Semiconductor structure and method of forming a semiconductor structure
By depositing a covering layer on the ruthenium conductive structure and forming a conductive structure, the problem of metal atom diffusion during the heat treatment of the conductive structure in the integrated circuit is solved, and the effects of reducing contact resistance and improving thermal stability are achieved.
Patent Information
- Application Number
- CN202110255869.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-05
- Filing Date
- 2021-03-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-03-09
AI Technical Summary
In integrated circuits, conductive structures lacking pads or barrier layers can easily lead to diffusion of metal atoms during thermal processing, increased contact resistance and material migration, making integration challenging.
Selectively depositing a capping layer, such as a tungsten layer, on the top surface of the ruthenium conductive structure, forming the capping layer to prevent outdiffusion of cobalt atoms, and exposing the capping layer by etching a stack of stop layers and dielectric layers, forming the conductive structure to surround the cobalt Diffusion barrier.
It effectively prevents cobalt atoms from migrating to the upper metallization layer, reduces contact resistance, improves thermal stability and reduces material migration, and enhances the integrity of the conductive structure.
Smart Images

Figure CN113161321B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to semiconductor structures and methods of forming semiconductor structures. Background Art
[0002] In an integrated circuit, conductive structures (e.g., metal contacts, vias, and lines) are electrically coupled to transistor regions, such as gate electrodes and source / drain terminals, to propagate electrical signals to and from the transistors. Depending on the complexity of the integrated circuit, the conductive structures may form multiple metal wiring layers. Summary of the invention
[0003] Some embodiments of the present application provide a semiconductor structure comprising: a substrate; a first metallization layer located on the substrate, wherein the first metallization layer includes a linerless conductive structure surrounded by a dielectric; a covering layer located on a top surface of the linerless conductive structure; and a second metallization layer located on the first metallization layer and including a conductive structure on the linerless conductive structure, wherein the covering layer is interposed between the top surface of the linerless conductive structure and a bottom surface of the conductive structure.
[0004] Other embodiments of the present application provide a semiconductor structure, comprising: a substrate; a first metallization layer, located on the substrate and comprising a linerless conductive structure surrounded by a dielectric; a covering layer, disposed on a top surface of the linerless conductive structure, wherein the covering layer has a dome shape with a base greater than a width of the linerless conductive structure; and a second metallization layer, located on the first metallization layer and comprising a conductive structure on the linerless conductive structure, wherein the linerless conductive structure is separated from the conductive structure by the covering layer.
[0005] Still other embodiments of the present application provide a method for forming a semiconductor structure, comprising: depositing a cobalt diffusion barrier layer on a linerless conductive structure comprising ruthenium, wherein depositing the cobalt diffusion barrier layer comprises forming the cobalt diffusion barrier layer self-aligned with the linerless conductive structure; depositing a stack comprising an etch stop layer and a dielectric layer on the cobalt diffusion barrier layer; forming an opening in the stack to expose the cobalt diffusion barrier layer; and forming a conductive structure on the cobalt diffusion barrier layer to surround the cobalt diffusion barrier layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0006] Aspects of the present invention are best understood from the following detailed description when read with the accompanying figures.
[0007] Figure 1 is a partial cross-sectional view of a metallization layer having a liner-less or barrier-less conductive structure, according to some embodiments.
[0008] Figure 2 is a partial cross-sectional view of a liner-less or barrier-less conductive structure according to some embodiments.
[0009] Figure 3 is a flow chart of a method for forming a capping layer on a liner-less or barrier-less conductive structure according to some embodiments.
[0010] FIG. 4A to FIG. 4D , Figure 4D' , Figure 4E and Figure 4E' are cross-sectional views of intermediate structures during various fabrication operations for forming a capping layer on a linerless or barrierless conductive structure, in accordance with some embodiments.
[0011] Figure 5 is a flow chart of a method for forming a capping layer on a liner-less or barrier-less conductive structure according to some embodiments.
[0012] FIG. 6A to FIG. 6E are cross-sectional views of intermediate structures during various fabrication operations for forming a capping layer on a linerless or barrierless conductive structure, in accordance with some embodiments.
[0013] Figure 7 is a flow chart of a method for forming a capping layer on a liner-less or barrier-less conductive structure according to some embodiments.
[0014] FIG. 8A to FIG. 8K are cross-sectional views of intermediate structures during various fabrication operations for forming a capping layer on a linerless or barrierless conductive structure, in accordance with some embodiments.
[0015] Fig. 9 is a flow chart of a method for forming a capping layer on a liner-less or barrier-less conductive structure according to some embodiments.
[0016] FIG. 10A to FIG. 10E are cross-sectional views of intermediate structures during various fabrication operations for forming a capping layer on a linerless or barrierless conductive structure, in accordance with some embodiments.
[0017] Fig.11 is a flow chart of a method for forming a capping layer on a liner-less or barrier-less conductive structure according to some embodiments.
[0018] FIG. 12A to FIG. 12I are cross-sectional views of intermediate structures during various fabrication operations for forming a capping layer on a linerless or barrierless conductive structure, in accordance with some embodiments.
[0019] Fig.13 is a flow chart of a method for forming a capping layer on a liner-less or barrier-less conductive structure according to some embodiments.
[0020] FIG. 14A to FIG. 14C are cross-sectional views of intermediate structures during various fabrication operations for forming a capping layer on a linerless or barrierless conductive structure, in accordance with some embodiments. DETAILED DESCRIPTION
[0021] The following disclosure provides many different embodiments or examples for implementing the different features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component is arranged between the first component and the second component so that the first component and the second component are not in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various examples. This repetition itself does not indicate the relationship between the various embodiments and / or configurations discussed.
[0022] Furthermore, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another (or additional) elements or components as shown in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should likewise be interpreted accordingly.
[0023] In some embodiments, the terms "about" and "substantially" may represent a value of a given amount that varies within 5% of the value (e.g., ±1%, ±2%, ±3%, ±4%, ±5% of the value). These values are merely examples and are not intended to be limiting. It should be understood that the terms "about" and "substantially" may refer to a percentage of a value as understood by a person skilled in the relevant art based on the teachings herein.
[0024] Active and passive devices in an integrated circuit (IC) are connected at a local level (e.g., within the same area of the IC) and a global level (e.g., between different areas of the IC) through multiple conductive structures such as metal contacts, metal vias, and metal lines. These conductive structures are formed in vertically stacked metallization (or interconnect) layers, which may include different conductive materials (e.g., different metal fills). When metallization layers with different conductive materials are stacked on top of each other, design considerations should be taken into account to avoid performance degradation due to undesirable interactions between the conductive materials.
[0025] A conductive structure without a barrier or liner layer (also referred to as a "linerless conductive structure" or "non-barrier conductive structure") can have a lower resistance than a conductive structure with a barrier or liner layer. This is because the liner or barrier layer (which can have a higher resistance than the metal fill layer in the conductive structure) consumes valuable space within the conductive structure. Therefore, by eliminating the liner or barrier layer in the conductive structure, the lower resistance metal fill can occupy the entire volume of the conductive structure and reduce the overall contact resistance of the conductive structure.
[0026] At the same time, due to the absence of a liner or barrier layer, when subjected to heat treatment, the linerless or barrierless conductive structure may not be able to prevent metal atoms from diffusing outward from the conductive structure below. For example, a ruthenium-filled linerless or barrierless conductive structure formed directly on a cobalt conductive structure may not be able to prevent cobalt from diffusing outward when the two structures are subjected to heat treatment. The out-diffused cobalt atoms can propagate to the upper metallization layer through the ruthenium linerless or barrierless conductive structure. The out-diffused cobalt atoms can increase the contact resistance of the "main" conductive structure (e.g., the ruthenium linerless or barrierless conductive structure and the upper metallization layer such as copper wiring). In addition, due to material migration, the out-diffused cobalt atoms can create voids in the cobalt conductive structure. The above-mentioned side effects of heat-driven cobalt diffusion make the integration of ruthenium-filled linerless or barrierless conductive structures challenging.
