Carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam

By using the carbon fiber bar and steel bar composite ICCP-SS system in seawater and sea sand concrete structures, the dual functions of FRP-steel composite bars are used to solve the problem of mechanical property degradation caused by steel bar corrosion in coastal environments and achieve higher mechanical properties. and durability.

CN113216512BActive Publication Date: 2024-10-15SHENZHEN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110539324.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-18
Publication Date
2024-10-15
Estimated Expiration
2041-05-18

AI Technical Summary

Technical Problem

Existing technologies cannot effectively solve the problem of mechanical property degradation caused by corrosion of reinforced concrete structures in coastal environments. ICCP technology can only inhibit corrosion but cannot restore the structural bearing capacity. SS technology cannot fundamentally solve the erosion of steel bars by harmful external and internal elements. .

Method used

The ICCP-SS seawater sea sand concrete beam composed of carbon fiber bars and steel bars is used, and the FRP-steel composite bars are used as the impressed current cathodic protection and structural reinforcement system. The carbon fiber bundles are wrapped around the FRP composite longitudinal bars, and the steel cages are connected to the FRP composite longitudinal bars. Carbon fiber bundles are used as anodes and steel bars are used as cathodes. The steel bars are protected by applied current and the structural bending reinforcement is provided through FRP longitudinal bars.

Benefits of technology

Prevent and delay corrosion of steel bars, improve the mechanical properties and durability of concrete structures, make up for the loss of structural bearing capacity caused by corrosion of steel bars, and significantly improve the performance of seawater and sand concrete structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113216512B_ABST
    Figure CN113216512B_ABST
Patent Text Reader

Abstract

The present invention discloses a carbon fiber bar and steel bar composite ICCP-SS seawater sea sand concrete beam, comprising: a seawater sea sand concrete layer; FRP-steel composite bars, embedded in the seawater sea sand concrete layer; the FRP-steel composite bars as an impressed current cathodic protection and structural reinforcement system; the FRP-steel composite bars include: FRP composite longitudinal bars; carbon fiber bundles, wrapped around the FRP composite longitudinal bars; steel cages, connected to the FRP composite longitudinal bars. On the one hand, the carbon fiber bundles are used as anodes and the steel bars are used as cathodes, and the steel bars in the seawater sea sand concrete composite plate are protected by impressed current, which can prevent and delay the corrosion of the steel bars; on the other hand, the FRP longitudinal bars can provide the function of structural bending reinforcement, which is used to compensate for and improve the loss of mechanical properties of the composite beam caused by steel bar corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of assembled structure engineering, and in particular to an ICCP-SS seawater and sea sand concrete beam composited with carbon fiber bars and steel bars. Background Art

[0002] The coastal areas are rich in seawater and sea sand resources. Using seawater and sea sand in concrete structures can effectively solve the problem of increasingly depleted river sand and freshwater resources and make full use of local resources. However, reinforced concrete structures using seawater and sea sand will have relatively serious corrosion problems, reducing the mechanical properties and durability of seawater and sea sand concrete structures.

[0003] Impressed Current Cathodic Protection (ICCP) is a technology that uses auxiliary anode materials to apply cathodic protection current to the steel bars inside the concrete structure, so that the potential shifts negatively to the corrosion-free area, thereby protecting the steel bars. It is recognized as an effective control method to prevent and delay steel corrosion; Structural Strengthening (SS) is a technology that uses structural reinforcement materials such as structural steel or fiber reinforced polymer (FRP) to jointly bear force and deformation with concrete structures, thereby improving or repairing the mechanical properties of the structure.

[0004] Among the existing technologies, although ICCP technology can inhibit the corrosion of steel bars in concrete structures in coastal environments, it cannot restore the deterioration of structural mechanical properties caused by steel bar corrosion; although SS technology can improve or restore the structural bearing capacity, it cannot fundamentally solve the continuous corrosion of steel bars by the external environment and internal harmful elements of concrete structures in coastal environments.

[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0006] The technical problem to be solved by the present invention is that, in view of the above-mentioned defects of the prior art, a carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam is provided, aiming to solve the problem of loss of structural bearing capacity due to steel bar corrosion in the prior art.

