel of a specific composition is used as a material, the shape of the exhaust valve consisting of a valve head and a shaft is formed by cold forging or warm forging after performing solid solution treatment, and aging treatment is performed at 600°C to 800°C for 0.5 to 4 hours. However, when this method is performed at 900°C to 1100°C, solid solution treatment cannot be sufficiently performed, which limits the high temperature characteristics of heat-resistant steel. When the manufactured valve is applied, holes or microcracks appear in the neck of the valve head when exposed to high temperatures of 700°C to 800°C for a long time.

[0007] Therefore, there is a need for research and development of a manufacturing method for an engine valve that does not cause an increase in material cost and valve weight, has improved physical properties (such as strength and fatigue life at high temperatures), has less durability deterioration even when exposed to high temperatures for a long time, and has improved creep life. Summary of the invention

[0008] The present disclosure provides a method for preparing an engine valve and an engine valve having improved physical properties such as strength and fatigue life at high temperatures, less durability degradation even when exposed to high temperatures for a long time, and improved creep life of the engine valve.

[0009] The technical problems to be solved by the present inventive concept are not limited to the above-mentioned problems, and any other technical problems not mentioned herein will be clearly understood by those skilled in the art to which the present disclosure pertains from the following description.

[0010] According to aspects of the present disclosure, a method for preparing an engine valve may include hot forging heat-resistant steel at about 1150°C to 1250°C to form a valve, aging the formed valve, hollowing the aged valve, nitriding and heating the hollow valve, and grinding the surface of the neck of the nitriding and heated valve to remove a nitride layer. According to another aspect of the present disclosure, an engine valve is provided, which is made of heat-resistant steel and has a hollow. The valve may include a nitride layer, and the nitride layer may be formed on the surface of the valve other than the neck of the valve. According to aspects of the present disclosure, an engine may include the above-mentioned engine valve. According to another aspect of the present disclosure, a vehicle may include the above-mentioned engine. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The above and other objects, features and advantages of the present disclosure will become more apparent from the following detailed description in conjunction with the accompanying drawings:

[0012] Figure 1 is an exploded cross-sectional view of each component of a conventional engine valve according to the prior art;

[0013] Figure 2 is a cross-sectional view of an engine valve according to an exemplary embodiment of the present invention; and

[0014] Figure 3A-3C 3 are scanning electron microscope (SEM) images of the valve heads of Example 1 and Comparative Examples 1 and 2 measured in Experimental Example 1. DETAILED DESCRIPTION

[0015] It should be understood that the terms "vehicle" or "vehicular" or other similar terms used herein generally include motor vehicles, such as passenger cars, including sport utility vehicles (SUVs), buses, trucks, various commercial vehicles, marine vessels including various watercraft, aircraft, etc., and include hybrid vehicles, electric vehicles, combustion, plug-in hybrid vehicles, hydrogen-powered vehicles and other alternative fuel vehicles (e.g., fuels derived from resources other than petroleum).

[0016] The terms used herein are only for the purpose of describing specific embodiments, and are not intended to limit the present disclosure. As used herein, the singular forms of "one", "an" and "the" are also intended to include plural forms, unless the context clearly indicates otherwise. It will also be understood that the terms "include" and / or "comprise" when used in this specification specify the presence of the features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or their groups. As used herein, the term "and / or" includes any and all combinations of one or more associated listed items.

[0017] Unless otherwise specified or apparent from the context, as used herein, the term "about" should be understood as being within the normal tolerance range in the art, such as within 2 standard deviations of the mean. "About" can be understood as being within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05%, or 0.01% of the stated value. Unless the context clearly indicates otherwise, all numerical values ​​provided herein are modified by the term "about".

[0018] Hereinafter, the present disclosure will be described in detail. As used herein, when a part is said to "comprise" a specific component, it means that it may further include other components, unless otherwise indicated, other components are not excluded. As used herein, when a component is "on" another component, this includes not only when one component is in contact with the other component, but also when the other component is present between the two components.