[0027] To address the above challenges, the embodiments described herein are directed to a ruthenium capping layer configured to prevent out-diffused cobalt atoms from migrating into an upper metallization layer (e.g., to copper wiring). In some embodiments, a capping layer is formed between the top surface of the ruthenium metal filler and the conductive structure of the upper metallization layer. In some embodiments, the capping layer described herein can also be used as a barrier layer for the upper metallization layer. For example, the capping layer described herein can prevent copper electromigration. In some embodiments, the capping layer comprises a pure metal or a metal nitride. In some embodiments, the capping layer has a low resistivity (e.g., less than about 150 μΩ·cm), a low solubility in ruthenium and cobalt, a melting point greater than about 600°C, and a formation temperature less than about 400°C.
[0028] According to some embodiments, Figure 1 is a partial cross-sectional view of a metallization or interconnect layer (also referred to herein as a "metallization layer") in an integrated circuit. By way of example and not limitation, Figure 1 The metallization layer includes a linerless conductive structure (such as a ruthenium conductive structure 100) formed on a source / drain (S / D) conductive structure (such as a cobalt conductive structure 105). The cobalt conductive structure 105 is formed on the S / D structure 110, which is further formed between the gate structures 115. The layout of the conductive structure described above is exemplary and not limiting. Other layouts of the conductive structure described above are possible and are within the spirit and scope of the present invention.
[0029] In some embodiments, the ruthenium conductive structure 100 is formed directly on the cobalt conductive structure 105 without an intermediate layer such as a liner or a barrier layer. Similarly, the ruthenium metal in the ruthenium conductive structure 100 is formed directly on surrounding layers such as an etch stop layer (ESL) 120 and a dielectric layer 125. In some embodiments, the cobalt conductive structure 105 includes a cobalt metal 105a surrounded by a liner 105b. Figure 1 As shown, liner layer 105b surrounds the sidewalls and bottom surface of cobalt metal 105a. In some embodiments, liner layer 105b is a cobalt diffusion barrier layer that prevents cobalt from diffusing into surrounding materials such as dielectric layer 130, ESL 135, gate structure 115, and S / D structure 110.
[0030] By way of example and not limitation, dielectric layers 125 and 130 may be interlayer dielectrics in which the above-described conductive structures are formed. In some embodiments, dielectric layers 125 and 130 include, for example, one or more silicon oxide-based dielectrics deposited using a high density chemical vapor deposition (HDCVD) process, a plasma enhanced chemical vapor deposition process (PECVD), a plasma enhanced atomic layer deposition process (PEALD), or any other suitable deposition process. By way of example and not limitation, dielectric layers 125 and 130 may be deposited to a thickness between about 100 nm and about 200 nm. The above-described deposition thickness ranges, deposition methods, and materials are exemplary and not limiting. Other materials, thickness ranges, or deposition methods may be used to form dielectric layers 125 and 130. These other materials, thickness ranges, or deposition methods are within the spirit and scope of the present invention.
[0031] In some embodiments, ESL 120 and 135 help to form openings for conductive structures in dielectric layers 125 and 130. The material used for ESL 120 and 135 can be selected from, for example, silicon nitride (SiN x ), silicon oxide (SiO x ), silicon oxynitride (SiON), silicon carbide (SiC), silicon carbonitride (SiCN), boron nitride (BN), silicon boron nitride (SiBN), silicon boron carbonitride (SiCBN), metal oxides, or combinations thereof. By way of example and not limitation, ESLs 120 and 135 may be deposited using low pressure chemical vapor deposition (LPCVD), PECVD, chemical vapor deposition (CVD), or any other suitable deposition process. In some embodiments, ESLs 120 and 135 have a thickness between about 3 nm and about 30 nm.
[0032] like Figure 1As shown, the silicide layer 140 is interposed between the S / D structure 110 and the cobalt conductive structure 105 to provide a low resistance path between the cobalt conductive structure 105 and the S / D structure 110. By way of example and not limitation, the silicide layer 165 may include nickel platinum silicide (NiPtSi), nickel silicide (NiSi), titanium silicide (TiSi), cobalt silicide (CoSi), tungsten silicide (WSi) or any suitable silicide with a thickness of about 4 nm.
[0033] The S / D structure 110 is formed in the top of the active region 145. In some embodiments, the active region 145 includes crystalline silicon (Si), germanium (Ge), a compound semiconductor (e.g., silicon carbide, gallium arsenide (GaAs), gallium phosphide (GaP), indium phosphide (InP), indium arsenide (InAs), indium antimonide (InSb)), an alloy semiconductor (e.g., SiGe, gallium arsenide phosphide (GaAsP), aluminum indium arsenide (AlInAs), aluminum gallium arsenide (AlGaAs), gallium indium arsenide (GaInAs), gallium indium phosphide (GaInP), gallium indium arsenide phosphide (GaInAsP)), or a combination thereof. In some embodiments, the active region 145 is a fin structure, for example, associated with one or more fin field effect transistors (finFETs).
[0034] By way of example and not limitation, active region 145 may be formed on substrate 180 (which may include Si). Alternatively, substrate 180 may include Ge; a compound semiconductor such as silicon carbide, GaAs, GaP, InP, InAs, and InSb; an alloy semiconductor such as SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and GaInAsP; or a combination thereof. In some embodiments, active region 145 is grown on substrate 180 or formed by etching substrate 180.
[0035] like Figure 1 As shown, the cobalt conductive structure 105 and the lower portion of the gate structure 115 are surrounded by a bottom dielectric 155 , which in turn is formed on the active region 145 , according to some embodiments.
[0036] According to some embodiments, Figure 1 The partial cross-sectional view shown is viewed along the x-direction (e.g., parallel to the zx plane). In some embodiments, the cobalt conductive structure is viewed along the y-direction (e.g., perpendicular to the Figure 1 By way of example and not limitation, the top width of the cobalt conductive structure 105 along the x-direction may be substantially equal to the top width of the ruthenium conductive structure 100 along the zx-direction. Figure 1 However, the width of the cobalt conductive structure 105 along the y direction may be greater than the bottom width of the ruthenium conductive structure 100 along the same direction. Figure 2 It is shown in Figure 2 FIG. 1 is an enlarged partial cross-sectional view of the ruthenium conductive structure 100 along the y direction. Figure 2 In the view of the ruthenium conductive structure 100 (e.g., along the y-direction), additional features of the ruthenium conductive structure 100 are visible, such as a hemispherical or arcuate anchor 200 embedded in the cobalt conductive structure 105. In some embodiments, the purpose of the anchor 200 is twofold: (i) to provide a larger contact area between the ruthenium conductive structure 100 and the underlying cobalt conductive structure 105, and (ii) to prevent damage to the ruthenium conductive structure 100 during the ruthenium planarization process. For example, the ruthenium conductive structure 100 can be "pulled out" during the planarization process.
[0037] As discussed above, the ruthenium conductive structure 100 is formed directly on the cobalt conductive structure 105 without an intermediate layer. For this reason, when the cobalt and ruthenium conductive structures are exposed to a thermal process such as an annealing process or during a process of forming additional layers or structures, cobalt atoms can diffuse from the cobalt conductive structure 105 to the ruthenium conductive structure 100. In some embodiments, cobalt and ruthenium do not form an alloy; instead, the cobalt atoms diffuse across the ruthenium grain boundaries 205. If not blocked at the top surface 210 of the ruthenium conductive structure 100, the out-diffused cobalt atoms can continue to migrate "upward" to the upper metallization layers disposed on the ruthenium conductive structure 100. For simplicity, these metallization layers are not shown in FIG. Figure 2 Shown in.