[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0008] A carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam, comprising:

[0009] Seawater and sea sand concrete layer;

[0010] FRP-steel composite bars are embedded in the seawater and sea sand concrete layer; the FRP-steel composite bars serve as an impressed current cathodic protection and structural reinforcement system;

[0011] The FRP-steel composite reinforcement comprises:

[0012] FRP composite longitudinal reinforcement;

[0013] A carbon fiber bundle is wound around the FRP composite longitudinal reinforcement;

[0014] A steel cage is connected with the FRP composite longitudinal reinforcement.

[0015] The carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam, wherein the steel cage comprises:

[0016] Longitudinal steel bars connected to the FRP composite longitudinal bars;

[0017] A plurality of stirrups are arranged on the longitudinal steel bars and arranged along the length direction of the longitudinal steel bars.

[0018] The carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam, wherein the longitudinal reinforcement is connected to the FRP composite longitudinal reinforcement through an insulating slot; the insulating slot includes:

[0019] A first sleeve, sleeved outside the longitudinal steel bar;

[0020] A second sleeve is sleeved outside the FRP composite longitudinal reinforcement;

[0021] A connecting rod, with two ends respectively connected to the first sleeve and the second sleeve.

[0022] The carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam, wherein the spacing between the first sleeve and the second sleeve is greater than 50 mm; and / or

[0023] The second sleeve is located at a position of the first sleeve toward the center of the stirrup.

[0024] The carbon fiber rib and steel bar composite ICCP-SS seawater and sea sand concrete beam, wherein the carbon fiber content in the carbon fiber bundle is 12K-50K.

[0025] The carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam, wherein the FRP composite longitudinal reinforcement is selected from one of glass fiber FRP composite longitudinal reinforcement, carbon fiber FRP composite longitudinal reinforcement, aramid fiber FRP composite longitudinal reinforcement, and basalt FRP composite longitudinal reinforcement.

[0026] The carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam, wherein the pitch of the carbon fiber bundle winding is greater than the diameter of the FRP composite longitudinal reinforcement; and / or

[0027] The carbon fiber bundle is bonded to the FRP composite longitudinal reinforcement by an epoxy resin adhesive.

[0028] A method for preparing a carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam, comprising the steps of:

[0029] Provide beam formwork, carbon fiber bundles, FRP composite longitudinal bars, steel cages and seawater sand concrete;

[0030] Winding the carbon fiber bundle on the FRP composite longitudinal reinforcement, and connecting the FRP composite longitudinal reinforcement and the steel cage to obtain FRP-steel composite reinforcement;

[0031] The FRP-steel composite reinforcement is placed in the beam formwork, and the seawater and sea sand concrete is poured in, and after curing treatment, a seawater and sea sand concrete layer is obtained;

[0032] The beam formwork is removed, and the carbon fiber bundle and the steel cage are connected by a power supply to protect the steel cage, thereby obtaining a carbon fiber bar and steel bar composite ICCP-SS seawater sand concrete beam.

[0033] The method for preparing the carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam, wherein the carbon fiber bundle is wound on the FRP composite longitudinal reinforcement, comprises:

[0034] Applying epoxy resin adhesive on the FRP composite longitudinal reinforcement, fixing one end of the carbon fiber bundle on the FRP composite longitudinal reinforcement with a binding tape, and winding the carbon fiber bundle until the other end of the carbon fiber bundle is bonded to the FRP composite longitudinal reinforcement;

[0035] The surface of the FRP composite longitudinal reinforcement wound around the carbon fiber bundle is subjected to sandblasting treatment.

[0036] The method for preparing the carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam, wherein the FRP-steel composite reinforcement is placed in the beam formwork, and the seawater sand concrete is poured in, and after curing treatment, a seawater sand concrete layer is obtained, comprising:

[0037] The FRP-steel composite reinforcement is placed in the beam formwork, and the seawater sand concrete is poured into the beam formwork and then smoothed by a layered pouring and vibrating method. A rough steel brush is used to roughen the concrete and the concrete is cured to obtain a seawater sand concrete layer.

[0038] Beneficial effects: On the one hand, the carbon fiber bundle is used as the anode and the steel bar is used as the cathode. The steel bars in the seawater and sea sand concrete composite slab are protected by an external current, which can prevent and delay the corrosion of the steel bars. On the other hand, the FRP longitudinal bars can provide structural bending reinforcement to compensate for and improve the loss of mechanical properties of the composite beam caused by steel bar corrosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a cross-sectional view of the seawater and sea sand concrete beam of the present invention.

