Detector for electromagnetic radiation and method of making the same
By introducing anchoring structures and perovskite liquefaction and recrystallization technology into the electromagnetic radiation detector, the difficulty of bonding between the perovskite layer and the electrode layer was solved, achieving good adhesion and large-area manufacturing.
Patent Information
- Application Number
- CN202110147712.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-04
- Filing Date
- 2021-02-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-02-03
AI Technical Summary
In the prior art, it is difficult to bond the perovskite layer on different substrates, especially when the thickness is greater than 100 μm. This leads to adhesion problems between the pixelated electrode layer and the perovskite layer in the electromagnetic radiation detector, affecting the performance of the detector.
By introducing an anchoring structure, a layer containing at least one perovskite is connected to a pixelated electrode layer, achieving good adhesion by utilizing the combination of perovskite liquefaction and recrystallization.
It improves the adhesion between the perovskite layer and the electrode layer, solves the problem of difficult bonding in the detector, and is suitable for large-area manufacturing.
Smart Images

Figure CN113281802B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a detector for electromagnetic radiation, comprising a pixelated first electrode layer, a second electrode and a first layer comprising at least one first perovskite, the first layer being located between the pixelated first electrode layer and the second electrode, and to a method for producing a corresponding detector. Background Art
[0002] Digital X-ray detectors have many possible applications, for example in medical diagnostics, where they are often used in 20×20 cm 2 Up to 43×43cm 2 Current detectors are based on amorphous silicon (indirect conversion) and amorphous selenium (direct conversion).
[0003] In direct conversion, X-ray quanta excite particles, which leads to the formation of electron-hole pairs. After the application of an electric field, these electron-hole pairs migrate towards the electrodes, where they are detected. The direct conversion of X-ray radiation in selenium is usually carried out in the kV range in the blocking direction with the aid of precharged layers up to 1 mm thick. In contrast to detection with the aid of indirect converters, which can be produced more easily and more cheaply, direct conversion usually achieves improved resolution.
[0004] In indirect conversion, an X-ray quantum excites a scintillating material (e.g., CsI:Tl, thallium-doped cesium iodide; or terbium-doped gadolinium oxysulfide), which causes the formation of visible photons. The photons can then be made, for example, into a stacked photodetector array, made, for example, of amorphous silicon (a-Si) photodiodes, which are used to convert the photons into electrical charges. After applying an electric field, the electrical charges can be detected at the photodetector electrodes.
[0005] An alternative to the two mentioned X-ray radiation detector technologies based on inorganic semiconductors are hybrid organic detectors, which are usually made from a liquid phase or powder. This enables the realization of X-ray radiation detectors with a resolution of 43×43 cm 2 Or larger sizes can be simply manufactured. Usually, inorganic absorber materials, such as quantum dots or scintillator particles, such as gadolinium oxysulfide, are introduced into an organic matrix. Organic semiconductors can be easily applied to large surfaces from the liquid phase or powder, and optical crosstalk can be minimized by direct introduction of inorganic scintillator materials. Hybrid X-ray detectors do not exist on the market at present. Due to the isotropic light emission in the scintillator, indirect converters usually have poor resolution compared to direct converters.
[0006] There are already various approaches to improving adhesion and ensuring electrical contact (pixel by pixel) in multilayer systems for detectors.
[0007] In particular, direct conversion X-ray detectors are usually manufactured by growing active materials directly on a backplane, such as a-Se by PECVD (plasma assisted chemical vapor deposition) or by bump bonding the active material on a backplane, such as CdTe or CZT (cadmium zinc telluride). Both methods do not have adhesion problems, but are expensive and time consuming. In addition, the commonly used starting materials are also expensive and, in the case of crystalline materials, are limited to a maximum wafer size if docking is not used.
[0008] Standardized connection technologies used in the semiconductor industry, such as bump bonding, cannot usually be easily transferred to other detector applications, such as to X-ray detectors, due to the small pixel area (partially less than 50 μm) and the extremely large number of pixels (up to 4000×4000 pixels). Likewise, due to short circuits of individual pixels, partially non-"connected" pixels (dead pixels) and insufficient contact areas in the pixels, anisotropically conductive and adhesive materials replaced by conductive particles (e.g. silver particles), such as conductive adhesives or thin films ACF (Anisotropic Conductive Film) are not used.
[0009] Semiconductor perovskites have recently been mentioned as novel detector materials. Semiconductor perovskites are low-cost materials for photovoltaics (PV), lasers, LEDs, and X-ray detection, for example in H. Wei et al., “Sensitive X-ray detectors made of methylammonium lead tribromide perovskite single crystals,” Nature Photonics 10, 2016, pp. 333-339, doi: 10.1038 / nphoton.2016.41; S. Shrestha et al., “High-performance direct conversion X-ray detectors based on sintered hybrid lead triiodide perovskite wafers,” Nature Photonics 11, 2017, pp. 436-440, doi: 10.1038 / nphoton.2017.94; and S. Yakunin et al., “Detection of X-ray photons by solution-processed lead halide perovskites,” Nature Photonics 9, 2015, pp. 444-449, doi: 10.1038 / nphoton.2015.82. However, there are also adhesion problems for these materials.
[0010] For example, in EP 3474339 A1, it is mentioned that a relatively thin adhesion layer is applied for a solution to this. As described in EP 3474339 A1, an adhesion layer can be applied, which can improve adhesion by its chemical and mechanical properties. Polyethylene dioxythiophene: sorbitol (Pedot: Sorbitol) is a material that has been frequently published for this. However, this approach is developed for thin layers with a thickness of several microns or less, and usually reaches its limit in the case of higher layers (>10 μm).
[0011] However, for improved sensitivity, thick X-ray detection layers of more than 100 μm should be provided. However, by application from the liquid phase or vapor deposition, large amounts of solvent are released and the surface roughness is difficult to control. Complete degassing of the solvent is not only technically demanding, but also problematic in terms of health and the environment.
[0012] WO 2016 / 091600 A1 and WO 2016 / 091442 A1 propose to produce thick detection layers containing perovskite using a soft sintering method.
[0013] However, bonding of thick perovskite layers (>100 μm) on different substrates (e.g. glass, polymer films, metal films) or functional substrates (e.g. a-Si or indium gallium zinc oxide (IGZO) backplanes for thin-film transistor (TFT) arrays on glass or flexible substrates) is difficult due to, for example, poor adhesion of the polycrystalline perovskite layer on the substrate itself.
[0014] Another way is to mechanically anchor two layers or components. EP 2973688 B1, for example, relates to a sensor component, which includes a form coupling feature (groove) on one component and a matching counterpart (protruding element) on the other component. Here, the form coupling feature is especially composed of a recess with at least two parallel walls. By means of the key-lock principle, the sensor component is fixed in two spatial directions to prevent slipping. The method described in US 10453763 B2 is based on a similar principle. This involves a packaging structure of an electronic device, which also has a structure such as a wall. Auxiliary material is applied to this preset structure to increase the adhesion of the packaging structure relative to the substrate of the electronic device; the planar electronic contact of the individual pixels is not taken into account here.
[0015] Another method for improving the adhesion of the individual components of an electronic system is to sinter the adhesive layer: DE 10 2009 040 627 proposes a method in which a structured mask layer is applied to a semiconductor chip. The openings produced by photoablation or etching are filled with a mass containing conductive particles, and a carrier layer is subsequently placed thereon. The mass is compressed by sintering, thereby improving the adhesion to the carrier layer and the chip.
[0016] A possible solution is also to apply the structured pixel electrodes directly onto the absorber layer by means of physical vapor deposition (PVD) or chemical vapor deposition (CVD) and subsequent structuring methods (e.g. photolithography, laser ablation, etc.). Standard solutions for anisotropic conductive films (ACF) can be used here. However, due to chemical incompatibility with developers and solvents and the extremely long laser structuring times (also due to the high number of pixels), this method is not suitable for absorber layers made of perovskites.
[0017] Therefore, there is still insufficient adhesion between perovskite absorber layers, for example in X-ray and / or gamma-ray detectors, and the corresponding readout electronics of the detector, especially in the case of layers with a thickness in the range of 1 μm-3000 μm. In this context, it should be particularly noted that in the case of coatings, the corresponding adhesion-promoting layer should be conductive or semiconducting, but should not short-circuit the pixels of the pixelated detector electrode with one another, but should only "connect" the pixels to the detection layer. Summary of the invention
[0018] The inventors have found that good adhesion between a layer comprising at least one first perovskite and a pixelated first electrode can be achieved when the following structure is introduced, which improves the adhesion between the two. In particular, the inventors have found that in detectors for electromagnetic radiation, in particular in pixelated X-ray and / or gamma radiation detectors / gamma ray detectors, adhesion problems between a pixelated electrode layer and a detection layer (also called absorber layer) comprising at least one perovskite can be avoided in that the layer comprising at least one first perovskite is connected to the pixelated electrode layer by means of a structure serving as an anchoring structure. To this end, good adhesion of the at least one first perovskite or a layer comprising it to the structure and thus also to the pixelated electrode layer or even to the pixelated substrate can be achieved in particular by means of a combination of liquefaction and recrystallization of the perovskite.
