Hafnium Oxide Corrosion Inhibitor
By using an aqueous etching solution containing alkaline ammonium compounds and peroxides, the problem of difficulty in removing TiSiN layer in semiconductor devices is solved, and high selective etching is achieved, which improves device performance.
Patent Information
- Application Number
- CN202080008270.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-01-11
- Filing Date
- 2020-01-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-01-10
AI Technical Summary
In the process of manufacturing semiconductor devices, it is difficult for the prior art to selectively remove the titanium nitride (TiSiN) layer without damaging the hafnium oxide (HfO2) layer, resulting in damage to electrical properties.
Using an etching solution containing water, alkaline ammonium compounds, peroxides, water miscible organic solvents and nitrogen-containing compounds, the TiSiN layer is selectively removed by contacting a composite semiconductor device of TiSiN and HfO2 to improve TiSiN relative to The etching rate of HfO2.
The preferential removal of the TiSiN layer is achieved, which significantly improves the etching selectivity of TiSiN/HfO2, avoids damage to the hafnium oxide layer, and improves the electrical performance of semiconductor devices.
Smart Images

Figure CN113287187B_ABST
Abstract
Description
[0001] This application claims priority to U.S. Provisional Patent Application No. 62 / 791,270, filed on January 11, 2019, the entire contents of which are incorporated herein by reference for all permitted purposes. Background of the Invention
[0003] The present invention relates to an aqueous etching solution for manufacturing semiconductor devices. More specifically, the present invention relates to an etching solution for selectively etching a sacrificial material layer such as titanium silicon nitride (TiSiN) in the process of manufacturing a semiconductor device including a polysilicon-based gate electrode formed on a high dielectric (high-k) material layer.
[0004] MOS field effect transistors with very thin gate dielectrics made of silicon dioxide may experience unacceptable gate leakage currents. Forming the gate dielectric from certain high-k dielectric materials (e.g., hafnium oxide) instead of silicon dioxide can reduce gate leakage. However, such dielectrics may be incompatible with polysilicon, the preferred material for making device gate electrodes. Placing a thin layer of titanium nitride or titanium silicon nitride, which is compatible with many high-k gate dielectrics, between the high-k gate dielectric and the polysilicon-based gate electrode can enable such a dielectric to be used with such a gate electrode. Unfortunately, the presence of such a layer may increase the threshold voltage of the transistor, which is undesirable, so it must be removed.
[0005] In the fabrication of certain devices (e.g., p-type devices), a titanium silicon nitride (TiSiN) layer is often employed over conventional metal gate materials (e.g., TaN and TiN) over a high-k hafnium oxide (HfO2) layer. In order to pattern the gate structure, a wet chemical etching composition having a high etch selectivity to TiSiN without damaging the hafnium oxide is preferred. If the wet chemical penetrates and causes at least partial removal of the HfO2, such damage will negatively impact the electrical performance of the device. Therefore, there is a need in the art for a wet chemical etching composition that will preferentially remove TiSiN over HfO2 without the above-mentioned disadvantages. SUMMARY OF THE INVENTION
[0007] The present disclosure satisfies this need, as the inventors have discovered a composition useful for selectively removing TiSiN relative to hafnium oxide.
[0008] In one aspect, an etching solution suitable for selectively removing TiSiN from microelectronic devices relative to HfO2 is provided, comprising: water; at least one alkaline ammonium compound selected from ammonium hydroxide, quaternary ammonium hydroxide, ammonium fluoride and quaternary ammonium fluoride; at least one peroxide; a water-miscible organic solvent; at least one selected from C 4-12nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; and optionally at least one chelating agent.
[0009] In another aspect, a method for selectively increasing the etching rate of TiSiN relative to HfO2 in a composite semiconductor device comprising TiSiN and HfO2 is provided, the method comprising the steps of: contacting the composite semiconductor device comprising TiSiN and HfO2 with an aqueous composition, wherein the aqueous composition comprises: water; at least one alkaline ammonium compound selected from ammonium hydroxide, quaternary ammonium hydroxide, ammonium fluoride and quaternary ammonium fluoride; at least one peroxide; a water-miscible organic solvent; at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines, and polyamines; and optionally at least one chelating agent; and rinsing the composite semiconductor device after at least partially removing the TiSiN, wherein the etch selectivity of the TiSiN relative to HfO2 is greater than 30.