[0038] In some embodiments, Figure 3 1 is a flow chart of a method 300 for forming a capping layer on a ruthenium conductive structure 100 to prevent out-diffused cobalt atoms from diffusing into an upper metallization layer such as a copper metallization layer. Other manufacturing operations may be performed between the various operations of the method 300 and may be omitted only for clarity and ease of description. These various operations are within the spirit and scope of the present invention. In addition, not all operations are required to implement the disclosure provided herein. They may be performed simultaneously or in conjunction with Figure 3 Those shown implement some operations in different orders.In some embodiments, one or more other operations may be implemented in addition to or in place of the operations currently described.
[0039] In some embodiments, Figure 2 Can be an intermediate starting structure for method 300 and subsequent methods described herein. In some embodiments, Figure 2 The ruthenium conductive structure 100 is shown after a planarization process (eg, after a chemical mechanical planarization (CMP) process).
[0040] refer to Figure 3 The method 300 begins at operation 305 and deposits a ruthenium conductive structure on a top surface (e.g., Figure 4AIn some embodiments, the selective deposition of a capping layer on the ruthenium conductive structure 100 can be achieved by appropriately selecting the capping layer material and adjusting its deposition process, so that the capping layer is substantially not formed on the dielectric layer 125. In some embodiments, the desired properties of the capping layer include, but are not limited to, a resistivity of less than about 150 μΩ·cm to minimize the reduction in contact resistance, a melting point of greater than about 600°C to improve thermal stability, and a formation temperature of about 400°C to minimize thermally driven cobalt out-diffusion. In some embodiments, the capping layer does not chemically react with ruthenium and cobalt, and does not form a ruthenium or cobalt alloy.
[0041] In some embodiments, the capping layer is a metal, such as tungsten, deposited using a chemical vapor deposition (CVD) process at a temperature in a range between about 300° C. and about 400° C. at a process pressure between about 1 Torr and about 10 Torr. In some embodiments, the tungsten deposit includes tungsten hexafluoride (WF 6 ) chemicals and hydrogen (H 2 ) to selectively form tungsten metal on the top surface 210 of the ruthenium conductive structure 100. In some embodiments, the thickness of the capping layer formed on the ruthenium conductive structure 100 is in the range between 1.5 nm and 10 nm. In some embodiments, the thickness of the capping layer on the dielectric layer 125 is substantially zero.
[0042] In some embodiments, a deposition temperature below about 400° C. promotes deposition selectivity and mitigates thermally driven cobalt outdiffusion. For example, a deposition temperature above about 400° C. can promote deposition of tungsten on the dielectric layer 125. In addition, a deposition temperature above about 400° C. can accelerate the outdiffusion of cobalt into and within the ruthenium conductive structure 100. On the other hand, a deposition temperature less than about 300° C. is insufficient to form a significant amount of tungsten on the ruthenium conductive structure 100.
[0043] In some embodiments, a capping layer thinner than about 1.5 nm may not block or prevent cobalt from outdiffusion from the ruthenium conductive structure 100, and a capping layer thicker than about 10 nm may adversely affect the combined resistance of the conductive structure. This is because the capping layer (e.g., a tungsten capping layer) has a higher resistance than ruthenium and cobalt.
[0044] In some embodiments, Figure 4B FIG. 4 shows a tungsten capping layer 400 selectively formed on the ruthenium conductive structure 100 according to operation 305 of method 300. Figure 4BAs shown, the cover layer 400 covers the top surface of the ruthenium conductive structure 100 along the y direction and overlaps with the portion M of the dielectric layer 125 surrounding the ruthenium conductive structure 100. The cover layer 400 has a base that is wider than the width of the ruthenium conductive structure 100 in the x and y directions. In some embodiments, the cover layer 400 has a dome shape (for example, the upper surface of the cover layer 400 is convex). In addition, the cover layer 400 is substantially self-aligned with the top surface of the ruthenium conductive structure 100, so that the cover layer 400 does not substantially cover the top surface of the dielectric layer 125, except for the portion of the dielectric layer 125 that is convex. Figure 4B 4. In some embodiments, the dome-like shape of the capping layer 400 is attributed to the growth kinetics of the selective tungsten deposition process described above. In some embodiments, the thickness T of the capping layer 400 is measured from the apex of the dome to the top surface 210 of the ruthenium conductive structure 100 and is measured to be between about 1.5 nm and 10 nm, as discussed above.
[0045] refer to Figure 3 , the method 300 continues with operation 310 and a process of depositing an etch stop layer (ESL) and a low-k dielectric on the capping layer 400. By way of example and not limitation, Figure 4C 3. The method 300 is shown after depositing ESL 405 and low-k dielectric 410 on capping layer 400 according to operation 310. Figure 4B In some embodiments, ESL 405 follows the contours of capping layer 400 and helps to form conductive structures in the upper metallization layer as discussed below. In some embodiments, ESL 405 is not in physical contact with ruthenium conductive structure 100 because capping layer 400 is interposed between ESL 405 and ruthenium conductive structure 100. In some embodiments, the upper surface of capping layer 400 is covered by ESL 405, such as Figure 4C shown.
[0046] By way of example and not limitation, ESL 405ESL includes SiN x 、SiO x , SiON, SiC, SiCN, BN, SiBN, SiCBN, or a combination thereof. In addition, the ESL 405 may have a thickness between about 3 nm and about 30 nm.
[0047] By way of example and not limitation, the low-k dielectric 410 has a dielectric constant (k value) of less than about 3.9 (e.g., about 3 or less), and may include a stack of dielectric layers such as a low-k dielectric and another dielectric. For example, a low-k dielectric (e.g., carbon-doped silicon oxide) and silicon carbide doped with nitrogen, a low-k dielectric (e.g., carbon-doped silicon oxide) and silicon carbide doped with oxygen, a low-k dielectric with silicon nitride (e.g., carbon-doped silicon oxide); or a low-k dielectric with silicon oxide (e.g., carbon-doped silicon oxide). In some embodiments, the low-k dielectric 410 is a porous material. By way of example and not limitation, the low-k dielectric 410 may be deposited at a thickness between about 100 nm and about 200 nm using a high density chemical vapor deposition (HDCVD) process, a plasma enhanced chemical vapor deposition process (PECVD), a plasma enhanced atomic layer deposition process (PEALD), or any other suitable deposition process.
[0048] The above-described deposition thickness ranges, deposition methods, and materials for ESL 405 and low-k dielectric 410 are exemplary and non-limiting. Thus, alternative materials, thickness ranges, or deposition methods may be used and are within the spirit and scope of the present invention.
[0049] refer to Figure 3 , method 300 continues with operation 315 and a process of etching openings in low-k dielectric 410 and ESL 405 to expose capping layer 400. By way of example and not limitation, the openings may be formed using a patterning process including photolithography and one or more etching operations. For example, a photoresist (not shown) may be deposited, exposed, and patterned to form an etching mask (not shown) on low-k dielectric 410. An etching operation may then be used to remove portions of low-k dielectric 410 and ESL 405 that are not covered by the patterned photoresist to form a Figure 4D In some embodiments, the opening 415 passes through the low-k dielectric 410 and the ESL 405 to expose the capping layer 400, such as Figure 4D In some embodiments, the top surface and sidewall surfaces of the ruthenium conductive structure 100 are not exposed by the opening 415. Figure 4D As shown; for example, dielectric layer 125 is not recessed during formation of opening 415.
[0050] In some embodiments, the opening 415 partially exposes the top surface of the cover layer 400. Figure 4D' In this case, after the opening 415 is formed, the ESL 405 continues to cover a portion of the cover layer 400 . In some embodiments, the cover layer 400 is partially embedded (eg, surrounded) by the unetched portion of the ESL 405 .