[0040] Figure 2 It is a structural schematic diagram of the beam formwork and FRP-steel composite reinforcement in the present invention.

[0041] Figure 3 It is a structural schematic diagram of the card slot in the present invention.

[0042] Description of reference numerals:

[0043] 1. Seawater and sea sand concrete layer; 2. Stirrups; 3. Longitudinal reinforcement; 4. Insulation slots; 5. Carbon fiber bundles; 6. FRP composite longitudinal reinforcement; 7. Beam formwork. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0045] Please also see Figure 1-Figure 3 The present invention provides some embodiments of carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beams.

[0046] FRP has the advantages of light weight, high strength, corrosion resistance, fatigue resistance, etc. It is a widely used material in SS technology. At the same time, carbon fiber has excellent conductivity and stable chemical properties and can be used as an auxiliary anode in ICCP technology. Therefore, FRP and carbon fiber materials can be developed into a combined material with ICCP function and SS function.

[0047] like Figure 1-Figure 2 As shown, the carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam of the present invention comprises:

[0048] Seawater and sea sand concrete layer 1;

[0049] FRP-steel composite bars are embedded in the seawater and sea sand concrete layer 1; the FRP-steel composite bars serve as an impressed current cathodic protection and structural reinforcement system;

[0050] The FRP-steel composite reinforcement comprises:

[0051] FRP composite longitudinal reinforcement 6;

[0052] A carbon fiber bundle 5 is wound around the FRP composite longitudinal reinforcement 6;

[0053] The steel cage is connected to the FRP composite longitudinal reinforcement 6.

[0054] It is worth noting that in the prior art, when using seawater and sea sand, the seawater is usually first desalinated, the sea sand is purified, and then the desalinated seawater and purified sea sand are used to make concrete. In addition, rust inhibitors are added and the surface coating of the steel bars is applied to prevent chloride ion corrosion. In the present application, the seawater and sea sand concrete layer 1 refers to a concrete structure formed using undesalinated seawater and / or unpurified sea sand as raw materials. It should be noted that the undesalinated seawater and unpurified sea sand in the present application can be used directly as raw materials. For example, cement is added to unpurified sea sand and then undesalinated seawater is added to form seawater and sea sand concrete. Since the seawater and sea sand concrete layer 1 is made of undesalinated seawater and / or unpurified sea sand, harmful media such as chlorides and sulfates exist inside the seawater and sea sand concrete layer 1. It should be noted that when preparing carbon fiber bar and steel bar composite ICCP-SS seawater sand concrete beams, the present application needs to use a power supply to connect the carbon fiber bundle and the steel cage, and perform protective treatment on the steel cage to remove harmful media, thereby actively intervening in the corrosion of the steel cage in the seawater sand concrete layer 1 rich in harmful media. The present application utilizes the dual functions of structural reinforcement and cathodic protection of FRP-steel composite bars as an impressed current cathodic protection and structural reinforcement system, and applies it to carbon fiber bar and steel bar composite ICCP-SS seawater sand concrete beams. Even when the seawater sand concrete layer is rich in harmful media or the external environment is harsh, the steel bars can be adequately protected. The steel cage refers to a cage structure formed by tying steel bars.

[0055] On the one hand, the carbon fiber bundle 5 is used as the anode and the steel bar is used as the cathode to protect the steel bars in the seawater-sand concrete composite slab through an external current, which can prevent and delay the corrosion of the steel bars; on the other hand, the FRP longitudinal bars can provide structural bending reinforcement to compensate for and improve the loss of mechanical properties of the composite beam caused by steel bar corrosion, and have better mechanical properties and durability than traditional seawater-sand concrete structures.

[0056] In a preferred implementation of the embodiment of the present invention, Figure 1-Figure 2 As shown, the steel cage comprises:

[0057] Longitudinal steel bars 3, connected to the FRP composite longitudinal bars 6;

[0058] A plurality of stirrups 2 are provided on the longitudinal reinforcement 3 and arranged along the length direction of the longitudinal reinforcement 3 .