[0019] Method for preparing engine valve

[0020] The method for preparing an engine valve according to an exemplary embodiment of the present disclosure may include forming the valve by hot forging, performing an aging treatment, a hollow treatment, performing a nitriding heat treatment, and removing a nitride layer. Specifically, when the engine burns, that is, when the engine is exposed to about 700°C to 800°C, the nitride layer diffuses and the density of the nitride layer decreases, generating pores or microcracks in the neck of the head of the nitriding heated valve. The preparation method of the present invention removes the nitride layer on the neck surface of the nitriding heated valve to improve the durability of the valve. In addition, the preparation method can perform hot forging at about 1150°C to 1250°C to fully perform a solid solution treatment, and thus the engine valve can be manufactured to have the maximum physical properties of heat-resistant steel at high temperatures.

[0021] forming

[0022] In this step, the heat-resistant steel may be hot forged at about 1150° C. to 1250° C. to form the valve. The heat-resistant steel is not particularly limited as long as it is a conventional heat-resistant steel. For example, the heat-resistant steel may include one or more selected from the group consisting of SUH35, SUH35NbW, NCF3015, and SUH330NM. In addition, the composition of the heat-resistant steel is shown in Table 1 below.

[0023] Table 1

[0024]

[0025] The treatment may include hot forging at about 1150° C. to 1250° C. for about 15 seconds to 25 seconds. At the above-mentioned treatment time during hot forging at the above-mentioned temperature, the carbides generated in the forging treatment are sufficient to undergo solid solution treatment, coarsening the grains, thereby improving the high temperature performance of the valve. When the hot forging temperature is lower than the above-mentioned range, the solid solution treatment is incomplete, and the carbides generated in the forging treatment cannot be completely solid solution treated, inhibiting the grain growth at high temperature.

[0026] Thereafter, the untreated carbides may coarsen during the aging treatment, reducing the strength of the manufactured valve at high temperatures. Meanwhile, when the hot forging temperature is higher than the above range, forging may occur due to spalling during the hot forging treatment, or grain coarsening due to excessive solution treatment may lead to insufficient carbide precipitation during the aging treatment, thereby reducing the strength of the manufactured valve at high temperatures.

[0027] Perform aging treatment

[0028] In this step, the formed valve is aged. Specifically, the aging treatment enhances the physical properties of the prepared valve at high temperatures, thereby generating sufficient precipitated carbides in the hot forging treatment. The aging treatment may be performed at about 740°C to 780°C for about 0.8 hours to 1.2 hours. When the aging treatment temperature is within the above range, carbide precipitation occurs sufficiently, and when the aging treatment time is outside the above range, carbide precipitation becomes unstable and high temperature characteristics are reduced.

[0029] Hollow processing

[0030] In this step, the valve after aging treatment is hollowed out. There is no particular limitation on the hollowing treatment as long as it is a hollowing treatment method generally used in the manufacture of valves. In addition, the preparation method may further include performing a surface treatment between the hollowing treatment and the nitriding heat treatment. Specifically, the surface treatment may be performed by grinding the surface of the valve after the hollowing treatment. In addition, the surface treatment improves the efficiency of the nitriding heat treatment to grind the surface of the valve after the hollowing treatment to improve the surface roughness.

[0031] Nitriding heat treatment

[0032] In this step, the valve after hollowing is subjected to nitriding heat treatment. Specifically, the nitriding heat treatment improves the wear resistance of the valve. The nitriding heat treatment generally includes salt bath soft nitride treatment or gas soft nitride treatment.

[0033] Removal of nitride layer

[0034] In this step, the surface of the neck of the nitrided heated valve is ground to remove the nitride layer. Generally, when exposed to a high temperature of about 700°C to 800°C for a long time, the nitride layer diffuses and the density decreases, thereby generating holes or microcracks on the surface. However, in this step, the nitride layer on the neck surface of the valve is removed, and therefore, there are no holes or microcracks on the surface, thereby improving the durability of the valve.