[0051] By way of example and not limitation, the etching process used to form opening 415 can be a two-step process during which low-k dielectric 410 and ESL 405 are sequentially etched using different dry etching chemistries. In some embodiments, the etching chemistry used to etch ESL 405 does not substantially etch dielectric layer 125 and capping layer 400.
[0052] In some embodiments, Figure 4D and Figure 4D' As shown, the opening 415 is formed to have a width in the y direction greater than the top width in the same direction of the ruthenium conductive structure 100. For example, the opening 415 may be wider than the ruthenium conductive structure 100 and the capping layer 400 in the y direction.
[0053] In some embodiments, the width of the opening 415 along the y direction may be substantially equal to the width of the cover layer 400 along the same direction. In some embodiments, the opening 415 and the conductive structure 100 may have substantially the same or different widths along the x direction. For example, along the x direction, the width of the opening 415 may be substantially equal to or greater than the width of the conductive structure 100.
[0054] In some embodiments, after forming the opening 415, the photoresist mask is removed from the low-k dielectric 410 using a wet etching process. Figure 4D and Figure 4D' The resulting structure is shown after forming openings 415 and removing the photoresist mask from the low-k dielectric 410 .
[0055] refer to Figure 3 , method 300 continues with operation 320 and a process of forming an upper metallized conductive structure in contact with the exposed capping layer 400. In some embodiments, the upper metallized conductive structure includes a barrier layer, a low-resistance liner layer, a seed layer, and a metal filler. By way of example and not limitation, the barrier layer may be a sputter-deposited tantalum nitride (TaN) layer, the low-resistance liner layer may be a sputter-deposited tantalum (Ta) layer, the seed layer may be a sputter-deposited copper (Cu) seed layer, and the metal filler may be electroplated copper. According to some embodiments, Figure 4E Shows Figure 4D The structure after forming the upper metallization conductive structure 420 including the barrier layer 420a and the metal filler 420b. According to some embodiments, Figure 4E' Shows Figure 4D' The structure after forming the upper metallization conductive structure 420 including the barrier layer 420a and the metal filler 420b. Figure 4E and Figure 4E' Not shown are the low resistance liner layer and the seed layer of the upper metallization conductive structure 420. In some embodiments, the upper metallization conductive structure 420 is a back end of line (BEOL) structure, such as a via or a line.
[0056] In some embodiments, the barrier layer 420a follows the curvature of the cover layer 400, such as Figure 4E and Figure 4E' According to some embodiments, Figure 4E and Figure 4E' The difference between Figure 4E' In the embodiment, the barrier layer 420a covers the cover layer 400. Figure 4D' The opening 415 is shown exposing a portion of the barrier layer 420. Other portions of the barrier layer 420 are embedded in the ESL 405 as discussed above.
[0057] In some embodiments, additional upper metal conductive structures similar to or different from the upper metal conductive structure 420 may be formed on each ruthenium conductive structure 100. In some embodiments, the tungsten capping layer 400 prevents or blocks cobalt atoms from diffusing into the upper metallization conductive structure 420 during subsequent thermal operations, such as annealing operations or layer formation operations involving thermal treatments.
[0058] In some embodiments, Figure 5 1 is a flow chart of a method 500 for forming a capping layer between a ruthenium conductive structure 100 and an upper metallization conductive structure. Other manufacturing operations may be omitted for clarity and ease of description only. These various operations are within the spirit and scope of the present invention. In addition, not all operations are required to implement the disclosure provided herein. Figure 5 Those shown implement some operations in different orders.In some embodiments, one or more other operations may be implemented in addition to or in place of the operations currently described.
[0059] refer to Figure 5 and Fig. 6A , method 500 begins with operation 505 and a process of depositing an etch stop layer and a low-k dielectric on the ruthenium conductive structure 100. In some embodiments, Figure 5 Operation 505 and Figure 3 The difference between operations 310 of the illustrated method 300 is that in operation 505 , the ESL 405 and the low-k dielectric 410 are deposited directly on the top surface 210 of the ruthenium conductive structure 100 and not on the capping layer formed in the previous operation. Figure 6B The resulting structure after operation 505 is shown.
[0060] refer to Figure 5 and Figure 6C, method 500 continues with operation 510 and a process of etching an opening 600 in low-k dielectric 410 and ESL 405 to expose ruthenium conductive structure 100. According to some embodiments, operation 510 is similar to operation 315 of method 300 discussed above. However, the difference between opening 415 and opening 600 is that opening 600 exposes the top surface of ruthenium conductive structure 100 instead of the capping layer. In some embodiments, the dimensions of opening 600 are similar to those of opening 415 discussed above.
[0061] refer to Figure 5 and Fig.6D The method 500 continues with operation 515 and a process of depositing a capping layer 610 in the opening 600 and on the ruthenium conductive structure 100. In some embodiments, the deposited capping layer 610 follows the topography of the opening 600. For example, the capping layer 610 is conformally deposited in the opening 600 to cover the sidewalls and bottom surface of the opening 600, such as Fig.6D As shown. In some embodiments, the capping layer 610 does not fill the opening 600 and extends above the top surface of the low-k dielectric 410. By way of example and not limitation, the capping layer 610 may be deposited using an atomic layer deposition (ALD) process, a CVD process, or another suitable process capable of depositing a conformal capping layer. In some embodiments, the capping layer 600 includes a W layer, a titanium nitride (TiN) layer, or a TaN layer.
[0062] By way of example and not limitation, WF 6 and H 2 W is deposited by CVD process of a mixture of W and W at a process pressure above about 10 Torr. 6 and diborane (H 2 B 6 ) ALD process may be used to deposit W. The CVD and ALD deposited W layer may be formed at a temperature in a range between about 300° C. and about 400° C. By way of example and not limitation, the W layer may be deposited using titanium tetrachloride (TiCl 4 ) and ammonia (NH 3 The TiN layer can be deposited by a CVD or ALD process using a tantalum tetrachloride (TaCl 4 ) and ammonia (NH 3 ) plasma CVD or ALD process at a temperature in a range between about 300° C. and about 400° C. In some embodiments, the capping layer 610 has a thickness in a range between about 1.5 nm and about 10 nm.
[0063] refer to Figure 5 and Fig. 6E, the method 500 continues with operation 520 and the process of forming the upper metallization conductive structure 420 in the opening 600 and on the capping layer 610. In some embodiments, operation 520 is similar to Figure 3 Operation 320 of method 300 is shown. Because there is no surface topography for capping layer 610 along the bottom surface of opening 600, an upper metallization conductive structure 420 is formed without stepped features, such as Figure 4E For example, method 500 produces an upper metallized conductive structure having a flat bottom surface.
[0064] In some embodiments, if the capping layer 610 is selected as a TaN layer as described above, a barrier layer 420a of the metallized conductive structure 420 may be optionally formed, depending on the deposition thickness of the TaN capping layer. For example, if the thickness of the capping layer 610 (e.g., thicker than about 1.5 nm) is sufficient to block cobalt and copper atoms, the barrier layer 420a may be omitted. On the other hand, if the thickness of the capping layer 610 (e.g., thinner than about 1.5 nm) is insufficient to block cobalt and copper atoms, the barrier layer 420a (e.g., a TaN layer) may be deposited on the TaN capping layer (e.g., capping layer 610) deposited by CVD or ALD by PVD.
[0065] In some embodiments, additional upper metal conductive structures similar to or different from the upper metal conductive structure 420 may be formed on each ruthenium conductive structure 100. In some embodiments, the capping layer 610 prevents or blocks cobalt atoms from diffusing into the upper metallization conductive structure 420 during subsequent thermal operations, such as annealing operations or layer formation operations involving thermal treatments.
