Stable modified polymer polyol dispersions

By using alkoxysilane group compounds as non-aqueous dispersants in modified polymer polyols, the problem of insufficient stability of polymer particles is solved, improving the performance of polyurethane materials and reducing formaldehyde release.

CN113004511BActive Publication Date: 2024-10-01REPSOL SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011472664.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-20
Filing Date
2020-12-15
Publication Date
2024-10-01
Estimated Expiration
2040-12-15

AI Technical Summary

Technical Problem

The stabilizers used to modify polymer polyols in the prior art are insufficient, causing the polymer particles to be unstable in the matrix polyol and prone to sedimentation or agglomeration, affecting the performance of the polyurethane material.

Method used

New compounds containing alkoxysilane groups are used as non-aqueous dispersants to form stable modified polymer polyol dispersions by reacting with polyether polyols to improve the stability of polymer particles.

Benefits of technology

Significantly improves the stability of modified polymer polyol dispersions, prevents settling and agglomeration, reduces formaldehyde release, and improves the performance and safety of polyurethane materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002836342920000031
    Figure BDA0002836342920000031
  • Figure BDA0002836342920000051
    Figure BDA0002836342920000051
  • Figure BDA0002836342920000061
    Figure BDA0002836342920000061
Patent Text Reader

Abstract

The present disclosure relates to novel compounds useful as dispersants and stabilizers for modified polymer polyol dispersions, stable modified polymer polyol dispersions obtained therefrom, and polyurethane materials prepared from the modified polymer polyol dispersions disclosed herein.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to novel compounds useful as dispersants and stabilizers for polymer-modified polyol dispersions. Background Art

[0002] Various modified polymer polyols are used as raw materials for the production of flexible polyurethane foams and other polyurethane products. They have a continuous phase consisting of one or more compounds with multiple hydroxyl groups ("base polyol") in which other polymers are dispersed in particle form.

[0003] Thus, examples of modified polymer polyols are:

[0004] - PolyHarnststoff dispersion (PHD) polyols, which are modified polymer polyols containing polyurea in dispersed form, which is the polycondensation product of polyamines and polyfunctional isocyanates;

[0005] - grafted polyether polyols synthesized by in situ free radical polymerization of vinyl monomers in liquid polyethers by a batch, semi-continuous or continuous process, wherein the vinyl monomers are generally selected from acrylonitrile, styrene, α-methylstyrene methyl methacrylate, hydroxyalkyl acrylates and methacrylates, vinyl chloride, etc.;

[0006] - polyisocyanate polyaddition (PIPA) polymer polyols, which are dispersions of polyurethane and / or polyurethane-urea particles in liquid polyether polyols, obtained by polymerization of alkanolamines with organic polyisocyanates in the presence of polyols;

[0007] - and recently described polymer polyols comprising a polyether carbonate polyol as base polyol, said polyether carbonate polyol (POPC) being obtainable by a process comprising the steps of copolymerizing one or more H-functional initiator substances, one or more alkylene oxides and carbon dioxide in the presence of a double metal cyanide catalyst (DMC).

[0008] In our previous patent application WO2019008140, a novel modified polymer polyol is disclosed, which comprises at least one base polyol and a stable dispersion of polymer particles in the at least one base polyol, and the modified polymer polyol can be obtained by a method comprising the following steps: preparing polymer particles by a polycondensation reaction of a and b as described below in the presence of the at least one base polyol:

[0009] a. at least one compound with at least one basic nitrogen atom, characterized in that there is at least one hydrogen atom attached to the nitrogen atom in the molecule;

[0010] b. at least one compound having a phosphorus atom selected from the group consisting of:

[0011] b1. a compound having a phosphorus atom selected from the group consisting of at least one hydroxyalkyl phosphine, at least one hydroxyalkyl phosphine salt, at least one hydroxyalkyl phosphine oxide and a combination thereof; or

[0012] b2. Condensation products of a mixture of compounds b1) with at least one compound having at least one basic nitrogen atom.

[0013] For the base polyols used to prepare these modified polymer polyols, they can be polyether polyols or polyester polyols. Polyether polyols can be commercially produced by polymerizing propylene oxide and / or ethylene oxide in the presence of a hydroxyl or amino initiator and a basic catalyst. Polyester polyols are prepared by the polycondensation reaction of multifunctional carboxylic acids and polyhydroxy compounds.

[0014] Among the polyether polyols, reactive polyether polyols and non-reactive polyether polyols can be distinguished. Reactive polyols are polyether polyols terminated with ethylene oxide (EO) and have a polyethylene oxide end block content of 5 to 20% by weight, so they have a high primary hydroxyl content (above 30%), while non-reactive polyols are polyether polyols terminated with propylene oxide (PO) and have mainly secondary hydroxyl groups. Secondary hydroxyl groups are less reactive than primary hydroxyl groups.

[0015] It is known in the art that PIPA and PHD polymer polyols prepared using polyether polyols containing primarily secondary hydroxyl groups result in the formation of polymer particles that are unstable in the base polyol.

[0016] Different methods for stabilizing modified polymer polyols have been proposed. Thus, the introduction of non-aqueous dispersants (NAD) stabilizers during the polymerization process is one of the proposed solutions. The stabilization of polymer dispersions in organic media is based on the principle of steric stabilization, which is ensured by the presence of non-aqueous dispersants (NAD) stabilizers. Thus, for example, in the case of grafted polyether polyols, the NAD comprises in the same chemical structure a segment with a strong affinity for carbocatenary vinyl polymers and a second segment with a strong affinity for liquid polyethers. The NAD is attached to the carbocatenary segments of the polymer at the surface of the solid polymer particles, and the polyether chains located outside the polymer particles in the continuous polyether medium form a steric hindrance, which prevents agglomeration of the polymer particles.

[0017] Different examples of NAD stabilizers are known in the art, however, in view of new developments and different methods of modifying polymer polyols and their different chemical and physical properties, there is currently a need for new stabilizers for modified polymer polyols (including at least one base polyol and a stable dispersion of polymer particles in the at least one base polyol). More specifically, there is a need to provide new stabilizers for modified polymer polyol dispersions (including at least one base polyol and a stable dispersion of polymer particles in the at least one base polyol, wherein the base polyol is a reactive or non-reactive polyether polyol). Summary of the invention

[0018] It has now been found that stable modified polymer polyol dispersions can be prepared by polymerizing one or more polymer particle precursors in the presence of at least one base polyol containing at least one novel alkoxysilane group-modified compound as described below used as a non-aqueous dispersant. The resulting modified polymer polyol dispersions show an improvement in their stability compared to those modified polymer dispersions prepared in the absence of the at least one novel alkoxysilane group-modified compound, i.e., the modified polymer polyol dispersions do not settle during extended storage or at least remain in dispersion form during mixing with other foam-forming ingredients.

[0019] The novel alkoxysilane group-modified compounds disclosed herein are used as non-aqueous dispersants (NADs) for modified polymer polyol dispersions, with the advantage that they are easily prepared under mild reaction conditions, and optionally, they can be prepared in situ in the reaction medium of the modified polymer polyol dispersion. In addition, the novel alkoxysilane group-modified compounds disclosed herein can be used to stabilize modified polymer polyols obtained using reactive polyether polyols or non-reactive polyether polyols as base polyols.

[0020] Therefore, according to the first aspect of the present disclosure, a novel alkoxysilane group-modified compound is provided. The novel alkoxysilane group-modified compound is suitable for use as a NAD stabilizer to prepare a modified polymer polyol dispersion.

[0021] The novel alkoxysilane group-modified compounds disclosed herein can be described as alkoxysilane-terminated polyether polyols having 1 to 8 hydroxyl groups per molecule and 1 to 2 (preferably 1) alkoxysilane groups per molecule. The novel alkoxysilane-terminated polyether polyols can be obtained by a method comprising the following steps: capping 1 to 2 (preferably 1) terminal hydroxyl groups of a polyether polyol having a functionality of 2 to 9 and an average molecular weight of 3000 to 25000 with a capping agent, wherein the capping agent is a compound having at least one alkoxysilane terminal group and at least one hydroxyl-reactive group; wherein the reaction of the capping agent with the polyether polyol is carried out in a molar ratio of 0.05 to 2.0 moles, preferably 0.2 to 1.8 moles, more preferably 0.5 to 1.5 moles, and particularly preferably 0.8 to 1.2 moles of the capping agent per 1 mole of the polyether polyol.

[0022] The novel alkoxysilane group-modified compound of the present invention can be obtained by the following reaction of a) and b):

[0023] a) at least one polyether polyol having a functionality of 2 to 9 and an average molecular weight of 3,000 to 25,000;

[0024] b) at least one alkoxysilane group-containing capping agent, which is a compound of formula (I):

[0025]

[0026] wherein R1, R2 and R3 are each independently selected from a linear or branched (C1-C6) alkyl group, a linear or branched (C1-C6) alkoxy group and a tri(C1-C3) alkylsilyloxy group; provided that at least one of R1, R2 and R3 is a (C1-C6) alkoxy group; and

[0027] wherein A is a group comprising a terminal functional group that can react with a hydroxyl group on a polyether polyol; and

[0028] The reaction of the alkoxysilane group-containing capping agent with the polyether polyol is carried out at a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.5 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the capping agent per 1 mol of the polyether polyol.

[0029] According to some preferred embodiments, A is a group comprising a terminal functional group reactive with a hydroxyl group on a polyether polyol, selected from -NCO and epoxy.

[0030] The alkoxysilane group-modified compounds disclosed herein can be used to stabilize modified polymer polyols; wherein the modified polymer polyol is a polymer polyol in which an organic filler is dispersed. The modified polymer polyol dispersion may preferably be a PIPA polyol, a PHD polyol, or any other polymer polyol known in the art. According to a particularly preferred embodiment, the modified polymer polyol dispersion is a polyol dispersion obtained using a mixture of hydroxyalkyl phosphines (e.g., [bis(hydroxymethyl)phosphino]methanol (THP)) and its derivatives (including salts, oxides, and hemiacetals) as polymer particle precursors.

[0031] It is known that when tetrakis(hydroxymethyl)phosphonium salts (THPX) are reacted with a base (e.g. KOH), a mixture of THP, formaldehyde, salt KX and water is obtained; in addition, depending on the alkaline conditions used, [bis(hydroxymethyl)phosphino]methanol (THPO, also known as tris(hydroxymethyl)phosphine oxide) can also be obtained as a by-product together with THP; in addition, THP and THPO can react with formaldehyde to form the corresponding hemiacetals (mono-, di- and tri-substituted hemiformals of THP and THPO can be found as reaction products). In some cases, the reaction can be carried out in the absence of a base, in which case unreacted THPX may be present in the reaction medium together with the resulting products. The amount of THPO formed depends on the reaction conditions. Alkaline pH values ​​favor the concentration of THPO. Therefore, depending on the conditions used, the reaction product between THPX and a base may be a complex mixture of phosphorus compounds (THP, THPO, their corresponding hemiformals and unreacted THPX), water, the corresponding salts and formaldehyde.

[0032] The chemical names and structures of the above-mentioned THP, THPX, THPO, and the mono-, di- and tri-substituted hemiformals of THP and THPO (mTHP, dTHP, tTHP, mTHPO and dTHPO) are as follows:

[0033]

[0034]

[0035]

[0036] It is desirable to reduce formaldehyde emission without compromising the stability of polyurethane materials prepared using modified polymer polyol dispersions prepared from mixtures of hydroxyalkyl phosphines and their derivatives (including salts, oxides and hemiacetals) as polymer particle precursors, i.e., without agglomeration and precipitation of polymer particles, in particular using modified polymer polyol dispersions prepared according to the method described in WO2019008140.

[0037] The free formaldehyde content can be reduced from a mixture of phosphorus-containing components (i.e. a mixture of THP, its salts, oxides and / or hemiformals) by distillation. Volatile compounds including formaldehyde can be distilled off at a distillation temperature of 50-120° C. under reduced pressure or atmospheric pressure. Unfortunately, the use of the resulting mixture of phosphorus-containing components in the preparation of modified polymer polyols according to the method described in patent application WO2019008140 leads to unstable modified polymer polyols due to agglomeration and precipitation of the polymer particles.

[0038] Therefore, the present disclosure also aims to use the alkoxysilane group-modified compounds disclosed herein in the preparation of modified polymer polyol dispersions, more specifically as stabilizers and dispersants for modified polymer polyol dispersions. Therefore, the alkoxysilane group-modified compounds disclosed herein can be used as dispersants and stabilizers for PHD polyols, PIPA polyols and preferably those modified polymer polyols prepared from mixtures of hydroxyalkyl phosphines and their derivatives (including salts, oxides and hemiacetals) as polymer particle precursors as disclosed in WO2019008140.

[0039] Another aspect of the present invention relates to a stable modified polymer polyol dispersion of polymer particles in a liquid polyol mixture, which can be obtained by a process comprising the steps of: preparing polymer particles by a or b in the presence of a liquid polyol mixture:

[0040] a. in the liquid polyol mixture and under polymerization conditions the following a.1) and a.2) or a.3) reaction

[0041] a.1) at least one compound with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule which is bonded to the nitrogen atom;

[0042] a.2) mixtures of compounds carrying phosphorus atoms, including [bis(hydroxymethyl)phosphino]methanol (THP) and optionally any derivatives thereof, such as tetrakis(hydroxymethyl)phosphonium salts (THPX), [bis(hydroxymethyl)phosphino]methanol (THPO) and its mono-, di- or tris-hemiacetals ({[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), {bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHPO), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHPO) and ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHPO);

[0043] a.3) a mixture of condensation products obtained by reaction of a mixture of compounds carrying phosphorus atoms as described above a.2) with a.1) at least one compound carrying at least one basic nitrogen atom;

[0044] Wherein, the at least one compound having at least one basic nitrogen atom a.1) is selected from

[0045] - melamine, trimethylolmelamine,

[0046] - those compounds of formula (VII) or formula (VIII); and

[0047] - mixtures thereof;

[0048] Wherein, the compound of formula (VII) is as follows:

[0049] R1-NH2 (VII)

[0050] Wherein, R1 is selected from -H, -(C1-C3)alkyl, (C1-C3)alkyl-CO-, NH2-CO-, -(CH2) n -NH2, -CN, -NH2, -SO2NH2, cyclohexyl, phenyl, -SO2OH and -NHCONHNH2; wherein n is an integer from 1 to 18;

[0051] The compound of formula (VIII) is as follows:

[0052]

[0053] wherein R2 is selected from NH=C<, O=C< and S=C<; R3 is selected from H, -CN, -NH2, -CONH2, -CONHCONH2 and -CONHCONHCONH2;

[0054] or

[0055] b. in the liquid polyol mixture and under polymerization conditions, optionally in the presence of a catalyst, reacting the following b.1) with b.2)

[0056] b.1) at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen or oxygen atom; preferably, the at least one co-reactant is selected from an amine, an alkanolamine or a diol;

[0057] b.2) at least one polyisocyanate;

[0058] The liquid polyol mixture comprises at least one base polyol and at least one alkoxysilane group-modified compound as described herein.