[0059] Specifically, the longitudinal steel bars 3 are arranged to extend along the length direction of the coastal sand concrete layer 1. The longitudinal steel bars 3 may be one or more. Figure 2 As shown, three longitudinal steel bars 3 are used. A plurality of stirrups 2 are arranged along the length direction of the longitudinal steel bars 3 , and the longitudinal steel bars 3 are located inside the stirrups 2 and connected to the stirrups 2 .

[0060] In a preferred implementation of the embodiment of the present invention, Figure 1-Figure 2 As shown, the longitudinal steel bar 3 is connected to the FRP composite longitudinal steel bar 6 through an insulating slot 4; the insulating slot 4 includes:

[0061] A first sleeve, sleeved outside the longitudinal steel bar 3;

[0062] A second sleeve, sleeved outside the FRP composite longitudinal reinforcement 6;

[0063] A connecting rod, with two ends respectively connected to the first sleeve and the second sleeve.

[0064] Specifically, the installation of the FRP composite longitudinal reinforcement 6 after being wound with carbon fiber needs to use a spacer or a slot made of insulating material to accurately fix the position of the FRP composite longitudinal reinforcement 6. There can be one or more FRP composite longitudinal reinforcements 6.

[0065] In a preferred implementation of the embodiment of the present invention, Figure 2-Figure 3 As shown, the distance between the first sleeve and the second sleeve is greater than 50 mm.

[0066] Specifically, the spacing between the FRP composite longitudinal reinforcement 6 and the stirrup 2 (or the longitudinal reinforcement 3) needs to be greater than 50 mm to prevent the carbon fiber bundle 5 from contacting the stirrup 2 (or the longitudinal reinforcement 3) and causing a short circuit when an external current is applied.

[0067] In a preferred implementation of the embodiment of the present invention, Figure 2-Figure 3 As shown, the second sleeve is located at a position of the first sleeve toward the center of the stirrup 2.

[0068] Specifically, the FRP composite longitudinal reinforcement 6 wrapped with carbon fiber is located above the longitudinal reinforcement 3 inside the reinforcement cage.

[0069] In a preferred implementation of the embodiment of the present invention, the carbon fiber content in the carbon fiber bundle 5 is 12K-50K.

[0070] Specifically, the carbon fiber content of the carbon fiber bundle 5 wound on the surface of the FRP bar can be selected from commonly used specifications on the market, such as 12K, 24K, 50K, etc., and needs to be adjusted according to actual needs.

[0071] In a preferred implementation of the embodiment of the present invention, the FRP composite longitudinal reinforcement 6 is selected from one of glass fiber FRP composite longitudinal reinforcement (GFRP), carbon fiber FRP composite longitudinal reinforcement (CFRP), aramid fiber FRP composite longitudinal reinforcement (AFRP), and basalt FRP composite longitudinal reinforcement.

[0072] Specifically, the FRP composite longitudinal reinforcement 6 can be various types of FRP composite longitudinal reinforcements currently available in the market.

[0073] In a preferred implementation of the embodiment of the present invention, Figure 2 As shown, the pitch of the winding of the carbon fiber bundle 5 is greater than the diameter of the FRP composite longitudinal reinforcement 6.

[0074] Specifically, when winding the carbon fiber bundle 5, the pitch needs to be greater than the diameter of the FRP composite longitudinal reinforcement 6 to avoid too few sandblasting areas, which would cause the FRP composite longitudinal reinforcement 6 after the carbon fiber winding to lose the bond with the subsequently poured seawater sand concrete.

[0075] In a preferred implementation of the embodiment of the present invention, the carbon fiber bundle 5 is bonded to the FRP composite longitudinal reinforcement 6 by an epoxy resin adhesive.

[0076] Specifically, the carbon fiber bundle 5 can be pasted on the FRP composite longitudinal reinforcement 6. When the epoxy resin adhesive is applied to the surface of the FRP composite longitudinal reinforcement 6, the amount of adhesive must be controlled to ensure that the surface fibers of the carbon fiber bundle 5 can be fully exposed when the carbon fiber bundle 5 is wound, so that it can fully contact with the seawater and sea sand concrete, thereby ensuring the effect of subsequent impressed current cathodic protection.