[0019] In a first aspect, the invention relates to a detector for electromagnetic radiation, in particular an X-ray detector and / or a gamma-ray detector, comprising:
[0020] a pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels,
[0021] - a second electrode, and
[0022] a first layer comprising at least one first perovskite, said first layer being located between said pixelated first electrode layer and said second electrode,
[0023] It also includes the following structure, which is at least partially located between the pixelated first electrode layer and the second electrode, and is at least partially arranged between the individual electrode pixels of the pixelated first electrode layer, so that the structure is at least partially arranged in the middle space between the individual electrode pixels away from the first electrode layer in the direction of the second electrode, wherein a layer containing at least one first perovskite is at least partially introduced into the structure.
[0024] Furthermore, a method for producing a detector for electromagnetic radiation, in particular an X-ray detector and / or a gamma-ray detector, is disclosed, the method comprising:
[0025] - providing a pixelated first electrode layer, the pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels;
[0026] - applying a structure at least partially to the intermediate spaces of the pixelated first electrode layer, wherein the structure is applied in such a way that the structure is at least partially arranged facing away from the first electrode layer in the intermediate spaces between the individual electrode pixels;
[0027] - introducing into said structure a first layer comprising at least one first perovskite; and
[0028] - applying a second electrode to the structure and / or to the first layer comprising at least one first perovskite; or
[0029] - providing a structure wherein the structure has an intermediate space;
[0030] - introducing a plurality of electrode pixels between the intermediate spaces of the structure, wherein the electrode pixels do not fill the structure, thereby forming a pixelated first electrode layer;
[0031] - introducing into said structure a first layer comprising at least one first perovskite; and
[0032] - applying a second electrode to the structure and / or to the first layer comprising at least one first perovskite.
[0033] Further aspects of the invention can be derived from the detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The accompanying drawings are intended to illustrate embodiments of the invention and facilitate a further understanding thereof. In conjunction with the description, the embodiments serve to explain the concept and principle of the invention. Further embodiments and a number of advantages mentioned can be derived with reference to the drawings. The elements of the drawings are not necessarily shown in proportion to one another. Unless otherwise indicated, in the drawings, identical, functionally identical and identically functioning elements, features and components are each provided with the same reference numerals.
[0035] Figure 1 An exemplary X-ray detector according to the present invention is schematically shown.
[0036] Figures 2 to 11 Different exemplary structures are schematically shown which can be used in the detector according to the invention.
[0037] exist Figures 12 to 14 Schematically, one method is shown by way of example how a first layer can be applied.
[0038] Figures 15 to 18 An exemplary first layer in a detector according to the invention is shown schematically.
[0039] exist Figures 19 to 22 Schematically, it is shown by way of example how a second layer can be applied to a first layer.
[0040] from Figures 23 to 25 It is shown schematically by way of example how the second layer can be applied.
[0041] Figures 26 to 28 A further method according to the invention is schematically shown, in which a first layer and a second layer are applied.
[0042] exist Fig.29 XRD data of perovskite before and after recrystallization are shown in FIG. DETAILED DESCRIPTION
[0043] Therefore, unless defined otherwise, technical and scientific expressions used herein have the same meaning as they are commonly understood by one of ordinary skill in the art to which the present invention pertains.
[0044] Unless stated otherwise or clear from the context, quantity specifications within the scope of the present invention relate to % by weight.
[0045] A first aspect of the invention relates to a detector for electromagnetic radiation, in particular an X-ray detector and / or a gamma-ray detector, comprising:
[0046] a pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels,
[0047] - a second electrode, and
[0048] a first layer comprising at least one first perovskite, said first layer being located between said pixelated first electrode layer and said second electrode,
[0049] It also includes the following structure, which is at least partially located between the pixelated first electrode layer and the second electrode, and is at least partially arranged between the individual electrode pixels of the pixelated first electrode layer, so that the structure is at least partially arranged in the middle space between the individual pixel electrodes away from the first electrode layer in the direction of the second electrode, wherein a layer containing at least one first perovskite is at least partially introduced into the structure.
[0050] Introducing the first layer comprising at least one first perovskite into the structure means in this context in particular that the first layer is introduced into a region extending between the structures above the electrode pixel. Although in the case of at least partially porous structures with porous materials, in which case it is theoretically possible to introduce the layer into the structural material (which is not excluded here), by introducing means in particular that the first layer comprising at least one first perovskite is introduced into a region which is defined by the structure and is located between parts of the structure, such as walls, in a grid, etc.
[0051] In the detector according to the present invention, the pixelated first electrode layer is not particularly limited. The pixelated first electrode layer here has a plurality of (i.e. 2 or more, for example 3, 4, 5, 6, 7, 8, 9, 10, 100, 1000 or more) electrode pixels or pixels, which can be electrically contacted. Neither the pixel size nor the material of the electrode pixel is particularly limited, and the following electrode pixels can be used, which have been used in detectors for electromagnetic radiation, especially X-ray detectors and / or gamma ray detectors so far. For example, an electrode pixel with a spacing of 98 μm with square electrode pixels can be used as an electrode pixel, which defines the electrode pixel, wherein other pixel sizes are also feasible. The material of the electrode pixel is not particularly limited and can, for example, contain conductive metal oxides, conductive polymers and / or metals for detecting electrons and / or holes generated by perovskites. Where there is a substrate, the substrate can be a pixelated substrate, and the electrode pixels of the pixelated first electrode layer are located on the pixelated substrate.
[0052] The pixelated first electrode layer comprises a plurality of electrode pixels and intermediate spaces between the electrode pixels or pixels, which intermediate spaces can form a grid structure. The intermediate spaces or the grid structure can here comprise a non-conductive material, which is not particularly restricted and which can, for example, also be the material of the substrate, for example if material is removed from the substrate (for example by etching, etc.) and the electrode pixels are introduced into the substrate, and / or the electrode pixels of the first electrode layer can also be isolated from each other in other ways, for example by a gas such as air, etc., for example if the electrode pixels are applied to a substrate.
[0053] In the detector according to the invention, the pixelated first electrode layer (and the second electrode and / or the first layer and possibly further layers and / or the substrate etc.) can be planar and / or curved, so that a planar or also curved detector can be produced.
[0054] In addition, the second electrode is also not particularly limited. According to a specific embodiment, the second electrode contains a conductive metal oxide, a conductive polymer and / or a metal. In the detector according to the present invention, the first electrode and the second electrode (or the first electrode layer and the second electrode) can be suitably connected as an anode and / or a cathode. According to a specific embodiment, the second electrode is formed in a planar manner. According to a specific embodiment, the second electrode is at least partially transparent or completely transparent to the electromagnetic radiation to be detected, and the electromagnetic radiation is not particularly limited and can be, for example, X-rays (wavelength ≥ 10pm and <10nm) and / or gamma rays (wavelength <10pm). For example, the second electrode can contain indium tin oxide (ITO), aluminum zinc oxide (aluminum doped zinc oxide, AZO), antimony tin oxide (antimony tin oxide, ATO) and / or fluorine tin oxide (FTO), or be composed of them.
[0055] As long as the structure is at least partially or completely arranged between the individual pixels of the pixelated first electrode layer, the structure is also not particularly limited. For this purpose, the structure can also be partially located on the electrode pixels of the pixelated first electrode layer, as long as the structure is at least partially located between two electrode pixels of the pixelated first electrode layer, that is, for example, so that the structure is directly arranged in the intermediate space or grid structure between the electrode pixels or on the material of the intermediate space or grid structure in the intermediate space or grid structure of the pixelated first electrode layer (for example, formed by the non-electrode material and / or gas, such as air, of the pixelated first electrode layer), and / or arranged above the intermediate space, that is, it is also arranged on the material of the intermediate space between the electrode pixels, such as the grid structure or its material. For this purpose, the structure is arranged so that the structure extends at least away from the pixelated first electrode layer in the direction toward the second electrode, that is, a three-dimensional structure is formed, which is at least between the pixelated first electrode layer and the second electrode. It is not excluded here that some parts of the structure are also located in the pixelated first electrode layer, for example, in the intermediate space, in order to ensure better anchoring of the structure. The structure forms an anchoring structure for at least some parts of the first layer, whereby the first layer can be better connected to the pixelated first electrode layer. By means of the structure, which is applied in particular as an electrically insulating structure, it is possible to increase the anchoring surface for the first layer on the pixelated first electrode layer and possibly also on the substrate.
[0056] Thus, according to a particular embodiment, the structure is at least partially or completely located in an area defined by an intermediate space or a grid structure of the pixelated first electrode layer between individual electrode pixels, wherein the structure can also be located in the intermediate space or the grid structure. It is not excluded that the structure is also partially located on and / or above the electrode pixels of the pixelated first electrode layer. The structure is located between the electrode pixels so that a 3D shape or a three-dimensional body is formed at least above the intermediate space of the pixelated first electrode layer in the direction of the second electrode. The shape of this body of the structure is not particularly limited.
