Method for manufacturing semiconductor element and method for manufacturing solar cell

By using an impurity diffusion composition of a silane compound polymer and an impurity diffusion component, a uniform impurity diffusion layer is formed, which solves the problems of complex processes and uneven impurity concentration in existing solar cell manufacturing, and realizes a simple and efficient selective emitter. Structural fabrication.

CN113169248BActive Publication Date: 2024-10-01TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980078538.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-07
Filing Date
2019-11-29
Publication Date
2024-10-01
Estimated Expiration
2039-11-29

AI Technical Summary

Technical Problem

In the existing solar cell manufacturing methods, the process of forming the selective emitter structure is complicated and requires multiple diffusion and etching. In addition, the inkjet method requires multiple inkjet heads and complex devices. It is difficult to control the diffusion concentration of impurities, resulting in impurities. The concentration is uneven.

Method used

An impurity diffusion composition containing a silane compound polymer and an impurity diffusion component is used to form impurity diffusion layers of different concentrations through coating and heat treatment. The silane compound polymer is used to suppress external diffusion and form a uniform impurity diffusion layer.

Benefits of technology

A simple method to manufacture solar cells with a selective emitter structure without complex equipment is realized. The impurity concentration has excellent in-plane uniformity, reducing process complexity and equipment requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113169248B_ABST
    Figure CN113169248B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a method for manufacturing a solar cell having a selective emitter structure, a method for manufacturing a semiconductor element having excellent in-plane uniformity of impurity concentration, and a method for manufacturing a solar cell without complex equipment and by a simple method. The present invention for achieving the above-mentioned object is a method for manufacturing a semiconductor element, which forms the same type of impurity diffusion layer regions on a semiconductor substrate with different impurity concentrations at two or more levels, wherein at least one or more impurity diffusion layer regions are formed by a method including: applying an impurity diffusion composition (a) to a semiconductor substrate to partially form an impurity diffusion composition film (b); and heating the impurity diffusion composition to diffuse impurities into the semiconductor substrate to form an impurity diffusion layer region (c), wherein the impurity diffusion composition (a) comprises (a-1) a polymer of a silane compound having a specific structure and (a-2) an impurity diffusion component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a semiconductor element and a method for manufacturing a solar cell, and in particular to a method for manufacturing a high-efficiency semiconductor element and a method for manufacturing a solar cell. Background Art

[0002] In conventional manufacturing of a solar cell having a pn junction, an n-type impurity is diffused on a p-type semiconductor substrate such as silicon to form an n-type diffusion layer, thereby forming a pn junction.

[0003] In recent years, a solar cell with a selective emitter structure has been disclosed, which is proposed to reduce the contact resistance with the electrode and suppress the recombination of carriers (Non-Patent Document 1). For example, in a solar cell with a selective emitter structure based on an n-type silicon substrate, a high-concentration p-type diffusion layer (p-type diffusion layer) is formed just below the electrode in the p-type diffusion layer on the light-receiving surface side. ++ A p-type diffusion layer with low to medium concentration is formed on the light-receiving surface other than directly below the electrode. + layer). It is known that in order to form a selective emitter structure, a complex process combining multiple diffusions and partial etching using a mask is required (Patent Document 1). In addition, the following methods have been proposed: in order to simplify the process, a method in which a diffusing agent of multiple impurity concentrations is applied to a substrate by an inkjet method and the impurities are diffused (Patent Document 2); a method in which a pattern is selectively formed on a substrate using a coating liquid containing an impurity diffusion component, and the substrate with the pattern is heat-treated in an atmosphere of a doping gas to form multiple impurity concentration regions (Patent Documents 3, 4, 5); a method in which a pattern is selectively formed on a substrate using a coating liquid containing an impurity diffusion component, and a phenomenon of external diffusion from the pattern caused by heat treatment is used to form multiple impurity concentration regions (Patent Documents 6, 7); etc.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-193350

[0007] Patent Document 2: Japanese Patent Application Publication No. 2004-221149

[0008] Patent Document 3: Japanese Patent Application Publication No. 2012-134571

[0009] Patent Document 4: Japanese Patent Application Publication No. 2015-50357

[0010] Patent Document 5: Japanese Patent Application Publication No. 2006-310368

[0011] Patent Document 6: Japanese Patent Application Publication No. 2017-22350

[0012] Patent Document 7: Japanese Patent Application No. 2002-503390

[0013] Non-patent literature

[0014] Non-patent document 1: E. Lee et al., “Exceeding 19% efficient 6-inch screen printed crystalline silicon solar cells with selective emitter”, Renewable Energy, Vol. 42 (June 2012), pp. 95-99 Summary of the invention

[0015] Problems to be solved by the invention

[0016] However, in the method described in Patent Document 1, in order to form a selective emitter structure, steps for pattern formation and etching are required, and there is a tendency for the number of steps to increase. In addition, in the inkjet method described in Patent Document 2, a dedicated device with multiple inkjet heads is required, and the control of the injection from each inkjet head also becomes complicated. In addition, the diffusion paste described in Patent Documents 3 to 5 does not sufficiently suppress the external diffusion of impurities from the paste film, so there is a problem of large deviations in the impurity diffusion concentration in the part other than the pattern forming part. In addition, in the methods described in Patent Documents 6 and 7, it is difficult to control the external diffusion, and there is still a problem of large deviations in the impurity diffusion concentration in the part other than the pattern forming part.

[0017] The present invention has been made in view of the above-mentioned conventional problems, and its purpose is to provide a method for manufacturing a solar cell having a selective emitter structure, a method for manufacturing a semiconductor element having excellent in-plane uniformity of impurity concentration, and a method for manufacturing a solar cell, which can be manufactured by a simple method without requiring complicated equipment.

[0018] Means for solving problems

[0019] In order to solve the above-mentioned problems, the manufacturing method of the semiconductor element of the present invention has the following structure. That is, a manufacturing method of a semiconductor element, the manufacturing method of the semiconductor element forms the same type of impurity diffusion layer regions on a semiconductor substrate with different impurity concentrations at two or more levels, wherein at least one or more impurity diffusion layer regions are formed by a method including the following steps: a step of applying an impurity diffusion composition (a) to the semiconductor substrate to partially form an impurity diffusion composition film (b); and a step of heating the impurity diffusion composition film (b) to diffuse impurities into the semiconductor substrate to form an impurity diffusion layer region (c), wherein the impurity diffusion composition (a) comprises:

[0020] (a-1) a polymer of a silane compound represented by the following general formula (1); and

[0021] (a-2) Impurity diffusion component.

[0022] [Chemistry 1]

[0023]

[0024] (In general formula (1), R 1 and R 2 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 1 and R 2 are the same or different. l1 represents an integer from 1 to 10000. )

[0025] Effects of the Invention

[0026] According to the present invention, a method for manufacturing a solar cell having a selective emitter structure, a method for manufacturing a semiconductor element having excellent in-plane uniformity of impurity concentration, and a method for manufacturing a solar cell can be provided without requiring complicated equipment and by a simple method. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a process cross-sectional view showing an example of the method for manufacturing a semiconductor element of the present invention.

[0028] Figure 2 It is a process cross-sectional view showing another example of the method for manufacturing a semiconductor element of the present invention.

[0029] Figure 3 The figures show the screen printing patterns and the sheet resistance value measurement sites used in the examples of the present invention. DETAILED DESCRIPTION

[0030] Hereinafter, first, the impurity diffusion compositions (a) and (d) used in the present invention are described, and then a preferred method for manufacturing a semiconductor element (selective emitter structure) is described with reference to the accompanying drawings. It should be noted that the following embodiments are illustrative only, and the present invention is not limited to these embodiments.

[0031] <Impurity-diffusing composition (a)>

[0032] The impurity-diffusing composition (a) used in the present invention contains (a-1) a polymer of a silane compound represented by the following general formula (1) as an essential component.

[0033] [Chemistry 2]

[0034]

[0035] In the general formula (1), R 1 and R 2 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 1 and R 2 They are the same or different. l1 represents an integer of 1 to 10000. From the viewpoint of the toughness of the film after film formation and the uniformity of the coating film thickness, it is preferably 5 to 9000, and more preferably 10 to 8000.

[0036] R in the general formula (1) 1 and R 2 The alkyl group with 1 to 6 carbon atoms, the alkoxy group with 1 to 6 carbon atoms, the alkenyl group with 2 to 10 carbon atoms, the acyloxy group with 2 to 6 carbon atoms, and the aryl group with 6 to 15 carbon atoms can be either unsubstituted or substituted, and can be selected according to the characteristics of the impurity diffusion composition.

[0037] As the substituted form of the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, or the acyloxy group having 2 to 6 carbon atoms, a structure in which the hydrocarbon is substituted with an amino group, a mercapto group, a hydroxyl group, a glycidyl group, a glycidyloxy group, or an isocyanate group is preferred. The number of substitutions is preferably 1 to 3, and more preferably 1.

[0038] As the substituted alkenyl group having 2 to 10 carbon atoms, preferred are structures in which hydrocarbon is substituted with an amino group, a mercapto group, a hydroxyl group, a glycidyl group, a glycidyloxy group, an isocyanate group, or a carbonyloxyalkyl group having 2 to 8 carbon atoms. The number of substitutions is preferably 1 to 3, and more preferably 1.

[0039] As a substituted body of an aryl group having 6 to 15 carbon atoms, a structure in which an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an acyloxy group having 2 to 5 carbon atoms, a carbonyloxyalkyl group having 2 to 7 carbon atoms, an amino group, a mercapto group, a hydroxyl group, a glycidyl group, a glycidyloxy group, or an isocyanate group is bonded to the aromatic ring is preferred; or a structure in which an acyloxy group having 2 to 5 carbon atoms, an amino group, a mercapto group, a hydroxyl group, a glycidyl group, a glycidyloxy group, or an isocyanate group is bonded to the aromatic ring via an alkyl group having 1 to 3 carbon atoms. The number of substitutions is preferably 1 to 3, and more preferably 1.

[0040] Specific examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, trifluoromethyl, 3,3,3-trifluoropropyl, 3-glycidoxypropyl, 3-aminopropyl, 3-mercaptopropyl, and 3-isocyanatepropyl.

[0041] Specific examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, and a tert-butoxy group.

[0042] Specific examples of the alkenyl group having 2 to 10 carbon atoms include a vinyl group, a 3-acryloxypropyl group, and a 3-methacryloxypropyl group.

[0043] Specific examples of the acyloxy group having 2 to 6 carbon atoms include acetoxy and the like.

[0044] Specific examples of the aryl group having 6 to 15 carbon atoms include phenyl, tolyl, p-hydroxyphenyl, p-phenylenyl, p-methoxyphenyl, 1-(p-hydroxyphenyl)ethyl, 2-(p-hydroxyphenyl)ethyl, 4-hydroxy-5-(p-hydroxyphenylcarbonyloxy)pentyl, and naphthyl.

[0045] From the viewpoint of easily suppressing outdiffusion from the impurity-diffusing composition, R 1 , R 2 At least one of the above represents any one of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms.

[0046] More preferably, R 1 represents any one of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and R 2 It represents any of a hydroxyl group and an alkoxy group having 1 to 6 carbon atoms.

[0047] The polymer of the silane compound is preferably a polymer of a silane compound represented by the following general formula (2) from the viewpoint of easily suppressing outdiffusion from the impurity-diffusing composition.

[0048] [Chemistry 3]

[0049]

[0050] In the general formula (2), R 3 represents an aromatic group having 6 to 15 carbon atoms, plural R 3 The same or different. 4represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 4 The same or different. 5 and R 6 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an acyloxy group having 2 to 6 carbon atoms, and a plurality of R 5 and R 6 n1 and m1 are integers of 1 to 9999, n1+m1 is an integer of 2 to 10000, and n1:m1=95:5 to 25:75. From the perspective of the toughness of the film after film formation, the preferred range of (n1+m1) is 5 to 9000, and more preferably 10 to 8000.

[0051] R in general formula (2) 3 The aryl group having 6 to 15 carbon atoms in the formula may be either an unsubstituted form or a substituted form, and may be selected according to the characteristics of the impurity diffusion composition. The preferred substituted form may be a structure similar to R 1 , R 2 Specific examples of the aryl group having 6 to 15 carbon atoms include the following: 1 , R 2 The aryl group in is the same aryl group.

[0052] R in general formula (2) 4 The alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, the alkenyl group having 2 to 10 carbon atoms, the acyloxy group having 2 to 6 carbon atoms, and the aryl group having 6 to 15 carbon atoms in the above-mentioned group may be either an unsubstituted group or a substituted group, and may be selected according to the characteristics of the impurity diffusion composition. The preferred substituted group may be a structure similar to R 1 , R 2 As specific examples thereof, there can be cited the same structure as R 1 , R 2 The specific example is the same as the example in .