[0077] The present invention provides a surface-wound carbon fiber FRP bar and steel bar composite seawater and sea sand concrete beam, which has the following beneficial effects compared with the prior art:

[0078] The present invention utilizes seawater sand to replace increasingly depleted resources such as freshwater river sand, and fully utilizes the abundant seawater sand resources in coastal areas for the casting of prefabricated composite slabs of reinforced concrete structures, thereby reducing material transportation costs, greatly improving the utilization efficiency of seawater sand resources, playing a positive role in protecting the ecological environment, and having great social and economic benefits.

[0079] The present invention adopts an ICCP-SS system based on FRP bars and carbon fiber bundles. On the one hand, the carbon fiber bundle 5 is used as the anode and the steel bar is used as the cathode. The steel bars in the seawater and sea sand concrete composite plate are protected by an external current, which can prevent and delay the corrosion of the steel bars. On the other hand, the FRP longitudinal bars can provide structural bending reinforcement, which is used to compensate for and improve the loss of mechanical properties of the composite beam caused by steel bar corrosion. Compared with the traditional seawater and sea sand concrete structure, it has better mechanical properties and durability.

[0080] Based on the carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam described in any of the above embodiments, the present invention also provides a preferred embodiment of a method for preparing a carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam:

[0081] The method for preparing the carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam according to the embodiment of the present invention comprises the following steps:

[0082] Step S100, providing beam formwork, carbon fiber bundles, FRP composite longitudinal bars, steel cages and seawater sand concrete.

[0083] Specifically, according to the length and cross-sectional size of the seawater and sea sand concrete beam, the FRP composite longitudinal reinforcement 6 of corresponding length and designed quantity is cut.

[0084] For example, according to the length and cross-sectional dimensions of the seawater sand concrete beam, two CFRP longitudinal bars are cut, the length of which is the length of the composite beam plus the anchorage length at both ends, and the diameter of the CFRP bar is 10 mm.

[0085] Step S200, winding the carbon fiber bundle on the FRP composite longitudinal reinforcement, and connecting the FRP composite longitudinal reinforcement and the steel cage to obtain FRP-steel composite reinforcement.

[0086] Specifically, the carbon fiber bundle 5 is spirally wound around the FRP composite longitudinal reinforcement 6. Specifically, the carbon fiber bundle 5 is wound from one end of the FRP composite longitudinal reinforcement 6 to the other end of the FRP composite longitudinal reinforcement 6, and then the FRP composite longitudinal reinforcement 6 is connected to the steel cage to form the FRP-steel composite reinforcement. In order to facilitate the connection of the power supply, one end of the carbon fiber bundle 5 is connected to the power conductor and protected by a plastic sleeve to prevent damage during the pouring process.

[0087] Step S200 specifically includes:

[0088] Step S210, applying epoxy resin adhesive on the FRP composite longitudinal reinforcement, fixing one end of the carbon fiber bundle to the FRP composite longitudinal reinforcement with a binding tape, and winding the carbon fiber bundle until the other end of the carbon fiber bundle is bonded to the FRP composite longitudinal reinforcement.

[0089] Step S220, sandblasting the surface of the FRP composite longitudinal reinforcement wrapped around the carbon fiber bundle.

[0090] Specifically, the carbon fiber bundle 5 needs to be tied to one end of the FRP composite longitudinal reinforcement 6 using a non-metallic strap, such as a plastic strap, and after the tying is completed, it needs to be fixed with an epoxy resin adhesive. The surface of the FRP composite longitudinal reinforcement 6 wrapped with the carbon fiber bundle 5 is sandblasted at the location where the epoxy resin adhesive is exposed to increase the bonding force between the FRP composite longitudinal reinforcement 6 and the subsequently poured seawater sand concrete. After the carbon fiber bundle 5 is wrapped, the epoxy resin is cured for the standard curing time.

[0091] The steel cage includes longitudinal steel bars 3 and stirrups 2. The longitudinal steel bars 3 and stirrups 2 are tied and connected to form a steel cage, and then the prepared FRP composite longitudinal bars 6 are installed on the tied longitudinal steel bars 3. The FRP composite longitudinal bars 6 maintain a certain distance from the longitudinal steel bars 3 and stirrups 2 to form FRP-steel composite bars.