[0057] exist Figures 2 to 11 2 schematically shows an exemplary shape of the structure in the form of a two-dimensional cross-sectional view. It is also clear from these figures how the structure 1.4 can be arranged at least partially between the electrode pixels 1.5. Figure 2 and Figure 3 For example, the following structure is shown in FIG. 1 , which gradually widens or narrows toward the second electrode (not shown, but located above it). This shape is obtained, for example, by using different photoresists (negative or positive photoresists) during manufacturing. Figures 4 to 6 The shapes shown in FIG. 1 can also be obtained, for example, by using different photoresists and / or by other methods explained below. For example, the shapes shown in FIG. 1 can be produced by means of a lift-off resist (LOR). Figure 6 The shape shown in .
[0058] As in Figures 7 to 9 As can be seen in FIG. 1 , in addition to different shapes, the size of the structure 1.4 can also vary: an example is that the structure 1.4 fits exactly between the electrode pixels 1.5 ( Figure 7 In another example, the structure 1.4 is wider than the spacing between the electrode pixels 1.5, that is, the intermediate space ( Figure 8 ); Alternatively, the structure 1.4 can also be narrower than the spacing between the electrode pixels 1.5, wherein the structure 1.4 can also be introduced into the intermediate space (this is not excluded in other figures; Fig. 9 ). In addition, as in Fig.10 and 11 As schematically shown in FIG. 1 , some parts of the structure 1.4 can also be added additionally above the active surface of the electrode pixel 1.5. Thus, the adhesion of the first layer can be further enhanced, but by reducing the active surface of the electrode pixel 1.5 that can be used for detection, the detection can also be reduced.
[0059] In addition, different shapes of the structure can also be obtained in other ways, for example by selective etching and / or laser ablation of the substrate and subsequently introducing electrode pixels into the etched and / or ablated areas of the substrate, wherein the material of the pixelated first electrode layer and the intermediate space of the structure can correspond to the material of the substrate, and / or by 3D printing. In this case, it is also feasible to use different polymers, ceramics, etc. as materials for the structure. Corresponding methods for selective etching are known, for example, from JD Zahn et al., "A direct plasmaetch approach to high aspect ratio polymer micromachining with applications in biomems and CMOS-mems", Technical Digest, MEMS 2002 IEEE International Conference, 15th IEEE International Conference on Microelectromechanical Systems, DOI: 10.1109 / MEMSYS.2002.984223. Exemplary methods for laser ablation are described, for example, in V. N. Tokarev et al., "High-aspect-ratio microdrilling of polymers with UV laser ablation: experiment with analytical model", Appl. Phys. A, 2002, DOI: 10.1007 / s00339-002-1511-8. Methods for 3D printing are known, for example, from A. Kain et al., "High aspect ratio-and 3D-printing of freestanding sophisticated structures", Procedie Chemistry 1, 2009, 750-753, DOI: 10.1016 / j.proche.2009.07.187.
[0060] The size of the structure is also not particularly limited. However, preferred is a structure having a height of 0.5 μm to 1500 μm, preferably 1 to 1000 μm, more preferably 2 μm to 500 μm, more preferably 3 μm to 300 μm, still more preferably 5 μm to 100 μm, still more preferably 7 μm to 70 μm, and especially 10 μm to 50 μm from the surface of the pixelated first electrode layer. Structures with a high aspect ratio (ratio of height to width) are also preferred, in particular if the structure extends as a "grid" and / or "wall" away from the surface of the pixelated first electrode layer, wherein the width of the wall and / or the width of the lateral struts of the grid can be, for example, 0.5 μm to 80 μm, preferably 1 to 50 μm, more preferably 2 μm to 35 μm, even more preferably 3 μm to 25 μm, even more preferably 4 μm to 15 μm, in particular 5 μm to 10 μm, wherein the width can be measured, for example, directly on the surface of the pixelated first electrode layer, in particular in the case of tapering or widening structures or otherwise irregularly shaped structures. It is also not excluded that the electrode pixels are filled into the structure during production, i.e. only after the structure has been produced. In this case, it is also possible to achieve higher aspect ratios. In the case where the structure is also located in the intermediate space, the electrode pixels are located almost in the structure, so that here the pixelated first electrode layer can also be formed by parts of the structure in the region of the intermediate space of the first pixelated electrode layer (here, the pixelated first electrode layer is then understood to be a layer having the same height as the height of the electrode pixels, which layer is imaginarily removed from the detector, wherein the material of the structure is then located between the electrode pixels and thus fills the intermediate space between the electrode pixels). Here, as in other cases also in the pixelated first electrode layer, the intermediate space has a height that corresponds to the height of the electrode pixels (also called pixel electrodes). The electrode pixels can here have a filling factor of the structure (i.e. in the region of the structure that is not filled with the material of the structure), which filling factor is, for example, up to 90%, but preferably <50%, preferably <10%, and more preferably <2%.
[0061] For example, electrode pixel sizes or pitches of 150 μm or more, structure widths of 50 μm or less, and / or structure heights of up to 1250 μm are feasible.
[0062] The material of the structure is likewise not particularly restricted, but is preferably electrically insulating in order to avoid short circuits between individual electrode pixels. The material of the structure can also be related to the manufacture of the structure itself. As mentioned above, the material of the structure can also correspond to the material of the intermediate space and possibly also to the material of the substrate, but can also be different, for example when applying a material or applying a resist in 3D printing.
[0063] Thus, for example, the structure can be produced by applying a resist, such as a photoresist, which can be structured appropriately by means of a model and / or a mask and can also be applied multiple times if necessary. The resist, such as a photoresist, is not particularly restricted. By appropriately selecting a resist, such as a photoresist, the adhesion of the first layer, and in particular the at least one first perovskite, to the structure can also be influenced. If the material is at least partially liquefied in the method according to the invention for recrystallization, this also includes the wetting behavior of the material of the first layer, in particular the at least one first perovskite. As mentioned above, the corresponding contents also apply to other materials in other manufacturing methods.
[0064] The different photoresists are not particularly limited and can be, for example, positive and negative or other structurable materials. Examples of positive photoresists or photoresists are, for example, AZ 10XT, AZ 12XT, AZ 40XT, AZ 4533, AZ 4562, AZ 9245, AZ 9260, AS IPS 6050, AZ P4110, AZ P4260, AZ P4903 and PL 177 from Microchemicals, Inc., and examples of negative photoresists are, for example, AZ 125nXT, AZ 125nXT (115CPS), AZ 15nXT (450CPS), AZ nLof 2020, AZ nLof 2035, AZ nLof 2070 and AZ nLof 5510 from Microchemicals, Inc. Other examples of photoresists and methods for structuring them are mentioned in "Thick-layer resists for surface micromachining" by B. Loechel, J. Micromech. Microeng, 10, 2000, 108-115. SU-8 is mentioned as another example of a photoresist, for example, in "SU-8: a photoresist for high-aspect-ratio and 3D submicron lithography" by A. del Campo and C. Greiner, J. Microchem. Microeng. 17, 2007, R81-R95.
[0065] The first layer comprising at least one first perovskite is likewise not particularly limited. The amount of the first perovskite in the first layer is also not particularly limited. According to a specific embodiment, the first layer comprises at least one first perovskite, the amount of the first perovskite being ≥30 wt. %, ≥50 wt. % or ≥70 wt. %, based on the first layer, or the first layer is substantially composed of the first perovskite (based on the first layer, for example, ≥90 wt. %, ≥95 wt. % or ≥99 wt. %); or the first layer is even composed of at least one first perovskite.
[0066] In the first layer, the at least one first perovskite is not particularly limited and can include one perovskite or multiple perovskites, such as 2, 3, 4, 5 or more perovskites. According to a specific embodiment, the first layer comprises one perovskite.
[0067] The first perovskite is not particularly limited. For example, organic-inorganic perovskites and pure inorganic perovskites can be used, which have an ABX3 structure, which has one or more cations (A + ), one or more B + Cation and one or more halides X - , which are not particularly limited. According to a specific embodiment, examples of suitable perovskites as the first perovskite are MAPbI3 (CH3NH3PbI3), MAPbBr3 (CH3NH3PbBr3), FAPbI3 (HC(NH2)2PbI3), MAPbICl2 (CH3NH3PbICl2), FAPbBr3 (HC(NH2)2PbBr3), EAPbI3 (CH3CH2NH3PbI3), PAPbI3 (CH3CH2CH2NH3PbI3), BA2PbI4 ((CH3CH2CH2CH2NH3)2Pb I4), PMA2PbI4 ((C6H5CH2NH3)2PbI4), PEA2PbI4 ((C6H5CH2CH2NH3)2PbI4), EAPbBr3 (CH3CH2NH3PbBr3), PAPbBr3 (CH3CH2CH2NH3PbBr3); their mixed halides; inorganic-organic perovskites with a mixture of A cations and halides X (X = Cl, I and / or Br), such as MAFAPbX3 (MA = CH3NH3, FA = HC(NH2)2), MAGAPbX3 (GA = guanidinium salt) , BAPAPbX3 (BA=CH3CH2CH2CH2NH3, PA=CH3CH2CH2NH3); organic halogenated mixtures in which the halogens are partially substituted by other halogens (e.g., halides having the formula I3-xClx or Br3-xClx, etc., such as MAPbI3-xClx or CH3NH3PbBr3-xClx); organic and / or organic-inorganic perovskites in which Pb is at least partially or even completely substituted by Sn, Cu, Ni, Bi, Co, Fe, Mn, Cr, Cd, Ge and / or Yb, and / or mixtures thereof; inorganic Perovskites and mixtures thereof, such as CsPbX3, wherein X=Cl, Br and / or I, and mixtures thereof, Cs3Bi2X9, wherein X=Cl, Br and / or I, and mixtures thereof, Cs3Sb2X, wherein X=Cl, Br and / or I, and mixtures thereof, Cs2AgBiX6, wherein X=Cl, Br and / or I, and mixtures thereof, Rb3Bi2X9, wherein X=Cl, Br and / or I, and mixtures thereof, Rb3Sb2X9, wherein X=Cl, Br and / or I, and mixtures thereof, CsSnI3; etc., and mixtures of the perovskites.