[0059] Thus, the stable modified polymer polyols of the present invention comprise a stable dispersion of polymer particles in a liquid polyol mixture comprising at least one base polyol and at least one alkoxysilane group-modified compound as described herein.

[0060] According to one aspect of the present disclosure, there is provided a method for preparing a stable modified polymer polyol dispersion, comprising preparing a liquid polyol mixture of at least one base polyol and at least one alkoxysilane group-modified compound as described herein, and adding a polymer particle precursor to obtain a polymer polyol dispersion in the liquid polyol mixture.

[0061] Thus, according to this aspect of the invention, there is provided a method of preparing a stable modified polymer polyol dispersion, the method comprising mixing the following materials simultaneously or sequentially in any order:

[0062] i. A polymer particle precursor comprising a mixture of:

[0063] - at least one compound a.1) having at least one basic nitrogen atom; and

[0064] - a mixture a.2) of compounds carrying phosphorus atoms as described herein or a mixture a.3) of condensation products

[0065] At least one of the groups consisting of;

[0066] ii. at least one base polyol;

[0067] iii. at least one compound modified with an alkoxysilane group as described herein.

[0068] According to a specific embodiment, the method comprises:

[0069] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described herein, thereby obtaining a liquid polyol mixture;

[0070] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0071] at least one compound a.1) with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule which is bonded to the nitrogen atom; and

[0072] mixtures a.2) of compounds carrying phosphorus atoms, including [bis(hydroxymethyl)phosphino]methanol (THP) and optionally any derivatives thereof, such as tetrakis(hydroxymethyl)phosphonium salts (THPX), [bis(hydroxymethyl)phosphino]methanol (THPO) and its mono-, di- or tris-hemiacetals ({[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), {bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHPO), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHPO) and ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHPO); or

[0073] mixtures a.3) of condensation products obtained by reaction of a mixture a.2) as described above with at least one compound a.1) having at least one basic nitrogen atom;

[0074] Wherein, the compound a.1) having at least one basic nitrogen atom is selected from

[0075] - melamine, trimethylolmelamine,

[0076] - those compounds of formula (VII) or formula (VIII); and

[0077] - mixtures thereof;

[0078] Wherein, the compound of formula (VII) is as follows:

[0079] R1-NH2 (VII)

[0080] Wherein, R1 is selected from -H, -(C1-C3)alkyl, (C1-C3)alkyl-CO-, NH2-CO-, -(CH2) n -NH2, -CN, -NH2, -SO2NH2, cyclohexyl, phenyl, -SO2OH and -NHCONHNH2; wherein n is an integer from 1 to 18;

[0081] The compound of formula (VIII) is as follows:

[0082]

[0083] Wherein, R2 is selected from NH=C<, O=C< and S=C<; R3 is selected from H, -CN, -NH2, -CONH2, -CONHCONH2 and -CONHCONHCONH2.

[0084] According to this first embodiment, the polymer particle precursor is therefore at least one compound a.1) carrying at least one basic nitrogen atom and a mixture a.2) or a mixture a.3); the resulting polymer particles have a high P and N content.

[0085] According to another embodiment, optionally in combination with one or more features of the various embodiments described above or below, the preparation of the modified polymer polyol comprises:

[0086] i. mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described herein, thereby obtaining a liquid polyol mixture;

[0087] ii. optionally in the presence of a catalyst and under polymerization conditions to the liquid polyol mixture obtained in i) simultaneously or in any order sequentially adding the following materials:

[0088] b.1) at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen or oxygen atom; and

[0089] b.2) At least one polyisocyanate.

[0090] Thus, this embodiment provides a polymer polyol blend comprising PIPA and / or PHD particles that have been formed in situ in a liquid polyol mixture containing at least one alkoxysilane group-modified compound as described herein.

[0091] In another aspect of the present disclosure, a method for preparing a polyurethane material is provided, wherein at least one polyisocyanate is reacted with an isocyanate-reactive component comprising at least one stable modified polymer polyol dispersion described herein, optionally in the presence of water and additives such as at least one blowing agent, at least one catalyst, and a surface-active product.

[0092] Another aspect of the present disclosure provides a polyurethane material obtainable by a process comprising the steps of reacting at least one polyisocyanate component with an isocyanate-reactive component comprising at least one stable modified polymer polyol disclosed herein in the presence of at least one catalyst and optionally at least one blowing agent.

[0093] Other aspects of the present disclosure relate to injection molded compositions or articles comprising the polyurethane material described above.

[0094] The modified polymer polyols of the present disclosure are useful in preparing polyurethane materials such as polyurethane foams, adhesives, elastomers, sealants, and coatings; preferably those polyurethane materials having flame retardant properties due to the high content of P and N in the dispersed polymer particles.

[0095] Another aspect of the present disclosure relates to a method of reducing formaldehyde emissions from a polyurethane material by using the modified polymer polyol dispersion described herein to prepare the polyurethane material.

[0096] Another object of the present disclosure is to provide a method for preparing polyurethane foam, wherein the formaldehyde emission measured by the UNE-ISO 16000-[clauses 3, 9 and 11] standard method is less than 100 (μg / m 3 ), preferably less than 10 (μg / m 3 ). The method comprises using the stable modified polymer polyol dispersion described herein to prepare a polyurethane foam. DETAILED DESCRIPTION

[0097] According to some embodiments, optionally in combination with one or more features of the various embodiments described above or below, the alkoxysilane group-modified compound is obtained by reacting a) with b):

[0098] a) at least one polyether polyol having a functionality of 2 to 9 and an average molecular weight of 3,000 to 25,000; and

[0099] b) at least one alkoxysilane group-containing capping agent, which is a compound of formula (I) above; and

[0100] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.5 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0101] Therefore, according to certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, a suitable alkoxysilane group-containing capping agent may be any alkoxysilane group-containing compound of formula (I), wherein A is a group comprising a terminal functional group capable of reacting with a hydroxyl group on a polyether polyol, and the terminal functional group capable of reacting with a hydroxyl group is selected from -NCO and epoxy.

[0102] According to certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, the compound of formula (I) is selected from those compounds, wherein the group A is selected from the group consisting of those compounds of formula (II), (III), (IV), (V) and (VI)

[0103]

[0104] in

[0105] The wavy line indicates the point of attachment to the Si atom in formula (I);

[0106] m, n, p, r, t and w are independently integers selected from 1 to 6;

[0107] q, s and v are independently integers selected from 1 to 4;

[0108] R4 is selected from -NCO, The group,

[0109] Among them, the asterisk indicates the point of connection to the rest of the group;

[0110] X is selected from -O- and -N(R5)-;

[0111] Wherein R5 is selected from H, linear or branched (C1-C6) alkyl, The group,

[0112] Among them, the asterisk indicates the connection point with the N atom;

[0113] x and z are independently an integer selected from 1 to 6;

[0114] R8, R9 and R10 are each independently selected from a linear or branched (C1-C6) alkyl group, a linear or branched (C1-C6) alkoxy group and a tri(C1-C3) alkylsilyloxy group; provided that at least one of R8, R9 or R10 is a (C1-C6) alkoxy group or a tri(C1-C3) alkylsilyloxy group; and

[0115] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0116] According to certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, the compound of formula (I) is a compound wherein R1, R2 and R3 are each independently selected from CH3-O-, CH3CH2-O-, CH3CH2CH2-O-, (CH3)2CH-O-, CH3CH2CH2CH2-O-, (CH3)3CH-O-, (CH3)2CHCH2-O-, CH3-, CH3CH2-, CH3CH2CH2-, (CH3)2CH-, CH3CH2CH2-, (CH3)3CH-, (CH3)2CHCH2-, (CH3)3CH-, (CH3)2CHCH2-, (CH3)3Si-O- and (CH3CH2)3Si-O-; provided that at least one of R1, R2 or R3 is (C1-C3)alkoxy.

[0117] In some specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the compounds of formula (I) are those wherein R1, R2 and R3 are each independently selected from CH3-O-, CH3CH2-O-, CH3-, CH3CH2- and (CH3)3Si-O-; provided that at least one of R1, R2 or R3 is selected from CH3-O- and CH3CH2-O-.

[0118] According to one embodiment of the present invention, optionally in combination with one or more features of the above or below various embodiments, the compound of formula (I) is selected from:

[0119]

[0120] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (II) described above.

[0121] In one embodiment, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from compounds of formula (II), wherein m is an integer from 1 to 6, specifically 1, 2, 3, 4, 5 or 6, more specifically 2 or 3; R4 is -NCO,

[0122] wherein the asterisk indicates the point of attachment to the remaining groups; and

[0123] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0124] According to a specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the compound of formula (I) is selected from (3-isocyanate propyl) trimethoxy silane (also known as 3-(trimethoxysilyl) propyl isocyanate), (3-isocyanate propyl) dimethoxy (methyl) silane, (3-isocyanate propyl) (methoxy) dimethyl silane, (3-isocyanate propyl) dimethoxyethyl silane, diethyl (3-isocyanate propyl) methoxy silane, (3-isocyanate propyl) triethoxy silane (also known as 3-(triethoxysilyl) propyl 1-isocyanate), diethoxy(3-isocyanatepropyl)methylsilane, ethoxy(3-isocyanatepropyl)dimethylsilane, (3-isocyanatepropyl)diethoxy(ethyl)silane, ethoxydiethyl(3-isocyanatepropyl)silane, trimethoxy(2-isocyanateethyl)silane, (2-isocyanateethyl)dimethoxy(methyl)silane, (2-isocyanateethyl)(methoxy)dimethylsilane, ethyl(2-isocyanateethyl)dimethoxysilane, diethyl(2-isocyanateethyl)methoxysilane, triethoxy(2-isocyanateethyl)silane silane, diethoxy(2-isocyanateethyl)methylsilane, ethoxy(2-isocyanateethyl)dimethylsilane, diethoxy(ethyl)(2-isocyanateethyl)silane, ethoxydiethyl(2-isocyanateethyl)silane, triethoxy(isocyanatemethyl)silane, (isocyanatemethyl)trimethoxysilane, trimethoxy({7-oxabicyclo[4.1.0]hept-3-yl}methyl)silane, triethoxy({7-oxabicyclo[4.1.0]hept-3-yl}methyl)silane, trimethoxy(2-{7-oxabicyclo[4.1.0]hept-3-yl}ethyl 1-{7-oxabicyclo[4.1.0]hept-3-yl}propyl)silane, trimethoxy(3-{7-oxabicyclo[4.1.0]hept-3-yl}propyl)silane, triethoxy(4-{7-oxabicyclo[4.1.0]hept-3-yl}butyl)silane and trimethoxy(4-{7-oxabicyclo[4.1.0]hept-3-yl}butyl)silane.

[0125] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (III) above. In one embodiment, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (III), wherein

[0126] n and p are independently an integer selected from 1 to 6, specifically 1, 2, 3, 4, 5 or 6, more specifically 2, 3 or 4; and

[0127] q is an integer selected from 1 to 4, specifically 1, 2, 3 or 4, more specifically 1 or 3.

[0128] According to one embodiment, optionally in combination with one or more features of the various embodiments described above or below, the group A is selected from those compounds of formula (III), wherein

[0129] n and p are independently integers selected from 1, 2, 3 or 4;

[0130] q is an integer selected from 1 or 3;

[0131] X is selected from -O- and -N(R5)-;

[0132] Wherein R5 is selected from H, linear or branched (C1-C6) alkyl, The group,

[0133] Among them, the asterisk indicates the connection point with the N atom;

[0134] x and z are independently an integer selected from 1 to 6;

[0135] R8, R9 and R10 are each independently selected from -CH3, -CH2CH3, -OCH3, -OCH2CH3, -O-Si(CH3)3 and -O-Si(CH2CH3)3; and

[0136] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0137] According to a specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the compound of formula (I) is selected from trimethoxy({3-[(oxiran-2-yl)methoxy]propyl})silane (also known as glycidyloxypropyl-trimethoxysilane), dimethoxy(methyl){3-[(oxiran-2-yl)methoxy]propyl}silane, methoxydimethyl{3-[(oxiran-2-yl)methoxy]propyl}silane, dimethoxy(ethyl){3-[(oxiran-2-yl)methoxy]propyl}silane, diethyl(methoxy){3-[(oxiran-2-yl)methoxy]propyl}silane, triethoxy({3-[(oxiran-2-yl)methoxy]propyl}silane}) silane (also known as glycidyloxypropyl-triethoxysilane), diethoxy(methyl){3-[(oxiran-2-yl)methoxy]propyl}silane, ethoxydimethyl{3-[(oxiran-2-yl)methoxy]propyl}silane, diethoxy-ethyl-[3-(oxiran-2-ylmethoxy)propyl]silane, ethoxydiethyl{3-[(oxiran-2-yl)methoxy]propyl}silane, trimethoxy({2-[(oxiran-2-yl)methoxy]ethyl}) silane, dimethoxy(methyl){2-[(oxiran-2-yl)methoxy]ethyl}silane, methoxydimethyl{2-[(oxiran-2-yl)methoxy]ethyl}silane, ethyldimethoxy{2- [(oxiran-2-yl)methoxy]ethyl}silane, diethyl(methoxy){2-[(oxiran-2-yl)methoxy]ethyl}silane, triethoxy({2-[(oxiran-2-yl)methoxy]ethyl})silane, diethoxy(methyl){2-[(oxiran-2-yl)methoxy]ethyl}silane, ethoxydimethyl{2-[(oxiran-2-yl)methoxy]ethyl}silane, diethoxy(ethyl){2-[(oxiran-2-yl)methoxy]ethyl}silane, diethoxy(ethyl){2-[(oxiran-2-yl)methoxy]ethyl}silane, trimethoxy({[(oxiran-2-yl)methoxy]methyl})silane, dimethoxy(methyl){[( oxiran-2-yl)methoxy]methyl} silane, methoxydimethyl{[(oxiran-2-yl)methoxy]methyl} silane, ethyldimethoxy{[(oxiran-2-yl)methoxy]methyl} silane, diethyl(methoxy){[(oxiran-2-yl)methoxy]methyl} silane, triethoxy({[(oxiran-2-yl)methoxy]methyl}) silane, diethoxy(methyl){[(oxiran-2-yl)methoxy]methyl} silane, ethoxydimethyl{[(oxiran-2-yl)methoxy]methyl} silane, diethoxy(ethyl){[(oxiran-2-yl)methoxy]methyl} silane, ethoxydiethyl{[(oxiran-2-yl)methoxy]methyl} silane,Butyl[(oxiran-2-yl)methyl][3-(trimethoxysilyl)propyl]amine, Butyl[(oxiran-2-yl)methyl][3-(triethoxysilyl)propyl]amine, Ethyl[(oxiran-2-yl)methyl][3-(trimethoxysilyl)propyl]amine, Ethyl[(oxiran-2-yl)methyl][3-(triethoxysilyl)propyl]amine, Methyl[(oxiran-2-yl)methyl][3-(triethoxysilyl)propyl]amine propyl] amine, methyl[(oxiran-2-yl)methyl][3-(triethoxysilyl)propyl]amine, N-[(oxiran-2-yl)methyl]-N-[3-(trimethoxysilyl)propyl]aniline, N-[(oxiran-2-yl)methyl]-N-[3-(triethoxysilyl)propyl]aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(triethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(triethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(triethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, 1-(trimethoxysilyl)methyl)aniline, N,N-bis((trimethoxysilyl)methyl)(oxiran-2-yl)methylamine and N,N-bis((triethoxysilyl)methyl)(oxiran-2-yl)methylamine.