[0092] For example, the surface of the CFRP longitudinal reinforcement is coated with the prepared epoxy resin adhesive, the continuous 50K carbon fiber bundle 5 is tied to one end of the CFRP longitudinal reinforcement with a plastic strap, and is wound to the other end of the CFRP longitudinal reinforcement with a pitch of 20 mm, and the carbon fiber bundle 5 is bonded to the surface of the CFRP longitudinal reinforcement through the resin on the surface of the CFRP longitudinal reinforcement; the amount of resin needs to be controlled during the winding and pasting process so that the carbon fiber filaments on the outer surface of the carbon fiber bundle 5 are fully exposed; after the winding of the carbon fiber bundle 5 is completed, the surface of the CFRP longitudinal reinforcement covered with resin is sandblasted to ensure the bonding of the CFRP longitudinal reinforcement with the subsequent pouring of concrete; one end of the carbon fiber bundle 5 is connected to the power-carrying wire and protected with a plastic casing to prevent damage during the pouring process; the epoxy resin adhesive is cured for a specified time, generally 24 hours.

[0093] Step S300, placing the FRP-steel composite reinforcement into the beam formwork, and pouring the seawater and sea sand concrete, and obtaining the seawater and sea sand concrete layer 1 after curing.

[0094] Specifically, the FRP-steel composite reinforcement is placed in the beam formwork 7, and then the seawater and sea sand concrete is poured into the beam formwork 7. After the seawater and sea sand concrete is cured, the seawater and sea sand concrete layer 1 is obtained.

[0095] Specifically, step S300 includes:

[0096] Step S310, placing the FRP-steel composite reinforcement into the beam formwork, using a layered pouring and layered vibration method, pouring the seawater sand concrete into the beam formwork and then smoothing it, using a rough steel brush to roughen it and perform a curing treatment to obtain a seawater sand concrete layer.

[0097] Specifically, the FRP-steel composite reinforcement is placed into the beam formwork 7, and the position of the longitudinal reinforcement 3 and the FRP composite longitudinal reinforcement 6 are fixed by using plastic slots; the mixed seawater and sea sand concrete is poured onto the top surface of the beam formwork 7, and after pouring, the top surface of the beam formwork 7 is smoothed, roughened with a coarse steel brush before initial setting, and the formwork is removed after initial curing.

[0098] For example, the cut longitudinal steel bars 3 and the CFRP longitudinal bars wrapped with carbon fiber bundles 5 pass through four insulating slots 4 to form a two-layer steel bar arrangement, and the positions of the upper CFRP longitudinal bars and the lower longitudinal steel bars 3 are controlled by the plastic sleeves on the insulating slots 4; stirrups 2 are made, and the stirrups 2, the fixed upper CFRP longitudinal bars and the lower longitudinal steel bars 3 are tied into an FRP-steel composite reinforcement cage, which is placed in the beam formwork 7, and the thickness of the protective layer is controlled by the longitudinal reinforcement holes on the side forms of the pads and the beam formwork 7 at both ends.

[0099] Pour the mixed seawater and sea sand concrete to the top surface of the beam formwork 7. To ensure the pouring quality, the pouring method can be adopted. After pouring, the top surface of the composite beam is smoothed, and roughened with a coarse steel brush before initial setting. The formwork is removed after initial curing.

[0100] Step S400, dismantling the beam formwork, connecting the carbon fiber bundle and the steel cage with a power supply to protect the steel cage, and obtaining a carbon fiber bar and steel bar composite ICCP-SS seawater sand concrete beam.

[0101] Specifically, after the formwork is removed, a conducting wire is welded to the ends of the stirrups 2 and / or longitudinal reinforcement 3 of the exposed seawater sand concrete beam and connected in parallel to the cathode of the DC power supply; the conducting wire connected to the carbon fiber bundle 5 is connected in parallel to the anode of the DC power supply; the DC power supply is turned on and an intensity of 10 mA / m is applied. 2 The DC current is used to protect the steel cage and prevent corrosion of the steel cage.

[0102] For example, it is necessary to weld the powered wires at the ends of the exposed stirrups 2 and the steel longitudinal bars 3 and connect them in parallel to the cathode of the DC power supply; connect the powered wires connected to the carbon fiber bundles 5 in parallel to the anode of the DC power supply; turn on the DC power supply and apply an intensity of 10mA / m 2 The direct current can protect the steel bars and prevent them from corrosion.