[0068] The layer thickness of the first layer is not particularly limited and can be less than or greater than the height of the structure on which the first layer is applied and introduced into the structure. In the case where the layer thickness is less than the height of the structure, the first layer is completely introduced into the structure and the individual parts of the first layer are separated from each other by the structure. The first layer can, for example, have a thickness of 0.5 μm to 1500 μm, preferably 1 μm to 1000 μm, more preferably 3 μm to 300 μm, even more preferably 4 μm to 200 μm, in particular 5 μm to 100 μm, more preferably 7 μm to 70 μm, even more preferably 10 μm to 50 μm.
[0069] According to a specific embodiment, the first layer is used for physical contact between the first and second electrodes, optionally with the aid of further layers, and optionally also as a detection layer in which electron-hole pairs are generated, so that, for example, no further detection layer is present. For this purpose, the detection layer is also introduced into the structure. By means of the structure, it is possible to achieve improved adhesion of the first layer containing at least one first perovskite, in particular the first perovskite, on the pixelated first electrode or, optionally, on other layers included.
[0070] A first layer comprising at least one first perovskite is at least partially introduced into the structure. In particular, according to a specific embodiment, the first layer contacts an electrode pixel of the pixelated first electrode layer or possibly another introduced layer, which can thus come into indirect contact with the pixelated first electrode layer.
[0071] The introduction of the first layer into the structure is not particularly limited, and the first layer can be introduced so that the first layer only partially fills the structure, the first layer can be introduced so that the first layer just fills the structure, i.e. is flush with the upper edge or the highest point of the structure, or the first layer can be introduced so that the first layer exceeds the structure, i.e. fills the structure and also partially or completely covers the structure. As described above, the form of the introduction, i.e. the filling in the case of incomplete filling, depends on the material of the structure.
[0072] Different examples of this different filling are given in Figures 15 to 18 . Here, an electrode pixel 3.3 is shown with a structure 3.2 and a first layer 3.6, which comprises, for example, a recrystallized first perovskite, as explained below. In a variant, the first layer 3.6 has a higher height than the structure 3.2, as shown in Fig.15 As shown in Fig.16 Another variant shown in FIG. 3 has a first layer 3.6 that is smaller in height than the structure 3.2. In addition, the first layer 3.6 can have a positive curvature. ( Fig.17 ) or negative curvature, such as in Fig.18 This depends, for example, on the wetting behavior (hydrophobic, hydrophilic) of the structure and / or of the pixelated first electrode layer, for example the electrode pixels.
[0073] According to a particular embodiment, the at least one first perovskite in the first layer comprising the at least one first perovskite is at least partially recrystallized, and in particular recrystallized, thereby making it possible to better connect the first layer to the structure.
[0074] The recrystallization is not particularly restricted here. In particular, the recrystallized first perovskite is different from the non-recrystallized first perovskite because the crystal structure changes during recrystallization. Accordingly, a corresponding first layer (also referred to herein as a recrystallized layer) with an at least partially or completely recrystallized perovskite can be easily distinguished from another layer, for example a second layer (also referred to herein as an absorber layer), with the same perovskite, because these layers have different morphologies, which can be easily detected by means of an X-ray electron microscope (REM) or a transmission electron microscope (TEM) based on images, in which the perovskite has not been recrystallized. The X-ray diffraction (XRD) spectra of the layers also differ.
[0075] Recrystallization can be carried out in different ways and methods, for example by melting with methylamine gas, in particular in the case of perovskites containing methylammonium ions, by pressure and / or temperature melting, wherein the method can be adapted to the perovskite used. For example, the first perovskite contains alkylammonium ions, in particular with 1 to 4 C atoms, more preferably methylammonium ions, and the treatment for producing the first layer is carried out with the aid of a gas containing methylamine, in particular with the aid of methylamine gas.
[0076] The treatment of perovskites containing methylammonium ions with the aid of methylamine (MA) gas has been published by Li et al. in 2017 (Li, C., S. Pang, H. Xu and G. Cui, Methylamine gas based synthesis and healing process toward upscaling of perovskite solar cells: Progress and perspective, Solar RRL, 1 (9), 1700076 (2017)). In their paper, they describe the liquefaction of a previously solid perovskite layer after the action of MA gas, and the subsequent recrystallization accompanied by a change in morphology once the MA gas is no longer contained in the atmosphere. Patent EP 3304611 B1 utilizes this phenomenon in order to prepare perovskites from precursors (including metal halides) applied to two different surfaces. In CN 10209088003 A, a process is described in which a single-crystalline perovskite powder is applied to a mesoporous layer, for example titanium oxide, and liquefied with the aid of MA gas. The perovskite enters the pores as a liquid intermediate phase and recrystallizes there.
[0077] In particular, treatment with MA gas is preferred, since the MA gas is technically easy to handle and only small amounts of MA gas are required (for example, at a pressure of 10 -6 mbar to 10 bar in a chamber with negative pressure, for example in a chamber with a volume of 1 L (for example 0.25 g of MA gas at a pressure of 200 mbar), which saves costs.
[0078] The first layer can also be applied and recrystallized multiple times layer by layer. The first layer containing at least one first liquefied and recrystallized perovskite can be used here in particular as an adhesion promoter between the pixelated first electrode layer or other layers optionally applied thereon, such as an electron conductor or hole conductor layer and a possible additional second or third layer, wherein the second layer or the third layer is used here as a thick absorber layer, for example, in the case of a second layer containing at least one second perovskite, as a thick perovskite absorber layer. Here, the structure is indirectly used to expand the anchoring surface for the final bonding of the second and / or third layer, wherein the second and / or third layer is generally better attached to the first layer than to the pixelated first electrode layer. By this bonding, it is particularly easy to produce a critical absorber layer thickness, which is particularly necessary in X-ray and / or gamma ray detectors. A layer-by-layer construction is feasible, wherein here, a separate second layer and / or third layer that can be manufactured in a separate process, for example by rolling, sintering, etc., can be applied, for example, with a larger layer thickness.
[0079] According to a particular embodiment, the first layer comprising at least one first perovskite at least fills the structure. This then enables improved bonding to further layers, such as the second or third layer or the second electrode, an optional electron-conducting layer or a hole-conducting layer, etc.
[0080] According to a particular embodiment, the detector for electromagnetic radiation according to the invention further comprises a second layer comprising at least one second perovskite, said second layer being located between the first layer comprising at least one first perovskite and said second electrode,
[0081] And / or further comprising a third layer comprising at least one scintillator, wherein the third layer is located between the first layer comprising at least one first perovskite and the second electrode.
[0082] According to a particular embodiment, the detector for electromagnetic radiation according to the invention further comprises a second layer comprising at least one second perovskite, said second layer being situated between said first layer comprising at least one first perovskite and said second electrode.
[0083] The second layer comprising at least one second perovskite is not particularly limited. The amount of the second perovskite in the second layer is also not particularly limited. According to a specific embodiment, the second layer comprises at least one second perovskite, the amount of the second perovskite is ≥30%, ≥50% or ≥70% based on the second layer, or the second layer is essentially composed of the second perovskite (based on the second layer, for example, ≥90% by weight, ≥95% by weight or ≥99% by weight); or the second layer even includes at least one second perovskite.
[0084] The second layer is in particular an absorbent layer for electromagnetic radiation. According to a specific embodiment, the second layer has a thickness (in the direction between the pixelated first electrode layer and the second electrode) of 5 μm to 5000 μm, preferably 10 μm to 3000 μm, more preferably 50 μm to 2000 μm, and even more preferably 100 μm to 1500 μm. The second layer can be manufactured as a separate layer, for example as a separately manufactured perovskite layer, and can be independent and non-independent, i.e., for example, during manufacture it is also in contact with the second electrode or an optional electron-conducting layer or hole-conducting layer, for example with an ITO or FTO electrode, wherein the second electrode can, for example, also be located on a transparent surface layer, such as glass.