[0035] The neck to be ground can be arranged about 10 mm to 40 mm from the inlet having the largest diameter of the valve. Figure 2 , the neck to be ground may be about 10mm to 40mm away from the inlet portion "i" having the maximum diameter, that is, the length "l" of the neck to be ground may be about 5mm to 20mm, or about 8mm to 15mm. In addition, the starting point of the neck to be ground may be about 10mm to 40mm or about 20mm to 30mm away from the inlet "i" having the maximum diameter, that is, the distance "m" between the inlet with the maximum diameter and the starting point of the neck to be ground may be about 10mm to 40mm or about 20mm to 30mm. This step may include grinding the surface of the neck to a depth of about 30μm to 70μm. The method for preparing an engine valve as described above can manufacture an engine valve that maintains existing materials and shapes to prevent an increase in material costs and the weight of the prepared valve and has improved durability.

[0036] Engine valve

[0037] In addition, an engine valve according to another exemplary embodiment of the present disclosure is a valve made of heat-resistant steel and having a hollow and including a nitride layer. The nitride layer may be formed on the surface of the valve except for the neck of the valve. Specifically, the neck may be set to be about 10mm to 40mm away from the inlet with the maximum diameter of the valve. In addition, there is no particular limitation on the heat-resistant steel as long as it is a conventional heat-resistant steel. For example, the heat-resistant steel may include one or more selected from the group consisting of SUH35, SUH35NbW, NCF3015 and SUH330NM.

[0038] Figure 2An engine valve "A" is shown, which may include a valve head "1", a hollow shaft "2" and a shaft end sealant "3". The engine valve "A" may include a nitride layer 10, and the neck of the valve head "1" does not include the nitride layer 10. The engine valve may have an average size of grains of an internal matrix of about 2μm to 5μm or about 2.5μm to 4.0μm. When the average size of the grains of the internal matrix is ​​within the above range, the high temperature creep rupture life is increased. In addition, the engine valve may not include coarsened grains having an average grain size greater than about 5μm.

[0039] In addition, when a static load of about 160 MPa is applied at about 800° C., the rupture time of the engine valve can be about 50 minutes to 70 minutes. The engine valve has excellent physical properties such as strength and fatigue life at a high temperature of about 700° C. to 800° C., so that its durable deterioration is reduced even when exposed to high temperature for a period of time, and the creep life is improved, and is therefore suitable for use as an exhaust valve for a high-power engine.

[0040] Engine and vehicle

[0041] The present disclosure provides an engine including the above-mentioned engine valve. The engine may be a high-power engine. Specifically, the high-power engine may have a power output of about 250hp to 450hp. Compared with conventional engines, high-power engines have higher exhaust temperatures, and the temperature to which the exhaust valve is exposed is also high, requiring the exhaust valve to have improved durability. The engine valve according to the present invention is suitable for use as an exhaust valve of a high-power engine because the durability is less reduced when the engine valve is exposed to high temperatures for a long time. In addition, the present disclosure provides a vehicle including the above-mentioned engine.

[0042] Hereinafter, the present disclosure will be described in more detail with reference to embodiments. However, the embodiments are only used to help understand the present disclosure, and the scope of the present disclosure is not limited to the embodiments in any sense.

[0043] Examples

[0044] Example 1 and Comparative Examples 1 and 2. Preparation of valve head

[0045] Steel grade SUH35NbW was hot forged at the temperature shown in Table 1 below, then cooled with air, and aged at 760° C. for 1 hour to prepare a valve head.

[0046] Experimental example 1.

[0047] For the valve heads of Example 1 and Comparative Examples 1 and 2, tensile strength, creep rupture time, and grain size at high temperature were measured in the following manner, and the results are shown in Table 2 and FIG. 3 .

[0048] (1) Tensile strength at high temperature

[0049] The high temperature tensile strength at 800°C was measured by the KS D 0026 test method.

[0050] (2) Creep rupture time

[0051] The head was heated to 800 °C by high-frequency induction heating, and a static load of 160 MPa was applied to measure the rupture time.

[0052] (3) Grain size

[0053] The grain size of the head was measured by the KS D 0205 test method.