[0103] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A carbon fiber reinforcement and steel bar composite ICCP-SS seawater sand concrete beam, characterized in that: include: Seawater and sea sand concrete layer; FRP-steel composite reinforcement, embedded in the seawater sand concrete layer; The FRP-steel composite reinforcement serves as an impressed current cathodic protection and structural reinforcement system; The FRP-steel composite reinforcement comprises: FRP composite longitudinal reinforcement; A carbon fiber bundle is wound around the FRP composite longitudinal reinforcement; A steel cage connected to the FRP composite longitudinal reinforcement; The steel cage comprises: Longitudinal steel bars connected to the FRP composite longitudinal bars; A plurality of stirrups are provided on the longitudinal steel bars and arranged along the length direction of the longitudinal steel bars; The longitudinal steel bar is connected to the FRP composite longitudinal steel bar through an insulating slot; the insulating slot includes: A first sleeve, sleeved outside the longitudinal steel bar; A second sleeve is sleeved outside the FRP composite longitudinal reinforcement; A connecting rod, two ends of which are respectively connected to the first sleeve and the second sleeve; The distance between the first sleeve and the second sleeve is greater than 50 mm; the distance between the FRP composite longitudinal reinforcement and the stirrup is greater than 50 mm; The second sleeve is located at a position of the first sleeve toward the center of the stirrup; The carbon fiber bundle is bonded to the FRP composite longitudinal reinforcement by an epoxy resin adhesive, and a sandblasting treatment is performed on the portion where the epoxy resin adhesive is exposed.

2. The carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam according to claim 1, characterized in that: The carbon fiber content in the carbon fiber bundle is 12K-50K.

3. The carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam according to claim 1, characterized in that: The FRP composite longitudinal reinforcement is selected from one of glass fiber FRP composite longitudinal reinforcement, carbon fiber FRP composite longitudinal reinforcement, aramid fiber FRP composite longitudinal reinforcement, and basalt FRP composite longitudinal reinforcement.

4. The carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam according to claim 1, characterized in that: The pitch of the carbon fiber bundle winding is greater than the diameter of the FRP composite longitudinal reinforcement.

5. A method for preparing a carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam as claimed in any one of claims 1 to 4, characterized in that: Includes steps: Provide beam formwork, carbon fiber bundles, FRP composite longitudinal bars, steel cages and seawater sand concrete; Winding the carbon fiber bundle on the FRP composite longitudinal reinforcement, and connecting the FRP composite longitudinal reinforcement and the steel cage to obtain FRP-steel composite reinforcement; The FRP-steel composite reinforcement is placed in the beam formwork, and the seawater and sea sand concrete is poured in, and after curing treatment, a seawater and sea sand concrete layer is obtained; The beam formwork is removed, and the carbon fiber bundle and the steel cage are connected by a power supply to protect the steel cage, thereby obtaining a carbon fiber reinforcement and steel reinforcement composite ICCP-SS seawater sand concrete beam; The step of winding the carbon fiber bundle on the FRP composite longitudinal reinforcement comprises: Applying epoxy resin adhesive on the FRP composite longitudinal reinforcement, fixing one end of the carbon fiber bundle on the FRP composite longitudinal reinforcement with a binding tape, and wrapping the carbon fiber bundle until the other end of the carbon fiber bundle is bonded to the FRP composite longitudinal reinforcement; The surface of the FRP composite longitudinal reinforcement wound around the carbon fiber bundle is subjected to sandblasting treatment.

6. The method for preparing the carbon fiber reinforcement and steel bar composite ICCP-SS seawater and sea sand concrete beam according to claim 5, characterized in that: The step of placing the FRP-steel composite reinforcement into the beam formwork and pouring the seawater-sand concrete into the beam formwork to obtain a seawater-sand concrete layer after curing, comprises: The FRP-steel composite reinforcement is placed in the beam formwork, and the seawater sand concrete is poured into the beam formwork and then smoothed by a layered pouring and vibrating method. A rough steel brush is used to roughen the concrete and the concrete is cured to obtain a seawater sand concrete layer.