[0138] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (IV) or (V) above. In one embodiment, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (IV) or (V), wherein

[0139] r and t are independently integers selected from 1, 2, 3 or 4; and

[0140] s is an integer selected from 1 to 3; and

[0141] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0142] According to a specific embodiment, optionally in combination with one or more features of the above or below various embodiments, the compound of formula (I) is selected from (oxiran-2-yl)methyl N-[3-(trimethoxysilyl)propyl]carbamate, (oxiran-2-yl)methyl-N-[3-(triethoxysilyl)propyl]carbamate, (oxiran-2-yl)methyl-N-[4-(trimethoxysilyl)butyl]carbamate, (oxiran-2-yl)methyl-N-[4-(triethoxysilyl)butyl]carbamate, (oxiran-2-yl)methyl-N-[2-(trimethoxysilyl)ethyl]carbamate, (oxiran-2-yl)methyl-N-[2-(triethoxysilyl)ethyl]carbamate carbamate, (oxiran-2-yl)methyl-N-[(trimethoxysilyl)methyl]carbamate, (oxiran-2-yl)methyl-N-[(triethoxysilyl)methyl]carbamate, 3-trimethoxysilylpropylcarbamoyloxirane-2-carboxylate, 3-triethoxysilylpropylcarbamoyloxirane-2-carboxylate, oxirane-2-carbonyl-N-[(trimethoxysilyl)methyl]carbamate, oxirane-2-carbonyl-N-[(triethoxysilyl)methyl]carbamate, oxirane-2-carbonyl-N-[4-(trimethoxysilyl)butyl]carbamate and oxirane-2-carbonyl-N-[4-(triethoxysilyl)butyl]carbamate.

[0143] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (VI) above.

[0144] In one embodiment, optionally in combination with one or more features of the various embodiments described above or below, group A is selected from those compounds of formula (VI), wherein

[0145] w is an integer selected from 1, 2, 3 or 4, specifically 2, 3 or 4;

[0146] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0147] According to a specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the compound of formula (I) is selected from 3-[3-(triethoxysilyl)propyl]tetrahydrofuran-2,5-dione

[0148]

[0149]

[0150] Therefore, according to certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, the alkoxysilane group-modified compound contains 1 to 8 hydroxyl groups per molecule, preferably 2 to 7, more preferably 3 to 6, and even more preferably 4 to 5 hydroxyl groups per molecule, and 1 to 2, preferably 1 alkoxysilane group per molecule.

[0151] According to a specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the functionality of the polyether polyol is 2 to 9, preferably 2 to 8, more preferably 3 to 7, and even more preferably 3 to 6. In some specific embodiments, the OH functionality is 2, 3, 4, 5, 6, 7, 8 or 9.

[0152] According to a specific embodiment, optionally in combination with one or more features of the above or below various embodiments, the average molecular weight of the polyether polyol is 3000 to 25000, preferably 6000 to 20000, more preferably 8000 to 15000, and even more preferably 11000 to 14000.

[0153] According to a specific embodiment, optionally in combination with one or more features of the above or below various embodiments, the polyether polyol has a hydroxyl value of 20-600 mg KOH / g, preferably 28-380 mg KOH / g, more preferably 28-80 mg KOH / g.

[0154] According to a specific embodiment, optionally in combination with one or more features of the above or below various embodiments, the viscosity of the polyether polyol at 25°C is 50 to 12500 mPa·s, preferably 200 to 8000 mPa·s, more preferably 450 to 5000 mPa·s, and even more preferably 500 to 2000 mPa·s.

[0155] According to certain specific embodiments, optionally in combination with one or more features of the above or below various embodiments, the polyether polyol is a polyether polyol having a functionality of 3 to 6, an average molecular weight of 6000 to 20000 and a viscosity of 25°C of 200 to 8000 mPa·s.

[0156] According to some specific embodiments of the present invention, optionally in combination with one or more features of the various embodiments described above or below, the polyether polyol does not contain an organic filler dispersed therein. Therefore, according to one embodiment, the first polyol is not or does not contain a modified polymer polyol because it has substantially no organic filler dispersed therein.

[0157] According to some specific embodiments of the present invention, optionally in combination with one or more features of the above or below various embodiments, the polyether polyol contains a certain amount of organic filler dispersed therein; therefore, in some embodiments, the polyether polyol contains an organic filler dispersed therein that can be 0 wt % to 50 wt %, preferably 0.01 wt % to 30 wt %, more preferably 0.02 wt % to 15 wt %, and even more preferably 0.5 wt % to 5 wt %. Examples of organic fillers are polyethylene, polypropylene and vinyl polymer particles, such as particles of acrylonitrile, polystyrene, methacrylonitrile, methyl methacrylate and styrene-acrylonitrile.

[0158] According to some specific embodiments of the present invention, optionally in combination with one or more features of the above or following various embodiments, the polyether polyol is a poly(ethylene oxide and / or propylene oxide) adduct of one of the following polyols: glycerol, sorbitol, trimethylolpropane, diethylene glycol, butanetriol, pentanetriol, hexanetriol and tetaerythriol.

[0159] According to a specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the polyether polyol is a polyether polyol terminated with ethylene oxide (EO) or propylene oxide (PO). In a specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the polyether polyol is a reactive polyether polyol, i.e., a polyether polyol terminated with ethylene oxide (EO), having a terminal primary hydroxyl content of 35 to 99.9%, 35 to 98%, 40 to 95%, 45 to 90%, 50 to 85%, 75 to 99%, 77 to 98% or 78 to 95% as measured by RMN-13C. According to some specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the polyether polyol is a reactive polyether polyol having a polyethylene oxide terminal block content of 5-20% by weight, preferably 10-19.5% by weight, preferably 12-19% by weight, and more preferably 13-18% by weight.

[0160] According to another specific embodiment, optionally in combination with one or more features of various embodiments described above or below, the polyether polyol is a non-reactive polyether polyol, ie, a propylene oxide (PO)-terminated polyether polyol.

[0161] In some specific embodiments of the present invention, optionally in combination with one or more features of the above or below various embodiments, the polyether polyol is a poly(ethylene oxide and / or propylene oxide) adduct of a polyol selected from glycerol, sorbitol, trimethylolpropane, diethylene glycol, butanetriol, pentanetriol, hexanetriol and tetaerythriol; wherein the functionality of the polyether polyol is 2 to 9 and the average molecular weight is 6000 to 20000.

[0162] In some specific embodiments of the present invention, optionally in combination with one or more features of the various embodiments described above or below, the alkoxysilane group-modified compound is obtained by reacting the following a) with b):

[0163] a) at least one polyether polyol having a functionality of 2 to 9 and an average molecular weight of 6000 to 20000, obtainable by reacting ethylene oxide and / or propylene oxide with a polyol selected from glycerol, sorbitol, trimethylolpropane, diethylene glycol, butanetriol, pentanetriol, hexanetriol and tetaerythriol;

[0164] b) at least one alkoxysilane group-containing capping agent, which is a compound of formula (I), wherein the group A is selected from

[0165] -Those compounds of formula (II), wherein m is an integer from 1 to 6; R4 is selected from -NCO,

[0166]

[0167] Among them, the asterisk indicates the point of connection to the rest of the group;

[0168] -Those compounds of formula (III), wherein n and p are independently integers selected from 1 to 6, q is an integer selected from 1 to 3, X is selected from -O- and -N(R5)-, wherein R5 is selected from H, linear or branched (C1-C6) alkyl, The group,

[0169] wherein the asterisk indicates the point of connection to the N atom; x and z are independently integers selected from 1 to 6; R8, R9 and R10 are each independently selected from -CH3, -CH2CH3, -OCH3, -OCH2CH3, -O-Si(CH3)3 and -O-Si(CH2CH3)3;

[0170] - those compounds of formula (IV) or (V) wherein r and t are independently integers selected from 1 to 4; s is an integer selected from 1 to 3; or

[0171] - those compounds of formula (VI) in which w is an integer selected from 1 to 4, for example 3-[3-(triethoxysilyl)propyl]tetrahydrofuran-2,5-dione and 3-[3-(trimethoxysilyl)propyl]tetrahydrofuran-2,5-dione; and

[0172] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent (of formula (I)) per 1 mol of the polyether polyol.

[0173] In some specific embodiments of the present invention, optionally in combination with one or more features of the various embodiments described above or below, the alkoxysilane group-modified compound can be obtained by reacting the following a) with b):

[0174] a) at least one polyether polyol as described above having a functionality of 2 to 9 and an average molecular weight of 3000 to 25000;

[0175] b) at least one alkoxysilane group-containing blocking agent of formula (I) selected from (3-isocyanatepropyl)trimethoxysilane, (3-isocyanatepropyl)dimethoxy(methyl)silane, (3-isocyanatepropyl)(methoxy)dimethylsilane, (3-isocyanatepropyl)dimethoxy-ethylsilane, 3-isocyanatepropyltriethoxysilane, (3-isocyanatepropyl)diethoxy(ethyl)silane, triethoxy(2- isocyanate ethyl) silane, triethoxy (isocyanate methyl) silane, trimethoxy ({3-[(oxiran-2-yl) methoxy] propyl}) silane, dimethoxy (methyl) {3-[(oxiran-2-yl) methoxy] propyl} silane, methoxydimethyl {3-[(oxiran-2-yl) methoxy] propyl} silane, dimethoxy (ethyl) {3-[(oxiran-2-yl) methoxy] propyl} silane, triethoxy ({3-[(oxiran-2-yl)methoxy]propyl})silane, diethoxy-ethyl-[3-(oxiran-2-ylmethoxy)propyl]silane, 3-(trimethoxysilyl)-N-(3-(trimethoxysilyl)propyl)-N-((oxiran-2-yl)methyl)propan-1-amine, 3-(triethoxysilyl)-N-(3-(triethoxysilyl)propyl)-N-((oxiran-2-yl)methyl)propan-1-amine methyl)propan-1-amine, N,N-bis((trimethoxysilyl)methyl)(oxiran-2-yl)methanamine, 3-trimethoxysilylpropylcarbamoyloxirane-2-carboxylate, 3-triethoxysilylpropylcarbamoyloxirane-2-carboxylate, 3-trimethoxysilylethylcarbamoyloxirane-2-carboxylate, and 3-triethoxysilylethylcarbamoyloxirane-2-carboxylate; and

[0176] The reaction of b) with a) is carried out in a molar ratio of 0.05 to 2.0 mol, preferably 0.2 to 1.8 mol, more preferably 0.50 to 1.5 mol, particularly preferably 0.8 to 1.2 mol of the end-capping agent per 1 mol of the polyether polyol.

[0177] Therefore, since the novel alkoxysilane group-modified compounds of the present invention can be obtained by reacting at least one polyether polyol described herein with at least one compound of formula (I), the novel alkoxysilane group-modified compounds can be described as capped polyether polyols, wherein 1 to 2 (preferably 1) hydroxyl groups of the polyether polyol react with the hydroxyl-reactive groups present in the capping agent containing alkoxysilane groups. According to some specific embodiments, the hydroxyl-reactive groups are NCO or epoxy groups. Thus, for example, when a polyether polyol having a functionality of 6 (i.e., the number of OH groups in the molecule is 6) is reacted with a compound of formula (I) in a molar ratio of 0.8 to 1.2 moles of the compound of formula (I) per 1 mole of the polyether polyol, the alkoxysilane group-modified compound thus obtained is a polyether polyol in which 1 hydroxyl group reacts with the hydroxyl-reactive groups present in the capping agent containing alkoxysilane groups of formula (I), while the remaining hydroxyl groups are free.

[0178] According to one embodiment, optionally in combination with one or more features of the various embodiments described above or below, the reaction of a) polyether polyol with b) compound of formula (I) is carried out in a temperature range of 0°C to 160°C, preferably 10°C to 120°C, particularly preferably 20°C to 80°C.

[0179] This reaction can be carried out in the presence of a catalyst. A person skilled in the art can determine any suitable catalyst according to the reactants.

[0180] In some embodiments, optionally in combination with one or more features of the various embodiments described above or below, the reaction may be carried out in the presence of a carbamateization catalyst known to the expert per se, such as a potassium-type catalyst, an organotin compound or an amine catalyst. Other catalysts may be used, for example a zinc-type catalyst. In some specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the potassium-type catalyst is selected from potassium acetate and potassium octoate; the organotin catalyst is selected from dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin diacetylacetonate, tin carboxylates (such as tin octoate, tin ricinoleate, tin neodecanoate); and the amine catalyst is selected from tertiary amines. In some embodiments, the reaction is carried out in the presence of at least one tin catalyst or at least one amino catalyst.

[0181] In another embodiment, optionally in combination with one or more features of the various embodiments described above or below, in particular when the compound of formula (I) has an epoxy group as a hydroxyl reactive group, the reaction can be carried out in the presence of a catalyst selected from: Lewis acids and Bronsted superacids ( superacid), such as BF3, PF5, SbF5, HPF6, HBF4, HSbF6, CF3SO3H, Al(CF3SO3)3, Y(CF3SO3)3, Nd(CF3SO3)3; anionic catalysts, such as NaOH, KOH, CsOH, Sr(OH)2, Ba(OH)2, calcium cyclohexaneate, calcium octoate, phosphazene salt compounds; coordination catalysts, such as alkyl aluminum and zinc and aluminum and zinc alkoxides [Ai(OR)3, Zn(OR)2], aluminum and zinc tetraphenylporphyrin salts, titanium alkoxides [Ti(OR)4], bimetallic catalysts (DMC) based on Zn3[Co(CN)6]3.

[0182] The reaction can be carried out continuously, for example in a static mixer or an extruder, or batchwise, for example in a stirred reactor.

[0183] The invention also relates to novel stable modified polymer polyol dispersions obtainable by polymerizing one or more polymer particle precursors in a liquid polyol mixture under polymerization conditions, characterized in that the liquid polyol mixture comprises at least one base polyol and at least one compound modified with alkoxysilane groups as described herein.

[0184] With respect to the base polyol used to prepare the modified polymer polyol dispersion and / or polyurethane foam of the present invention, the base polyol may be of any suitable type known in the art.