[0085] With regard to the connection, the composition of the second layer does not have to correspond to the composition of the first layer, but can correspond to the composition of the first layer. In particular, the at least one first perovskite and the at least one second perovskite can be identical or different. According to a particular embodiment, the at least one first perovskite corresponds to the at least one second perovskite. Losses during detection, for example losses with respect to the read signal or due to thermal stresses caused by process treatments, etc., can thus be avoided.
[0086] According to a particular embodiment, the second layer is in contact with the first layer and / or the structure, and in particular with the first layer.By using perovskites in both layers, good adhesion can be achieved.
[0087] According to a particular embodiment, the detector for electromagnetic radiation according to the invention further comprises a third layer comprising at least one scintillator, said third layer being situated between the first layer comprising at least one first perovskite and the second electrode.
[0088] The third layer is not particularly limited here. According to a specific embodiment, the third layer has a thickness (in the direction between the pixelated first electrode layer and the second electrode) of 5 μm to 5000 μm, preferably 10 μm to 3000 μm, more preferably 50 μm to 2000 μm, and even more preferably 100 μm to 1500 μm. The third layer can be manufactured as a separate layer, for example as a separately manufactured scintillator layer, and can be independent and non-independent, i.e., for example, during manufacturing, it is also in contact with the second electrode or an optional electron conduction layer or hole conduction layer, for example, in contact with an ITO or FTO electrode, wherein the second electrode can, for example, also be located on a transparent surface layer, such as glass.
[0089] According to a particular embodiment, said third layer is in contact with said first layer and / or said structure, and in particular with said first layer.
[0090] In an embodiment having a first layer and a third layer, the third layer is used in particular as a detection layer for high-energy radiation, such as X-ray radiation and / or gamma radiation, and the first layer is used for indirect detection by conversion of photons generated in the third layer.
[0091] The scintillator of the third layer is not particularly limited. For example, CsI:Tl, thallium-doped cesium iodide, or terbium-doped gadolinium oxysulfide, barium fluoride (BaF2), bismuth germanate (BGO), beryllium fluoride (BeF3), quantum dots, scintillating perovskite nanocrystals, etc. are suitable for use as scintillators.
[0092] According to a particular embodiment, a second layer comprising at least one second perovskite is included, wherein the at least one second perovskite is at least partially not recrystallized. Recrystallization is not required for the second layer, since the second layer can be manufactured in a simpler manner, for example by sintering or rolling.
[0093] According to a particular embodiment, the detector for electromagnetic radiation according to the invention further comprises an electron-conducting layer and / or a hole-conducting layer between the pixelated first electrode layer and the second electrode. A plurality of electron-conducting layers and / or hole-conducting layers can also be included in the detector.
[0094] Here, the electron-conducting layer and / or hole-conducting layer is not particularly restricted, and in the detector according to the invention, only one electron-conducting layer, only one hole-conducting layer or an electron- and hole-conducting layer can be present. The electron-conducting layer and / or the hole-conducting layer represent here an intermediate layer, which is also called an interlayer. An interlayer is correspondingly an intermediate layer, which acts as an electron transport (or hole blocking (HBL)) layer, i.e. as an electron-conducting layer, or as a hole transport (or electron blocking (EBL)) layer, i.e. as a hole-conducting layer.
[0095] The material for such an electron conductive and / or hole conductive layer is not particularly limited, and materials used in a commonly used electron conductive layer and / or hole conductive layer can be used.
[0096] Exemplary electron-conducting layers (HBL) can, for example, comprise the following materials, for example, with ≥30 wt. %, ≥50 wt. % or ≥70 wt. %, based on the electron-conducting layer; the electron-conducting layer consists essentially of these materials (for example, ≥90 wt. %, ≥95 wt. % or ≥99 wt. %, based on the electron-conducting layer); or even consists of these materials (wherein the following list is non-exclusive and also includes mixtures and isomeric mixtures of the materials mentioned, for example, binary, ternary, quaternary mixtures, etc.): fullerene derivatives, such as C60 PCBM ([6,6]-phenyl C61 butyric acid methyl ester), C70 PCBM ([6,6]-phenyl C71 butyric acid methyl ester), bis-C60 PCBM (bis-[6,6]-phenyl C61 butyric acid methyl ester), C60oQDM (o-quinodimethane C60 monoadduct), bis-C60-OQDM (o-quinodimethane C60 bisadduct), ICMA (indene C60 monoadduct, ICBA (indene C60 bisadduct), fullerol (C60(OH)44)); other acceptors including polymers and small molecules, such as compounds based on indacene and dithiophene (Dithienoindacen-basierte Verbindungen), such as: 3,9-bis(2-methylene-(3-(1,1-dicyanomethylidene)-indanone))-5,5,11,11-tetra(4-hexylphenyl)-dithieno[2,3-d:2',3'-d']-s-indaceno[1,2-b:5,6-b']dithiophene)(ITIC), IT-M(ITIC-M; 3,9-bis(2-methylene-((3-(1,1-dicyanomethylidene)-6,7-methyl)-indanone))-5,5,11,11-tetra(4-hexylphenyl)-dithieno[2,3-d:2',3'-d']-s-indaceno[1,2-b:5,6-b']dithiophene), IT-DM(ITIC-DM; 3,9-bis(2-methylene-((3-(1,1-dicyanomethylene)-6,7-dimethyl)-indanone))-5,5,11,11-tetrakis(4-hexylphenyl)-dithieno[2,3-d:2',3'-d']-s-indacen[1,2-b:5,6-b']dithiophene) and IDTBR((5Z,5'Z)-5,5'-((7 ,7'-(4,4,9,9-tetraoctyl-4,9-dihydro-s-indacene[1,2-b:5,6-b']dithiophene-2,7-diyl)bis(benzo[c][1,2,5]thiadiazole-7,4-diyl))bis(methylidene))bis(3-ethylthiazolidine-2,4-dione)); compounds based on perylene imide, such as TPB (tert-butylpyridine, C9H 13N), SdiPDI-Se (a perylene imide derivative modified by inserting a selenene unit into the bay position), NIDCS-HO ((2E,2'E)-3,3'-(2,5-bis(hexyloxy)-1,4-phenylene)bis(2-(5-(4-(N-(2-ethylhexyl)-1,8-naphthalimido)-thiophen-2-yl)acrylonitrile)); compounds based on diketopyrrolopyrroles, such as DPP6 (dipeptidyl aminopeptidase-like protein 6), 6,6'-(benzo[c][1,2,5]thiadione oxadiazole-4,7-diylbis([2,2'-bithiophene]-5',5-diyl))bis(2,5-bis(2-ethylhexyl)-3-(thiophene-2-yl)-2,5-dihydropyrrolo[3,4-c]pyrrole-1,4-dione)(DTDfBT(DPP)2), 6,6',6",6"'-(9,9'-spirobis[fluorene]-2,2',7,7'-tetrayltetra(thiophene-5,2-diyl))tetra(2,5-bis(2-ethylhexyl)-3-(5 -phenylthiophene-2-yl)-2,5-dihydropyrrolo[3,4-c]pyrrole-1,4-dione)(SF(DPPB)4); PFN(poly[(9,9-bis(3'-(N,N-dimethylamino)-propyl)-2,7-fluorene)-alt-2,7-(9,9-dioctylfluorene)]), PFN-OX(poly[9,9-bis(60-(N,N-diethylamino)propyl)-fluorene-alt-9,9-bis-(3-ethyl(oxetane-3- ethoxy)-hexyl)-fluorene]), PFO (poly(9,9-di-n-octylfluorenyl-2,7-diyl)), PPDIDTT (poly([N,N'-bis(2-decyl-tetradecyl)-3,4,9,10-peryleneimide-1,7-diyl]-alt-(dithieno[3,2-b:2',3'-d]thiophene-2,6-diyl)}), TPBi (1,3,5-tri(N-phenylbenzimidazol-2-yl)benzene); metal oxides, such as TiO x SnO x wait.