[0053] R in general formula (2) 5 and R 6 The alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, the alkenyl group having 2 to 10 carbon atoms, and the acyloxy group having 2 to 6 carbon atoms in the formula (A) may be either an unsubstituted form or a substituted form, and may be selected according to the characteristics of the impurity diffusion composition. The preferred substituted form may be a structure similar to R 1 , R 2As specific examples thereof, there can be cited the same structure as R 1 , R 2 The specific example is the same as the example in .

[0054] Specific examples of the organosilanes that can be used as a raw material for the polymer of the silane compound represented by the general formula (1) include tetramethoxysilane, tetraethoxysilane, tetraacetoxysilane and other tetrafunctional silanes, methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltri-n-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, ethyltri-n-butoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, The present invention also includes trifunctional silanes such as 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, trifluoromethyl trimethoxysilane, trifluoromethyl triethoxysilane, 3,3,3-trifluoropropyl trimethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl triethoxysilane, and 3-mercaptopropyl trimethoxysilane, and bifunctional silanes such as dimethyl dimethoxysilane, dimethyl diethoxysilane, dimethyl diacetoxysilane, di-n-butyl dimethoxysilane, (3-glycidoxypropyl) methyl dimethoxysilane, and (3-glycidoxypropyl) methyl diethoxysilane. It should be noted that these organosilanes may be used alone or in combination of two or more. Among these organosilanes, trifunctional silane is preferably used from the viewpoint of easily suppressing outdiffusion from the impurity-diffusing composition.

[0055] As the silane compound represented by the general formula (2), the silane compound having R 3 and R 4 Specific examples of the organosilane as a raw material of the unit are preferably phenyltrimethoxysilane, phenyltriethoxysilane, p-hydroxyphenyltrimethoxysilane, p-tolyltrimethoxysilane, p-phenylyltrimethoxysilane, p-methoxyphenyltrimethoxysilane, 1-(p-hydroxyphenyl)ethyltrimethoxysilane, 2-(p-hydroxyphenyl)ethyltrimethoxysilane, 4-hydroxy-5-(p-hydroxyphenylcarbonyloxy)pentyltrimethoxysilane, diphenyldimethoxysilane, 1-naphthyltrimethoxysilane, 2-naphthyltrimethoxysilane, 1-naphthyltriethoxysilane, 2-naphthyltriethoxysilane, and anthracenetrimethoxysilane. Among them, from the perspective of cost, organosilanes having a monocyclic aromatic group such as phenyl are more preferred than organosilanes having a polycyclic aromatic group such as naphthalene and anthracene.

[0056] As the compound having R which can be used as the general formula (2) 5 and R 6 Specific examples of the organosilane as a raw material for the unit include the same organosilane as the raw material for the polymer of the silane compound represented by the general formula (1). Among them, trifunctional silane is preferably used from the aspect of easily suppressing the outdiffusion from the impurity-diffusing composition.

[0057] The polymer of the silane compound represented by the general formula (2) is a polysiloxane containing 25 to 95 mol % of units of aromatic groups having 6 to 15 carbon atoms in terms of Si atoms. That is, n1:m1=95:5 to 25:75. By being within this range, the effect of suppressing the external diffusion of impurity diffusion components and reducing organic residues when removing impurity diffusion components after heat treatment is improved. In addition, by being within this range, in an impurity diffusion composition to which a thermal decomposition component such as a thickener is added, the pores generated by thermal decomposition can be filled by the reflux effect of siloxane, and a dense film with few pores can be formed. Therefore, it is not easily affected by the atmosphere during diffusion, and a high shielding property against other impurities can be obtained.

[0058] The terminal group is preferably any one of hydrogen, hydroxyl, alkyl having 1 to 6 carbon atoms, alkoxy having 1 to 6 carbon atoms, acyloxy having 1 to 6 carbon atoms, and alkenyl having 2 to 10 carbon atoms.

[0059] The polymer of the silane compound represented by the general formula (2) may be a block copolymer or a random copolymer as long as it contains the respective constituent components in the above-specified ratio.

[0060] From the perspective of suppressing outward diffusion and further improving masking properties, the unit containing an aromatic group having 6 to 15 carbon atoms is more preferably 35 mol% or more, and more preferably 40 mol% or more. In addition, in order not to be affected by the atmosphere or film thickness and not to generate residues, the unit containing an aromatic group is preferably 80 mol% or less. That is, n1:m1=80:20 to 35:65 is more preferred, and n1:m1=80:20 to 40:60 is more preferred.

[0061] The polymer of the silane compound represented by the general formula (1) or (2) can be obtained, for example, by subjecting the organosilane compound to hydrolysis and subjecting the hydrolyzate to a condensation reaction in the presence of a solvent or in the absence of a solvent. Various conditions of the hydrolysis reaction, such as acid concentration, reaction temperature, reaction time, etc., can be appropriately set in consideration of the scale of the reaction, the size and shape of the reaction vessel, etc. For example, it is preferred that an acid catalyst and water are added to the organosilane compound in a solvent for 1 to 180 minutes, followed by reaction at room temperature to 110° C. for 1 to 180 minutes. By conducting the hydrolysis reaction under such conditions, a violent reaction can be suppressed. The reaction temperature is more preferably 30 to 130° C.

[0062] The hydrolysis reaction is preferably carried out in the presence of an acid catalyst. As an acid catalyst, halogenated hydrogen-based inorganic acids such as hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, nitric acid, phosphoric acid, hexafluorophosphoric acid, hexafluoroantimonic acid, boric acid, tetrafluoroboric acid, chromic acid, sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, acetic acid, citric acid, formic acid, gluconic acid, lactic acid, oxalic acid, tartaric acid, pyruvic acid, citric acid, succinic acid, fumaric acid, malic acid, etc. can be exemplified. In the present invention, from the aspect of doping, the acid catalyst preferably does not contain atoms other than silicon, hydrogen, carbon, oxygen, nitrogen, and phosphorus as much as possible, and preferably uses an acid catalyst of phosphoric acid, formic acid, acetic acid, and carboxylic acid.

[0063] Among them, phosphoric acid is preferred.

[0064] The preferred content of the acid catalyst is 0.1 to 5 parts by mass relative to 100 parts by mass of all the organosilane compounds used in the hydrolysis reaction. By setting the amount of the acid catalyst within the above range, the hydrolysis reaction can be easily controlled so as to proceed necessarily and sufficiently.

[0065] The solvent used in the hydrolysis reaction of the organosilane compound and the condensation reaction of the hydrolyzate is not particularly limited, and can be appropriately selected in consideration of the stability, coating properties, volatility, etc. of the resin composition. In addition, two or more solvents can be combined, or the reaction can be carried out under solvent-free conditions. Specific examples of solvents include alcohols such as methanol, ethanol, propanol, isopropanol, butanol, isobutanol, tert-butanol, 1-methoxy-2-propanol, pentanol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxy-1-butanol, 1-tert-butoxy-2-propanol, and diacetone alcohol; glycols such as ethylene glycol and propylene glycol; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monopropyl ether. , propylene glycol tert-butyl ether, propylene glycol n-butyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethyl ether, diethylene glycol methyl ethyl ether, dipropylene glycol n-butyl ether, dipropylene glycol monomethyl ether, diisopropyl ether, di-n-butyl ether, diphenyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, ethylene glycol monobutyl ether and other ethers; methyl ethyl ketone, acetylacetone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, 2-heptanone, diisopropyl ketone Ketones such as butanone, cyclohexanone, and cycloheptanone; amides such as dimethylformamide and dimethylacetamide; isopropyl acetate, ethyl acetate, propyl acetate, butyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, ethyl acetoacetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, diethylene glycol monoethyl ether acetate Acetic esters such as glycol butyl ether acetate, 1,3-butanediol diacetate, diethylene glycol ethyl ether acetate, dipropylene glycol methyl ether acetate, methyl lactate, ethyl lactate, butyl lactate, triacetyl glycerol, etc.; aromatic or aliphatic hydrocarbons such as toluene, xylene, hexane, cyclohexane, ethyl benzoate, naphthalene, 1,2,3,4-tetrahydronaphthalene, γ-butyrolactone, N-methyl-2-pyrrolidone, N,N-dimethylimidazolidinone, dimethyl sulfoxide, propylene carbonate, etc.

[0066] In the present invention, from the viewpoint of solubility and printability, preferred examples include diethylene glycol methyl ethyl ether (boiling point 176°C), ethylene glycol monoethyl ether acetate (boiling point 156.4°C), ethylene glycol monomethyl ether acetate (boiling point 145°C), methyl lactate (boiling point 145°C), ethyl lactate (boiling point 155°C), diacetone alcohol (boiling point 169°C), propylene glycol monomethyl ether acetate (boiling point 145°C), 3-methoxy-3-methyl-1-butanol (boiling point 174°C), dipropylene glycol monomethyl ether (boiling point 188°C), dipropylene glycol n-butyl ether (boiling point 22 9℃), γ-butyrolactone (boiling point 204℃), diethylene glycol monoethyl ether acetate (boiling point 217℃), diethylene glycol butyl ether acetate (boiling point 246℃), ethyl acetoacetate (boiling point 181℃), N-methyl-2-pyrrolidone (boiling point 204℃), N,N-dimethylimidazolidinone (boiling point 226℃), dipropylene glycol methyl ether acetate (boiling point 213℃), 1,3-butanediol diacetate (boiling point 232℃), diisobutyl ketone (boiling point 168℃), propylene glycol tert-butyl ether (boiling point 151℃), propylene glycol n-butyl ether (boiling point 170℃).

[0067] In the case where a solvent is generated by the hydrolysis reaction, the hydrolysis can also be carried out under solvent-free conditions. It is also preferred to further add a solvent after the reaction is completed to adjust the appropriate concentration as a resin composition. In addition, it is also possible to distill and remove the generated alcohol etc. in an appropriate amount under heating and / or reduced pressure after the hydrolysis according to the purpose, and then add a suitable solvent.

[0068] The amount of the solvent used in the hydrolysis reaction is preferably 80 parts by mass or more and 500 parts by mass or less relative to 100 parts by mass of the total organosilane compound. By making the amount of the solvent within the above range, the hydrolysis reaction can be easily controlled so that it is necessary and sufficient to proceed. In addition, the water used in the hydrolysis reaction is preferably ion-exchanged water. The amount of water can be arbitrarily selected, and is preferably used in the range of 1.0 to 4.0 moles relative to 1 mole of Si atoms.

[0069] The impurity diffusion composition (a) used in the present invention comprises an impurity diffusion component (a-2) for forming an impurity diffusion layer in a semiconductor substrate. As an n-type impurity diffusion component, a compound containing a Group 15 element is preferred, and a phosphorus compound is preferred. As a p-type impurity diffusion component, a compound containing a Group 13 element is preferred, and a boron compound is preferred.

[0070] When the impurity diffusion composition (a) is used in the method for manufacturing a semiconductor element of the present invention, there is an advantage that when a diffusion layer of the same type of impurities with different concentrations is formed by thermal diffusion using gas, coating, etc. in a region where the impurity diffusion layer region (c) is not formed, the diffusion of the impurity diffusion layer region (c) is further advanced compared to the case where only the same thermal history is applied. It is presumed that this is due to the additional supply of the same type of impurities to the impurity diffusion layer region (c). This effect is particularly significantly confirmed in p-type impurities. As a result, there is an advantage that the processing conditions for obtaining the same diffusion layer state can be made milder.

[0071] Examples of the phosphorus compound include phosphorus pentoxide, phosphoric acid, polyphosphoric acid, methyl phosphate, dimethyl phosphate, trimethyl phosphate, ethyl phosphate, diethyl phosphate, triethyl phosphate, propyl phosphate, dipropyl phosphate, tripropyl phosphate, butyl phosphate, dibutyl phosphate, tributyl phosphate, phenyl phosphate, diphenyl phosphate, triphenyl phosphate and other phosphoric acid esters, methyl phosphite, dimethyl phosphite, trimethyl phosphite, ethyl phosphite, diethyl phosphite, triethyl phosphite, propyl phosphite, dipropyl phosphite, tripropyl phosphite, butyl phosphite, dibutyl phosphite, tributyl phosphite, phenyl phosphite, diphenyl phosphite, triphenyl phosphite and other phosphoric acid esters, etc. Among them, phosphoric acid, phosphorus pentoxide or polyphosphoric acid is preferred from the aspect of doping property.