[0185] The representative matrix polyol that can be used for preparing the modified polymer polyol of the present disclosure can comprise any type of polyol known in the art, and comprises those polyols as herein described and any other commercially available polyol.Representative polyol comprises polyether polyol, polyester polyol, polymer polyol, polyhydroxy-terminated acetal resin, hydroxy-terminated amine, polyalkylene carbonate type polyol, acrylic acid polyol, polyphosphate type polyol and the polyol comprising polyether carbonate polyol (POPC).Suitable polymer polyol comprises PDH polyol, PIPA polyol, SAN polyol, copolymer polyol and the polymer polyol comprising polyether carbonate polyol (POPC) as matrix polyol.All other types of other polyols (for example, the polyol derived from renewable resources, i.e. so-called natural oil polyol or NOP) can also be pure or mixed, as long as it has suitable physicochemical properties.

[0186] According to one embodiment, optionally in combination with one or more features of various embodiments described above or below, preferred base polyols are selected from polyether polyols, PDH polyols, PIPA polyols, SAN polyols and polyols containing polyether carbonate polyols (POPC). Some particularly preferred base polyols are selected from polyether carbonate polyols (POPC) and polyether polyols.

[0187] In a preferred embodiment, optionally in combination with one or more features of various embodiments described above or below, the base polyol comprises at least one ethylene oxide (EO) or propylene oxide (PO) terminated polyether polyol.

[0188] According to one embodiment, optionally in combination with one or more features of various embodiments described above or below, suitable base polyols may have an OH functionality of 2 to 10, in other embodiments, an OH functionality of 2 to 8, more specifically 2 to 6, and even more specifically 3 to 6. In some embodiments, the OH functionality is 2, 3, 4, 5, 6, 7, 8, 9 or 10.

[0189] According to one embodiment, optionally in combination with one or more features of the above or below various embodiments, a suitable base polyol is a reactive polyether polyol, i.e., an ethylene oxide (EO) terminated polyether polyol, having a terminal primary hydroxyl content of 35 to 99.9%, 35 to 99.9%, 35 to 98%, 40 to 95%, 45 to 90%, 50 to 85%, 75 to 99%, 77 to 98% or 78 to 95% as measured by RMN-13C. According to some embodiments, optionally in combination with one or more features of the above or below various embodiments, the base polyol is a reactive polyether polyol, having a polyethylene oxide terminal block content of 5-20% by weight, preferably 10-19.5% by weight, preferably 12-19% by weight, and more preferably 13-18% by weight.

[0190] According to another specific embodiment, optionally in combination with one or more features of various embodiments described above or below, the base polyol is a non-reactive polyether polyol.

[0191] In some embodiments, optionally in combination with one or more features of the various embodiments described above or below, the molecular weight (MW) of the base polyol is from 150 to 12,000, preferably from 200 to 11,500, more preferably from 250 to 10,500. Some base polyols of the present invention have a molecular weight (MW) of from 300 to 4,000, particularly from 350 to 2,000, more particularly from 400 to 1,000. In other specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the MW of the base polyol may be from 3,000 to 12,000, specifically from 4,500 to 12,000, more specifically from 4,600 to 10,000, or even more specifically from 5,000 to 9,000. Some specific embodiments (optionally in combination with one or more features of the various embodiments described above or below) relate to base polyols having a molecular weight (MW) of from 400 to 3,000; or, in certain specific embodiments, base polyols have a molecular weight of from 4,500 to 12,000.

[0192] In some embodiments, optionally in combination with one or more features of the above or below various embodiments, the viscosity of the base polyol at 25°C is 50 to 25000 mPa·s, preferably 65 to 9500 mPa·s, more preferably 150 to 8000 mPa·s. In some embodiments, optionally in combination with one or more features of the above or below various embodiments, the viscosity of the base polyol at 25°C is 250 to 6500 mPa·s, in particular 400 to 2000 mPa·s, 420 to 1800 mPa·s, 450 to 1600 mPa·s, 470 to 1500 mPa·s.

[0193] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, the hydroxyl value (iOH) of the base polyol is 5 to 1800 mg KOH / g, 5 to 1500 mg KOH / g, 7 to 1400 mg KOH / g, 8 to 1300 mg KOH / g, 9 to 1200 mg KOH / g, or 10 to 1100 mg KOH / g. In other embodiments, the iOH of the base polyol is 5 to 800 mg KOH / g, 10 to 600 mg KOH / g, 15 to 500 mg KOH / g, 25 to 460 mg KOH / g. In certain specific embodiments, the iOH of the base polyol is 20 to 80 mg KOH / g, 25 to 70 mg KOH / g, 26 to 65 mg KOH / g, or 26 to 58 mg KOH / g. And in certain embodiments, the iOH of the base polyol is 80 to 700 mg KOH / g, 81 to 650 mg KOH / g, 90 to 550 mg KOH / g, 120 to 520 mg KOH / g. In some examples, the iOH of the base polyol is 28-280 mg KOH / g; according to other examples, the iOH is 28-56 mg KOH / g, and in other examples, the iOH is 160-490 mg KOH / g.

[0194] It is well known in the art to use mixed polyols to change the reactivity of the system or to impart the desired properties of the resulting polyurethane. Therefore, according to one embodiment of the present disclosure, optionally in combination with one or more features of the above or following various embodiments, a mixture of a matrix polyol, a mixture of a polymer polyol, or a mixture of a matrix polyol and a polymer polyol may also be used.

[0195] According to some embodiments, optionally in combination with one or more features of the various embodiments described above or below, a modified polymer polyol dispersion is obtained using at least one co-reactant b.1) having at least one hydrogen attached to a nitrogen or oxygen atom as described above and at least one polyisocyanate as a polymer particle precursor.

[0196] In those embodiments in which the polymer particle precursor is as defined in b.1) (i.e., at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen or oxygen atom), the modified polymer polyol dispersion obtained therefrom is a PIPA polyol or a PHD polyol. Thus, according to some embodiments, optionally in combination with one or more features of various embodiments described above or below, at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen group is used.

[0197] If a PHD polymer polyol is desired, the co-reactants to form the PHD may include amines such as ammonia, aniline, and substituted anilines and fatty amines. The co-reactants to form the PHD may also include diamines (e.g., ethylenediamine, 1,6-hexamethylenediamine), alkanolamines, and hydrazine.

[0198] If a PIPA polymer polyol is desired, the coreactants to form the PIPA may include: glycols such as diethylene glycol, triethylene glycol, and polyethylene glycol; and alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, triisopropanolamine, 2-(2-aminoethoxyethanol), hydroxyethylpiperazine, monoisopropanolamine, diisopropanolamine, and mixtures thereof. Other alkanolamines contemplated include N-methylethanolamine, phenylethanolamine, and ethylene glycolamine.

[0199] It is also possible to provide co-reactants to form PHD and PIPA to form hybrid PHD-PIPA particles.

[0200] At least one co-reactant that forms a PHD and / or PIPA polymer is added to the blend at a concentration of about 2% to about 40%, preferably about 5% to about 30%, by weight of the total weight of the polyol blend. All individual values ​​and subranges within about 2% to about 40% by weight are included and disclosed herein; for example, the solids content can be a lower limit of 2, 3, 4, 5, 8, 10, 15, 20, 25, or 30% by weight to an upper limit of 20, 25, 30, 35, or 40% by weight relative to the weight of the polymer polyol.

[0201] According to some embodiments, a catalytic amount of organic metal can be used. The organic metal compound that can be used as catalyst includes compounds of bismuth, lead, tin, titanium, iron, antimony, uranium, cadmium, cobalt, thorium, aluminum, mercury, zinc, nickel, cerium, molybdenum, vanadium, copper, manganese, zirconium, chromium, etc. Some examples of these metal catalysts include bismuth nitrate, bismuth neodecanoate, 2-ethylhexanoic acid lead, lead benzoate, lead oleate, dibutyltin dilaurate, tributyltin, butyltin trichloride, dimethyltin, dimethyltin dineodecanoate, stannous chloride, stannous octoate, stannous oleate, stannous ricinoleate, di(2-ethylhexanoic acid) dibutyltin, zinc octoate, zinc ricinoleate, ferric chloride, antimony trichloride, antimony glycolate, tin glycolate, ferric acetylacetonate, etc. Catalyst can promote the reaction of the primary hydroxyl group of diisocyanate and alkanolamine.

[0202] The at least one polyisocyanate b.2) that can be used in the present invention includes aliphatic, cycloaliphatic, araliphatic and aromatic isocyanates. Examples of suitable aromatic polyisocyanates include 4,4'-, 2,4'- and 2,2'-isomers of diphenylmethane diisocyanate (MDI), their blends and polymeric and monomeric MDI blends, toluene-2,4- and 2,6-diisocyanate (TDI), meta- and para-phenylene diisocyanate, chlorophenylene 2,4-diisocyanate, phenylene-4,4'-diisocyanate, 3,3'-dimethyldiphenyl-4,4'-diisocyanate, 3-dimethyldiphenyl-methane-4,4'-diisocyanate and 2,4,4'-triisocyanatodiphenyl ether. Mixtures of polyisocyanates can be used, for example commercial mixtures of 2,4- and 2,6-isomers of toluene diisocyanate. Crude polyisocyanates may also be used in the practice of the present invention, such as crude toluene diisocyanate obtained by phosgenation of a toluenediamine mixture or crude diphenylmethane diisocyanate obtained by phosgenation of crude methylene dianiline. TDI / MDI blends may also be used. Examples of aliphatic polyisocyanates include ethylene diisocyanate, 1,6-hexamethylene diisocyanate, isophorone diisocyanate, cyclohexane-1,4-diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, saturated analogs of the above aromatic polyisocyanates, and mixtures thereof.

[0203] According to certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, the mixture a.2) of compounds carrying phosphorus atoms comprises:

[0204] I. [bis(hydroxymethyl)phosphino]methanol (THP) at a concentration of 0-99.9 mol%, 20-95 mol%, 30-90 mol%, 35-85 mol%, 50-75 mol% or 60-72 mol%;

[0205] II. tetrakis(hydroxymethyl)phosphonium salt (THPX) at a concentration of 0-50 mol%, 0-30 mol%, 0.05-15 mol%, 0.1-10 mol%, 0.1-7.5 mol%, 0.2-5 mol% or 0.5-6.6 mol% THPX;

[0206] III. [Bis(hydroxymethyl)phosphoryl]methanol (THPO), at a concentration of 0-99.9 mol%, 0-40 mol%, 1-15 mol%, 2-12 mol% or 2-7 mol% THPO;

[0207] IV. {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), at a concentration of 0-80 mol%, 0.1-60 mol%, 0.2-45 mol%, 0.4-40 mol%, 0.5-30 mol% or 1-25 mol% mTHP;

[0208] V. {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP) at a concentration of 0-30 mol%, 0.1-20 mol%, 0.2-15 mol% or 0.25-10 mol% dTHP;

[0209] VI. ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP) at a concentration of 0-15 mol%, 0.05-5 mol%, 0.075-2 mol% or 0.1-1 mol% tTHP;

[0210] VII. {[Bis(hydroxymethyl)phosphoryl]methoxy}methanol (mTHPO) at concentrations of 0-20 mol%, 0.05-10 mol%, 0.1-6.5 mol%, 0-6.1 mol% mTHPO;

[0211] VIII. {Bis[(hydroxymethoxy)methyl]phosphoryl}methanol (dTHPO) at a concentration of 0-10 mol%, 0.05-5 mol%, 0.1-1 mol% dTHPO; and

[0212] IX. ({bis[(hydroxymethoxy)methyl]phosphoryl}methoxy)methanol (tTHPO), concentration 0-4 mol%, 0.01-1 mol%, 0.05-0.2 mol%, 0-0.5 mol% tTHPO;

[0213] X. optionally at least one other compound containing a phosphorus atom;

[0214] The total amount of compounds having phosphorus atoms in the mixture is 100 mol%.

[0215] According to some specific embodiments, optionally in combination with one or more features of the above or below various embodiments, the mixture of compounds with phosphorus atoms includes a tetrakis(hydroxymethyl)phosphonium salt (THPX) at a concentration of 0-50 mol%; wherein the counter ion (X) of the salt is a monovalent, divalent or trivalent ligand selected from chloride, bromide, iodine, sulfate, phosphate, hydrogen phosphate, dihydrogen phosphate, hydroxide, acetate, oxalate and citrate.

[0216] In certain embodiments, optionally in combination with one or more features of various embodiments described above or below, the hydroxyalkyl phosphonium salt is selected from the group consisting of tetrakis(hydroxymethyl)phosphonium chloride, bis(tetrakis(hydroxymethyl)phosphonium sulfate) (THPS), tetrakis(hydroxymethyl)phosphonium phosphate (THPP(3:1)), tetrakis(hydroxymethyl)phosphonium monohydrogen phosphate (THPP(2:1)), tetrakis(hydroxymethyl)phosphonium dihydrogen phosphate (THPP(1:1)), tetrakis(hydroxymethyl)phosphonium hydroxide (THPOH), tetrakis(hydroxymethyl)phosphonium oxalate (THPOx), and tetrakis(hydroxymethyl)phosphonium acetate (THPA).

[0217] Specific examples of hydroxyalkylphosphonium salts are tetrakis(hydroxymethyl)phosphonium chloride (THPC) and bis[tetrakis(hydroxymethyl)phosphonium] sulfate (THPS).

[0218] In the case of using a hydroxyalkylphosphonium salt, it may be necessary to treat it with a base to obtain the corresponding hydroxyalkylphosphine. The base may be an organic base or an inorganic base, which is preferably selected from KOH, NaOH, Ca(OH)2, Mg(OH)2, Ba(OH)2, triethylamine (NEt3), tributylamine (NBu3). Alternatively, the hydroxyalkylphosphonium salt may be treated with a basic ion exchange resin. Both strong and weak ion exchange resins are suitable for this process. Examples of strong bases are IRN78 or A26. Examples of weak bases are IRA 67, MP-62 and VP OC1065.

[0219] As mentioned above, when a hydroxyalkylphosphonium salt reacts with a base, the corresponding hydroxyalkylphosphine, the corresponding salt, the corresponding aldehyde and water are obtained, while other phosphorus compounds may appear as reaction products. THPO is usually obtained as a by-product together with THP. In addition, THP and THPO can react with formaldehyde to form the corresponding hemiformals. Mono-, di- and tri-substituted hemiformals of THP and THPO can be found as reaction products.

[0220] In general, it is desirable to reduce the formaldehyde content in the modified polyol for preparing polyurethane materials. However, it has been observed that when the formaldehyde content is reduced (for example, by distilling it off together with the solvent and volatiles in the mixture of phosphorus compounds) and the resulting mixture is used for preparing modified polymer polyols according to the method described in WO2019008140, the resulting polymer particles may agglomerate and precipitate, producing unstable dispersions. The alkoxysilane group-modified compounds disclosed herein can be used to disperse and stabilize those modified polymer polyol dispersions, and the modified polymer polyol dispersions can be used to prepare polyurethane materials showing reduced formaldehyde release.