[0097] Exemplary hole-conducting layers (EBL) can, for example, comprise the following materials, for example ≥30 wt.-%, ≥50 wt.-% or ≥70 wt.-%, based on the electron-conducting layer; consist essentially of these materials (for example ≥90 wt.-%, ≥95 wt.-% or ≥99 wt.-%, based on the electron-conducting layer); or even consist of these materials (wherein the following list is non-exclusive and also includes mixtures of the materials mentioned, for example binary, ternary, quaternary mixtures, etc.):
[0098] Poly(3-hexylthiophene-2,5-diyl) (P3HT),
[0099] Poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene] (MEH-PPV),
[0100] Poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene](MDMO-PPV), CN-PPV, CN-MEH-PPV, other phthalocyanines,
[0101] poly[(9,9-di-n-octylfluorenyl-2,7-diyl)-alt-(benzo[2,1,3]thiadiazole-4,8-diyl]] (F8BT), polyfluorene (PF), poly[2,1,3-benzothiadiazole-4,7-diyl[4,4-bis(2-ethylhexyl)-4H-cyclopenta[2,1-b:3,4-b']dithiophene-2,6-diyl]] (PCPDTBT), squarylium cyanine (e.g., symmetrical squarylium cyanine, e.g., having a terminal end with an alcohol functional group) Terminated hydrazone or diazabis-squarylium, PTT) (polythieno[3,4-b]thiophene), poly(5,7-bis(4-decyl-2-thienyl)-thieno(3,4-b)dithiazol-thiophene-2,5) (PDDTT); polymers based on diketopyrrolopyrroles, such as poly{2,2'-[(2,5-bis(2-hexyldecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)dithiophene]-5, 5'-diyl-alt-thiophene-2,5-diyl} (PDPP3T), poly[[2,5-bis(2-hexyldecyl)-2,3,5,6-tetrahydro-3,6-dioxapyrrolo[3,4c]pyrrole-1,4-diyl]-alt-[3',3"-dimethyl-2,2':5',2"-p-thiophene]-5,5"-diyl] (PMDPP3T), poly{2,2'-[(2,5-bis(2-hexyldecyl)-3,6-dioxopyrrolo[3,4c]pyrrole-1,4-diyl] ,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)dithiophene]-5,5'-diyl-alt-thiophene-2,5-diyl} (PDPP5T), poly[2,6-4,8-di(5-ethylhexylthienyl)benzo[1,2-b;3,4-b]dithiophene-alt-5-dibutyloctyl-3,6-bis(5-bromothien-2-yl)pyrrolo[3,4-c]pyrrole-1,4-dione] (PBDTT-DPP);
[0102] Dithienosilole-based polymers, such as poly[(4,4-bis(2-ethylhexyl)dithieno[3,2-b:2',3'-d]silole)-2,6-diyl-alt-(4,7-bis(2-thienyl)-2,1,3-benzothiadiazole)-5,5'-diyl] (PSBTBT),
[0103] 7,7'-(4,4-bis(2-ethylhexyl)-4H-silane[3,2-b:4,5-b']bithiophene-2,6-diyl)bis(6-fluoro-4-(5'-hexyl-[2,2'-bithiophene]-5-yl)benzo[c][1,2,5]thiadiazole)(p-DTS(FBTTh2)2),
[0104] poly[2,7-(9,9-dioctyl-dibenzosilyl)-alt-4,7-bis(thiophen-2-yl)benzo-2,1,3-thiadiazole] (PSiFDTBT); benzodithiophene-based polymers, such as poly[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl-alt-3-fluoro-2-[[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophene-4,6-diyl] (PTB7),
[0105] Poly[(2,6-(4,8-bis(5-(2-ethylhexyl)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione))]))(PBDB-T),
[0106] Poly{2,6'-4,8-di(5-ethylhexylthienyl)benzo[1,2-b;3,4-b]dithiophene-alt-5-dibutyloctyl-3,6-bis(5-bromothiophen-2-yl)pyrrolo[3,4-c]pyrrole-1,4-dione (PBDTT-DPP), poly[4,8-bis(5-(2-ethylhexyl)thiophen-2-yl)benzo[1,2-b;4,5-b']dithiophene-2,6-diyl-alt-(4-(2-ethylhexyl)-3-fluorothieno[3,4-b]thiophene-)-2-carboxy-2-6-diyl)] (PBDTT-FTTE),
[0107] Poly[(4,8-bis-(2-ethylhexyloxy)-benzo(1,2-b:4,5-b')dithiophene)-2,6-diyl-alt-(4-(2-ethylhexyl)-thieno[3,4-b]thiophene-)-2-6-diyl)] (PBDTTT-CF), polybenzothiadiazole(thiophene)-stat-benzodithiophene(thiophene)-8 (PBTZT-stat-BDTT-8) and other polymers and copolymers and small molecules having an absorption maximum between 320-800 nm; polytriarylamines and their derivatives,
[0108] Poly[[2,5-bis(2-octyldodecyl)-2,3,5,6-tetrahydro-3,6-dioxapyrrolo[3,4-c]pyrrole-1,4-diyl]-alt2[[2,2'-(2,5-thiophene)bithieno[3,2-b]thiophene]-5,5'-diyl]] (DPP(P)), polyaniline (PANI),
[0109] Poly[[4,8-bis-(2-ethylhexyloxy)-benzo(1,2-b:4,5-b')dithiophene)-2,6-diyl-alt-(4-(2-ethylhexyl)-thieno[3,4-b]thiophene)-2-6-diyl]] (PBDTTT-C),
[0110] Poly[N29-heptyl-decyl-2,7-carbazole-alt-3,6-bis(thiophen-5-yl)-2,5-dioctyl-2,5-dihydropyrrolo[3,4-]pyrrole-1,4-dione] (PCBTDPP),
[0111] Poly[[9-(1-octylnonyl)-9H-carbazole-2,7-diyl]-2,5-thiophenediyl-2,1,3-benzothiadiazole-4,7-diyl-2,5-thiophenediyl] (PCDTBT),
[0112] Poly[2,5-bis(2-octyldodecyl)pyrrolo[3,4-c]pyrrole-1,4(2H,5H)-dione-(E)-1,2-di(2,2'-bithiophene-5-yl)ethylene] (PDPPDBTE),
[0113] Perfluoro(4-methyl-3,6-dioxaoctan-7-ene)sulfonyl fluoride (PFI),
[0114] Poly(4-styrene sulfonate) grafted-polyaniline (PSS-g-PANI),
[0115] Copolymer of 2'-butyloctyl-4,6-dibromo-3-fluorothieno[3,4-b]thiophene-2-carboxylate (TT-BO), copolymer of 3',4'-dichlorobenzyl-4,6-dibromo-3-fluorothieno[3,4-b]thiophene-2-carboxylate (TT-DCB) and 2,6-bis(trimethyltin)-4,8-bis(2-ethylhexyloxy)benzo[1,2-b:4,5-b′]dithiophene (BDT-EH) (PTB-DCB21); N2,N2,N2',N2',N7,N7,N7',N7'-octyl (4-Methoxyphenyl)-9,9'-spirobis[9H-fluorene]-2,2',7,7'-tetraamine (spiro-OMeTAD), poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)] (TFB), N4,N4'-di(naphthalen-1-yl)-N4,N4'-bis(4-vinylphenyl)biphenyl-4,4'-diamine (VNPB), 1,4-bis(4-sulfobutyloxy)benzene and thiophene fraction (PhNa-1T); metal oxides such as NiO x 、MoO x wait.
[0116] An electron-conducting layer and / or a hole-conducting layer can, for example, be arranged between the pixelated first electrode layer and the first layer, between the first layer and the optional second and / or third layer, preferably to a lesser extent between the optional second layer and the optional third layer (preferably to a lesser extent) and / or between the optional second layer and the second electrode.
[0117] According to a particular embodiment, the detector for electromagnetic radiation according to the invention further comprises a substrate on which a pixelated first electrode layer is present, wherein the substrate preferably has a plurality of transistors, wherein further preferably at least one transistor respectively contacts an electrode pixel of the pixelated first electrode layer.
[0118] The substrate is not particularly limited and can be, for example, a pixelated substrate. In particular, the substrate is used for contacting electrode pixels and / or for stabilizing the detector, but also simplifies its manufacture. The substrate can be a substrate that is usually present in a detector, in particular an X-ray detector and / or a gamma ray detector.
[0119] The transistor is also not particularly limited and can be, for example, a TFT. A plurality of transistors can also contact the electrode pixel.
[0120] According to certain embodiments, a surface layer, for example glass and / or an encapsulation, may also be present on the second electrode.
[0121] The detector according to the invention is in particular designed to be planar. For the detector according to the invention, in particular simple solutions such as the use of anisotropic conductive films (ACF) or conductive inks cannot be used, since a "planar" contact with the first layer via the electrode pixels must be ensured, rather than a point-by-point contact. According to a specific embodiment, planar means here that the surface of the electrode pixel in contact with the first layer is greater than 60%, preferably >80%, further preferably >90%, for example greater than 95%, more than 99% or even 100%, of the surface of the electrode pixel.
[0122] exist Figure 1 An exemplary detector according to the invention is schematically shown in , wherein an exemplary layer arrangement is shown there, here for example an X-ray detector and / or a gamma ray detector. The substrate 1.6 comprises a transistor 1.7, for example a thin film transistor (TFT) in an active matrix drive scheme. The transistor 1.7 contacts the electrode pixels 1.5, which form a structured pixelated first electrode layer. There are intermediate spaces between the electrode pixels 1.5, above which the structure 1.4 is located, here for example as a grid for an anchoring structure. In and above the structure 1.4 there is a first layer 1.3 comprising at least one recrystallized first perovskite. On the first layer 1.3 there is a second layer 1.4, which comprises at least one second perovskite, which corresponds here to at least one first perovskite. Above it there is a second electrode 1.1 and an encapsulation portion 1.8.
[0123] For the detector Figure 1 In addition to the layer structure shown by way of example in the embodiment, one or more interlayers may be present in the structure, i.e. electron-conducting layers and / or hole-conducting layers having electron-conducting and / or hole-conducting (hole / electron-blocking) functions. Possible positions for one or more interlayers are, for example, between the electrode pixel 1.5 and the first layer 1.3, between the first layer 1.3 and the second layer 1.2, preferably to a lesser extent, and / or between the second layer 1.2 and the second electrode 1.1.