[0072] Examples of the boron compound include boric acid, boron trioxide, methylboric acid, phenylboric acid, trimethyl borate, triethyl borate, tripropyl borate, tributyl borate, trioctyl borate, and triphenyl borate.

[0073] In addition to the polymer of the silane compound, the impurity diffusion composition (a) used in the present invention may also contain a binder resin. Preferred specific examples include polyvinyl alcohol, polyacrylamide, polyvinyl pyrrolidone, polyethylene oxide, polysulfone, cellulose ether, carboxymethyl cellulose, hydroxyethyl cellulose, ethyl cellulose, gelatin, starch, dextrin, poly(meth)acrylic acid, poly(meth)acrylate, poly(dimethylaminoethyl)acrylate, polybutadiene, polystyrene, polybutyral, etc., but are not limited thereto. They may be used alone or in combination of two or more.

[0074] When the polymer of the silane compound (a-1) in the impurity diffusion composition (a) is a polymer of the silane compound represented by the general formula (2), a particularly preferred resin may be polyvinyl alcohol (a-3) having a saponification degree of 20 mol% or more and less than 50 mol%. Polyvinyl alcohol is a component used to form a complex with the impurity diffusion component (a-2), especially the p-type impurity diffusion component, to form a uniform coating when applied. By making the saponification degree of the polyvinyl alcohol greater than 20%, the stability of the complex with the impurity diffusion component (a-2) is improved, and the diffusibility and diffusion uniformity are further improved. In addition, by making the saponification degree of the polyvinyl alcohol less than 50%, the solubility in organic solvents is easily improved. The impurity diffusion composition (a) containing the polymer of the silane compound represented by the general formula (2) has low solubility in water and a high proportion of organic solvent in the solvent, so that the solubility in organic solvents is sometimes very important. Even in this case, by setting the saponification degree of polyvinyl alcohol to 20% or more and less than 50%, a very stable complex can be formed in an organic solvent system, and an impurity diffusion composition can be provided that can further improve the diffusion uniformity of impurities and further promote the diffusion process. The composition that can further promote the diffusion process has the advantage that the processing conditions for obtaining the same diffusion layer state can be milder.

[0075] From the viewpoint of solubility and complex stability, the average degree of polymerization of polyvinyl alcohol is preferably 150 to 1000. In the present invention, the average degree of polymerization and saponification degree are values ​​measured in accordance with JIS K 6726 (1994). The saponification degree is a value measured by the back titration method described in the JIS.

[0076] The impurity diffusion composition (a) used in the present invention preferably contains a solvent. As preferred specific examples, there can be mentioned: acetone, methyl ethyl ketone, methyl n-propyl ketone, methyl isopropyl ketone, methyl n-butyl ketone, methyl isobutyl ketone, methyl n-amyl ketone, methyl n-hexyl ketone, diethyl ketone, diacetone, diisobutyl ketone, trimethyl nonanone, cyclohexanone, cyclopentanone, methylcyclohexanone, 2,4-pentanedione, acetone acetone and other ketone solvents; diethyl ether, methyl ethyl ether, methyl n-propyl ether, diisopropyl ether, tetrahydrofuran, methyl tetrahydrofuran, dioxane, dimethyl dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol di-n-propyl ether, ethylene glycol dibutyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol methyl n-propyl ether, diethyl ether Ethylene glycol methyl n-butyl ether, diethylene glycol di-n-propyl ether, diethylene glycol di-n-butyl ether, diethylene glycol methyl n-hexyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, triethylene glycol methyl n-butyl ether, triethylene glycol di-n-butyl ether, triethylene glycol methyl n-hexyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, tetraethylene glycol methyl n-butyl ether, tetraethylene glycol di-n-butyl ether, tetraethylene glycol methyl n-hexyl ether, tetraethylene glycol di-n-butyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol di-n-propyl ether, propylene glycol dibutyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, dipropylene glycol methyl ethyl ether, dipropylene glycol methyl n-butyl ether, dipropylene glycol di-n-propyl ether, dipropylene glycol di Ether solvents such as butyl ether, dipropylene glycol methyl n-hexyl ether, tripropylene glycol dimethyl ether, tripropylene glycol diethyl ether, tripropylene glycol methyl ethyl ether, tripropylene glycol methyl n-butyl ether, tripropylene glycol di-n-butyl ether, tripropylene glycol methyl n-hexyl ether, tetrapropylene glycol dimethyl ether, tetrapropylene glycol diethyl ether, tetrapropylene glycol methyl ethyl ether, tetrapropylene glycol methyl n-butyl ether, tetrapropylene glycol di-n-butyl ether, tetrapropylene glycol methyl n-hexyl ether, tetrapropylene glycol di-n-butyl ether; methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, n-pentyl acetate, sec-pentyl acetate, 3-methoxybutyl acetate, methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, 2-(2-butoxy)acetate Ester solvents such as ethyl acetate, benzyl acetate, cyclohexyl acetate, methyl cyclohexyl acetate, nonyl acetate, methyl acetoacetate, ethyl acetoacetate, diethylene glycol methyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, dipropylene glycol ethyl ether acetate, ethylene glycol diacetate, methoxytriethylene glycol acetate, ethyl propionate, n-butyl propionate, isopentyl propionate, diethyl oxalate, di-n-butyl oxalate, methyl lactate, ethyl lactate, n-butyl lactate, n-pentyl lactate, ethylene glycol methyl ether propionate, ethylene glycol ethyl ether propionate, ethylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, γ-butyrolactone, and γ-valerolactone;Acetonitrile, N-methylpyrrolidone, N-ethylpyrrolidone, N-propylpyrrolidone, N-butylpyrrolidone, N-hexylpyrrolidone, N-cyclohexylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and other non-protonic polar solvents; methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylpropanol butyl alcohol, secondary amyl alcohol, tert-amyl alcohol, 3-methoxybutanol, 3-methoxy-3-methylbutanol, n-hexanol, 2-methylpentanol, secondary hexanol, 2-ethylbutanol, secondary heptanol, n-octanol, 2-ethylhexanol, secondary octanol, n-nonanol, n-decanol, secondary undecyl alcohol, trimethyl nonanol, secondary tetradecanol, secondary heptadecanol, phenol, cyclohexanol, methylcyclohexanol, benzyl alcohol, isobornyl cyclohexanol, ethylene glycol, 1, Alcohol solvents such as 2-propylene glycol, 1,3-butylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, etc.; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether (cellosolve), ethylene glycol monophenyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-n-hexyl ether, ethoxylated triethylene glycol, tetraethylene glycol mono-n-butyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether , tripropylene glycol monomethyl ether and other glycol monoether solvents; α-terpinene, α-terpineol, myrcene, alloocimene, limonene, dipentene, α-pinene, β-pinene, terpineol, carvone, ocimene, phellandrene and other terpene solvents; isobornyl cyclohexanol, isobornyl phenol, 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, p-menthenyl phenol, and water. These can be used alone or in combination of two or more. ;

[0077] When the (a-1) silane compound polymer in the impurity-diffusing composition (a) has a structure represented by the general formula (2), the proportion of water is preferably 20% by mass or less based on the total solvent in consideration of the solubility of the silane compound polymer.

[0078] In particular, from the perspective of further improving printability when using screen printing or spin coating printing, a solvent having a boiling point of 100° C. or higher is preferred. When the boiling point is 100° C. or higher, for example, when the impurity-diffusing composition is printed on a printing plate used in the screen printing method, it is easy to suppress the impurity-diffusing composition from drying and fixing on the printing plate.

[0079] The content of the solvent having a boiling point of 100° C. or higher is preferably 20% by mass or more relative to the total amount of the solvent. Examples of the solvent having a boiling point of 100° C. or higher include diethylene glycol methyl ethyl ether (boiling point 176° C.), ethylene glycol monoethyl ether acetate (boiling point 156.4° C.), ethylene glycol monomethyl ether acetate (boiling point 145° C.), methyl lactate (boiling point 145° C.), ethyl lactate (boiling point 155° C.), diacetone alcohol (boiling point 169° C.), propylene glycol monomethyl ether acetate (boiling point 145° C.), 3-methoxy-3-methyl-1-butanol (boiling point 174° C.), dipropylene glycol monomethyl ether (boiling point 188° C.), dipropylene glycol n-butyl ether (boiling point 229° C.), γ-butyrolactone (boiling point 204° C.), diethylene glycol monoethyl ether acetate Ester (boiling point 217°C), diethylene glycol butyl ether acetate (boiling point 246°C), ethyl acetoacetate (boiling point 181°C), N-methyl-2-pyrrolidone (boiling point 204°C), N,N-dimethylimidazolidinone (boiling point 226°C), dipropylene glycol methyl ether acetate (boiling point 213°C), 1,3-butanediol diacetate (boiling point 232°C), diisobutyl ketone (boiling point 168°C), propylene glycol tert-butyl ether (boiling point 151°C), propylene glycol n-butyl ether (boiling point 170°C), acetylacetone (boiling point 140°C), diethylene glycol monobutyl ether (boiling point 171°C), diethylene glycol monobutyl ether acetate (boiling point 245°C).

[0080] The impurity diffusion composition (a) used in the present invention may contain a surfactant. By containing a surfactant, coating unevenness is improved and a uniform coating film can be obtained. As the surfactant, a fluorine-based surfactant or a silicone-based surfactant is preferably used.

[0081] Specific examples of fluorine-based surfactants include 1,1,2,2-tetrafluorooctyl (1,1,2,2-tetrafluoropropyl) ether, 1,1,2,2-tetrafluorooctyl hexyl ether, octaethylene glycol di (1,1,2,2-tetrafluorobutyl) ether, hexaethylene glycol (1,1,2,2,3,3-hexafluoropentyl) ether, octapropylene glycol di (1,1,2,2-tetrafluorobutyl) ether, hexapropylene glycol di (1,1,2,2,3,3-hexafluoropentyl) ether, sodium perfluorododecyl sulfonate, 1,1,2,2,8,9,9 A fluorine-based surfactant composed of a compound having a fluorinated alkyl group or a fluorinated alkylene group at least at one of a terminal, a main chain, and a side chain, such as 10,10-decafluorododecane, 1,1,2,2,3,3-hexafluorodecane, N-[3-(perfluorooctanesulfonylamide)propyl]-N,N'-dimethyl-N-carboxymethyleneammonium betaine, perfluoroalkylsulfonamidopropyltrimethylammonium salt, perfluoroalkyl-N-ethylsulfonylglycine salt, bis(N-perfluorooctanesulfonyl-N-ethylaminoethyl) phosphate, and monoperfluoroalkylethyl phosphate. In addition, commercially available products include Megaface F142D, Megaface F172, Megaface F173, Megaface F183, Megaface F444, Megaface F475, Megaface F477 (all manufactured by Dainippon Ink & Chemicals Co., Ltd.), Eftop EF301, Eftop303, Eftop 352 (manufactured by Shin-Akita Chemicals Co., Ltd.), Fluorad FC-430, Fluorad FC-431 (manufactured by Sumitomo 3M Co., Ltd.), AashiGuard AG710, Surflon S-382, Surflon SC-101, Surflon SC-102, Surflon SC-103, Surflon SC-104, Surflon SC-105, Surflon Fluorine-based surfactants such as SC-106 (manufactured by Asahi Glass Co., Ltd.), BM-1000, BM-1100 (manufactured by Yusho Co., Ltd.), NBX-15, FTX-218, DFX-218 (manufactured by NEOS Co., Ltd.)

[0082] Examples of commercially available silicone surfactants include SH28PA, SH7PA, SH21PA, SH30PA, and ST94PA (all manufactured by Dow Corning Toray Co., Ltd.), BYK067A, BYK310, BYK322, BYK331, BYK333, and BYK355 (manufactured by BYK Chemical Japan Ltd.).

[0083] When the surfactant is contained, the content is preferably 0.0001 to 1 mass % in the impurity-diffusing composition.

[0084] The impurity-diffusing composition (a) used in the present invention preferably contains a thickener to adjust the viscosity, so that it can be applied in a more precise pattern by a printing method such as screen printing.