[0066] In some embodiments, Figure 7 1 is a flow chart of a method 700 for forming a capping layer between a ruthenium conductive structure 100 and an upper metallized conductive structure. Other manufacturing operations may be omitted for clarity and ease of description only. These various operations are within the spirit and scope of the present invention. In addition, not all operations are required to implement the disclosure provided herein. Figure 7 Those shown implement some operations in different orders.In some embodiments, one or more other operations may be implemented in addition to or in place of the operations currently described.
[0067] refer to Figure 7 and Fig. 8A , method 700 begins with operation 705 and the process of recessing the ruthenium conductive structure 100 relative to the surrounding dielectric layer 125. According to some embodiments, Figure 8BThe ruthenium conductive structure 100 after operation 705 is shown. In some embodiments, the ruthenium conductive structure 100 is recessed using a selective etch-back process. In some embodiments, the recess height R can be controlled by the etch-back process conditions such as etching time. According to some embodiments, the recess height R is equal to or less than about 5 nm to prevent excessive removal of low-resistance ruthenium metal, high contact resistance, and performance degradation. In some embodiments, the selective etch-back process includes a wet etching chemistry, such as hypochlorous acid (HClO), which does not substantially etch the dielectric layer 125. In some embodiments, the etch-back process forms a top surface for the ruthenium conductive structure 100 having a substantially flat middle portion and a raised edge portion due to its isotropic nature, such as Figure 8B In some embodiments, the groove height R is measured from point A of the horizontal portion of the ruthenium conductive structure to the top surface of the dielectric layer 125, as shown in FIG. Figure 8B In some embodiments, point A is located in the middle of the ruthenium conductive structure 100 .
[0068] refer to Figure 5 and Figure 8C The method 700 continues with operation 710 and a process of depositing a capping layer 800 on the recessed ruthenium conductive structure 100 and the surrounding dielectric layer 125. In some embodiments, the capping layer 800 is blanket deposited so that it fills the recess formed by operation 705, such as Figure 8C As shown. For example and not limitation, the capping layer 800 including W, TiN or TaN can be deposited using a CVD or PVD deposition process. For example, WF 6 and H 2 CVD W is deposited at a process pressure greater than about 10 Torr at a temperature in a range between 300° C. and 400° C. By way of example and not limitation, PVD TiN may be deposited by sputtering Ti metal and then exposing the sputtered metal to a nitrogen-based plasma (e.g., nitrogen plasma or ammonia plasma). Similarly, PVD TaN may be deposited by sputtering Ta metal and then exposing the sputtered metal to a nitrogen-based plasma (e.g., nitrogen plasma or ammonia plasma). In some embodiments, the capping layer 800 is deposited at a thickness between about 1.5 nm and about 5 nm to mitigate the impact on contact resistance and provide adequate protection for cobalt diffusion.
[0069] refer to Figure 5 and Fig.8D , method 700 continues with operation 715 and a process of removing a portion of capping layer 800 from the top surface of dielectric layer 125. By way of example and not limitation, capping layer 800 may be removed using a planarization process such as a CMP process. In some embodiments, after capping layer 800 is removed from dielectric layer 125, the top surfaces of capping layer 800 and dielectric layer 125 are substantially coplanar, such as Fig.8DIn addition, the capping layer 800 substantially fills the region between the top surface of the recessed ruthenium conductive structure 100 and the top surface of the dielectric layer 125. Because the top surface of the ruthenium conductive structure 100 is not flat, the thickness of the capping layer 800 may vary between the middle and sidewall portions of the ruthenium conductive structure 100. For example, referring to Fig.8D , the capping layer 800 has a thickness T greater than the vertical sidewall of the ruthenium conductive structure 100 2 The thickness T of the ruthenium conductive structure 100 toward the center (eg, above point A) is 1 (For example, T 1 >T 2 ). In some embodiments, T 1 / T 2 The ratio between T and t may be greater than about 1 and less than about 2. In some embodiments, T 1 Basically equal to Figure 8B The groove height R shown (eg, T 1 =R).
[0070] refer to Figure 7 The method 700 continues with operation 720 and a process of forming an upper metallization conductive structure on the capping layer 800. In some embodiments, forming the upper metallization conductive structure includes, for example, depositing and then patterning the ESL 405 and the low-k dielectric 410 to form an opening 805 exposing the capping layer 800, such as Fig. 8E In addition, a barrier layer 420a and a metal filler 420b are deposited to form Fig.8F As shown and previously discussed Figure 4E and Fig. 6E The upper metallization conductive structure 420 discussed above. In some embodiments, the opening 805 is similar to Figure 4D and Fig.6D Openings 415 and 600 are shown.
[0071] Similar to Fig. 6E The upper metallization conductive structure 420 is shown, Fig.8F The upper metallization conductive structure 420 in FIG. 4 has a flat bottom morphology.
[0072] In some embodiments, additional upper metal conductive structures similar to or different from the upper metal conductive structure 420 may be formed on each ruthenium conductive structure 100. In some embodiments, the capping layer 800 prevents or blocks cobalt atoms from diffusing into the upper metallization conductive structure 420 during subsequent thermal operations, such as annealing operations or layer formation operations involving thermal treatments.
[0073] In some embodiments, the selective etching back process of operation 705 enables the ruthenium conductive structure 100 to have a convex top surface, such as Figure 8GIn this case, the groove height R is measured between the top surface of the sidewall of the ruthenium conductive structure 100 and the top surface of the dielectric layer 125, as shown in FIG. Figure 8G As shown. In some embodiments, the groove height R is equal to or less than about 5 nm to prevent excessive removal of low-resistance ruthenium metal, high contact resistance, and performance degradation. In some embodiments, the selective etch-back process includes an etching process that does not substantially etch the dielectric layer 125. For example, the etching process may include an ion bombardment process and a plasma etching process implemented when a bias voltage is applied to the substrate.
[0074] In subsequent operations 710 and 715, the capping layer 800 is blanket deposited and planarized, respectively. Figure 8H and Figure 8I As shown. Since the top surface of the ruthenium conductive structure 100 has a convex shape, T 2 Greater than T 1 (For example, T 2 >T 1 ). In some embodiments, T 2 / T 1 The ratio between T and t may be greater than about 1 and less than about 2. In some embodiments, T 2 Basically equal to Figure 8G The groove height R shown (eg, T 2 =R). After planarization, the top surface of the cover layer 800 is substantially flat. Figure 8I Subsequently, an upper metallization conductive structure 420 in contact with the cover layer 800 may be formed according to operation 720, as shown in FIG. Figure 8J and Figure 8K shown.
[0075] According to some embodiments, Fig. 9 is based on Figure 7 1. The method 900 is a flow chart of the method 900 of the method 700 shown in FIG. The differences between the method 900 and the method 700 include the deposition method of the capping layer, in which the capping layer is selectively deposited on the recessed portion of the ruthenium conductive structure 100, and there is no removal process for removing the capping layer from the dielectric layer 125. For example, the method 900 begins with operation 905, which is similar to operation 705 of the method 700. Therefore, the intermediate ruthenium conductive structure 100 of the method 900 corresponding to operation 905 is Fig. 10A and Fig. 10B Similar to method 700 Fig. 8A and Figure 8B .
[0076] refer to Fig. 9 and Fig. 10C The method 900 continues with operation 910 and a process of selectively depositing a capping layer 1000 on the recessed ruthenium conductive structure. According to some embodiments, operation 910 is similar to Figure 3 Operation 305 of method 300 is shown, where the capping layer is a metal such as tungsten deposited using a selective CVD process at a temperature in a range between about 300 Torr and about 400 Torr at a process pressure between about 1 Torr and about 10 Torr. In some embodiments, the tungsten deposition includes WF 6 Chemical substances and H 2 , to achieve a desired deposition selectivity on the ruthenium conductive structure 100. In some embodiments, the thickness of the capping layer formed on the ruthenium conductive structure 100 is in a range between 1.5 nm and 5 nm. In some embodiments, the thickness of the capping layer on the dielectric layer 125 is substantially zero.