[0221] In one embodiment of the present invention, optionally in combination with one or more features of the various embodiments described above or below, examples of suitable at least one compound a.1) with at least one basic nitrogen atom (characterized in that there is at least one hydrogen atom attached to the nitrogen atom in the molecule) are selected from melamine, trimethylolmelamine, those compounds of formula (VII) or formula (VIII) as described above, and mixtures thereof.

[0222] According to some specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the compounds of formula (VII) are those wherein R1 is selected from H, methyl, CN, CH3-CO-, NH2-CO-.

[0223] In another specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the compounds with at least one basic nitrogen atom are those of formula (VIII) wherein R2 is selected from O=C<, S=C< and R3 is H.

[0224] Specific examples of compounds with at least one basic nitrogen atom, characterized by the presence of at least one hydrogen atom bonded to the nitrogen atom in the molecule, are NH3, aliphatic and alicyclic primary amines, aliphatic and alicyclic primary and secondary polyamines, aromatic primary, secondary and tertiary amines and polyamines, such as cyanamide, guanidine, 2-cyanoguanidine, methylamine, ethylenediamine, diethylenetriamine, hexamethylenediamine, hydrazine, tert-octylamine, cyclohexylamine, trimethylolmelamine, urea, thiourea, aniline and polyethyleneimine. NH3, cyanamide, melamine, urea, thiourea, diethylenetriamine, hydrazine and ethylenediamine are particularly preferred examples.

[0225] The person skilled in the art is aware of methods and suitable media in order to solubilize compounds with at least one basic nitrogen atom, if necessary.

[0226] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, a method for preparing a modified polymer polyol dispersion comprises:

[0227] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0228] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0229] a.1) at least one compound as described above with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule which is bonded to the nitrogen atom; and

[0230] a.2) A mixture of compounds containing phosphorus atoms, comprising

[0231] I. [bis(hydroxymethyl)phosphino]methanol (THP) at a concentration of 0-99.9 mol%, 20-95 mol%, 30-90 mol%, 35-85 mol%, 50-75 mol% or 60-72 mol%;

[0232] II. tetrakis(hydroxymethyl)phosphonium salt (THPX) at a concentration of 0-50 mol%, 0-30 mol%, 0.05-15 mol%, 0.1-10 mol%, 0.1-7.5 mol%, 0.2-5 mol% or 0.5-6.6 mol% THPX;

[0233] III. [Bis(hydroxymethyl)phosphoryl]methanol (THPO), at a concentration of 0-99.9 mol%, 0-40 mol%, 1-15 mol%, 2-12 mol% or 2-7 mol% THPO;

[0234] IV. {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), at a concentration of 0-80 mol%, 0.1-60 mol%, 0.2-45 mol%, 0.4-40 mol%, 0.5-30 mol% or 1-25 mol% mTHP;

[0235] V. {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP) at a concentration of 0-30 mol%, 0.1-20 mol%, 0.2-15 mol% or 0.25-10 mol% dTHP;

[0236] VI. ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP) at a concentration of 0-15 mol%, 0.05-5 mol%, 0.075-2 mol% or 0.1-1 mol% tTHP;

[0237] VII. {[Bis(hydroxymethyl)phosphoryl]methoxy}methanol (mTHPO) at concentrations of 0-20 mol%, 0.05-10 mol%, 0.1-6.5 mol%, 0-6.1 mol% mTHPO;

[0238] VIII. {Bis[(hydroxymethoxy)methyl]phosphoryl}methanol (dTHPO) at a concentration of 0-10 mol%, 0.05-5 mol%, 0.1-1 mol% dTHPO; and

[0239] IX. ({bis[(hydroxymethoxy)methyl]phosphoryl}methoxy)methanol (tTHPO), concentration 0-4 mol%, 0.01-1 mol%, 0.05-0.2 mol% tTHPO;

[0240] X. optionally at least one other compound containing a phosphorus atom;

[0241] The total amount of compounds having phosphorus atoms in the mixture is 100 mol%.

[0242] or

[0243] a.3) a mixture of condensation products obtained by reaction of a mixture of compounds carrying phosphorus atoms as described above a.2) with a.1) at least one compound carrying at least one basic nitrogen atom;

[0244] Therein, the compound a.1) having at least one basic nitrogen atom is selected from melamine, trimethylolmelamine, those compounds of the formula (VII) or (VIII) as described above, and mixtures thereof.

[0245] According to certain specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, a method for preparing a modified polymer polyol comprises:

[0246] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0247] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0248] At least one compound a.1) having at least one basic nitrogen atom selected from:

[0249] - melamine, trimethylolmelamine,

[0250] - those compounds of formula (VII) in which R1 is selected from H, methyl, -CN, CH3CO-, NH2-CO-;

[0251] - those compounds of formula (VIII) in which R2 is selected from O=C<, S=C<; R3 is H; and

[0252] - mixtures thereof;

[0253] and

[0254] Mixtures a.2) of compounds containing phosphorus atoms, comprising:

[0255] I. [bis(hydroxymethyl)phosphino]methanol (THP) at a concentration of 0-99.9 mol%, 20-95 mol%, 30-90 mol%, 35-85 mol%, 50-75 mol% or 60-72 mol%;

[0256] II. tetrakis(hydroxymethyl)phosphonium salt (THPX) at a concentration of 0-50 mol%, 0-30 mol%, 0.05-15 mol%, 0.1-10 mol%, 0.1-7.5 mol%, 0.2-5 mol% or 0.5-6.6 mol% THPX;

[0257] III. [Bis(hydroxymethyl)phosphoryl]methanol (THPO), at a concentration of 0-99.9 mol%, 0-40 mol%, 1-15 mol%, 2-12 mol% or 2-7 mol% THPO;

[0258] IV. {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), at a concentration of 0-80 mol%, 0.1-60 mol%, 0.2-45 mol%, 0.4-40 mol%, 0.5-30 mol% or 1-25 mol% mTHP;

[0259] V. {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP) at a concentration of 0-30 mol%, 0.1-20 mol%, 0.2-15 mol% or 0.25-10 mol% dTHP;

[0260] VI. ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP) at a concentration of 0-15 mol%, 0.05-5 mol%, 0.075-2 mol% or 0.1-1 mol% tTHP;

[0261] VII. {[Bis(hydroxymethyl)phosphoryl]methoxy}methanol (mTHPO) at concentrations of 0-20 mol%, 0.05-10 mol%, 0.1-6.5 mol%, 0-6.1 mol% mTHPO;

[0262] VIII. {Bis[(hydroxymethoxy)methyl]phosphoryl}methanol (dTHPO) at a concentration of 0-10 mol%, 0.05-5 mol%, 0.1-1 mol% dTHPO; and

[0263] IX. ({bis[(hydroxymethoxy)methyl]phosphoryl}methoxy)methanol (tTHPO), concentration 0-4 mol%, 0.01-1 mol%, 0.05-0.2 mol% tTHPO;

[0264] X. optionally at least one other compound containing a phosphorus atom;

[0265] The total amount of compounds having phosphorus atoms in the mixture is 100 mol%.

[0266] According to certain specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, a method for preparing a modified polymer polyol comprises:

[0267] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0268] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0269] At least one compound a.1) having at least one basic nitrogen atom selected from:

[0270] - melamine, trimethylolmelamine,

[0271] - those compounds of formula (VII) in which R1 is selected from H, methyl, -CN, CH3CO-, NH2-CO-;

[0272] - those compounds of formula (VIII) in which R2 is selected from O=C<, S=C<; R3 is H; and

[0273] - mixtures thereof;

[0274] as well as

[0275] Mixtures a.2) of compounds containing phosphorus atoms, comprising:

[0276] I. [Bis(hydroxymethyl)phosphino]methanol (THP), concentration 35-85 mol %

[0277] II. Tetrakis(hydroxymethyl)phosphonium salt (THPX), concentration 0.5-6.6 mol%,

[0278] III. [Bis(hydroxymethyl)phosphoryl]methanol (THPO), concentration 2-12 mol %

[0279] IV. {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), concentration 1-25 mol %

[0280] V. {Bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), concentration 0.25-10 mol %

[0281] VI. ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), concentration 0-15 mol%

[0282] VII. {[Bis(hydroxymethyl)phosphoryl]methoxy}methanol (mTHPO), concentration 0-20 mol%

[0283] VIII. {Bis[(hydroxymethoxy)methyl]phosphoryl}methanol (dTHPO), concentration 0-10 mol %

[0284] IX. ({bis[(hydroxymethoxy)methyl]phosphoryl}methoxy)methanol (tTHPO), concentration 0-4 mol%

[0285] X. optionally at least one other compound containing a phosphorus atom;

[0286] The total amount of compounds having phosphorus atoms in the mixture is 100 mol%.

[0287] According to some embodiments, optionally in combination with one or more features of the various embodiments described above or below, a method for preparing a modified polymer polyol comprises:

[0288] i. mixing at least one tetrakis (hydroxymethyl) phosphonium salt (THPX) with an aqueous or alcoholic base solution, preferably at a temperature of 0°C to 60°C;

[0289] ii. optionally filtering the resulting solution;

[0290] iii. distilling off the solvent and volatiles, in particular formaldehyde, thereby obtaining a mixture a.2) of compounds carrying phosphorus atoms, which comprises [bis(hydroxymethyl)phosphino]methanol (THP), tetrakis(hydroxymethyl)phosphonium salt (THPX), [bis(hydroxymethyl)phosphino]methanol (THPO), ({[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), {bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHPO), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHPO) and ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHPO);

[0291] iv. optionally filtering the resulting solution;

[0292] v. optionally oxidizing the product obtained in iii or the solution obtained in iv, wherein the oxidation can be carried out by simple heat treatment in an air atmosphere or by using an oxidizing agent (such as hydrogen peroxide), thereby obtaining a mixture a.2) having a high content of oxidized components;

[0293] vi. mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0294] vii. preparing polymer particles in the presence of the liquid polyol mixture obtained in vi by reacting the liquid polyol mixture obtained in vi by adding the following substances simultaneously or sequentially in any order:

[0295] at least one compound a.1) with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule attached to the nitrogen atom and is chosen from melamine, trimethylolmelamine, those compounds of formula (VII) or (VIII) as described above, and mixtures thereof; and

[0296] - a mixture a.2 of compounds carrying phosphorus atoms obtained in iii), the filtered solution obtained in iv, the oxidized mixture obtained in v or a mixture thereof.

[0297] According to certain embodiments, optionally in combination with one or more features of various embodiments described above or below, the aqueous or alcoholic base solution used in step i above can be selected from KOH, NaOH, Ca(OH)2, Mg(OH)2, Ba(OH)2, triethylamine (NEt3), tributylamine (NBu3). Alternatively, the hydroxyalkylphosphonium salt can be treated with a basic ion exchange resin. Both strong ion exchange resins and weak ion exchange resins are suitable for this process. Examples of strong bases are IRN78 or A26. Examples of weak bases are IRA 67, MP-62 and VP OC1065.

[0298] According to certain embodiments, optionally in combination with one or more features of various embodiments described above or below, the distillation step is performed under vacuum and at a temperature of 25-99°C, preferably 40-90°C, more preferably 60-80°C.

[0299] The molar ratio of the compound with phosphorus to the compound with at least one basic nitrogen atom used depends on the functionality of the compound with at least one basic nitrogen atom. The skilled person will know how to adjust the molar ratio according to the description and examples of the present invention to obtain a solid product.

[0300] The compound with at least one basic nitrogen atom can be added to the reactor as a solid, a gas or dissolved in a suitable solvent. An aqueous solution of an amine is preferred.

[0301] The reaction can be carried out under atmospheric pressure, vacuum or pressure. In addition, the reaction can be carried out under an inert (nitrogen, argon) or oxidizing atmosphere (air).

[0302] Agitation must be vigorous to ensure particle formation and avoid product agglomeration.

[0303] As regards the specific conditions for carrying out the method of the invention, a person skilled in the art will know how to adjust the parameters of each of the steps indicated above according to the description and examples of the invention.

[0304] In certain embodiments, optionally in combination with one or more features of the various embodiments described above or below, a method for preparing a modified polymer polyol dispersion comprises:

[0305] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0306] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0307] at least one compound a.1) with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule which is bonded to the nitrogen atom; and

[0308] - Mixtures of condensation products as described above a.3).

[0309] The condensation product a.3) is obtained by reacting the mixture a.2) with at least one compound a.1) having at least one basic nitrogen atom, the compound a.1) being selected from melamine, trimethylolmelamine, those compounds of the formula (VII) or (VIII) as described above, and mixtures thereof; wherein the condensation reaction is carried out at a temperature of 2 to 140° C., preferably 25 to 120° C., more preferably 40 to 100° C., particularly preferably 60 to 90° C. The person skilled in the art knows how to adjust the temperature conditions depending on the compound a.1) used in the process.

[0310] According to certain specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the preparation of the modified polymer polyol comprises:

[0311] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0312] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0313] At least one compound a.1) having at least one basic nitrogen atom selected from

[0314] - melamine, trimethylolmelamine,

[0315] - those compounds of formula (VII) in which R1 is selected from H, methyl, -CN, CH3CO-, NH2-CO-;

[0316] - those compounds of formula (VIII) in which R2 is selected from O=C<, S=C<; R3 is H; and

[0317] - mixtures thereof;

[0318] as well as

[0319] • A mixture a.3) of condensation products which is obtainable at a temperature of 2-140°C, preferably 25-120°C, more preferably 40-100°C, particularly preferably 60-90°C.

[0320] According to certain specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the preparation of the modified polymer polyol comprises:

[0321] i) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0322] ii) adding the following substances simultaneously or in any order to the liquid polyol mixture obtained in i):

[0323] At least one compound a.1) having at least one basic nitrogen atom selected from

[0324] - melamine, trimethylolmelamine,

[0325] - those compounds of formula (VII) in which R1 is selected from H, methyl, -CN, CH3CO-, NH2-CO-;

[0326] - those compounds of formula (VIII) in which R2 is selected from O=C<, S=C<; and R3 is H; and

[0327] - mixtures thereof;

[0328] as well as

[0329] • A mixture a.3) of condensation products which is obtainable at a temperature of 2-140°C, preferably 25-120°C, more preferably 40-100°C, particularly preferably 60-90°C.