[0085] Examples of the thickener include organic thickeners such as cellulose, cellulose derivatives, starch, starch derivatives, polyvinyl pyrrolidone, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyurethane resins, polyurea resins, polyimide resins, polyamide resins, epoxy resins, polystyrene resins, polyester resins, synthetic rubber, natural rubber, polyacrylic acid, various acrylic resins, polyethylene glycol, polyethylene oxide, polypropylene glycol, polypropylene oxide, silicone oil, sodium alginate, xanthan gum polysaccharides, gellan gum polysaccharides, guar gum polysaccharides, carrageenan polysaccharides, locust bean gum polysaccharides, carboxyvinyl polymers, hydrogenated castor oil-based, hydrogenated castor oil-based and fatty acid amide wax-based, special fatty acid-based, oxidized polyethylene-based, mixtures of oxidized polyethylene-based and amide-based, fatty acid-based polycarboxylic acids, phosphate ester surfactants, salts of long-chain polyaminoamide and phosphoric acid, and special modified polyamide-based. In the case of inorganic materials, there can be exemplified bentonite, montmorillonite, magnesium montmorillonite, iron montmorillonite, iron magnesium montmorillonite, beidellite, aluminum beidellite, saponite, aluminum saponite, synthetic hectorite, aluminum silicate, aluminum magnesium silicate, organic hectorite, fine-particle silicon oxide, colloidal alumina, calcium carbonate, etc. Two or more of them may be used in combination.

[0086] Examples of commercially available cellulose-based thickeners include 1110, 1120, 1130, 1140, 1150, 1160, 1170, 1180, 1190, 2200, 2260, 2280, and 2450 (all manufactured by Daicel Finechem Co., Ltd.).

[0087] Examples of commercially available polysaccharide thickeners include Viscarin PC209, Viscarin PC389, SeaKem×P8012 (all manufactured by FMC Chemicals Co., Ltd.), CAM-H, GJ-182, SV-300, LS-20, LS-30, XGT, XGK-D, G-100, and LG-10 (all manufactured by Mitsubishi Corporation).

[0088] Examples of commercially available acrylic thickeners include #2434T, KC7000, and KC1700P (all manufactured by Kyoeisha Chemical Co., Ltd.), AC-10LHPK, AC-10SHP, 845H, and PW-120 (all manufactured by Toagosei Co., Ltd.).

[0089] Examples of commercially available hydrogenated castor oil-based thickeners include Disparlon 308, NAMLON T-206 (both manufactured by Kusumoto Chemicals Co., Ltd.), T-20SF, and T-75F (both manufactured by Ito Oil Products Co., Ltd.).

[0090] Examples of commercially available oxidized polyethylene thickeners include D-10A, D-120, D-120-10, D-1100, DS-525, and DS-313 (all manufactured by Ito Oil Manufacturing Co., Ltd.), Disparlon 4200-20, Disparlon PF-911, Disparlon PF-930, Disparlon 4401-25X, Disparlon NS-30, Disparlon NS-5010, Disparlon NS-5025, Disparlon NS-5810, Disparlon NS-5210, and Disparlon NS-5310 (all manufactured by Kusumoto Chemicals Co., Ltd.), and FLOWNON SA-300 and FLOWNON SA-300H (all manufactured by Kyoeisha Chemical Co., Ltd.).

[0091] Examples of commercially available amide thickeners include T-250F, T-550F, T-850F, T-1700, T-1800, and T-2000 (all manufactured by Ito Oil Manufacturing Co., Ltd.), Disparlon 6500, Disparlon 6300, Disparlon 6650, Disparlon 6700, and Disparlon 3900EF (all manufactured by Kusumoto Chemicals Co., Ltd.), Talen 7200, Talen 7500, Talen 8200, Talen 8300, Talen 8700, Talen 8900, Talen KY-2000, KU-700, Talen M-1020, Talen VA-780, Talen VA-750B, Talen 2450, Flownon SD-700, and Flownon SDR-80, FLOWNON EC-121 (both manufactured by Kyoeisha Chemical Co., Ltd.), and the like.

[0092] Examples of commercially available bentonite thickeners include BEN-GEL, BEN-GEL HV, BEN-GEL HVP, BEN-GEL F, BEN-GEL FW, BEN-GEL BRITE 11, BEN-GEL A, BEN-GEL W-100, BEN-GEL W-100U, BEN-GEL W-300U, BEN-GEL SH, MULTIBEN, Esben, Esben C, Esben E, Esben W, Esben P, Esben WX, ORGANITE, and ORGANITE D (all manufactured by Hojun Co., Ltd.).

[0093] Examples of commercially available fine-particle silica thickeners include AEROSIL R972, AEROSIL R974, AEROSIL NY50, AEROSIL RY200S, AEROSIL RY200, AEROSIL RX50, AEROSIL NAX50, AEROSIL RX200, AEROSIL RX300, AEROSIL VPNKC130, AEROSIL R805, AEROSIL R104, AEROSIL R711, AEROSIL OX50, AEROSIL 50, AEROSIL 90G, AEROSIL 130, AEROSIL 200, AEROSIL 300, and AEROSIL 380 (all manufactured by NIPPON AEROSIL Co., Ltd.), WACKER HDK S13, WACKER HDK V15, WACKER HDK N20, and WACKER HDK N20P, WACKER HDK T30, WACKER HDK T40, WACKER HDK H15, WACKER HDK H18, WACKER HDK H20, WACKER HDK H30 (the above are manufactured by Asahi Kasei Co., Ltd.), etc.

[0094] From the perspective of forming a dense film and reducing residue, the thickener preferably has a 90% thermal decomposition temperature of 400°C or less. Specifically, polyethylene glycol, polyethylene oxide, polypropylene glycol, polypropylene oxide, and various acrylate resins are preferred, among which polyethylene oxide, polypropylene oxide, or acrylate resins are preferred. From the perspective of storage stability, acrylate resins are particularly preferred. Here, the 90% thermal decomposition temperature refers to the temperature at which the weight of the thickener is reduced by 90% due to thermal decomposition. The 90% thermal decomposition temperature can be measured using a thermogravimetric measuring device (TGA) or the like.

[0095] Examples of the acrylic resin include polyacrylates such as polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polymethyl acrylate, polyethyl acrylate, polypropyl acrylate, polybutyl acrylate, polyhydroxyethyl methacrylate, polybenzyl methacrylate, and polyglycidyl methacrylate, and copolymers thereof. In the case of the copolymer, the acrylic component may be 60 mol% or more in terms of polymerization ratio, and other copolymerizable components such as polyacrylic acid and polystyrene may be copolymerized.

[0096] In addition, as for polyethylene oxide and polypropylene oxide, copolymers of these two are also preferred. Acrylic resins, polyethylene oxide, and polypropylene oxide are preferably highly thickening in that they have a weight average molecular weight of 100,000 or more.

[0097] The content of these thickeners in the impurity-diffusing composition is preferably 3% by mass or more and 20% by mass or less. By being within this range, a dense film can be easily formed while obtaining a sufficient viscosity adjustment effect.

[0098] From the aspect of screen printability, the impurity diffusion composition (a) in the present invention preferably contains a thixotropic agent that imparts thixotropy. Here, imparting thixotropy refers to increasing the ratio (η1 / η2) of the viscosity (η1) at low shear stress to the viscosity (η2) at high shear stress. By containing a thixotropic agent, the pattern accuracy of screen printing can be improved. It is speculated that this is based on the following reasons. That is, it is speculated that the impurity diffusion composition containing a thixotropic agent has a low viscosity at high shear stress, so it is not easy to block the screen during screen printing, and the viscosity is high at low shear stress, so it is not easy to cause bleeding just after printing and thickening of the pattern line width.

[0099] As thixotropic agent, specifically, cellulose, cellulose derivatives, sodium alginate, xanthan gum polysaccharides, gellan gum polysaccharides, guar gum polysaccharides, carrageenan polysaccharides, locust bean gum polysaccharides, carboxyvinyl polymers, hydrogenated castor oil system, hydrogenated castor oil system and fatty acid amide wax system, special fatty acid system, oxidized polyethylene system, the mixture of oxidized polyethylene system and amide system, fatty acid system polycarboxylic acid, phosphate ester surfactant, long chain polyaminoamide and phosphoric acid salt, special modified polyamide system, bentonite, montmorillonite, magnesium montmorillonite, iron montmorillonite, iron magnesium montmorillonite, beidellite, aluminum beidellite, soapstone, aluminum soapstone, synthetic hectorite, aluminum silicate, magnesium aluminum silicate, organic hectorite, micro-silicon oxide, colloidal alumina, calcium carbonate etc. can be illustrated. Thixotropic agent can be used alone, and thixotropic agent more than two kinds can also be combined. In addition, it is more preferably used in combination with the above-mentioned thickener to obtain higher effect.

[0100] The viscosity of the impurity diffusion composition in the present invention is not limited and can be appropriately changed according to the printing method and film thickness. Here, for example, in the case of screen printing, which is one of the preferred printing methods, the viscosity of the impurity diffusion composition is preferably 5,000 mPa·s or more. This is because it is possible to suppress the bleeding of the printed pattern and obtain a good pattern. A further preferred viscosity is 10,000 mPa·s or more. There is no particular upper limit, but from the perspective of storage stability and handling, it is preferably 100,000 mPa·s or less. Here, regarding the viscosity, when it is less than 1,000 mPa·s, it is a value measured at a rotation speed of 20 rpm using an E-type digital viscometer based on JIS Z8803 (1991) "Solution Viscosity-Determination Method", and when it is more than 1,000 mPa·s, it is a value measured at a rotation speed of 20 rpm using a B-type digital viscometer based on JIS Z 8803 (1991) "Solution Viscosity-Determination Method". Thixotropy can be obtained from the viscosity ratio at different rotation speeds obtained by the above viscosity measurement method. In the present invention, the ratio (η2 / η20) of the viscosity at a rotation speed of 20 rpm (η20) to the viscosity at a rotation speed of 2 rpm is defined as thixotropy. In order to form a pattern with good precision by screen printing, the thixotropy is preferably 2 or more, and more preferably 3 or more.

[0101] In the present invention, the solid content concentration of the impurity diffusion composition (a) is not particularly limited, and the preferred range is 1 mass % to 90 mass %. If the concentration is lower than this range, the coating film thickness becomes too thin, and it is sometimes difficult to obtain the desired doping and masking properties; if the concentration is higher than this range, the storage stability is sometimes reduced.

[0102] <Impurity-diffusing composition (d)>

[0103] In the present invention, a first preferred embodiment of the impurity-diffusing composition (d) is that the impurity-diffusing composition (d) contains (d-1) a polymer of a silane compound and (d-2) an impurity-diffusing component.

[0104] The silane compound polymer (d-1) includes polycondensates, polyaddition products, polyadducts, and the like of monomers containing Si atoms.

[0105] In the first preferred embodiment of the impurity-diffusing composition (d), the silane compound polymer (d-1) is preferably a polymer of a silane compound represented by the following general formula (3).

[0106] [Chemistry 4]

[0107]

[0108] In the general formula (3), R 7 and R 8represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 7 and R 8 They are the same or different. l2 represents an integer of 1 to 10000. From the viewpoint of the toughness of the film after film formation, it is preferably 5 to 10000, and more preferably 10 to 10000.

[0109] R in formula (3) 7 and R 8 The alkyl group with 1 to 6 carbon atoms, the alkoxy group with 1 to 6 carbon atoms, the alkenyl group with 2 to 10 carbon atoms, the acyloxy group with 2 to 6 carbon atoms, and the aryl group with 6 to 15 carbon atoms can be either unsubstituted or substituted, and can be selected according to the characteristics of the impurity diffusion composition.

[0110] Specific examples of the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, the alkenyl group having 2 to 10 carbon atoms, the acyloxy group having 2 to 6 carbon atoms, and the aryl group having 6 to 15 carbon atoms include: 1 , R 2 The specific example is the same as the example in .

[0111] From the viewpoint of easily suppressing outdiffusion from the impurity-diffusing composition, R 7 , R 8 At least one of the above represents any one of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms.

[0112] More preferably, R 7 represents any one of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and R 8 It represents any of a hydroxyl group and an alkoxy group having 1 to 6 carbon atoms.

[0113] In the first preferred embodiment of the impurity-diffusing composition (d), the polymer of the silane compound (d-1) is more preferably a polymer of a silane compound represented by the following general formula (4) from the viewpoint of easily suppressing outdiffusion from the impurity-diffusing composition.

[0114] [Chemistry 5]

[0115]

[0116] In the general formula (4), R 9represents an aromatic group having 6 to 15 carbon atoms, plural R 9 The same or different. 10 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 10 The same or different. 11 and R 12 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an acyloxy group having 2 to 6 carbon atoms, and a plurality of R 11 and R 12 They are the same or different. n2 and m2 represent integers of 1 to 9999, n2+m2 is an integer of 2 to 10000, and n2:m2=95:5 to 25:75.

[0117] From the viewpoint of toughness of the film after film formation, the preferred range of (n2+m2) is 5 to 10,000, more preferably 10 to 10,000.