[0077] As discussed above, because the top surface of the recess of the ruthenium conductive structure 100 is not flat, the capping layer 1000 is deposited so that it follows the contour of the ruthenium conductive structure 100. By way of example and not limitation, the top surface of the capping layer 1000 may also be non-flat (e.g., concave), such as Fig. 10C As shown. Therefore, the top surfaces of the cover layer 1000 and the dielectric layer 125 are not coplanar. In some embodiments, the top surface curvature of the cover layer 1000 is substantially equal to or less than the top surface curvature of the ruthenium conductive structure 100. Therefore, the thickness of the cover layer 1000 across the top surface of the ruthenium conductive structure 100 may be substantially non-conformal. For example, T 1 Can be equal to or greater than T 2 (For example, T 1 ≥T 2 ), wherein T is measured at point A located in the middle of the ruthenium conductive structure 100 as discussed above 1 .
[0078] refer to Fig. 9 , method 900 continues with operation 915 and a process of forming an upper metallization conductive structure on cover layer 1000. According to some embodiments, operation 915 is similar to operation 720 of method 700. Therein, ESL 405 and low-k dielectric 410 are first deposited on dielectric layer 125 and cover layer 1000 and then patterned to form opening 1005 exposing cover layer 1000, as shown in FIG. Fig. 10D In addition, a barrier layer 420a and a metal filler 420b are deposited in the opening 1005 to form Fig. 10E The upper metallized conductive structure 420 is shown. In some embodiments, due to the top surface morphology of the cover layer 1000, the bottom surface of the upper metallized conductive structure 420 may have Fig. 10E The convex part 1010 shown. For example, Fig. 10E The bottom surface of the upper metallized conductive structure 420 may not be as Fig.8F As flat as in.
[0079] In some embodiments, if the groove height R is Figure 8B and Fig. 10B If they are equivalent, Fig.8D The thickness T shown 1 Can be greater than Fig. 10C The thickness T shown 1 In some embodiments, you can adjust Figure 8B and Fig. 10B The groove height R shown is such that Fig.8D and Fig. 10C The resulting thickness T of the cover layers 800 and 1000 shown in 1 It is quite.
[0080] According to some embodiments, Fig.11 is based on Figure 5 1100 of method 500. The difference between method 1100 and method 500 is the additional recessing operation for the ruthenium conductive structure, as discussed below. In some embodiments, method 1100 begins with operations 1105 and 1110, which are similar to corresponding operations 505 and 510 of method 500. Therefore, the operations corresponding to operations 1105 and 1110 are as follows: Fig. 12A , Fig. 12B and Fig. 12C Similar to the operations corresponding to operations 505 and 510 Fig. 6A , Figure 6B and Figure 6C In some embodiments, Fig. 12C The opening 1200 shown is similar to Figure 6C Opening 600 is shown.
[0081] refer to Fig.11 , method 1100 continues with operation 1115 and a process of recessing the ruthenium conductive structure 100 relative to the surrounding dielectric layer 125. In some embodiments, aspects of operation 1115 are similar to operation 705 of method 700. For example, the ruthenium conductive structure 100 can be recessed using a selective etch back process including a wet etch chemistry such as hypochlorous acid (HClO) that does not substantially etch the dielectric layer 125. In some embodiments, the recess height R is controlled by the etch back process conditions such as etching time, and is equal to or less than about 5 nm to prevent excessive removal of low resistance ruthenium metal, high contact resistance, and performance degradation, as discussed above. In some embodiments, and due to its isotropic nature, the etch back process forms a concave top surface for the ruthenium conductive structure 100, such as Fig.12D In some embodiments, the groove height R is higher above the inflection point A and shorter above the vertical sidewall surface of the ruthenium conductive structure 100 .
[0082] refer to Fig.11, method 1100 continues with operations 1120 and 1125, which are similar to operations 515 and 520 of method 500 described above. For example, Fig.12E The deposited capping layer 1210 is shown to follow the top surface morphology of the ruthenium conductive structure 100 and cover the sidewalls and bottom surface of the opening 1200. In some embodiments, the capping layer 1210 does not fill the opening 1200 and extends above the top surface of the low-k dielectric 410. For example, the capping layer 1210 can be deposited using an ALD process, a CVD process, or another suitable process capable of depositing a conformal capping layer. In some embodiments, the capping layer 1210 includes a W layer, a titanium nitride (TiN) layer, or a TaN layer. In some embodiments, the thickness of the capping layer 1210 is substantially constant on the top surface of the ruthenium conductive structure 100.
[0083] As discussed above, you can use WF 6 and H 2 The CVD process of the mixture is at a process pressure above about 10 Torr and utilizes WF 6 and H 2 B 6 W can be deposited by an ALD process using CVD. The W layer deposited by CVD and ALD can be formed at a temperature ranging between about 300° C. and about 400° C. In addition, the W layer can be deposited by using TiCl 4 and NH 3 The TiN layer is deposited by a plasma CVD or ALD process at a temperature ranging between about 300° C. and about 400° C. The TiN layer can be deposited by using TaCl 4 and NH 3 The plasma CVD or ALD process deposits the TaN layer at a temperature ranging between about 300° C. and about 400° C. In some embodiments, the capping layer 1210 has a thickness ranging between about 1.5 nm and about 5 nm to mitigate the impact on contact resistance and provide adequate protection for cobalt diffusion, as discussed above.
[0084] Subsequently, an upper metallization conductive structure 420 may be formed over the capping layer 1210, as shown above. Fig.12F As shown and described in operations 520 and 320. In some embodiments, if the capping layer 1210 is selected as a TaN layer as described above, the formation of the barrier layer 420a may be optional, depending on the deposition thickness of the TaN capping layer. For example, if the thickness of the capping layer 1210 (e.g., thicker than about 1.5 nm) is sufficient to block cobalt and copper atoms, the barrier layer 420a may be omitted. On the other hand, if the thickness of the capping layer 1210 (e.g., thinner than about 1.5 nm) is insufficient to block cobalt and copper atoms, an additional TaN barrier layer 420a may be deposited by PVD on the TaN capping layer (e.g., capping layer 1210) deposited by CVD or ALD.
[0085] In some embodiments, and with reference to Fig.12F Due to the top surface morphology of the cover layer 1210, the bottom surface of the upper metallized conductive structure 420 may produce a similar Fig. 10E Male component 1220 of male component 1010 is shown.
[0086] As discussed above, the material selection for the capping layer and the deposition method are based on the desired characteristics, such as selectivity, uniformity, or gap fill. For example, if selective deposition is desired regardless of the underlying topography (e.g., as described in methods 300 and 900), a CVD process may be used to deposit the capping layer using WF. 6 and H 2 The W capping layer is deposited at a temperature in a range between about 300° C. and about 400° C. and a process pressure between about 1 Torr and 10 Torr. If uniform or conformal deposition is desired regardless of the underlying topography (e.g., as described in methods 500 and 1100), the W capping layer, TiN capping layer, or TaN capping layer may be deposited using a CVD or ALD process. Additionally, if blanket deposition is desired (e.g., as described in method 700), the W capping layer, TiN capping layer, or TaN capping layer may be deposited using a CVD or PVD process.