[0330] According to some embodiments, optionally in combination with one or more features of the various embodiments described above or below, the preparation of the modified polymer polyol comprises:

[0331] i) mixing at least one tetrakis(hydroxymethyl)phosphonium salt (THPX) with an aqueous or alcoholic base solution, preferably at a temperature of 0° C. to 60° C.;

[0332] ii) optionally filtering the resulting solution;

[0333] iii) distilling off the solvent and volatiles, thereby obtaining a mixture of compounds carrying phosphorus atoms as described above a.2);

[0334] iv) optionally filtering the resulting solution;

[0335] v) optionally oxidizing the product obtained in iii or the solution obtained in iv, wherein the oxidation can be carried out by simple thermal treatment in an air atmosphere or by using an oxidizing agent (for example hydrogen peroxide), thereby obtaining a mixture a.2) having a high content of oxidized components;

[0336] vi) reacting the mixture a.2) of compounds obtained in iii), the filtered solution obtained in iv), the oxidized mixture obtained in v) or a mixture thereof with at least one compound a.1) having at least one basic nitrogen atom, wherein the compound a.1) is characterized by the presence of at least one hydrogen atom attached to a nitrogen atom in the molecule and is selected from melamine, trimethylolmelamine, those compounds of formula (VII) or (VIII) as described above, and mixtures thereof, to obtain a mixture a.3) of condensation products; the reaction is preferably carried out at a temperature of 2-140° C., preferably 25-120° C., more preferably 40-100° C., most preferably 60-90° C.;

[0337] vii) mixing at least one base polyol with at least one compound modified with alkoxysilane groups as described above, thereby obtaining a liquid polyol mixture;

[0338] viii) preparing polymer particles in the presence of the liquid polyol mixture obtained in vii) by reacting the liquid polyol mixture obtained in vii) by adding simultaneously or sequentially in any order:

[0339] at least one compound a.1) with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule attached to the nitrogen atom and is selected from melamine, trimethylolmelamine, those compounds of formula (VII) or (VIII) as described above and mixtures thereof; and

[0340] vi) a mixture of the condensation products obtained in a.3).

[0341] According to some specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the aqueous or alcoholic base solution used in the above step i) is selected from KOH, NaOH, Ca(OH)2, Mg(OH)2, Ba(OH)2, triethylamine (NEt3), tributylamine (NBu3). Alternatively, the hydroxyalkylphosphonium salt can be treated with a basic ion exchange resin. Both strong ion exchange resins and weak ion exchange resins are suitable for this process. Examples of strong bases are IRN78 or A26. Examples of weak bases are IRA 67, MP-62 and VP OC1065.

[0342] According to certain specific embodiments, optionally in combination with one or more features of the various embodiments described above or below, the condensation product obtained by the reaction of the mixture of compounds a.2 obtained in iii), the filtered solution obtained in iv), the oxidized mixture obtained in v), or a mixture thereof with at least one compound a.1) having at least one basic nitrogen atom (selected from melamine, trimethylolmelamine, those compounds of formula (VII) or formula (VIII) as described above, and mixtures thereof) can be obtained at a temperature of 2-140° C., preferably 25-120° C., more preferably 40-100° C., most preferably 60-90° C. A person skilled in the art will know how to adjust the temperature and reaction time to complete the condensation reaction according to the description and examples herein.

[0343] The stable modified polymer polyol dispersion obtained according to the above method is a polyol having well-dispersed polymer particles having a high content of nitrogen and phosphorus.

[0344] In some embodiments, optionally in combination with one or more features of various embodiments described above or below, the stable modified polymer polyol dispersion comprises 5 wt % to 95 wt %, 10 wt % to 90 wt %, 15 wt % to 80 wt %, 20 wt % to 70 wt % dispersed polymer particles.

[0345] Thus, the phosphorus content of the dispersed polymer particles in the at least one polyol is from 0.1 to 50% by weight, preferably from 5 to 40% by weight, most preferably from 13 to 35% by weight. The nitrogen content of the dispersed polymer particles in the at least one polyol is from 0.1 to 40% by weight, preferably from 5 to 40% by weight, most preferably from 7 to 30% by weight. The total content of nitrogen and phosphorus is from 0.1 to 90% by weight, preferably from 10 to 70% by weight, most preferably from 20 to 60% by weight.

[0346] According to a specific embodiment of the present disclosure, the polymer particles dispersed in the at least one polyol may be further oxidized using a suitable oxidant such as manganate, permanganate, peroxide and molecular oxygen; preferably, the oxidant is molecular oxygen and / or hydrogen peroxide.

[0347] After the polycondensation reaction has occurred, an oxidation step is performed by introducing at least one oxidizing agent into the medium. If hydrogen peroxide is used as the oxidizing agent, it can be added as an aqueous solution to the modified polymer polyol containing a stable dispersion of polymer particles in the base polyol. If molecular oxygen is used as the oxidizing agent, air can be bubbled into the system after the polymer particles have been formed to perform the oxidation.

[0348] The polyol composition of the present invention comprises polymer particles, wherein at least 90% by volume have a particle size of 30 μm or less, preferably 0.5 μm to 20 μm, more preferably 0.6 μm to 15 μm, even more preferably 0.8 μm to 10 μm (particle size measured using a mastersizer 3000 from Malvern Instruments equipped with a hydro SM dispersion accessory using ethanol as eluent).

[0349] Particle size distributions can be trimodal, bimodal, unimodal, and different independent distributions can also be found.

[0350] The polymer-modified polyols of the present disclosure are useful in preparing polyurethane materials such as polyurethane foams, adhesives, elastomers, sealants, and coatings; preferably those polyurethane materials having flame retardant properties.

[0351] As regards the specific conditions for carrying out the method of the invention, a person skilled in the art will know how to adjust the parameters of each of the steps indicated above according to the description and examples of the invention.

[0352] In the preparation of polyurethane foam, polyisocyanates, water and additives conventionally used to make polyurethane foam can be used in combination with the modified polymer polyol of the present disclosure, and the amount and reaction conditions will vary depending on the type of polyurethane foam to be prepared and the desired properties. The skilled person is aware of the different types of reactants, catalysts and conditions required to prepare polyurethane foam.

[0353] Due to the presence of dispersed polymer particles with high P and N contents, the modified polymer polyols of the present invention provide flame retardant properties to the polyurethanes obtained by their use. In addition, the presence of dispersed polymer particles with high P and N contents will provide enhanced oxidation, thermal and UV stability to the polyurethanes obtained by their use. This enhanced stability is particularly suitable for polyurethane foams to reduce scorching and discoloration.

[0354] In addition, the modified polymer polyols of the present invention exhibit reduced formaldehyde content. Thus, when used to prepare polyurethane foams, the resulting foams exhibit low formaldehyde emissions.

[0355] In the preparation of polyurethane foam, polyisocyanates, water and additives conventionally used to make polyurethane foam can be used in combination with the modified polymer polyol of the present disclosure, and the amount and reaction conditions will vary depending on the type of polyurethane foam to be prepared and the desired properties. The skilled person is aware of the different types of reactants, catalysts and conditions required to prepare polyurethane foam.

[0356] Therefore, polyisocyanates that can be used in combination with the modified polymer polyols of the present disclosure to prepare polyurethane foams are well known in the art. Examples of suitable isocyanates include 4,4'-, 2,4'- and 2,2'-isomers of diphenylmethane diisocyanate (MDI), blends thereof, and polymeric and monomeric MDI blends, toluene-2,4- and 2,6-diisocyanates (TDI), and TDI / MDI blends can also be used.

[0357] The polyisocyanates may be used with an isocyanate index of 60 to 140, preferably 80 to 120, most preferably 90 to 110. The isocyanate index is defined as the ratio of isocyanate groups to isocyanate-reactive hydrogen atoms present in the polyurethane formulation. Thus, the isocyanate index represents the percentage of isocyanate actually used in the formulation relative to the amount of isocyanate theoretically required to react with the amount of isocyanate-reactive hydrogen used in the formulation.

[0358] The blowing agent can be selected from any blowing agent commonly known in the art. The main blowing agent is carbon dioxide generated by decarboxylation of carbamic acid generated by the reaction of water with isocyanate. Depending on regulations and target foam properties, alternative blowing agents (ABA) such as liquid carbon dioxide, methylene chloride, HCFC, pentane, etc. can be used.

[0359] The concentration of the blowing agent in the expandable polymer composition is preferably 0 to 120 wt %, more preferably 0 to 40 wt %, and even more preferably 0 to 10 wt %, relative to the total weight of the expandable polymer mixture.

[0360] Any known catalyst may be used, including amine compounds such as triethylenediamine, N-methylmorpholine, N,N-dimethylcyclohexylamine, pentamethyldiethylenetriamine, tetramethylethylenediamine, bis(dimethylaminoethyl)ether, 1-methyl-4-dimethylaminoethyl-piperazine, 3-methoxy-N-dimethylpropylamine, N-ethylmorpholine, dimethylethanolamine, N-cocomorpholine, N,N-dimethyl-N',N'-dimethylisopropylpropylenediamine, N,N-diethyl-3-diethylamino-propylamine, and dimethylbenzylamine. Metal catalysts based on tin, zinc, bismuth, and other metals may be used in the foam formulation, such as tin octoate, dibutyltin dilaurate, zinc octoate, and other similar compounds.

[0361] The amount of catalyst in the formulation may be 0 to 4%, preferably 0 to 2%, most preferably 0 to 1%.Another option is to use a self-catalytic polyol based on a tertiary amine initiator instead of an amine catalyst, thereby reducing volatile organic compounds in the foam.

[0362] Other additives that may be employed in the preparation of polyurethane polymers are fillers (e.g., talc, silica, titanium dioxide, magnesium oxide, calcium carbonate, carbon black, graphite, magnesium silicate or clays such as kaolinite and montmorillonite); flame retardants (e.g., halogenated flame retardants such as hexabromocyclododecane and brominated polymers; or phosphorus flame retardants such as triphenyl phosphate, dimethyl methylphosphonate, red phosphorus or aluminum diethylphosphinate); acid scavengers (e.g., calcium stearate, magnesium oxide, zinc oxide, tetrasodium pyrophosphate or hydrotalcite); antioxidants (e.g., hindered phenols, phosphites and mixtures thereof); and pigments and foaming agent stabilizers. Silicone surfactants may be required to stabilize the foam formulation and these products are available from major players in the market such as EVONIK, MOMENTIVE, AIR PRODUCTS, STRUKSILON, etc.

[0363] Polyurethane foam can be prepared by any known method. Thus, for example, polyurethane foam can be formed by a so-called prepolymer process, in which a stoichiometric excess of polyisocyanate is first reacted with a high equivalent polyol to form a prepolymer, which is then reacted with a chain extender and / or water in a second step to form the desired foam. Foaming methods may also be suitable. A so-called one-shot method may also be used. In such a one-shot method, polyisocyanate and all isocyanate-reactive components are simultaneously put together and reacted. Three widely used one-shot methods suitable for use herein include a block foam method, a high resilience block foam method, a molded foam method, and a box foam method.

[0364] Slabstock foam can be prepared by mixing the foam ingredients and dispensing them into a trough or other pouring plate where the reaction mixture reacts, rises freely relative to the atmosphere (sometimes beneath a membrane or other flexible cover), and solidifies. In common commercial-scale slabstock foam production, the foam ingredients (or their various mixtures) are pumped separately to a mixing head where they are mixed and dispensed onto a conveyor lined with paper or plastic. Foaming and curing occur on the conveyor to form foam blocks.

[0365] High resilience slabstock foam (HR slabstock foam) can be made by methods similar to those used to make conventional slabstock foam, but using higher equivalent weight polyols.

[0366] The shaped foam can be produced according to the present invention by transferring the reactants (a polyol composition comprising a copolyester, a polyisocyanate, a blowing agent and a surfactant) into a closed mold made of steel, aluminum or epoxy resin, where a foaming reaction occurs to produce a shaped foam. Either the so-called "cold forming" method (where the mold is not preheated to a temperature significantly above ambient temperature) or the "hot forming" method (where the mold is heated to promote curing) can be used. The cold forming method is preferred for producing high resilience shaped foam.

[0367] The box foam process consists in the discontinuous production of foam with a simple mixer (for mixing the foam ingredients previously weighed with a scale) or with a machine capable of metering and mixing the quantities of each product required to prepare a foam block, in both cases the liquid resulting from the mixture of all the ingredients is poured into a mold of defined block dimensions.

[0368] According to the present disclosure, any type of flexible (conventional, high resilience, viscoelastic foam), semi-flexible or rigid polyurethane foam can be prepared using the modified polymer polyols of the present disclosure, provided that the reactants, catalysts and additives forming the polyurethane foam are selected and processed in an appropriate known manner.

[0369] The polyurethane foams prepared from the stable modified polymer polyols of the present disclosure exhibit densities of 4 to 120 kg / m 3 , preferably 15 to 80 kg / m 3 , most preferably 20 to 60 kg / m 3 .

[0370] The use of the modified polymer polyols of the present disclosure in the preparation of polyurethane foams can improve the flame retardancy and heat aging resistance of the foams obtained therefrom. Therefore, depending on the desired combustion test, the polyurethane foam obtained may not require any other flame retardant additives, although any other known flame retardant additives can be used in combination with the modified polymer polyols of the present disclosure when preparing polyurethane foams.

[0371] The use of the modified polymer polyols of the present disclosure in the preparation of polyurethane foams produces foams that retain their flame retardancy longer than foams prepared using liquid flame retardant additives, thereby avoiding known migration problems.

[0372] The modified polymer polyols of the present disclosure exhibit relatively low viscosity and high phosphorus and nitrogen contents. Thus, the modified polymer polyols are particularly useful for preparing polyurethane foams having improved flame retardant properties and reduced solids content.

[0373] Furthermore, using the modified polymer polyols of the present disclosure in rigid foams reduces the thermal conductivity values ​​of the foams, thereby increasing the thermal insulation capabilities of the foams.

[0374] In the context of this disclosure, the term "modified polymer polyol" is also referred to as "polymer-polyol dispersion" or "polymer polyol", which refers to a dispersion of polymer particles, i.e., a dispersion of organic fillers, in a continuous phase composed of one or more compounds having multiple hydroxyl groups ("base polyol").

[0375] In the context of the present invention, when referring to compounds with basic nitrogen atoms, the term "functionality" is used herein to represent the number average functionality of the compound (the number of hydrogen atoms connected to the nitrogen atom in each molecule). When referring to a base polyol, the term "functionality" is used herein to represent the number average functionality (the number of hydrogen atoms in each molecule) of the polyol composition, assuming that it is the number average functionality (the number of active hydrogens in each molecule) of the initiator used in its preparation. Although in reality, due to some terminal unsaturations, the actual functionality will usually be slightly lower, but for the purpose of characterizing the base polyol, the functionality of the polyol is the functionality of the initiator used for its preparation.

[0376] In the context of the present invention, the term "iOH" refers to the hydroxyl number (iOH), which is defined as the number of milligrams of potassium hydroxide required to completely hydrolyze the fully phthalated derivatives made from 1 gram of polyol. The hydroxyl number is determined according to ASTM D4274-16.

[0377] According to the present disclosure, the term "stable polyol" or "stable polymer-modified polyol" refers to a dispersion of polymer particles in the at least one polyol which does not settle out or at least remains in dispersion when mixed with other foam-forming ingredients.

[0378] According to some examples of the present disclosure, the method should allow the production of highly stable modified polymer polyols in which the dispersed particles are smaller (and therefore less prone to sedimentation). Unexpectedly, the modified polymer polyols are stable even when the base polyol is a non-reactive polyether polyol (i.e., having primarily secondary hydroxyl groups).

[0379] In the context of the present invention, the term "molecular weight" of a polyol is calculated using the following formula.