[0118] R in general formula (4) 9 The aryl group having 6 to 15 carbon atoms in the formula (R) may be either an unsubstituted form or a substituted form, and may be selected according to the characteristics of the impurity-diffusing composition. Specific examples of the aryl group having 6 to 15 carbon atoms include: 1 , R 2 The specific example is the same as the example in .

[0119] R in general formula (4) 10 The alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, the alkenyl group having 2 to 10 carbon atoms, the acyloxy group having 2 to 6 carbon atoms, and the aryl group having 6 to 15 carbon atoms in the impurity diffusion composition may be either unsubstituted or substituted, and may be selected according to the characteristics of the impurity diffusion composition. Specific examples thereof include: 1 , R 2 The specific example is the same as the example in .

[0120] R in general formula (4) 11 and R 12 The alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, the alkenyl group having 2 to 10 carbon atoms, and the acyloxy group having 2 to 6 carbon atoms in the impurity diffusion composition may be either unsubstituted or substituted, and may be selected according to the characteristics of the impurity diffusion composition. Specific examples thereof include: 1 , R 2 The specific example is the same as the example in .

[0121] Specific examples of the organosilane used as a raw material for the polymer of the silane compound represented by the general formula (3) include the same organosilanes as the specific examples of the organosilane used as a raw material for the polymer of the silane compound represented by the general formula (1).

[0122] Among these organosilanes, trifunctional silane is preferably used from the viewpoint of easily suppressing outdiffusion from the impurity-diffusing composition.

[0123] As the silane compound represented by the general formula (4), 9 and R 10 Specific examples of the organosilane as a raw material of the unit include: 3 and R 4 Specific examples of the organosilane as a raw material of the unit are the same as the organosilane.

[0124] As the compound having R which can be used as the general formula (4) 11 and R 12 Specific examples of the organosilane as a raw material for the unit include the same organosilane as the specific example of the organosilane as a raw material for the polymer of the silane compound represented by the general formula (1). Among them, trifunctional silane is preferably used from the aspect of easily suppressing the outdiffusion from the impurity-diffusing composition.

[0125] The polymer of the silane compound represented by the general formula (4) is a polysiloxane containing 25 to 95 mol % of units of aromatic groups having 6 to 15 carbon atoms in terms of Si atoms. That is, n2:m2=95:5 to 25:75. By being within this range, the effect of suppressing the external diffusion of impurity diffusion components and reducing organic residues when removing impurity diffusion components after heat treatment is improved. In addition, by being within this range, in an impurity diffusion composition to which a thermal decomposition component such as a thickener is added, the pores generated by thermal decomposition can be filled by the reflux effect of siloxane, and a dense film with few pores can be formed. Therefore, it is not easily affected by the atmosphere during diffusion, and a high shielding property against other impurities can be obtained.

[0126] The terminal group is preferably any one of hydrogen, hydroxyl, alkyl having 1 to 6 carbon atoms, alkoxy having 1 to 6 carbon atoms, acyloxy having 1 to 6 carbon atoms, and alkenyl having 2 to 10 carbon atoms.

[0127] The polymer of the silane compound represented by the general formula (2) may be a block copolymer or a random copolymer as long as it contains the respective constituent components in the above-specified ratio.

[0128] From the perspective of suppressing outward diffusion and further improving the masking property, the unit containing an aromatic group having 6 to 15 carbon atoms is more preferably 35 mol% or more, and more preferably 40 mol% or more. In addition, in order not to be affected by the atmosphere or film thickness and not to generate residues, the unit containing an aromatic group is preferably 80 mol% or less. That is, n2:m2=80:20 to 40:60 is particularly preferred.

[0129] The polymers of the silane compounds represented by the general formulae (3) and (4) can be obtained, for example, by hydrolyzing an organic silane compound and subjecting the hydrolyzate to a condensation reaction in the presence of a solvent or in the absence of a solvent. The specific method is the same as that for the polymers of the silane compounds represented by the general formulae (1) and (2).

[0130] Specific examples of the impurity-diffusing component (d-2) contained in the first preferred embodiment of the impurity-diffusing composition (d) are the same as those of the impurity-diffusing component contained in the impurity-diffusing composition (a).

[0131] In addition, when the polymer of the silane compound (d-1) in the impurity-diffusing composition (d) has a structure represented by the general formula (4), it may also contain polyvinyl alcohol (d-3) having a saponification degree of 20 mol% or more and less than 50 mol%. Specific examples of (d-3) are the same as those of (a-3).

[0132] The first preferred embodiment of the impurity-diffusing composition (d) may also contain a solvent, a surfactant, a thickener, and a thixotropic agent. Specific examples are the same as those of the solvent, surfactant, thickener, and thixotropic agent contained in the impurity-diffusing composition (a).

[0133] In the present invention, a second preferred embodiment of the impurity diffusion composition (d) is that the impurity diffusion composition (d) comprises (d-4) at least one resin selected from the group consisting of polyvinyl alcohol and polyether oxide, (d-5) an impurity diffusion component and (d-6) water accounting for more than 25% by mass in all solvents.

[0134] In a second preferred embodiment of the impurity-diffusing composition (d), at least one resin selected from the group consisting of polyvinyl alcohol and polyethylene oxide (d-4) is a component for forming a complex with the impurity-diffusing component (d-5) and forming a uniform coating when applied. From the perspective of the formation of a complex with the impurity-diffusing component (d-5) and the stability of the formed complex, at least one resin selected from the group consisting of polyvinyl alcohol and polyethylene oxide (d-4) is more preferably polyvinyl alcohol.

[0135] From the perspective of solubility and complex stability, the average degree of polymerization of polyvinyl alcohol is preferably 150 to 1000. In addition, from the perspective of solubility in water and complex stability, the saponification degree of polyvinyl alcohol is preferably 70 to 95 mol%. In the present invention, the average degree of polymerization and saponification degree are values ​​measured in accordance with JIS K6726 (1994), and the saponification degree is a value measured by back titration.

[0136] From the viewpoint of complex stability, the resin (d-4) contained in the impurity-diffusing composition is preferably 80 mass % or more, preferably 90 mass % or more, and most preferably 95 mass % or more of all the resins contained in the impurity-diffusing composition.

[0137] In view of heat diffusion and suppression of organic residues on the substrate after removal of the impurity-diffusing composition, the amount of the resin (d-4) is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass, based on the entire impurity-diffusing composition.

[0138] In the second preferred embodiment of the impurity-diffusing composition (d), specific examples of the impurity-diffusing component (d-5) are the same as those of the impurity-diffusing component contained in the impurity-diffusing composition (a).

[0139] Specific examples of the solvent, surfactant, thickener, and thixotropic agent are the same as those contained in the impurity-diffusing composition (a).

[0140] <Method for manufacturing semiconductor element (selective emitter)>

[0141] The method for manufacturing a semiconductor element of the present invention is a method for manufacturing a semiconductor element in which the same type of impurity diffusion layer regions are formed on a semiconductor substrate at two or more levels of different impurity concentrations, wherein at least one or more levels of impurity diffusion layer regions are formed by a method comprising the following steps: a step of applying an impurity diffusion composition (a) to a semiconductor substrate to partially form an impurity diffusion composition film (b); and a step of heating the impurity diffusion composition film (b) to diffuse impurities into the semiconductor substrate to form an impurity diffusion layer region (c), wherein the impurity diffusion composition (a) comprises (a-1) a polymer of a silane compound represented by the above general formula (1) and (a-2) an impurity diffusion component. The different impurity concentrations referred to herein refer to impurity diffusion layers having an impurity concentration difference of 1×10 17 / cm 3 As described above, the difference in sheet resistance value of the portion of the substrate surface where the impurity diffusion layer region is formed is 10Ω / □ or more.

[0142] A first preferred embodiment of the method for manufacturing a semiconductor device of the present invention preferably includes the step of diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed, using the impurity-diffusing composition film (b) as a mask.

[0143] Hereinafter, a first preferred embodiment of the method for manufacturing a semiconductor element of the present invention will be described with reference to the drawings. It should be noted that these are merely examples, and the method for manufacturing a semiconductor element of the present invention is not limited to these.

[0144] First, if Figure 1 As shown in (i), the impurity-diffusing composition (a) is partially applied onto the semiconductor substrate 1 to form a pattern 4 of the impurity-diffusing composition film (b).

[0145] As the semiconductor substrate, for example, a substrate having an impurity concentration of 10 15 ~10 16 Atom / cm 3 n-type single crystal silicon, polycrystalline silicon, and crystalline silicon substrates mixed with other elements such as germanium and carbon. P-type crystalline silicon or semiconductors other than silicon can also be used. The semiconductor substrate is preferably 50 to 300 μm thick and approximately quadrilateral with a side of 100 to 250 mm. In addition, in order to remove the slice damage and natural oxide film, it is preferred to etch the surface in advance using a hydrofluoric acid solution or an alkaline solution.

[0146] Examples of the method for coating the impurity-diffusing composition (a) include spin coating, screen printing, inkjet printing, slit coating, spray coating, relief printing, and gravure printing.

[0147] After the impurity-diffusing composition (a) is applied by these methods, the semiconductor substrate coated with the impurity-diffusing composition (a) is preferably dried at 50 to 260° C. for 30 seconds to 30 minutes using a hot plate, an oven, or the like to form a pattern of the impurity-diffusing composition film (b).

[0148] The drying temperature is more preferably 180 to 260° C. from the viewpoint of promoting the curing of the polymer of the silane compound and improving the in-plane uniformity of the impurity concentration after diffusion by suppressing the volatilization of the impurities such as sublimation. From the same viewpoint, the oxygen concentration during drying is preferably 15 to 25%.

[0149] The film thickness of the impurity-diffusing composition film (b) after drying is preferably 100 nm or more from the viewpoint of the diffusibility of impurities, and is preferably 3 μm or less from the viewpoint of the residue after etching.

[0150] Then, if Figure 1As shown in (ii), the impurities are heated and diffused into the semiconductor substrate to form an impurity diffusion layer region (c). The impurities can be diffused by a known thermal diffusion method, such as electric heating, infrared heating, laser heating, microwave heating, etc.

[0151] The time and temperature of thermal diffusion can be appropriately set to obtain the desired diffusion characteristics such as impurity diffusion concentration and diffusion depth. For example, by heating and diffusing at 800°C to 1200°C for 1 to 120 minutes, a surface impurity concentration of 10 19 ~10 21 diffusion layer.

[0152] However, as the diffusion temperature increases, the defect density of the silicon substrate increases, the lifetime decreases, and the light conversion efficiency of the solar cell tends to decrease. Therefore, in order to form the same diffusion layer state, it is preferable to perform the diffusion under milder conditions.

[0153] The diffusion atmosphere is not particularly limited and can be carried out in the air, or inert gases such as nitrogen and argon can be used to appropriately control the amount of oxygen in the atmosphere. From the perspective of shortening the diffusion time, it is preferred that the oxygen concentration in the atmosphere be 3% or less. In addition, if necessary, the film can be fired at a temperature of 200°C to 850°C before diffusion to decompose and remove organic matter in the impurity diffusion composition film (b).

[0154] Next, as described above, the process preferably includes the step of using the impurity-diffusing composition film (b) as a mask to diffuse impurities into a portion where the impurity-diffusing composition film (b) is not formed. Specifically, for example, Figure 1 (iv-1)~ Figure 1 As shown in (iv-3), the pattern of the impurity-diffusing composition film (b) is used as a mask to form an impurity diffusion layer region (f) having the same conductivity as the impurity diffusion layer region (c) but a different impurity concentration in the unpatterned portion.

[0155] In a first preferred embodiment of the method for manufacturing a semiconductor element of the present invention, the step of diffusing impurities into a portion where the impurity diffusion composition film (b) is not formed (the step of forming an impurity diffusion layer region (f)) can be performed after the impurity diffusion composition film (b) is heated to diffuse the impurities into the above-mentioned semiconductor substrate to form an impurity diffusion layer region (c).

[0156] As a specific example of a method for diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed, there can be mentioned: after ions containing an impurity-diffusing component are implanted onto the semiconductor substrate 1 having a pattern of the impurity-diffusing composition film (b), Figure 1A method of annealing (iv-1) by heating a semiconductor substrate 1 having a pattern of an impurity-diffusing composition film (b) in an atmosphere containing an impurity-diffusing component (iv-2); and forming an impurity-diffusing composition film (e) by applying an impurity-diffusing composition (d) to a portion of the semiconductor substrate 1 having a pattern of an impurity-diffusing composition film (b) where the impurity-diffusing composition film (b) is not formed (iii-1)). Figure 1 (iii-3)), methods of electric heating, infrared heating, laser heating, microwave heating (iv-3); etc.