[0087] In some embodiments, the selective etch-back process used to recess the ruthenium conductive structure 100 relative to the surrounding dielectric layer 125 in operation 1115 causes the ruthenium conductive structure 100 to have a convex top surface, such as Figure 12G In some embodiments, Figure 12G Similar to the above discussion Fig. 8E , except for the ESL and low-k dielectrics 405 and 410. Similar to Figure 8G ,exist Figure 12G In the embodiment, the groove height R is measured between the top surface of the sidewall of the ruthenium conductive structure 100 and the top surface of the dielectric layer 125, as shown in FIG. Figure 12G As shown. In some embodiments, the groove height R is equal to or less than about 5nm to prevent excessive removal of low-resistance ruthenium metal, high contact resistance and performance degradation. In some embodiments, the selective back etching process includes an etching process that does not substantially etch low-k dielectric 410, ESL 405 or dielectric layer 125. For example, the etching process may include an ion bombardment process or a plasma etching process. In some embodiments, a bias voltage may be applied to the substrate during the etching process. For example, the bias voltage applied may be between about 100V and about 1100V, between about 150V and about 1050V, between about 200V and about 1000V, or any suitable bias voltage. In some embodiments, increasing the bias voltage may result in excessive removal of low-resistance ruthenium metal.
[0088] In subsequent operations 1120 and 1125, a blanket deposition of a capping layer 1210 is performed, such as Fig.12H Similar to Fig.12E , Fig.12H The capping layer 1210 in FIG. 1 follows the top surface topography of the conductive structure 100 and covers the sidewalls and bottom surface of the opening 1200 . In some embodiments, the capping layer 1210 does not fill the opening 1200 and extends over the top surface of the low-k dielectric 410 .
[0089] Subsequently, an upper metallization conductive structure 420 may be formed over the capping layer 1210, such as Fig.12I As shown. In some embodiments, if the capping layer 1210 is selected as a TaN layer as described above, the formation of the barrier layer 420a may be optional, depending on the deposition thickness of the TaN capping layer. For example, if the thickness of the capping layer 1210 (e.g., thicker than about 1.5 nm) is sufficient to block cobalt and copper atoms, the barrier layer 420a may be omitted. On the other hand, if the thickness of the capping layer 1210 (e.g., thinner than about 1.5 nm) is insufficient to block cobalt and copper atoms, an additional TaN barrier layer 420a may be deposited by PVD on the TaN capping layer (e.g., capping layer 1210) deposited by CVD or ALD.
[0090] In some embodiments, and with reference to Fig.12I Due to the top surface topography of the capping layer 1210, the bottom surface of the upper metallized conductive structure 420 can produce a convex feature 1225 with a convex bottom surface topography that follows the top surface topography of the underlying ruthenium conductive structure 100. In some embodiments, the bottom surface of the feature 1225 is substantially flat and does not follow the top surface topography of the underlying ruthenium conductive structure 100.
[0091] In some embodiments, Fig.13 is a flowchart of method 1300, which is Fig.11 According to some embodiments, method 1300 has corresponding operations similar to method 1100. One exception between methods 1300 and 1100 is operation 1315, which is different from operation 1115. More specifically, in operation 1315, as opposed to recessing ruthenium conductive structure 100, dielectric layer 125 is partially etched. In some embodiments, Fig.14A The following diagram shows the Fig. 12CDuring operation 1315, dielectric layer 125 is partially etched by an amount H to expose a portion of the sidewall surface of ruthenium conductive structure 100. In some embodiments, the ratio of the etched height H to the thickness of dielectric layer 125 can be between about 5% and about 35%, between about 10% and about 30%, between about 15% and about 25%, or any suitable ratio. In some embodiments, the etching process of operation 1315 does not substantially etch ESL 405 and low-k dielectric 410. In some embodiments, the etching process of operation 1315 results in rounded top corners for ruthenium conductive structure 100, such as by Fig.14A As shown by the dashed circle 1330 in FIG. In some embodiments, the precursor of the etching process of operation 1315 may include boron trichloride, chlorine, hydrogen bromide, any suitable precursor, or a combination thereof.
[0092] In operation 1320, a blanket deposit of a capping layer 1210 is performed in the opening 1200, such as Fig. 14B Similar to Fig.12E , Fig. 14B The capping layer 1210 in FIG. 1 follows the top surface topography of the conductive structure 100 and covers the sidewalls and bottom surface of the opening 1200. In some embodiments, the capping layer 1210 does not fill the opening 1200 and extends over the top surface of the low-k dielectric 410. In addition, the capping layer 1200 fills the space between the sidewall surface of the conductive structure 100 and the dielectric layer 125 as shown by the dashed circle 1335.
[0093] Subsequently, an upper metallization conductive structure 420 may be formed over the capping layer 1210 according to operation 1325, such as Fig. 14C As shown. In some embodiments, if the capping layer 1210 is selected as a TaN layer as described above, the formation of the barrier layer 420a may be optional, depending on the deposition thickness of the TaN capping layer. For example, if the thickness of the capping layer 1210 (e.g., thicker than about 1.5 nm) is sufficient to block cobalt and copper atoms, the barrier layer 420a may be omitted. On the other hand, if the thickness of the capping layer 1210 (e.g., thinner than about 1.5 nm) is insufficient to block cobalt and copper atoms, an additional TaN barrier layer 420a may be deposited by PVD on the TaN capping layer (e.g., capping layer 1210) deposited by CVD or ALD.
[0094] In some embodiments, and with reference to Fig. 14C Due to the top surface topography of the capping layer 1210 , the bottom surface of the upper metallization conductive structure 420 may produce a convex feature 1340 that follows the top surface topography of the underlying ruthenium conductive structure 100 .
[0095] Various embodiments described herein are directed to a ruthenium capping layer configured to prevent out-diffused cobalt atoms from migrating into an upper metallization layer (e.g., to copper wiring). In some embodiments, a capping layer is formed between the top surface of the ruthenium metal filler and the conductive structure of the upper metallization layer. In some embodiments, the capping layer described herein is also used as a copper electromigration barrier for the upper metallization layer. In some embodiments, the capping layer comprises a pure metal (e.g., W) or a metal nitride (e.g., TiN and TaN). In some embodiments, the capping layer has a low resistivity (e.g., less than about 150 μΩ·cm), a low solubility in ruthenium and cobalt, a melting point greater than about 600°C, and a formation temperature less than about 400°C. In some embodiments, a capping layer is selectively deposited on the top surface of the ruthenium conductive structure. In some embodiments, a capping layer is blanket deposited on the ruthenium conductive structure. In some embodiments, the ruthenium conductive structure is recessed before forming the capping layer.
[0096] In some embodiments, a structure includes: a substrate; and a first metallization layer located on the substrate, wherein the first metallization layer includes a linerless conductive structure surrounded by a dielectric. The structure also includes: a cover layer located on a top surface of the linerless conductive structure; and a second metallization layer located on the first metallization layer, wherein the second metallization layer includes a conductive structure on the linerless conductive structure. In addition, the cover layer is interposed between the top surface of the linerless conductive structure and the bottom surface of the conductive structure.
[0097] In some embodiments, a structure includes a substrate having a first metallization layer formed thereon, wherein the first metallization layer has a linerless conductive structure surrounded by a dielectric. The structure also includes: a cover layer located on a top surface of the linerless conductive structure and not in contact with the dielectric. In addition, the structure includes: a second metallization layer located on the first metallization layer, wherein the second metallization layer includes a conductive structure on the linerless conductive structure. In addition, the linerless conductive structure is separated from the conductive structure by the cover layer.
[0098] In some embodiments, the method includes: depositing a cobalt diffusion barrier layer on a linerless conductive structure including ruthenium, wherein depositing the cobalt diffusion barrier layer includes forming the cobalt diffusion barrier layer self-aligned with the linerless conductive structure. The method also includes: depositing a stack having an etch stop layer and a dielectric layer on the cobalt diffusion barrier layer; and forming an opening in the stack to expose the cobalt diffusion barrier layer. Finally, the method includes: forming a conductive structure on the cobalt diffusion barrier layer.