[0380]

[0381] Here, “functionality” refers to the functionality of the polyol, that is, the average number of hydroxyl groups per polyol molecule; the hydroxyl number (iOH) is calculated according to ASTM D4274-16.

[0382] In the context of the present invention, Haake TM Viscotester TM The rheometer obtains viscosity measurements (in mPa·s) at 25°C.

[0383] The formaldehyde emission of polyurethane foams was determined according to the UNE-ISO 16000-[clauses 3, 9 and 11] standard method following the CertiPUR instructions for flexible polyurethane foams.

[0384] The solids content of the modified polymer polyol was calculated using the following formula.

[0385]

[0386] In the context of the present disclosure, the term "weight %" refers to the percentage of each component in a combination or composition relative to the total weight.

[0387] The modified polymer polyol "obtainable" by the process of the present invention is used herein to define the modified polymer polyol by the process of obtaining it, and refers to the product obtainable by the preparation process defined herein. For the purposes of the present invention, the expressions "obtainable", "obtained" and equivalent expressions are used interchangeably, and in any case, the expression "obtainable" includes the expression "obtained".

[0388] For the purpose of the present invention, any range given includes the lower and upper endpoints of the range. Unless otherwise specified, the given ranges (eg, temperature, time, size, etc.) should be considered as approximate.

[0389] Although only a certain number of embodiments are disclosed herein, other substitutions, modifications, uses and / or equivalents are possible. In addition, all possible combinations of the embodiments are also covered. Therefore, the scope of the present disclosure should not be limited by the specific embodiments, but should only be determined by a fair reading of the attached claims.

[0390] The following examples are provided to illustrate embodiments of the present invention but are not intended to limit the scope thereof. Unless otherwise indicated, all parts and percentages are by weight.

[0391] Example

[0392] The following materials were used:

[0393] - Polyol A - a polyether polyol (PO / EO) initiated with sorbitol (functionality 6), with a hydroxyl value of 29.5 mgKOH / g, a polyethylene oxide end block content of 16.2 wt%, 81% primary hydroxyl groups, and a viscosity of 1500 mPa·s at 25°C.

[0394] - Polyol B - polyether polyol (PO / EO) initiated with glycerol (functionality 3), hydroxyl value of 48 mgKOH / g, content of polyethylene units randomly distributed along the central backbone of the polyol of 12 wt%, viscosity of 560 mPa·s at 25°C.

[0395] - Polyol C - polyether polyol (PO) initiated with glycerol (functionality 3) with a hydroxyl value of 56 mgKOH / g and a viscosity of 470 mPa·s at 25°C.

[0396] - Polyol D - a glycerol (functionality 3) initiated polyether polyol (PO / EO) with a hydroxyl value of 28 mgKOH / g, a polyethylene oxide end block content of 14 wt %, and a viscosity of 1100 mPa·s at 25°C.

[0397] - Polyol E - polyether polyol (PO / EO) initiated with glycerol (functionality 3), hydroxyl value of 55 mgKOH / g, content of polyethylene units randomly distributed along the polyol central skeleton of 15 wt%, content of polyethylene units as terminal blocks of 5.8 wt%, viscosity at 25°C of 500 mPa·s.

[0398] - Polyol F - a glycerol (functionality 3) initiated polyether polyol (PO / EO) having a hydroxyl value of 35 mgKOH / g, a polyethylene oxide end block content of 18 wt %, and a viscosity of 870 mPa·s at 25°C.

[0399] - Polyol G - a glycerol (functionality 3) initiated polyether polyol (PO / EO) with a hydroxyl value of 28 mgKOH / g, a polyethylene oxide end block content of 15 wt %, and a viscosity of 1100 mPa·s at 25°C.

[0400] - THPS - tetrakis(hydroxymethyl)phosphonium sulfate (70-75 wt % in water), available from Sigma Aldrich.

[0401] -KOH - Potassium hydroxide (≥85%), available from Sigma Aldrich.

[0402] -(3-isocyanatopropyl)triethoxysilane (also known as 3-(triethoxysilyl)propyl isocyanate) (95%), available from Sigma Aldrich.

[0403] -(3-isocyanatopropyl)trimethoxysilane (also known as 3-(trimethoxysilyl)propyl isocyanate) (>97%), available from TCI Europe.

[0404] - DBTL - dibutyltin dilaurate (95%), available from Sigma Aldrich.

[0405] - PRO1 - stannous neodecanoate, available from Evonik Industries.

[0406] -Tetrafluoroboric acid solution (48%), available from Sigma Aldrich.

[0407] -Trimethoxy({3-[(oxiran-2-yl)methoxy]propyl})silane (also known as glycidyloxypropyl-trimethoxysilane) (97%), available from Acros Organics.

[0408] - Urea (98%), available from Sigma Aldrich.

[0409] - Melamine (99%), available from Sigma Aldrich.

[0410] - -29-Stannic octoate, available from Evonik Industries.

[0411] - 33-33 wt % solution of triethylenediamine in dipropylene glycol, available from Evonik Industries.

[0412] - BDE - 70% solution of bis(2-dimethylaminoethyl) ether in dipropylene glycol, available from Evonik Industries.

[0413] - Niax L-620LV - a silicone surfactant for polyurethane foams available from Momentive.

[0414] - TCPP - tris(chloroisopropyl) phosphate, available from Shekoy chemicals.

[0415] -Melamine, available from BASF.

[0416] - TDI-80 - toluene diisocyanate (80 / 20), available from Borsodchem.

[0417] - TDI 65 - toluene diisocyanate (65 / 35), available from Borsodchem.

[0418] Example 1. Preparation of NAD-stabilizer A

[0419] 112.68 g of polyol A and 2.32 g of 3-(triethoxysilyl)propyl isocyanate were placed in a 3-necked glass flask reactor equipped with mechanical stirring. The temperature was raised to 100° C. and maintained for 48 hours under stirring and nitrogen atmosphere. After this period of time, the temperature was raised to 120° C. and maintained at this temperature for 23 hours. The reaction mixture was stirred at 2270 cm / s for 1 h. -1 The complete reaction of 3-(triethoxysilyl)propyl isocyanate was detected by the complete disappearance of the isocyanate infrared band at . The obtained product, NAD-stabilizer A, was a viscous light yellow liquid.

[0420] Example 2. Preparation of NAD-stabilizer B

[0421] 116.68 g of polyol A, 2.32 ml of 3-(triethoxysilyl)propyl isocyanate and 34 mg of dibutyltin dilaurate were placed in a 3-necked glass flask reactor equipped with mechanical stirring. The temperature was raised to 80° C. and maintained for 30 minutes under stirring and nitrogen atmosphere. The complete disappearance of the isocyanate band in the infrared spectrum confirmed the completion of the reaction. A transparent liquid (NAD-stabilizer B) was obtained as the reaction product.

[0422] Example 3. Preparation of NAD-Stabilizer C

[0423] 149.98 g of polyol A, 2.57 g of 3-(triethoxysilyl)propyl isocyanate and 67.6 mg of KOSMOS PRO1 were mixed in a 3-necked glass flask reactor equipped with mechanical stirring. The temperature was raised to 80° C. and maintained for 30 minutes under stirring and nitrogen atmosphere. The complete disappearance of the isocyanate band in the infrared spectrum confirmed the completion of the reaction. A transparent liquid (NAD-stabilizer C) was obtained as the reaction product.

[0424] Example 4. Preparation of NAD-Stabilizer D

[0425] In a glass reactor equipped with a mechanical stirrer, 34.8 mg of tetrafluoroboric acid solution (48%) was added to 61.54 g of polyol A. After stirring for 5 minutes, 1.42 g of 3-glycidyloxypropyl-trimethoxysilane was added to the mixture, and the reaction temperature was raised to 50° C. The temperature was maintained at 50° C. for 3 hours. The resulting product (NAD-stabilizer D) was a transparent liquid.

[0426] Example 5. Preparation of THP mixture A

[0427] The KOH solution with a concentration of 0.166 g / mL is prepared by dissolving 87.04 g of KOH in 420 ml of ethanol. 390 mL of this solution is slowly added to 323.3 g of THPS solution (76.1%). After complete precipitation, sulfate is filtered out and the filter cake is washed with another 100 ml of pure methanol. Under the conditions of 130 ° C. for the temperature of the heating surface (the temperature of the film), 1.0-1.1 kPa, 300 rpm of the rotor speed and about 10 mL / min of the feed rate, a short-path distillation apparatus (model "KDL5" is manufactured by UIC GmbH) is used for distillation to perform thin film distillation. 101 g of product is collected. The composition of the product is analyzed by 31 P-NMR. The results are shown in Table 1. Other minor components may be present.

[0428] Table 1

[0429]

[0430] Example 6. Preparation of THP mixture B

[0431] 1500.3 g of THPS (tetrakis (hydroxymethyl) phosphonium sulfate solution (75%)) was placed in a glass reactor equipped with a mechanical stirrer. 1686 mL of a 0.186 g / mL KOH solution (369 g of KOH flakes in 1300 g of methanol) was slowly added to the THPS to precipitate potassium sulfate. After complete precipitation, the sulfate was filtered off and the volatile compounds in the resulting solution were distilled in a rotary evaporator at a temperature of 100° C. for 75 minutes to reduce the pressure to 25 mbar, which was maintained for another 15 minutes.

[0432] The mol% distribution of the different THP derivatives was determined by 31P-NMR. The results are shown in Table 2. Other minor components may be present.

[0433] Table 2

[0434]

[0435] Example 7. Preparation of THP mixture C

[0436] 700.1 g of THPS (tetrakis (hydroxymethyl) phosphonium sulfate solution (75%)) was placed in a glass reactor equipped with a mechanical stirrer. 779 mL of a 0.188 g / mL KOH solution (172.2 g of KOH flakes in 600 g of methanol) was slowly added to the THPS to precipitate potassium sulfate. After complete precipitation, the sulfate was filtered off and the volatile compounds in the resulting solution were distilled in a rotary evaporator at a temperature of 50° C. for 120 minutes to reduce the pressure to 25 mbar, which was maintained for another 15 minutes.

[0437] The mol% distribution of the different THP derivatives was determined by 31P-NMR. The results are shown in Table 3. Other minor components may be present.

[0438] Table 3

[0439]

[0440] Example 8. Preparation of THP mixture D

[0441] 301.5 g of THPS (tetrakis (hydroxymethyl) phosphonium sulfate solution (75%)) were placed in a glass reactor equipped with a mechanical stirrer. KOH solution (55.1 g of KOH flakes in 38.6 g of methanol) was slowly added to THPS to precipitate potassium sulfate. The sulfate was filtered off and the volatile compounds in the resulting solution were distilled in a rotary evaporator at a temperature of 100° C. for 50 minutes to reduce the pressure to 20 mbar, which was maintained for another 15 minutes. A turbid liquid product was obtained, which was cooled to 25° C. and filtered again to obtain a clear product.

[0442] The mol% distribution of THP derivatives was determined by 31P-NMR. The results are shown in Table 4. Other minor components may be present.

[0443] Table 4

[0444]

[0445] Example 9. Preparation of THP mixture E

[0446] A solution of 205 g of KOH and 143 g of MiliQ water was prepared. 494 g of THPS was weighed in a beaker equipped with a mechanical stirrer. 186 g of the previous KOH / H2O solution was slowly added to the THPS. The resulting product was filtered through a POBEL No. 4 porous plate to obtain 434 g of solution and 240 g of filter cake. The volatile compounds were removed in a rotary evaporator at 15 mbar and 100°C in hot oil for 1 hour, and the resulting product was filtered again. 187 g of product was obtained. The product was redissolved in 200 g of water, and the resulting solution was heated at 60°C in an air atmosphere (1 bar) for 24 hours and at 100°C for another 8 hours. Finally, the product was vacuum dried (15 mbar, 100°C) for 1 hour. 183 g of product was obtained.

[0447] The mol% distribution of THP derivatives was determined by 31P-NMR. The results are shown in Table 5. Other minor components may be present.

[0448] Table 5

[0449]

[0450] Example 10. Comparative Example

[0451] 90.2 g of polyol B and 8.35 g of THP mixture A were placed in a glass reactor equipped with mechanical stirring and the temperature was raised to 100° C. After the temperature reached 100° C., a solution of 6.09 g of urea in 9 mL of water preheated to 40° C. was added to the reactor. The pressure was reduced to 400 mbar to remove volatile compounds. After the volatiles were distilled, the temperature was raised to 120° C. and maintained under vacuum for 3 hours. Finally, the temperature was raised to 140° C. and placed under vacuum at this temperature for 1 hour.

[0452] The modified polymer polyol was not stable and the particles settled quickly.

[0453] Example 11. Preparation of Stable Modified Polymer Polyols

[0454] 90.2 g of polyol B, 4.47 g of NAD-stabilizer A and 8.37 g of THP mixture A were placed in a glass reactor equipped with mechanical stirring and the temperature was raised to 100° C. After the temperature reached 100° C., a solution of 6.06 g of urea in 9 mL of water preheated to 40° C. was added to the reactor under vigorous stirring. Then, volatile compounds were removed under vacuum (400 mbar). After the volatile compounds were removed, the temperature was raised to 120° C. and the reaction was maintained at this temperature for 3 hours under vacuum. Then, the temperature was raised to 140° C. and maintained at this temperature for 1 hour.

[0455] The obtained product is a white stable modified polymer polyol with a viscosity of 805 MPa·s. The particle size is bimodal, with the largest part ranging from 0.675 to 8.68 μm, centered at 3.12 μm. The smaller part is particles ranging from 0.01 to 0.675 μm, centered at 0.376 μm.

[0456] Table 6 below summarizes the different examples carried out following the procedure described in Example 11.

[0457] Table 6

[0458]

[0459]

[0460] Example 31. THP / urea premix

[0461] 89.5 g of polyol B, 3.3 g of dispersant D are placed in a glass reactor equipped with mechanical stirring, and the temperature is raised to 80° C. In another reactor equipped with mechanical stirring, 17.2 g of urea, 16.9 g of THP mixture D and 7 g of water are heated to 80° C. to obtain a clear solution. The temperature is maintained at 80° C. for 30 minutes so that the THP mixture reacts with the urea to form a so-called precondensate. The clear solution of the precondensate is added to the reactor under vigorous stirring. Then, volatile compounds are removed under vacuum (400 mbar). After removing the volatile compounds, the temperature is raised to 120° C. and the reaction is maintained at this temperature for 3 hours under vacuum. Then, the temperature is raised to 140° C. and maintained at this temperature for 1 hour.

[0462] Example 32. THP / melamine premix

[0463] 16.98 g of THP mixture D and 4.35 g of melamine were reacted at 90° C. with stirring until a clear solution was obtained. Then, a solution of 80° C. urea (6.88 g) in 8 g of water was added to the precondensation product of melamine and THP with stirring. The resulting clear mixture containing THP-melamine precondensate and urea was added to a glass reactor containing 90.1 g of polyol B and 3.14 g of NAD-stabilizer D with vigorous stirring. Then, the volatile compounds were removed under vacuum (400 mbar). After the volatile compounds were removed, the temperature was raised to 120° C. and the reaction was kept at this temperature under vacuum for 3 hours. Then, the temperature was raised to 140° C. and kept at this temperature for 1 hour.