[0157] In the first preferred embodiment of the method for producing a semiconductor composition of the present invention, a first more preferred embodiment is that the step of diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed is a step of implanting ions containing an impurity-diffusing component.

[0158] In the ion implantation process, boron is implanted at an energy of 1 to 40 keV and 0.5 to 5 eV. 15 1 / cm 2 The dose is preferably between 3 and 10 keV, 1.5 and 3e 15 1 / cm 2 The resistance of the impurity diffusion layer region (f) implanted with boron after recovery is 30 to 300 ohm / square (Ω / □), preferably 60 to 100 ohm / square.

[0159] Phosphorus is implanted at an energy of 1 to 40 keV and 0.5 to 5 eV. 15 1 / cm 2 The dose is preferably between 10 keV and 2.5 and 4 e 15 1 / cm 2 The resistance of the impurity diffusion layer region (f) implanted with phosphorus after recovery is 10 to 300 ohm / square (Ω / □), preferably 30 to 120 ohm / square.

[0160] Recovery (activation of the implanted dopant) can be performed by annealing the semiconductor substrate with the pattern of the impurity-diffusing composition film (b) in an inert atmosphere (N2, Ar) at a high temperature (800-1100°C).

[0161] By setting the energy, dose and temperature conditions of ion implantation, the impurity concentration of the impurity diffusion layer region (f) can be set higher than the impurity concentration of the impurity diffusion layer region (c), or it can be set lower than the impurity concentration of the impurity diffusion layer region (c).

[0162] In a first preferred embodiment of the method for manufacturing a semiconductor element of the present invention, the step of diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed (the step of forming an impurity diffusion layer region (f)) can also be performed simultaneously with the step of heating the impurity-diffusing composition film (b) to diffuse the impurities into the above-mentioned semiconductor substrate.

[0163] For example, Figure 1 As shown in (i), the impurity-diffusing composition (a) can be partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b), and then the impurity-diffusing composition film (b) can be partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b). Figure 1 (ii) the diffusion process Figure 1 (iii-1) ion implantation, through Figure 1 The annealing of (iv-1) forms the impurity diffusion layer region (f) and the impurity diffusion layer region (c) at the same time. In addition, as described later, in the second more preferred embodiment and the third more preferred embodiment, the impurity diffusion layer region (f) and the impurity diffusion layer region (c) may also be formed at the same time.

[0164] In the first preferred embodiment of the method for manufacturing a semiconductor device of the present invention, in a second more preferred embodiment, the step of diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed is a step of heating in an atmosphere containing an impurity-diffusing component.

[0165] When heating is performed in an atmosphere containing an impurity diffusion component, for example, boron tribromide (BBr3) is bubbled in the case of a p-type, phosphorus oxychloride (POCl3) is bubbled in the case of an n-type, and N2 is circulated, thereby forming an atmosphere containing an impurity diffusion component, and heating a semiconductor substrate with a pattern of an impurity diffusion composition film (b) in the atmosphere, thereby forming an impurity diffusion layer region (f). By setting the gas pressure and heating conditions, the impurity concentration of the impurity diffusion layer region (f) can be set to be higher than the impurity concentration of the impurity diffusion layer region (c), and can also be set to be lower than the impurity concentration of the impurity diffusion layer region (c).

[0166] At this time, in order to avoid mixing of other components, after forming the pattern of the impurity-diffusing composition film (b), it is preferred to continuously perform the diffusion process based on the same batch diffusion device. Figure 1 (ii) The impurity diffusion layer region (c) is formed by the diffusion process and based on Figure 1 (iv-2) Formation of the heated impurity diffusion layer region (f).

[0167] In addition, in Figure 1 As shown in (i), the impurity-diffusing composition (a) is partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b), and then the impurity-diffusing composition film (b) may be partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b). Figure 1 (ii) through the diffusion process Figure 1The heating in (iv-2) simultaneously forms the impurity diffusion layer region (f) and the impurity diffusion layer region (c).

[0168] In addition, in Figure 1 As shown in (i), the impurity-diffusing composition (a) is partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b), and then the impurity-diffusing composition film (b) may be partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b). Figure 1 (ii) the diffusion process and put it into Figure 1 In the heating furnace of (iv-2), the impurity diffusion layer region (c) is first formed by heating only in an inert gas, and then a gas containing an impurity diffusion component is directly introduced into the furnace and heated under conditions different from those of the heating conditions using only the inert gas, thereby forming an impurity diffusion layer region (f) having an impurity concentration different from that of the impurity diffusion layer region (c) in one batch.

[0169] In the first preferred embodiment of the method for manufacturing a semiconductor element of the present invention, the third more preferred embodiment is: the process of diffusing impurities to the portion where the impurity diffusion composition film (b) is not formed is a process of applying the impurity diffusion composition (d) to the portion where the impurity diffusion composition film (b) is not formed on the semiconductor substrate where the impurity diffusion composition film (b) is formed, and heating the formed impurity diffusion composition film (e).

[0170] Examples of the method for coating the impurity-diffusing composition (d) include spin coating, screen printing, inkjet printing, slit coating, spray coating, relief printing, and gravure printing.

[0171] Examples of the step of heating the impurity-diffusing composition film (e) include electric heating, infrared heating, laser heating, and microwave heating.

[0172] In particular, it is preferable that the impurity-diffusing composition (d) is applied so as to cover the pattern of the impurity-diffusing composition film (b) because impurities can be diffused well at the interface between the impurity-diffusing composition film (b) and the impurity-diffusing composition film (e). In order to achieve good impurity diffusion at the interface, it is most preferable to apply the impurity-diffusing composition (d) to the entire surface of the substrate so as to cover the pattern of the impurity-diffusing composition film (b).

[0173] After the impurity-diffusing composition (d) is applied by these methods, the semiconductor substrate 1 coated with the impurity-diffusing composition (d) is preferably dried at 50 to 200° C. for 30 seconds to 30 minutes using a hot plate, an oven, or the like to form an impurity-diffusing composition film (e).

[0174] Then, if Figure 1As shown in (iv-3), impurities are diffused into the semiconductor substrate 1 to form an impurity diffusion layer region (f). The impurity diffusion method can utilize a known thermal diffusion method, such as electric heating, infrared heating, laser heating, microwave heating, etc.

[0175] The time and temperature of thermal diffusion can be appropriately set to obtain the desired diffusion characteristics such as the impurity diffusion concentration and diffusion depth. For example, by heating and diffusing at 800°C to 1200°C for 1 to 120 minutes, a surface impurity concentration of 10 19 ~10 21 diffusion layer.

[0176] However, as the diffusion temperature increases, the defect density of the silicon substrate increases, the lifetime decreases, and the light conversion efficiency of the solar cell tends to decrease. Therefore, in order to form the same diffusion layer state, it is preferable to perform the diffusion under milder conditions.

[0177] The diffusion atmosphere is not particularly limited, and the diffusion may be carried out in the air, or an inert gas such as nitrogen or argon may be used to appropriately control the amount of oxygen in the atmosphere. From the perspective of shortening the diffusion time, it is preferred that the oxygen concentration in the atmosphere be 3% or less. In addition, if necessary, the film may be fired at a temperature of 200° C. to 850° C. before diffusion to decompose and remove organic matter in the impurity diffusion composition film (e).

[0178] At this time, by adjusting the impurity concentration of the impurity diffusion composition (d) and the film thickness of the impurity diffusion composition film (e), the impurity concentration of the impurity diffusion layer region (f) can be set to be higher than the impurity concentration of the impurity diffusion layer region (c), or it can be set to be lower than the impurity concentration of the impurity diffusion layer region (c).

[0179] In addition, in Figure 1 As shown in (i), the impurity-diffusing composition (a) is partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b), and then the impurity-diffusing composition film (b) may be partially applied to the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b). Figure 1 (ii) the diffusion process Figure 1 The impurity-diffusing composition film (e) of (iii-3) is formed by Figure 1 The heating in (iv-3) simultaneously forms the impurity diffusion layer region (f) and the impurity diffusion layer region (c).

[0180] Among the first to third more preferred aspects of the first preferred aspect of the method for manufacturing a semiconductor element of the present invention, the third more preferred aspect is more preferred from the perspective of improving the uniformity of the impurity diffusion concentration in the impurity diffusion layer regions (c) and (f).

[0181] Then, if Figure 1As shown in (v), the impurity diffusion composition films (b) and (e) formed on the surface of the semiconductor substrate 1 can be removed by a known etching method. The material used for etching is not particularly limited, and for example, it is preferred to contain at least one of hydrogen fluoride, ammonium, phosphoric acid, sulfuric acid, and nitric acid as an etching component, and contain water, an organic solvent, etc. as other components. Through the above process, two impurity diffusion layers of the same type and different impurity diffusion concentrations can be formed on the semiconductor substrate.

[0182] In a second preferred embodiment of the method for manufacturing a semiconductor element of the present invention, after forming an impurity diffusion layer region (f) using at least one step selected from the group consisting of a step of implanting ions containing an impurity diffusion component into a semiconductor substrate, a step of heating in an atmosphere containing an impurity diffusion component, and a step of coating an impurity diffusion composition (d) on the entire surface and heating the formed impurity diffusion composition film (e), the method further comprises the following steps: a step of coating an impurity diffusion composition (a) to partially form an impurity diffusion composition film (b); and a step of heating the impurity diffusion composition film (b) to diffuse impurities into the semiconductor substrate to form an impurity diffusion layer region (c).

[0183] Hereinafter, a second preferred embodiment of the method for manufacturing a semiconductor element of the present invention will be described with reference to the drawings. It should be noted that these are merely examples, and the method for manufacturing a semiconductor element of the present invention is not limited to these.

[0184] First, if Figure 2 (ii-1)~ Figure 2 As shown in (ii-3), an impurity diffusion layer region (f) is formed on the semiconductor substrate 1.

[0185] As a specific example of a method for forming the impurity diffusion layer region (f), there can be cited: after ions containing an impurity diffusion component are implanted onto the semiconductor substrate 1 ( Figure 1 (ii-1)) annealing; (ii-2) heating the semiconductor substrate 1 in an atmosphere containing an impurity diffusion component; (iii) applying the impurity diffusion composition (d) to the entire surface of the semiconductor substrate 1 to form an impurity diffusion composition film (e) ( Figure 2 (i-3)), methods of electric heating, infrared heating, laser heating, microwave heating (ii-3); etc.

[0186] The respective details can be performed by the same method as described above.

[0187] Then, if Figure 2 As shown in (iii), the impurity-diffusing composition (a) is partially applied onto the semiconductor substrate 1 to form a pattern of the impurity-diffusing composition film (b).

[0188] The pattern formation can be performed in detail by the same method as described above.

[0189] Then, if Figure 2 As shown in (iv), impurities are diffused into the semiconductor substrate 1 to form an impurity diffusion layer region (c).

[0190] The impurity diffusion can be performed in detail by the same method as described above.

[0191] A third preferred embodiment of the method for manufacturing a semiconductor element of the present invention includes the following steps: a step of coating an impurity diffusion composition (d) on the entire surface of a semiconductor substrate to form an impurity diffusion composition film (e), coating an impurity diffusion composition (a) thereon to partially form an impurity diffusion composition film (b); and a step of heating them simultaneously to diffuse impurities into the semiconductor substrate to simultaneously form impurity diffusion layer regions (c) and (f).

[0192] Hereinafter, a third preferred embodiment of the method for manufacturing a semiconductor element of the present invention will be described with reference to the drawings. It should be noted that these are merely examples, and the method for manufacturing a semiconductor element of the present invention is not limited to these.

[0193] For example, in Figure 2 As shown in (i-3), after the impurity-diffusing composition (d) is applied to the entire surface of the semiconductor substrate 1 to form an impurity-diffusing composition film (e), it is not necessary to Figure 2 (ii-3) is carried out by the diffusion step Figure 2 (iii) the patterning of the impurity-diffusing composition film (b), by Figure 2 The heating in (iv) simultaneously forms the impurity diffusion layer region (f) and the impurity diffusion layer region (c).

[0194] In the second preferred embodiment and the third preferred embodiment of the method for manufacturing a semiconductor element of the present invention, for example, finally, Figure 2 As shown in (v), the impurity-diffusing composition films (b) and (e) formed on the surface of the semiconductor substrate 1 are removed by a known etching method. The same method as described above can be used for details.