[0054] Table 2

[0055]

[0056] As shown in Table 2 and Figure 3, the valve head of Example 1 has excellent tensile strength at 800°C, long creep rupture time and appropriate grain size. On the other hand, Comparative Example 1 hot forged at low temperature and Comparative Example 2 hot forged at high temperature lack tensile strength at high temperature, and the grains are too small or too large.

[0057] Example 2. Preparation of engine valve

[0058] The valve head of Example 1 was hollowed out, ground on its surface by a conventional processing method for surface treatment, and nitrided and heated by a salt bath soft nitriding method. Then, a neck with a length of 10 mm at 20 mm from the inlet with the maximum diameter of the valve was ground to a depth of 50 μm to remove the nitride layer, thereby forming an engine valve.

[0059] Comparative Example 3

[0060] An engine valve was prepared in the same manner as in Example 2, except that the nitride layer of the neck portion was not removed.

[0061] Experimental Example 2: Evaluation of high temperature fatigue performance of engine valves

[0062] The engine valves of Example 2 and Comparative Example 3 were heated to 800° C. by high-frequency induction heating, and a static load of 160 MPa was applied until they were broken. The results are shown in Table 3.

[0063] Table 3

[0064] High temperature fatigue performance Example 2 <![CDATA[6.3X10 5 ]]> Comparative Example 3 <![CDATA[3.2X10 5 ]]>

[0065] As shown in Table 3, it can be seen that the engine valve of Example 2 in which the nitride layer of the head and neck is removed has a significant advantage in high temperature fatigue performance compared with Comparative Example 3 in which the nitride layer of the neck is not removed.

[0066] As described above, the engine valve prepared by the method for preparing an engine valve maintains the existing material and shape without increasing the material cost and the weight of the prepared valve, and has excellent durability. Specifically, it is shown that the engine valve according to the present disclosure has excellent physical properties, such as strength and fatigue life at high temperatures of 700° C. to 800° C., has less durability degradation even when exposed to high temperatures for a long time, and has improved creep life, and is suitable for use as an exhaust valve for a high-power engine.

[0067] The method for manufacturing an engine valve according to the present disclosure can be formed into an engine valve that maintains existing materials and shapes without increasing the cost of materials and the weight of the manufactured valve, and has improved durability. Specifically, the engine valve according to the present disclosure has excellent physical properties, such as strength and fatigue life at high temperatures of 700° C. to 800° C., has less durability degradation even when exposed to high temperatures for a long time, and has improved creep life, and is suitable for use as an exhaust valve for a high-power engine.

[0068] Although the present disclosure has been described above with reference to exemplary embodiments and the accompanying drawings, the present disclosure is not limited thereto, and those skilled in the art to which the present disclosure belongs may make various modifications and changes to the present disclosure without departing from the spirit and scope of the present disclosure as claimed in the appended claims.

Claims

1. A method for preparing an engine valve, The following steps are involved: Hot forging of heat-resistant steel at 1150°C to 1250°C for valve forming; Aging of the molded valves; Hollow out the aged valves; The hollow valve is ground to perform surface treatment; Nitriding heating is performed on the surface treated hollow valve; The surface of the valve neck that has been heated by nitriding is ground to remove the nitride layer. Therein, the neck to be ground is arranged to be 10 mm to 40 mm away from the inlet having the maximum diameter of the valve.

2. The method according to claim 1, in, The molded valve is aged at 740°C to 780°C for 0.8 to 1.2 hours.

3. The method according to claim 1, in, The molding of the valve includes hot forging at 1,150° C. to 1,250° C. for 15 seconds to 25 seconds.

4. The method according to claim 1, in, Removing the nitride layer includes grinding the surface of the neck portion to a depth of 30 μm to 70 μm.

Citation Information

Patent Citations

  • Preparing method of engine valve

    KR1020210071623A

  • Method for manufacturing hollow sodium inflating valve with closed disc end

    CN103990944A

  • Large crankshaft

    EP3401412A1

  • Forming hollow metallic parts

    GB1386702A

  • Rust proof structure of metallic sliding parts

    JP1995188897A