[0464] The results obtained for the stable modified polymer polyols are shown in Table 7 below.

[0465] Table 7

[0466]

[0467]

[0468]

[0469] Example 33. Preparation of polyurethane foam

[0470] The batch was prepared by mixing water and amine according to the foam recipe shown in Table 8. The polyol and silicone were mixed in a paper cup at a speed of 5000 rpm for 50 seconds. The corresponding amount of batch was added to the polyol / silicone mixture and stirred, and tin octoate was added after 5 seconds and stirred for another 5 seconds. Then the isocyanate was added and stirred for 10 seconds.

[0471] The resulting mixture was poured into a 30.4×21.8×16.7 cm aluminum mold protected with kraft paper at 23°C and the mixture was allowed to react in the mold for 5 minutes, and the rising curve was monitored by the Foamat equipment. The resulting foam was removed from the mold and cured in an oven at 100°C for 15 minutes. After this curing step, the foam was stored at 23°C and 50% relative humidity for at least 24 hours.

[0472] The prepared compositions are shown in Table 8 below.

[0473] Table 8

[0474]

[0475] Polymer foams. Combustion behavior.

[0476] The foams were analyzed in accordance with standard UL94 (horizontal burning foam material test).

[0477]

Claims

1. Use of an alkoxysilane-terminated polyether polyol having 1 to 8 hydroxyl groups in each molecule and 1 to 2 alkoxysilane groups in each molecule in the preparation of a modified polymer polyol dispersion, which can be obtained by a process comprising the following steps: capping 1 to 2 terminal hydroxyl groups of a polyether polyol a) having a functionality of 2 to 9 and an average molecular weight of 3000 to 25000 calculated using the following formula with a capping agent b), wherein the capping agent b) is a compound of formula (I) having at least one alkoxysilane terminal group and at least one hydroxyl-reactive group; in, "Functionality" means the functionality of the polyol, i.e., the average number of hydroxyl groups per polyol molecule; the hydroxyl number (iOH) is calculated according to ASTM D4274-16; wherein the reaction of the end-capping agent and the polyether polyol is carried out at a molar ratio of 0.05 to 2.0 moles of the end-capping agent per 1 mole of the polyether polyol; Wherein, the compound of formula (I) has the following formula: wherein R1, R2 and R3 are each independently selected from a linear or branched (C1-C6) alkyl group, a linear or branched (C1-C6) alkoxy group and a tri(C1-C3) alkylsilyloxy group; provided that at least one of R1, R2 or R3 is a (C1-C6) alkoxy group; and wherein A is selected from the group consisting of compounds of formula (II), (III), (IV), (V) and (VI): in, The asterisk indicates the point of attachment to the Si atom in formula (I); m, n, p, r, t and w are independently integers selected from 1 to 6; q, s and v are independently integers selected from 1 to 4; R4 is selected from -NCO, The group, Among them, the asterisk indicates the point of connection to the rest of the group; X is selected from -O- and -N(R5)-; Wherein R5 is selected from H, linear or branched (C1-C6) alkyl, The group, Among them, the asterisk indicates the connection point with the N atom; x and z are independently an integer selected from 1 to 6; R8, R9 and R10 are each independently selected from a linear or branched (C1-C6) alkyl group, a linear or branched (C1-C6) alkoxy group and a tri(C1-C3) alkylsilyloxy group; provided that at least one of R8, R9 or R10 is a (C1-C6) alkoxy group or a tri(C1-C3) alkylsilyloxy group; and wherein the reaction of b) with a) is carried out at a molar ratio of 0.05 to 2.0 moles of the compound of formula (I) per 1 mole of the polyether polyol; Wherein, the modified polymer polyol dispersion is a stable modified polymer polyol dispersion of polymer particles in a liquid polyol mixture; Wherein, the stable modified polymer polyol dispersion can be obtained by a method comprising the following steps: preparing polymer particles by a or b in the presence of the liquid polyol mixture: a. in the liquid polyol mixture and under polymerization conditions, reacting the following a.1) with a.2) or a.3): a.1) at least one compound with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule which is bonded to the nitrogen atom; a.2) mixtures of compounds containing phosphorus atoms, including [bis(hydroxymethyl)phosphino]methanol (THP), tetrakis(hydroxymethyl)phosphonium salts (THPX), [bis(hydroxymethyl)phosphino]methanol (THPO), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), {bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHPO), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHPO) and ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHPO); a.3) a mixture of condensation products obtained by reaction of a mixture of compounds carrying phosphorus atoms as described above a.2) with a.1) at least one compound carrying at least one basic nitrogen atom; Wherein, the compound a.1) having at least one basic nitrogen atom is selected from - melamine, trimethylolmelamine, - those compounds of formula (VII) or formula (VIII); and - mixtures thereof; Wherein, the compound of formula (VII) is as follows: R1-NH2 (VII) Wherein, R1 is selected from -H, -(C1-C3)alkyl, (C1-C3)alkyl-CO-, NH2-CO-, -(CH2) n -NH2, -CN, -NH2, -SO2NH2, cyclohexyl, phenyl, -SO2OH and -NHCONHNH2; wherein n is an integer from 1 to 18; The compound of formula (VIII) is as follows: wherein R2 is selected from NH=C<, O=C< and S=C<; R3 is selected from H, -CN, -NH2, -CONH2, -CONHCONH2 and -CONHCONHCONH2; or b. in the liquid polyol mixture and under polymerization conditions, optionally in the presence of a catalyst, reacting the following b.1) with b.2) b.1) at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen or oxygen atom; b.2) at least one polyisocyanate; The liquid polyol mixture comprises at least one base polyol and at least one alkoxysilane-terminated polyether polyol.

2. A stable modified polymer polyol dispersion of polymer particles in a liquid polyol mixture, wherein: The stable modified polymer polyol dispersion can be obtained by a method comprising the following steps: preparing polymer particles by a or b in the presence of the liquid polyol mixture: a. in the liquid polyol mixture and under polymerization conditions, reacting the following a.1) with a.2) or a.3): a.1) at least one compound with at least one basic nitrogen atom, characterized in that at least one hydrogen atom is present in the molecule which is bonded to the nitrogen atom; a.2) mixtures of compounds containing phosphorus atoms selected from [bis(hydroxymethyl)phosphino]methanol (THP), tetrakis(hydroxymethyl)phosphonium salts (THPX), [bis(hydroxymethyl)phosphino]methanol (THPO), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), {bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHPO), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHPO) and ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHPO); a.3) a mixture of condensation products obtained by reaction of a mixture of compounds carrying phosphorus atoms as described above a.2) with a.1) at least one compound carrying at least one basic nitrogen atom; Wherein, the at least one compound having at least one basic nitrogen atom a.1) is selected from - melamine, trimethylolmelamine, - those compounds of formula (VII) or formula (VIII); and - mixtures thereof; Wherein, the compound of formula (VII) is as follows: R1-NH2 (VII) Wherein, R1 is selected from -H, -(C1-C3)alkyl, (C1-C3)alkyl-CO-, NH2-CO-, -(CH2) n -NH2, -CN, -NH2, -SO2NH2, cyclohexyl, phenyl, -SO2OH and -NHCONHNH2; wherein n is an integer from 1 to 18; The compound of formula (VIII) is as follows: wherein R2 is selected from NH=C<, O=C< and S=C<; R3 is selected from H, -CN, -NH2, -CONH2, -CONHCONH2 and -CONHCONHCONH2; or b. in the liquid polyol mixture and under polymerization conditions, optionally in the presence of a catalyst, reacting the following b.1) with b.2) b.1) at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen or oxygen atom; b.2) at least one polyisocyanate; The liquid polyol mixture comprises at least one base polyol and at least one alkoxysilane-terminated polyether polyol as defined in claim 1.

3. The stable modified polymer polyol dispersion of claim 2, which can be obtained by a method comprising the following steps: i. mixing said at least one base polyol with at least one alkoxysilane-terminated polyether polyol as defined in claim 1, thereby obtaining a liquid polyol mixture; ii. adding the following materials simultaneously or in any order to the liquid polyol mixture obtained in i): a.1) at least one compound with at least one basic nitrogen atom, characterized in that There is at least one hydrogen atom attached to a nitrogen atom in the molecule; and a.2) A mixture of compounds containing phosphorus atoms, comprising: I. [Bis(hydroxymethyl)phosphino]methanol (THP), concentration 0-99.9 mol%, II. Tetrakis (hydroxymethyl) phosphonium salt (THPX), concentration 0-50 mol%, III. [Bis(hydroxymethyl)phosphoryl]methanol (THPO), concentration 0-99.9 mol%, IV. {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), concentration 0-80 mol % V. {Bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), concentration 0-30 mol % VI. ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), concentration 0-15 mol% VII. {[Bis(hydroxymethyl)phosphoryl]methoxy}methanol (mTHPO), concentration 0-20 mol% VIII. {bis[(hydroxymethoxy)methyl]phosphoryl}methanol (dTHPO) at a concentration of 0-10 mol%, and IX. ({bis[(hydroxymethoxy)methyl]phosphoryl}methoxy)methanol (tTHPO), concentration 0-4 mol%; The sum of compounds with phosphorus atoms in the mixture is 100 mol %; or a.3) a mixture of condensation products obtained by reaction of a mixture as described above under a.2) with a.1) at least one compound having at least one basic nitrogen atom; Wherein, the compound a.1) having at least one basic nitrogen atom is selected from: - melamine, trimethylolmelamine, - those compounds of formula (VII) or formula (VIII) as defined in claim 2; and - A mixture thereof.

4. The stable modified polymer polyol dispersion of claim 2, wherein The at least one compound having at least one basic nitrogen atom is a.1) selected from - melamine, trimethylolmelamine, - those compounds of formula (VII) in which R1 is selected from H, methyl, -CN, CH3CO-, NH2-CO-; - those compounds of formula (VIII) in which R2 is selected from O=C<, S=C<; and R3 is H; and - mixtures thereof; and The mixture a.2) of compounds containing phosphorus atoms comprises: I. [Bis(hydroxymethyl)phosphino]methanol (THP), concentration 35-85 mol % II. Tetrakis(hydroxymethyl)phosphonium salt (THPX), concentration 0-30 mol%, III. [Bis(hydroxymethyl)phosphoryl]methanol (THPO), concentration 0-40 mol % IV. {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), concentration 0-80 mol % V. {Bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), concentration 0-30 mol % VI. ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), concentration 0-15 mol% VII. {[Bis(hydroxymethyl)phosphoryl]methoxy}methanol (mTHPO), concentration 0-20 mol% VIII. {bis[(hydroxymethoxy)methyl]phosphoryl}methanol (dTHPO) at a concentration of 0-10 mol%, and IX. ({bis[(hydroxymethoxy)methyl]phosphoryl}methoxy)methanol (tTHPO), concentration 0-4 mol%; The total amount of compounds having phosphorus atoms in the mixture is 100 mol%.

5. The stable modified polymer polyol dispersion of claim 2, wherein The at least one compound having at least one basic nitrogen atom is a.1) selected from - melamine, trimethylolmelamine, - those compounds of formula (VII) in which R1 is selected from H, methyl, -CN, CH3CO-, NH2-CO-; - those compounds of formula (VIII) in which R2 is selected from O=C<, S=C<; and R3 is H; and - mixtures thereof; and The mixture of condensation products a.3) is as defined in claim 2.

6. The stable modified polymer polyol dispersion of claim 2, which can be obtained by a process comprising the steps of: i. mixing said at least one base polyol with at least one alkoxysilane-terminated polyether polyol as defined in claim 1, thereby obtaining a liquid polyol mixture; ii. optionally in the presence of a catalyst and under polymerization conditions, to the liquid polyol mixture obtained in i) simultaneously or in any order, adding the following materials: b.1) at least one co-reactant having an equivalent weight of up to 400 and at least one active hydrogen attached to a nitrogen or oxygen atom, the co-reactant being selected from an amine, an alkanolamine or a diol; and b.2) At least one polyisocyanate.

7. A method for preparing a stable modified polymer polyol dispersion, the method comprising: i. mixing at least one tetrakis (hydroxymethyl) phosphonium salt (THPX) with an aqueous or alcoholic solution of a base; ii. optionally filtering the resulting solution; iii. distilling off the solvent and volatiles, thereby obtaining a mixture a.2) of compounds carrying a phosphorus atom, wherein the compound carrying a phosphorus atom is selected from [bis(hydroxymethyl)phosphino]methanol (THP), tetrakis(hydroxymethyl)phosphonium salt (THPX), [bis(hydroxymethyl)phosphino]methanol (THPO), ({[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHP), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHP), {bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHP), {[bis(hydroxymethyl)phosphino]methoxy}methanol (mTHPO), {bis[(hydroxymethoxy)methyl]phosphino}methanol (dTHPO) and ({bis[(hydroxymethoxy)methyl]phosphino}methoxy)methanol (tTHPO); iv. optionally filtering the resulting solution; v. optionally oxidizing the product obtained in iii or the solution obtained in iv, thereby obtaining a mixture a.2) having a high content of oxidized components; vi. mixing at least one base polyol with at least one alkoxysilane-terminated polyether polyol as defined in claim 1, thereby obtaining a liquid polyol mixture; vii. preparing polymer particles in the presence of the liquid polyol mixture obtained in vi by reacting the liquid polyol mixture obtained in vi by adding the following substances simultaneously or in any order: at least one compound a.1) having at least one basic nitrogen atom, characterized in that at least one hydrogen atom attached to the nitrogen atom is present in the molecule and is selected from those compounds of formula (VII) or (VIII); and - a mixture a.2) of compounds containing phosphorus atoms obtained in iii or iv, a mixture a.2) of the oxidation obtained in v, or a mixture thereof; Wherein, the compound of formula (VII) is as follows: R1-NH2 (VII) Wherein, R1 is -H, -(C1-C3)alkyl, (C1-C3)alkyl-CO-, NH2-CO-, -(CH2) n -NH2, -CN, -NH2, -SO2NH2, cyclohexyl, phenyl, -SO2OH or -NHCONHNH2; wherein n is an integer from 1 to 18; The compound of formula (VIII) is as follows: Wherein, R2 is selected from NH=C<, O=C< and S=C<; R3 is selected from H, -CN, -NH2, -CONH2, -CONHCONH2 and -CONHCONHCONH2.

8. A method for preparing a polyurethane material, wherein: The method comprises reacting at least one polyisocyanate with an isocyanate-reactive component comprising at least one stable modified polymer polyol dispersion according to any one of claims 2 to 6 in the presence of at least one catalyst and optionally additives.

9. A polyurethane material obtainable by the process according to claim 8.

10. An article comprising the polyurethane material according to claim 9.