[0099] Some embodiments of the present application provide a semiconductor structure, comprising: a substrate; a first metallization layer located on the substrate, wherein the first metallization layer includes a linerless conductive structure surrounded by a dielectric; a capping layer located on a top surface of the linerless conductive structure; and a second metallization layer located on the first metallization layer and including a conductive structure on the linerless conductive structure, wherein the capping layer is between the top surface of the linerless conductive structure and the bottom surface of the conductive structure. In some embodiments, the top surface of the linerless conductive structure is located below the top surface of the dielectric, and wherein the top surface of the capping layer is coplanar with the top surface of the dielectric. In some embodiments, the capping layer has a dome shape. In some embodiments, the bottom surface of the capping layer is flat. In some embodiments, the top surface of the linerless conductive structure and the top surface of the capping layer are not coplanar with the top surface of the dielectric. In some embodiments, the capping layer contacts the bottom surface and sidewall surfaces of the conductive structure. In some embodiments, the capping layer includes tungsten, titanium nitride, or tantalum nitride. In some embodiments, the linerless conductive structure includes ruthenium.
[0100] Some other embodiments of the present application provide a semiconductor structure, comprising: a substrate; a first metallization layer located on the substrate and including a linerless conductive structure surrounded by a dielectric; a capping layer disposed on a top surface of the linerless conductive structure, wherein the capping layer has a dome shape with a base greater than a width of the linerless conductive structure; and a second metallization layer located on the first metallization layer and including a conductive structure on the linerless conductive structure, wherein the linerless conductive structure is separated from the conductive structure by the capping layer. In some embodiments, the capping layer is embedded in the bottom of the conductive structure. In some embodiments, the top surface of the capping layer is not coplanar with the dielectric. In some embodiments, a portion of the bottom surface of the capping layer is coplanar with the dielectric and is wider than the linerless conductive structure. In some embodiments, the capping layer comprises tungsten. In some embodiments, the capping layer covers a first portion of the dielectric, and the conductive structure covers a second portion of the dielectric different from the first portion. In some embodiments, the bottom surface of the conductive structure is not flat. In some embodiments, the linerless conductive structure comprises ruthenium metal, and wherein the capping layer comprises a metal selectively deposited on the ruthenium metal.
[0101] Some other embodiments of the present application provide a method of forming a semiconductor structure, comprising: depositing a cobalt diffusion barrier layer on a linerless conductive structure including ruthenium, wherein depositing the cobalt diffusion barrier layer comprises forming the cobalt diffusion barrier layer self-aligned with the linerless conductive structure; depositing a stack including an etch stop layer and a dielectric layer on the cobalt diffusion barrier layer; forming an opening in the stack to expose the cobalt diffusion barrier layer; and forming a conductive structure on the cobalt diffusion barrier layer to surround the cobalt diffusion barrier layer. In some embodiments, forming the cobalt diffusion barrier layer comprises: depositing a tungsten layer using a chemical vapor deposition process at a temperature in a range between about 300° C. and about 400° C. and at a process pressure between about 1 Torr and about 10 Torr. In some embodiments, the chemical vapor deposition process comprises tungsten hexafluoride and hydrogen. In some embodiments, depositing the cobalt diffusion barrier layer comprises: depositing a metal having a melting point greater than about 600° C. and a resistivity less than about 150 μΩ·cm.
[0102] It should be understood that the detailed description section, rather than the abstract, is intended to be used to interpret the claims. The abstract of the disclosure section may set forth one or more but not all contemplated exemplary embodiments and, thus, is not intended to limit the dependent claims.
[0103] The features of several embodiments are disclosed above so that those skilled in the art can better understand aspects of the present invention. It should be understood by those skilled in the art that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. It should also be appreciated by those skilled in the art that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the appended claims.
Claims
1. A semiconductor structure comprising: substrate; a first metallization layer disposed on the substrate, wherein the first metallization layer comprises a linerless conductive structure, a first portion of the linerless conductive structure is surrounded by a dielectric and in physical contact with the dielectric, and a second portion of the linerless conductive structure is surrounded by a metal; a cover layer disposed on a top surface of the linerless conductive structure; and The second metallization layer is located on the first metallization layer and includes a conductive structure on the linerless conductive structure, wherein the cover layer is between the top surface of the linerless conductive structure and the bottom surface of the conductive structure.
2. The semiconductor structure according to claim 1, wherein: The top surface of the linerless conductive structure is below a top surface of the dielectric, and wherein a top surface of the capping layer is coplanar with the top surface of the dielectric.
3. The semiconductor structure according to claim 2, wherein: The cover layer has a dome shape.
4. The semiconductor structure according to claim 3, wherein: The bottom surface of the cover layer is flat.
5. The semiconductor structure according to claim 1, wherein: The top surface of the linerless conductive structure and the top surface of the capping layer are not coplanar with a top surface of the dielectric.
6. The semiconductor structure according to claim 1, wherein: The capping layer contacts the bottom surface and sidewall surfaces of the conductive structure.
7. The semiconductor structure according to claim 1, wherein: The capping layer includes tungsten, titanium nitride or tantalum nitride.
8. The semiconductor structure according to claim 1, wherein: The linerless conductive structure includes ruthenium.
9. A semiconductor structure comprising: substrate; a first metallization layer disposed on the substrate and comprising a linerless conductive structure, wherein a first portion of the linerless conductive structure is surrounded by and in physical contact with a dielectric and a second portion of the linerless conductive structure is surrounded by metal; a covering layer disposed on a top surface of the linerless conductive structure, wherein the covering layer has a dome shape having a base greater than a width of the linerless conductive structure; and A second metallization layer is located on the first metallization layer and includes a conductive structure on the linerless conductive structure, wherein the linerless conductive structure is separated from the conductive structure by the cover layer.
10. The semiconductor structure according to claim 9, wherein: The cover layer is embedded in the bottom of the conductive structure.
11. The semiconductor structure according to claim 9, wherein: A top surface of the capping layer is not coplanar with the dielectric.
12. The semiconductor structure according to claim 9, wherein: A portion of the bottom surface of the capping layer is coplanar with the dielectric and is wider than the linerless conductive structure.
13. The semiconductor structure according to claim 9, wherein: The capping layer includes tungsten.
14. The semiconductor structure according to claim 9, wherein: The capping layer covers a first portion of the dielectric, and the conductive structure covers a second portion of the dielectric different from the first portion.
15. The semiconductor structure according to claim 9, wherein: The bottom surface of the conductive structure is not flat.
16. The semiconductor structure according to claim 9, wherein: The linerless conductive structure includes a ruthenium metal, and wherein the capping layer includes a metal selectively deposited on the ruthenium metal.
17. A method of forming a semiconductor structure, comprising: depositing a cobalt diffusion barrier layer on a linerless conductive structure including ruthenium, wherein depositing the cobalt diffusion barrier layer includes forming the cobalt diffusion barrier layer self-aligned with the linerless conductive structure; depositing a stack including an etch stop layer and a dielectric layer on the cobalt diffusion barrier layer; forming an opening in the stack to expose the cobalt diffusion barrier layer; and A conductive structure is formed on the cobalt diffusion barrier layer to surround the cobalt diffusion barrier layer.
18. The method according to claim 17, wherein: Forming the cobalt diffusion barrier layer includes depositing a tungsten layer using a chemical vapor deposition process at a temperature ranging between about 300° C. and about 400° C. and at a process pressure between about 1 Torr and about 10 Torr.
19. The method according to claim 18, wherein: The chemical vapor deposition process includes tungsten hexafluoride and hydrogen.
20. The method according to claim 17, wherein: Depositing the cobalt diffusion barrier layer includes depositing a metal having a melting point greater than about 600° C. and a resistivity less than about 150 μΩ·cm.