[0124] Furthermore, a method for producing a detector for electromagnetic radiation, in particular an X-ray detector and / or a gamma-ray detector, is disclosed, the method comprising:
[0125] - providing a pixelated first electrode layer, the pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels;
[0126] - applying a structure at least partially to the intermediate spaces of the pixelated first electrode layer, wherein the structure is applied in such a way that the structure is at least partially arranged facing away from the first electrode layer in the intermediate spaces between the individual electrode pixels;
[0127] - introducing into said structure a first layer comprising at least one first perovskite; and
[0128] - applying a second electrode to the structure and / or to the first layer comprising at least one first perovskite; or
[0129] - providing a structure wherein the structure has an intermediate space;
[0130] - introducing a plurality of electrode pixels between the intermediate spaces of the structure, wherein the electrode pixels do not fill the structure, thereby forming a pixelated first electrode layer;
[0131] - introducing into said structure a first layer comprising at least one first perovskite; and
[0132] - applying a second electrode to the structure and / or to the first layer comprising at least one first perovskite.
[0133] According to a particular embodiment, the steps are performed in the order presented.
[0134] The method according to the invention can in particular be used to produce the detector according to the invention. Accordingly, the description of the detector according to the invention according to a specific embodiment also relates to the method according to the invention, and vice versa. In particular, the different layers and materials used to produce the detector in the method according to the invention can be identical to those already described in conjunction with the detector according to the invention, and vice versa. The method according to the invention has the advantage that it can be easily scaled up to large areas (e.g. 43×43 cm 2 )superior.
[0135] The method according to the present invention may firstly comprise the following steps:
[0136] I) - providing a pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels;
[0137] - applying a structure at least partially to the intermediate spaces of the pixelated first electrode layer, wherein the structure is applied in such a way that the structure is at least partially arranged remote from the first electrode layer on the intermediate spaces between the individual electrode pixels;
[0138] or steps
[0139] II) - providing a structure having an intermediate space;
[0140] - introducing a plurality of electrode pixels between the intermediate spaces of the structure, wherein the electrode pixels do not fill the structure, thereby forming a pixelated first electrode layer.
[0141] The two methods can be distinguished, for example, with regard to the production of the structure. Variant I) is advantageous, for example, in methods in which the structure is subsequently applied, such as, for example, in the case of resists, in particular photoresists, or in 3D printing. Variant II) is suitable, however, for methods in which parts of the substrate are removed, etc., in order to produce the structure, such as, for example, in etching or laser ablation, as described above.
[0142] Providing a pixelated first electrode layer, which can be obtained as described above, and providing a structure in variant II), which can also be obtained as described above, for example based on a substrate, are not particularly restricted. Applying the structure in variant I) can be carried out as described above, for example by coating a resist, such as a photoresist, if necessary also in multiple layers, and / or by 3D printing, etc. In variant II, the introduction of electrode pixels can be carried out, for example, in the following manner: the material of the electrode pixels is introduced as described above into the area between the "intermediate spaces" of the pixelated first electrode layer (the intermediate spaces are therefore defined as above in this embodiment), for example also on the contact part of the substrate, and liquefaction and resolidification (for example melting and resolidification), introduction of solid electrode pixels, solidification from the gas phase, evaporation from a solution, etc., and is not particularly restricted, and can also be carried out from a precursor of the electrode material, for example during precipitation.
[0143] In both methods, a first layer comprising at least one first perovskite is then introduced. This step is also not particularly limited. For example, a material for a first layer comprising at least one first perovskite, such as at least one first perovskite material and / or its precursor, can be introduced into the structure as a powder and liquefied and solidified again there. The composition of the introduced material does not have to correspond to the final composition of the final first layer. When the precursor is introduced, after manufacturing at least one first perovskite, it can also be liquefied and solidified again in order to recrystallize it. Here, at least one first perovskite or first layer can be well connected to the structure and fixed on the structure because good wetting can be achieved by the liquid phase. Liquefaction is not particularly limited here and can be carried out by the action of methylamine gas (MA gas), pressure and / or temperature as described above in conjunction with the detector. Then, solidification and then recrystallization can be carried out again by removing MA gas and / or other corresponding temperature and / or pressure changes accordingly, wherein this can be adapted to at least one first perovskite.
[0144] exist Figures 12 to 14 The corresponding method is schematically shown in Fig.12As shown in FIG. 3 , a first electrode layer 3.3 including electrode pixels is present on a substrate 3.4. Structure 3.2 is located as an anchoring structure above the interspace of the first electrode layer 3.3. The material for the first layer is introduced into the structure 3.2 as a powder 3.1, for example as a perovskite powder or as a precursor material for a perovskite, and is optionally also applied, as in this case Fig.12 Subsequently, Fig.13 In the step shown in FIG. 1 , the powder is liquefied by the action of MA gas, temperature T, etc., so that a liquid first layer 3.5 is formed. Fig.14 In the step shown in , the liquid first layer is recrystallized to form a recrystallized first layer 3.6. The recrystallized first layer then has good adhesion to the first electrode layer 3.3 and good electrical contact of the individual electrode pixels on its surface, which is, for example, greater than 60%, preferably >80%, further preferably >90%, for example greater than 95%, greater than 99% or even 100% of the area of the electrode pixels.
[0145] In such a method, the material for the first layer, for example at least one first perovskite and / or a precursor thereof, can be applied, liquefied and recrystallized one or more times in order to achieve a desired filling height or thickness of the first layer.
[0146] Alternatively, only a portion of the first layer can also be liquefied, for example by means of MA gas, temperature and / or pressure, and this liquefied portion can be brought into contact with the structure and preferably ultimately with the pixelated first electrode layer, and the liquefied portion of the first layer can then be recrystallized. As described above, after recrystallization, a structure is formed which has a combination of a first layer and a second layer, which have the same perovskite molecules in different crystal structures, so that a corresponding layer thickness is then also obtained, for example a total of 5 μm to 5000 μm, preferably 10 μm to 3000 μm, further preferably 50 μm to 2000 μm, even more preferably 100 μm to 1500 μm, and if necessary, a height of the structure as given above can also be obtained. Thus, the absorber layer is partially liquefied here and is directly connected to the anchoring structure.
[0147] exist Figures 23 to 25 The corresponding method is schematically shown in Fig.23 As shown in FIG. 5 , the pixelated first electrode layer 5.3 is located on a substrate 5.4 and there is a structure 5.2 thereon above the intermediate spaces between the electrode pixels. The first layer 5.6 is partially liquefied by MA gas, temperature, etc., so that a liquefied portion 5.8 is formed. Fig.24As shown in FIG, the liquefied portion 5.8 is then placed in contact with or on the structure 5.2 and the pixelated first electrode layer 5.3. Thereafter, the liquefied portion 5.8 solidifies and as shown in FIG. Fig.25 As shown in FIG. 5 , a recrystallized portion 5 . 9 of the first layer 5 . 6 is formed.
[0148] Hybrid forms and derivatives of these two methods are also possible if, for example, a second layer containing at least one second perovskite and / or a third layer containing at least one scintillator is additionally applied, resulting in a detector with a thick absorber layer, the adhesion of which to the pixelated first electrode layer is improved by the first layer.
[0149] An exemplary derivative is Figures 19 to 22 Here, as in Fig.19 As shown in, a second layer 5.6 comprising at least one second perovskite is provided as a thick absorber layer, wherein the second perovskite can be the same as or different from the at least one first perovskite, and the thickness of the absorber layer is, for example, 10μm-3000μm, preferably 50μm-2000μm, and more preferably 100μm-1500μm, wherein the absorber layer can be manufactured in a separate process, for example by sintering, rolling or a high-temperature process, so that decoupling of the process for manufacturing the detection layer is possible.
[0150] Furthermore, a substrate 5.4 is provided with a pixelated first electrode layer 5.3 and a structure 5.2, here for example as a grid structure, wherein the first layer 5.1 is located in and above the structure 5.2, and here for example the first layer can have a liquid or already recrystallized first perovskite. Fig. 20 In the step shown in , a part of the first layer 5.1 is reliquefied by MA gas and / or (optionally) at a pressure (depending on the material, especially perovskite, for example 1 MPa-300 MPa, preferably 2 MPa-100 MPa, more preferably 3 MPa-50 MPa) and / or temperature (depending on the material, especially perovskite, for example 0-600° C.), so that a liquefied layer 5.7 is formed. The given pressures and temperatures can also be applied in other corresponding methods. As in Fig.21 As shown in FIG. 5 , the second layer is applied or positioned on the liquefied layer 5.7, wherein the second layer adheres well to the liquefied layer 5.7. After the liquefied layer 5.7 solidifies, the first layer 5.1 with recrystallized perovskite is formed again, as shown in FIG. Fig. 22 As a result, the second layer 5 . 6 is also fixed.
[0151] exist Figures 26 to 28 A "hybrid approach" is shown, where the hybrid approach means Figures 19 to 22and a mixed type of methods 23 to 25.