[0195] The method for manufacturing a semiconductor element of the present invention can also be applied to photovoltaic elements such as solar cells, or semiconductor devices having patterned impurity diffusion regions on the semiconductor surface, such as transistor arrays, diode arrays, photodiode arrays, sensors, etc.

[0196] The method for producing a solar cell of the present invention includes the method for producing a semiconductor element of the present invention.

[0197] An example of a method for obtaining a solar cell from a semiconductor element obtained by the method for producing a semiconductor element of the present invention using the method for producing a solar cell of the present invention is as follows.

[0198] As a method for manufacturing a solar cell of the present invention, it is preferred to provide a passivation film for suppressing surface recombination and preventing light reflection on the semiconductor element obtained by the method for manufacturing a semiconductor element of the present invention. For example, as a passivation film for an n-type diffusion layer, SiO2 obtained by heat treatment in a high temperature oxygen atmosphere above 700°C and a silicon nitride film for protecting the film can be provided. Alternatively, only SiN x Film. In this case, it can be formed by a plasma CVD method using a mixed gas of SiH4 and NH3 as a raw material. At this time, hydrogen diffuses into the crystal, and orbitals that do not contribute to the bonding of silicon atoms, that is, dangling bonds, are bonded with hydrogen to passivate defects (hydrogen passivation). More specifically, it is formed under the conditions of a mixed gas flow ratio of NH3 / SiH4 of 0.05 to 1.0, a pressure of the reaction chamber of 13.3 to 266.6 Pa (0.1 to 2 Torr), a temperature during film formation of 300°C to 550°C, and a frequency for plasma discharge of 100 kHz or more.

[0199] Next, a metal paste for the light-receiving surface electrode is printed on the anti-reflection film of the light-receiving surface by screen printing, and a metal paste is printed on the passivation film of the n-type diffusion layer, and dried to form a light-receiving surface electrode. The metal paste for the light-receiving surface electrode has metal particles and glass particles as essential components, and contains a resin binder, other additives, etc. as needed. The metal paste used at this time is preferably a metal paste suitable for the p-type diffusion layer and a metal paste suitable for the n-type diffusion layer. As for the metal particles, Ag and Al are preferably used.

[0200] Next, the electrode is heat treated (fired) to complete the solar cell element. When the heat treatment (fired) is performed for several seconds to several minutes in the range of 600°C to 900°C, the anti-reflection film as an insulating film on the light-receiving side is melted by the glass particles contained in the metal paste for the electrode, and then the silicon surface is also partially melted, and the metal particles (such as silver particles) in the paste form a contact portion with the semiconductor substrate and solidify. As a result, the light-receiving surface electrode formed is connected to the semiconductor substrate. This is called fire through.

[0201] The light-receiving surface electrode is usually composed of a busbar electrode and a finger electrode intersecting the busbar electrode. Such a light-receiving surface electrode can be formed by screen printing of the above-mentioned metal paste, or plating of electrode materials, evaporation of electrode materials by electron beam heating in a high vacuum, etc. The busbar electrode and the finger electrode can be formed by a known method.

[0202] Example

[0203] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. It should be noted that the compounds used are referred to by abbreviations as follows.

[0204] KBM-13: Methyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0205] KBM-103: Phenyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0206] GBL: gamma-butyrolactone

[0207] BYK-333: Silicone surfactant (manufactured by BYK Chemical Co., Ltd.)

[0208] SH30PA: Silicone surfactant (manufactured by Dow Corning Toray Co., Ltd.)

[0209] <Evaluation method>

[0210] Sheet resistance (surface resistance) uniformity (impurity diffusion concentration uniformity)

[0211] For the semiconductor substrates in Examples 1 to 14 and Comparative Examples 1 to 4, the impurity-diffusing composition was removed. Figure 3 The sheet resistance values ​​of the indicated locations (A to D, E to M) were measured using a four-probe sheet resistance measuring apparatus RT-70V (manufactured by Napson Corporation).

[0212] The average value, maximum value and minimum value of A~D are set as A1, B1 and C1, and the average value, maximum value and minimum value of E~M are set as A2, B2 and C2. If the deviation (B1-C1) / A1×100 and (B2-C2) / A2×100 are both within 20%, it is qualified; if it exceeds 20%, it is unqualified.

[0213] Mixing example 1

[0214] <Synthesis of Silica Compound Polymer Solution>

[0215] Into a 2000 mL three-necked flask, 164.93 g of KBM-13, 204.07 g of KBM-103, and 363.03 g of GBL were charged. While stirring at 40 °C, an aqueous formic acid solution prepared by dissolving 1.215 g of formic acid in 130.76 g of water was added over 30 minutes. After the addition was completed, the mixture was stirred at 40 °C for 1 hour, then heated to 70 °C and stirred for 30 minutes. Thereafter, the oil bath was heated to 115 °C. One hour after the start of heating, the internal temperature of the solution reached 100 °C, and then it was heated and stirred for 1 hour (internal temperature: 100 - 110 °C). The resulting solution was cooled using an ice bath to obtain a polymer of the silica compound. The solid content concentration of the polymerization solution was 39.8 mass%.

[0216] <Preparation of p-Type Impurity Diffusion Composition>

[0217] 4.39 g of the polymer of the silica compound synthesized above, 1.47 g of boric acid, 12.55 g of GBL, and BYK-333 at 300 ppm relative to the total solution were added, and the mixture was stirred well until homogeneous to obtain p-type impurity diffusion composition A.

[0218] Mixing Example 2

[0219] <Synthesis of Polymer Solution of Silica Compound>

[0220] Into a 500 mL three-necked flask, 112.47 g of 3-glycidoxypropyltrimethoxysilane and 130.47 g of diethylene glycol monomethyl ether were charged and heated to 40 °C. Then, a mixed solution of 0.24 g of concentrated sulfuric acid and 42.83 g of water was added dropwise. After the addition was completed, the mixture was continuously stirred at 40 °C for 1 hour. Then, it was heated to 70 °C and stirred for 1 hour 20 minutes. Then, it was heated to 100 °C and stirred for 1 hour. Thereafter, the temperature of the oil bath was raised to 120 °C and stirred. After stirring at 120 °C for 1 hour, it was cooled to below 40 °C to obtain a polymer solution of the silica compound.

[0221] <Preparation of p-Type Impurity Diffusion Composition>

[0222] To a 500 mL three-necked flask, 58.55 g of 3-methoxy-3-methylbutanol and 4.22 g of polyvinyl alcohol (manufactured by JAPANVAM&POVAL CO., LTD., degree of polymerization 300, saponification degree 85%) were successively added. The temperature was raised to 80 °C by heating, and then 36.00 g of added water was added dropwise. After the addition was completed, stirring was continued at 80 °C until the polyvinyl alcohol was completely dissolved. Then, 0.73 g of boron trioxide was added, and stirring was continued at 80 °C for 1 hour. Then, it was cooled to below 40 °C, and 20 g of the polymer solution of the synthesized silica compound was added dropwise. Stirring was continued for 1 hour to obtain p-type impurity diffusion composition B.

[0223] Mixing Example 3

[0224] <Preparation of p-Type Impurity Diffusion Composition>

[0225] To a 300 mL three-necked flask, 73.74 g of water, 113.4 g of propylene glycol monomethyl ether, and 9.3 g of polyvinyl alcohol (manufactured by JAPANVAM&POVAL CO., LTD., degree of polymerization 300, saponification degree 85%) were successively added. The temperature was raised to 80 °C by heating, and stirring was continued at 80 °C until the polyvinyl alcohol was completely dissolved. Then, 1.793 g of boron trioxide was added, and stirring was continued at 80 °C for 1 hour. Then, it was cooled to below 40 °C, 0.01 g of SH30PA was added, and stirring was continued for 1 hour to obtain p-type impurity diffusion composition C.

[0226] Mixing Example 4

[0227] <Synthesis of Particles Containing Impurity Diffusion Component>

[0228] B2O3, SiO2, Al2O3, and CaO (all manufactured by High Purity Chemical Research Institute Co., Ltd.) were weighed in a molar ratio of 40 mol%, 45 mol%, 5 mol%, and 10 mol% for the composition of B2O3, SiO2, Al2O3, and CaSO4, respectively. After mixing with an agate mortar, it was placed in a platinum crucible and held at 1500 °C for 2 hours using a glass melting furnace. After that, it was rapidly cooled to obtain a glass block. After crushing it with an agate mortar, it was crushed using a planetary ball mill to obtain glass particles with a spherical particle shape, an average particle size of 0.35 μm, and a softening point of about 800 °C.

[0229] <Preparation of p-Type Impurity Diffusion Composition>

[0230] 10 g of the above glass particles, 6 g of ethyl cellulose, and 84 g of terpineol were mixed to form a paste to obtain p-type impurity diffusion composition D.

[0231] Mixing Example 5

[0232] <Preparation of p-Type Impurity Diffusion Composition>

[0233] 4.39 g of a GBL solution containing 40% trimethoxysilane, 1.47 g of boric acid, 12.55 g of GBL, and 300 ppm of BYK-333 relative to the total solution were thoroughly stirred until homogeneous to obtain p-type impurity diffusion composition E.

[0234] Mixing Example 6

[0235] <Synthesis of Polymer Solution of Silica Compound>

[0236] 183.25 g of KBM-13 (methyltrimethoxysilane), 266.75 g of KBM-103 (phenyltrimethoxysilane), and 403.36 g of GBL were placed in a 2000 mL three-necked flask. While stirring at 40°C, an aqueous formic acid solution prepared by dissolving 0.45 g of formic acid in 145.29 g of water was added over 30 minutes. After the addition was complete, the mixture was stirred at 40°C for 1 hour, then heated to 70°C and stirred for 30 minutes. Thereafter, the oil bath was heated to 115°C. One hour after the start of heating, the internal temperature of the solution reached 100°C, and then it was heated and stirred for 1 hour (internal temperature 100 - 110°C). The resulting solution was cooled using an ice bath to obtain a polymer solution of the silica compound.

[0237] <Preparation of p-Type Impurity Diffusion Composition>

[0238] 13.42 g of the polymer of the silica compound synthesized above, 1.31 g of boric acid, 11.63 g of polyvinyl alcohol with a saponification degree of 49% (manufactured by JAPAN VAM&POVAL CO., LTD.) (hereinafter referred to as polyvinyl alcohol (49)), 3.9 g of AEROSIL VPNKC130 (manufactured by NIPPON AEROSIL Co., Ltd.) as particulate silica, 24.64 g of GBL, 35.1 g of terpineol, and 10 g of water were mixed and thoroughly stirred until homogeneous to obtain p-type impurity diffusion composition F.

[0239] Mixing Example 7

[0240] The saponification degree of polyvinyl alcohol was made 70%, and p-type impurity diffusion composition G was obtained in the same manner as in Mixing Example 6 except for this.

[0241] Example 1

[0242] As a substrate, a semiconductor substrate made of n-type single crystal silicon with a side of 156 mm was prepared, and both surfaces were alkali-etched to remove the slice damage and natural oxide. At this time, countless concave and convex surfaces with a typical width of 40 to 100 μm and a depth of about 3 to 4 μm were formed on both sides of the semiconductor substrate, which was used as a coating substrate (sheet resistance value: 200Ω / □).

[0243] Here, the p-type impurity diffusion composition A is printed by screen printing. The printing pattern is a square of 4 cm×4 cm. Figure 3 The alignment was performed in the manner of configuration (screen printing machine (Micro-tec Co., Ltd. TM-750 model), screen mask (manufactured by SUS Co., Ltd., 400 mesh, line diameter 23 μm)).

[0244] After the p-type impurity diffusing composition was screen-printed, the substrate was heated in air on a hot plate at 140° C. for 5 minutes and then heated in an oven at 230° C. for 30 minutes to form a pattern having a thickness of about 1.5 μm.

[0245] Next, the patterned substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.) and maintained at 950°C for 30 minutes in an atmosphere of 19 L / min nitrogen and 0.6 L / min oxygen to form an impurity diffusion layer. In this state, the temperature in the furnace was lowered to 920°C, and nitrogen 19 L / min, oxygen 0.06 L / min, and boron tribromide (BBr3) bubbled with nitrogen 0.06 L / min were introduced to make the furnace an atmosphere containing impurity diffusion components, and impurity diffusion was performed in the portion where the pattern was not formed. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0246] Example 2

[0247] The same coating substrate as that in Example 1 was used as the coating substrate.

[0248] Here, a pattern having a thickness of about 1.5 μm was formed by the same method as in Example 1 using the p-type diffusion layer forming composition A.