[0152] As in Fig.26 As shown in Fig.23 A second layer 5.6 having a liquefied portion 5.8 is provided, wherein the liquefied portion can be produced by MA gas, temperature, etc. Furthermore, on a substrate 5.4 having a pixelated first electrode layer 5.3 and a structure 5.2, the first layer 5.1 is partially liquefied to provide a liquefied layer 5.7 (corresponding to Fig.19 ), also provided by means of MA gas, temperature, etc. The liquefied layer 5.7 is in contact with the liquefied portion 5.8, as in Fig. 27 After recrystallization, as shown in Fig.28 Thus, a portion of the second layer and a portion of the first layer are liquefied and brought into contact with each other in order to fix the layers accordingly on the pixelated first electrode layer, wherein the second layer is the main absorber layer and the first layer is used to promote adhesion.
[0153] Also included in the method according to the invention are other hybrid forms and variants which are not described in detail in conjunction with the figures but result in the same detector, in which the first perovskite, in particular at least one recrystallized first perovskite, is directly connected to the structure completely or partially in the first layer, i.e., for example, methods with other filling levels in the structure, etc.
[0154] Immediately after applying the first layer and optionally the second and / or third layer, the second electrode is applied, wherein this is likewise not subject to particular restrictions. It is also not excluded that the second electrode is previously applied to the non-liquefied part of the first layer, as proposed in the above-mentioned variant with liquefied parts, and the second or third layer is applied.
[0155] According to a particular embodiment, introducing the first layer comprising at least one first perovskite comprises at least partially recrystallizing the at least one first perovskite. Thus, as described above, the adhesion of the first layer is improved.
[0156] According to a particular embodiment, the structure is filled with at least a first layer comprising at least one first perovskite. As described above, the bonding of the other layers is thus improved.
[0157] According to a particular embodiment, a second layer comprising at least one second perovskite and / or a third layer comprising at least one scintillator is applied to the first layer comprising at least one first perovskite. The materials of the layers correspond to the materials already mentioned in connection with the detector.
[0158] According to a specific embodiment, a second layer is applied which contains at least one second perovskite, wherein the at least one second perovskite at least partially no longer crystallizes. This allows for a decoupling of the production of the second layer which is primarily used as an absorber layer (e.g. by sintering, rolling or high-temperature processes etc.) and the application to a further detector (e.g. in the form of a backplane).
[0159] According to a specific embodiment, an electron-conducting layer and / or a hole-transporting layer is also introduced between the pixelated first electrode layer and the second electrode. As explained above in conjunction with the detector, this can be applied during the method at suitable locations, i.e. to the pixelated first electrode layer, the first layer, the second and / or third layer, etc. The materials of the layers correspond to the materials already mentioned in conjunction with the detector.
[0160] According to a particular embodiment, the pixelated first electrode is applied to a substrate. This is not particularly limited and can be constructed as above in connection with the detector.
[0161] According to a special embodiment, the substrate has a plurality of transistors, wherein preferably the pixelated first electrode layer is applied in such a way that at least one transistor in each case contacts an electrode pixel of the pixelated first electrode layer.
[0162] Also disclosed are the use of a structure for improving the adhesion between a pixelated electrode layer comprising a plurality of electrode pixels and a layer comprising at least one first perovskite, in particular a detection layer, wherein both the pixelated electrode layer and the layer comprising at least one first perovskite are in contact with the structure, and in particular their use in detectors, in particular in X-ray detectors and / or gamma-ray detectors.
[0163] As long as it makes sense, the above-mentioned embodiments, designs and improvements can be combined with each other arbitrarily. Other feasible designs, improvements and embodiments of the present invention also include combinations of features of the present invention described above or below with respect to the embodiments that are not mentioned in detail. In particular, those skilled in the art also add individual aspects as improvements or supplements to the corresponding basic forms of the present invention.
[0164] The present invention is further explained in detail below with reference to different examples thereof. However, the present invention is not limited to these examples.
[0165] On the first electrode layer of the pixel having an electrode made of, for example, ITO or Pt, Figure 3 The electrode pixels are formed by SU-8 as a photoresist. Figures 12 to 14 , MAPI (CH3NH3PbI3) is introduced into the structure as the first perovskite in powder form, liquefied and recrystallized by means of MA gas. Figures 19 to 22, a second layer of MAPI is applied, which is produced as an absorber layer by means of sintering, wherein the first layer is liquefied again and recrystallized after contact with the second layer, and a second electrode of Cr or Ti is applied thereon. This results in improved adhesion compared to a structure without structuring.
[0166] As from Fig.29 It can be seen from the XRD spectrum shown in , in which the angle 2θ in degrees is plotted relative to the intensity I in counts c, that the first layer of MAPI 12 treated with MA gas has eight additional peaks 1 to 8 compared to the untreated MAPI 11 of the second layer, from which the structural changes of the crystals of MAPI in the first layer are revealed.
[0167] Since in the example the same material is used in the first layer as in the second layer, no losses in the read signal and no thermal stresses caused by the process can be observed during use in the X-ray detector.
Claims
1. A detector for electromagnetic radiation, the detector comprising: a pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels, - a second electrode, and - a first layer comprising at least one first perovskite, said first layer being located between said pixelated first electrode layer and said second electrode, It also includes the following structure, which is at least partially located between the pixelated first electrode layer and the second electrode, and is at least partially arranged between the individual electrode pixels of the pixelated first electrode layer, so that the structure is at least partially arranged on the intermediate space between the individual pixel electrodes in the direction toward the second electrode away from the first electrode layer, wherein the first layer containing at least one first perovskite fills and covers the structure.
2. The detector for electromagnetic radiation according to claim 1, It is characterized in that The detector is an X-ray detector and / or a gamma-ray detector.
3. A detector for electromagnetic radiation according to claim 1 or 2, The at least one first perovskite in the first layer comprising at least one first perovskite is at least partially recrystallized.
4. A detector for electromagnetic radiation according to claim 1 or 2, It also includes a second layer comprising at least one second perovskite, which is located between the first layer comprising at least one first perovskite and the second electrode, and / or also includes a third layer comprising at least one scintillator, which is located between the first layer comprising at least one first perovskite and the second electrode.
5. A detector for electromagnetic radiation according to claim 4, The second layer includes at least one second perovskite, wherein the at least one second perovskite is at least partially non-recrystallized.
6. A detector for electromagnetic radiation according to claim 1 or 2, It also includes an electron conducting layer and / or a hole conducting layer, wherein the electron conducting layer and / or the hole conducting layer is located between the pixelated first electrode layer and the second electrode.
7. A detector for electromagnetic radiation according to claim 1 or 2, Also included is a substrate on which the pixelated first electrode layer exists.
8. A detector for electromagnetic radiation according to claim 7, The substrate has a plurality of transistors.
9. A detector for electromagnetic radiation according to claim 8, At least one of the transistors is respectively in contact with an electrode pixel of the pixelated first electrode layer.
10. A method for manufacturing a detector for electromagnetic radiation, the method comprising: - providing a pixelated first electrode layer, the pixelated first electrode layer comprising a plurality of electrode pixels and intermediate spaces between the individual electrode pixels; - applying a structure at least partially to the intermediate spaces of the pixelated first electrode layer, wherein the structure is applied in such a way that it is arranged at least partially facing away from the first electrode layer in the intermediate spaces between the individual electrode pixels; - introducing a first layer comprising at least one first perovskite into the structure, wherein the first layer comprising at least one first perovskite fills and covers the structure; and - applying a second electrode to the structure and / or to the first layer comprising at least one first perovskite; or - providing a structure, wherein the structure has an intermediate space; - introducing a plurality of electrode pixels between the intermediate spaces of the structure, wherein the electrode pixels do not fill the structure, thereby forming a pixelated first electrode layer; - introducing a first layer comprising at least one first perovskite into the structure, wherein the first layer comprising at least one first perovskite fills and covers the structure; and - applying a second electrode to the structure and / or to the first layer comprising at least one first perovskite.
11. The method according to claim 10, The method is used for producing an X-ray detector and / or a gamma-ray detector.
12. The method according to claim 10 or 11, Wherein introducing the first layer comprising at least one first perovskite comprises at least partially recrystallizing the at least one first perovskite.
13. The method according to claim 10 or 11, Wherein at least the structure is filled with the first layer comprising at least one first perovskite.
14. The method according to claim 10 or 11, Therein, a second layer comprising at least one second perovskite and / or a third layer comprising at least one scintillator is applied to the first layer comprising at least one first perovskite.
15. The method according to claim 14, The second layer is applied which contains at least one second perovskite, wherein the at least one second perovskite is at least partially not recrystallized.
16. The method according to claim 10 or 11, In this case, an electron-conducting layer and / or a hole-conducting layer is / are introduced between the pixelated first electrode layer and the second electrode.
17. The method according to claim 10 or 11, Therein, the pixelated first electrode layer is applied to a substrate.
18. The method according to claim 17, The substrate has a plurality of transistors.
19. The method according to claim 18, The pixelated first electrode layer is applied in such a way that at least one transistor in each case contacts an electrode pixel of the pixelated first electrode layer.