[0249] Next, the patterned substrate was placed in an ion implantation apparatus and implanted with an energy of 10 keV and 2e 15 1 / cm 2 After that, the patterned substrate was placed in a diffusion furnace and maintained at 950°C for 30 minutes in an atmosphere of 19 L / min nitrogen and 0.6 L / min oxygen to form an impurity diffusion layer. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0250] Example 3

[0251] The same coating substrate as that in Example 1 was used as the coating substrate.

[0252] Here, a pattern having a thickness of about 1.5 μm was formed by the same method as in Example 1 using the p-type diffusion layer forming composition A.

[0253] Next, the patterned substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.), and nitrogen gas 19 L / min, oxygen gas 0.06 L / min, and boron tribromide (BBr3) bubbled with nitrogen gas 0.06 L / min were introduced to form an atmosphere containing impurity diffusion components in the furnace, and impurity diffusion was simultaneously performed in the patterned portion and the non-patterned portion at 950° C. for 30 minutes. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0254] Example 4

[0255] The same coating substrate as that in Example 1 was used as the coating substrate.

[0256] Here, a pattern having a thickness of about 1.5 μm was formed by the same method as in Example 1 using the p-type diffusion layer forming composition A.

[0257] The p-type impurity diffusion composition B was applied to the entire surface of the substrate by spin coating, and the rotation speed was adjusted so that the film thickness was 500 nm. The substrate was heated in air with a hot plate at 140° C. for 5 minutes.

[0258] The patterned substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.), and the impurities of the patterned portion and the non-patterned portion were diffused at 950°C for 30 minutes in an atmosphere of 19 L / min nitrogen and 0.6 L / min oxygen. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0259] Example 5

[0260] The same procedure as in Example 4 was carried out until the measurement of the sheet resistance value, except that the p-type impurity-diffusing composition B was changed to the p-type impurity-diffusing composition C.

[0261] Example 6

[0262] The same coating substrate as that in Example 1 was used as the coating substrate.

[0263] The substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.), and nitrogen gas at 19 L / min, oxygen gas at 0.06 L / min, and boron tribromide (BBr3) bubbled with nitrogen gas at 0.06 L / min were introduced to create an atmosphere in the furnace containing impurity diffusion components, and impurities were diffused over the entire surface of the substrate at 920°C for 30 minutes.

[0264] Next, a pattern having a thickness of about 1.5 μm was formed on the substrate using the p-type diffusion layer forming composition A by the same method as in Example 1.

[0265] Next, the patterned substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.) and maintained at 950°C for 30 minutes in an atmosphere of 19 L / min nitrogen and 0.6 L / min oxygen to form an impurity diffusion layer. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0266] Example 7

[0267] The same coating substrate as that in Example 1 was used as the coating substrate.

[0268] The substrate was placed in an ion implantation device and ion implanted at an energy of 10 keV and 2e 15 1 / cm 2 After that, the substrate was placed in a diffusion furnace and maintained at 920° C. for 30 minutes in a nitrogen atmosphere to form an impurity diffusion layer.

[0269] Next, a pattern having a thickness of about 1.5 μm was formed on the substrate using the p-type diffusion layer forming composition A by the same method as in Example 1.

[0270] Next, the patterned substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.) and maintained at 950°C for 30 minutes in an atmosphere of 19 L / min nitrogen and 0.6 L / min oxygen to form an impurity diffusion layer. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0271] Example 8

[0272] The same coating substrate as that in Example 1 was used as the coating substrate.

[0273] The p-type impurity diffusion composition B was applied to the entire surface of the substrate by spin coating, and the rotation speed was adjusted so that the film thickness was 500 nm. The substrate was heated in air with a hot plate at 140° C. for 5 minutes.

[0274] Next, a pattern having a thickness of about 1.5 μm was formed on the substrate using the p-type diffusion layer forming composition A by the same method as in Example 1.

[0275] Next, the patterned substrate was placed in a diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd.) and maintained at 950°C for 30 minutes in an atmosphere of 19 L / min nitrogen and 0.6 L / min oxygen to form an impurity diffusion layer. After the diffusion was completed, the substrate was immersed in a 5% hydrofluoric acid solution for 5 minutes, washed with water to remove the impurity diffusion film, and the sheet resistance value was measured.

[0276] Example 9

[0277] The same procedure as in Example 1 was carried out until the measurement of the sheet resistance value, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition F.

[0278] Example 10

[0279] The same procedure as in Example 2 was carried out until the measurement of the sheet resistance value, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition F.

[0280] Embodiment 11

[0281] The same procedure as in Example 3 was carried out until the measurement of the sheet resistance value, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition F.

[0282] Example 12

[0283] The same procedure as in Example 4 was carried out up to the measurement of the sheet resistance value, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition F.

[0284] Embodiment 13

[0285] The same procedure as in Example 5 was carried out up to the measurement of the sheet resistance value, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition F.

[0286] Embodiment 14

[0287] The same procedure as in Example 1 was carried out, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition G, up to the measurement of the sheet resistance value.

[0288] Comparative Example 1

[0289] The same procedure as in Example 1 was carried out, except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition D, up to the measurement of the sheet resistance value.

[0290] Comparative Example 2

[0291] The same procedure as in Example 1 was carried out except that the p-type impurity-diffusing composition A was changed to the p-type impurity-diffusing composition E, up to the measurement of the sheet resistance value.

[0292] Comparative Example 3

[0293] The measurement of the sheet resistance value was carried out in the same manner as in Example 1 except that the boron tribromide (BBr 3 ) was stopped and the furnace was not made into an atmosphere containing the impurity diffusing component.

[0294] Comparative Example 4

[0295] The same procedure as in Example 4 was carried out until the measurement of the sheet resistance value, except that the p-type impurity diffusing composition B was not applied on the substrate on which the pattern of the p-type diffusion layer forming composition A was formed.

[0296] The evaluation results are shown in Table 1.

[0297] [Table 1]

[0298]

Table 1

[0299]

[0300] Explanation of symbols

[0301] 1 Semiconductor substrate

[0302] 2 Ion implantation

[0303] 3 Gases containing impurity diffusion components

[0304] 4. Pattern of impurity diffusion composition film (b)

Claims

1. A method for manufacturing a semiconductor element, wherein the method comprises forming an impurity diffusion layer region of the same type on a semiconductor substrate with two or more different impurity concentrations, wherein: At least one level or more of the impurity diffusion layer region is formed by a method comprising the steps of: applying an impurity diffusion composition (a) to a semiconductor substrate to partially form an impurity diffusion composition film (b); and heating the impurity diffusion composition film (b) to diffuse impurities into the semiconductor substrate to form an impurity diffusion layer region (c). The impurity-diffusing composition (a) comprises: (a-1) a polymer of a silane compound represented by the following general formula (1); (a-2) impurity diffusion components; and (a-3) polyvinyl alcohol having a saponification degree of 20 mol% or more and less than 50 mol%, [Chemistry 1] In the general formula (1), R 1 and R 2 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 1 and R 2 are the same or different; l1 represents an integer from 1 to 10000.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The polymer of the silane compound is a polymer of the silane compound represented by the following general formula (2): [Chemistry 2] In the general formula (2), R 3 represents an aromatic group having 6 to 15 carbon atoms, plural R 3 Respectively the same or different; R 4 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 4 Respectively the same or different; R 5 and R 6 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an acyloxy group having 2 to 6 carbon atoms, and a plurality of R 5 and R 6 are the same or different; n1 and m1 represent integers from 1 to 9999, n1+m1 is an integer from 2 to 10000, and n1:m1=95:5 to 25:

75.

3. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: The method includes the step of using the impurity-diffusing composition film (b) as a mask to diffuse impurities into a portion where the impurity-diffusing composition film (b) is not formed.

4. The method for manufacturing a semiconductor device according to claim 3, wherein: The step of diffusing impurities into the portion where the impurity-diffusing composition film (b) is not formed is performed after heating the impurity-diffusing composition film (b) to diffuse the impurities into the semiconductor substrate to form the impurity diffusion layer region (c).

5. The method for manufacturing a semiconductor device according to claim 3, wherein: The step of diffusing the impurities into the portion where the impurity-diffusing composition film (b) is not formed is performed simultaneously with the step of heating the impurity-diffusing composition film (b) to diffuse the impurities into the semiconductor substrate.

6. The method for manufacturing a semiconductor element according to claim 4 or 5, wherein: The step of diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed is a step of implanting ions containing an impurity-diffusing component.

7. The method for manufacturing a semiconductor element according to claim 4 or 5, wherein: The step of diffusing impurities into the portion where the impurity-diffusing composition film (b) is not formed is a step of heating in an atmosphere containing an impurity-diffusing component.

8. The method for manufacturing a semiconductor device according to claim 4 or 5, wherein: The step of diffusing impurities into a portion where the impurity-diffusing composition film (b) is not formed is a step of applying an impurity-diffusing composition (d) onto a portion where the impurity-diffusing composition film (b) is not formed on a semiconductor substrate where the impurity-diffusing composition film (b) is formed, and heating the formed impurity-diffusing composition film (e).

9. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: After forming an impurity diffusion layer region (f) using at least one step selected from the group consisting of a step of implanting ions containing an impurity diffusion component into a semiconductor substrate, a step of heating in an atmosphere containing an impurity diffusion component, and a step of coating an impurity diffusion composition (d) on the entire surface and heating the formed impurity diffusion composition film (e), the method includes the following steps: a step of coating an impurity diffusion composition (a) to partially form an impurity diffusion composition film (b); and a step of heating the impurity diffusion composition film (b) to diffuse impurities into the semiconductor substrate to form an impurity diffusion layer region (c).

10. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: The method comprises the following steps: coating an impurity-diffusing composition (d) on the entire surface of a semiconductor substrate to form an impurity-diffusing composition film (e), coating an impurity-diffusing composition (a) thereon to partially form an impurity-diffusing composition film (b); and heating them simultaneously to diffuse impurities into the semiconductor substrate to simultaneously form impurity diffusion layer regions (c) and (f).

11. The method for manufacturing a semiconductor device according to claim 8, wherein: The impurity-diffusing composition (d) comprises: (d-1) a polymer of a silane compound; and (d-2) Impurity diffusion component.

12. The method for manufacturing a semiconductor device according to claim 9, wherein: The impurity-diffusing composition (d) comprises: (d-1) a polymer of a silane compound; and (d-2) Impurity diffusion component.

13. The method for manufacturing a semiconductor device according to claim 10, wherein: The impurity-diffusing composition (d) comprises: (d-1) a polymer of a silane compound; and (d-2) Impurity diffusion component.

14. The method for manufacturing a semiconductor device according to any one of claims 11 to 13, wherein: (d-1) The polymer of the silane compound is a polymer of the silane compound represented by the following general formula (3), [Chemistry 3] In the general formula (3), R 7 and R 8 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 7 and R 8 are the same or different; l2 represents an integer from 1 to 10000.

15. The method for manufacturing a semiconductor device according to any one of claims 11 to 13, wherein: (d-1) The polymer of the silane compound is a polymer of the silane compound represented by the following general formula (4), [Chemistry 4] In the general formula (4), R 9 represents an aromatic group having 6 to 15 carbon atoms, plural R 9 Respectively the same or different; R 10 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an acyloxy group having 2 to 6 carbon atoms, and an aryl group having 6 to 15 carbon atoms, and a plurality of R 10 Respectively the same or different; R 11 and R 12 represents any one of a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an acyloxy group having 2 to 6 carbon atoms, and a plurality of R 11 and R 12 are the same or different; n2 and m2 represent integers from 1 to 9999, n2+m2 is an integer from 2 to 10000, and n2:m2=95:5 to 25:

75.

16. The method for manufacturing a semiconductor device according to claim 8, wherein: The impurity-diffusing composition (d) comprises: (d-4) at least one resin selected from the group consisting of polyvinyl alcohol and polyether oxide; (d-5) impurity diffusion components; and (d-6) a solvent, 25% by mass or more of the entire solvent is water.

17. The method for manufacturing a semiconductor device according to claim 9, wherein: The impurity-diffusing composition (d) comprises: (d-4) at least one resin selected from the group consisting of polyvinyl alcohol and polyether oxide; (d-5) impurity diffusion components; and (d-6) a solvent, 25% by mass or more of the entire solvent is water.

18. The method for manufacturing a semiconductor device according to claim 10, wherein: The impurity-diffusing composition (d) comprises: (d-4) at least one resin selected from the group consisting of polyvinyl alcohol and polyether oxide; (d-5) impurity diffusion components; and (d-6) a solvent, 25% by mass or more of the entire solvent is water.

19. A method for manufacturing a solar cell, comprising the method for manufacturing a semiconductor element according to any one of claims 1 to 18.