[0010] In another aspect, an etching solution suitable for selectively removing TiSiN relative to hafnium oxide from a microelectronic device is provided, comprising, consisting essentially of, or consisting of: about 3.7 to about 4.5 weight percent, or about 3.7 to about 5.5 weight percent, of at least one pure alkaline ammonium compound selected from ammonium hydroxide, quaternary ammonium hydroxide, ammonium fluoride, and quaternary ammonium fluoride; about 3.9 to about 4.5 weight percent, of at least one pure peroxide; about 7 to about 12 weight percent, or about 10 to about 15 weight percent, of a water-miscible organic solvent; about 0.4 to about 0.6 weight percent, or about 0.4 to about 0.8 weight percent, of at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; water; and optionally at least one chelating agent.
[0011] In another aspect, an etching solution suitable for selectively removing polysilicon relative to silicon oxide from a microelectronic device is provided, comprising, consisting essentially of, or consisting of: about 4.1% by weight ammonium hydroxide (pure); about 4.3% hydrogen peroxide (pure); about 0.4 to about 1.2% by weight ammonium fluoride (pure); about 10% water-miscible organic solvent; about 0.3 to about 0.5% or from about 0.3 to about 0.8% of at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; water; and optionally at least one chelating agent.
[0012] The embodiments of the present invention may be used alone or in combination with each other. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a graphical illustration of the HfO2 loss determined by XPS analysis comparing SC1 to the compositions disclosed herein; and
[0015] Figure 2 is a graphical illustration of the Si remaining on the substrate as determined by XPS analysis comparing SC1 to the compositions disclosed herein. DETAILED DESCRIPTION OF THE INVENTION
[0017] All references, including publications, patent applications, and patents, cited herein are hereby incorporated by reference to the same extent as if each reference were individually and specifically indicated to be incorporated by reference and were set forth in its entirety herein.
[0018] In the context of describing the present invention (especially in the context of the following claims), the use of the terms "one" and "a kind of" and "the" and similar references is interpreted as covering the singular and plural, unless otherwise specified herein or clearly contradicted by the context. Unless otherwise specified, the terms "comprising", "having", "including" and "containing" should be interpreted as open terms (i.e., meaning "including but not limited to"). Unless otherwise specified herein, the reference to the numerical range herein is intended only as a shorthand method for individually referring to each individual value falling within the range, and each individual value is incorporated into the specification as if it were stated separately herein. Unless otherwise specified herein or clearly contradicted by the context, all methods described herein can be performed in any suitable order. Unless otherwise stated, the use of any and all embodiments or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the present invention without limiting the scope of the present invention. Any language in the specification should not be interpreted as indicating that any unclaimed element is essential for the implementation of the present invention. The term "comprising" used in the specification and claims includes the narrower language of "substantially consisting of..." and "consisting of..."
[0019] Embodiments of the present invention are described herein, including the best mode known to the inventor for implementing the present invention. By reading the foregoing description, the changes of those embodiments will become apparent to those of ordinary skill in the art. The inventor expects that the technician will appropriately adopt such changes, and the inventor intends that the present invention be implemented in a manner different from that specifically described herein. Therefore, the present invention includes all modifications and equivalents of the subject matter recorded in the appended claims when applicable law allows. In addition, unless otherwise specified herein or clearly contradictory to the context, the present invention encompasses any combination of all possible variations of the above-mentioned elements.
[0020] The present invention generally relates to compositions for selectively removing TiSiN relative to hafnium oxide from microelectronic devices having hafnium oxide and TiSiN materials thereon during their fabrication.
[0021] For ease of reference, "microelectronic device" or "semiconductor device" corresponds to the manufacture of semiconductor substrates for microelectronic, integrated circuit or computer chip applications, such as wafers, flat panel displays, phase change memory devices, solar panels and other products, including solar substrates, photovoltaic devices and micro-electromechanical systems (MEMS). Solar substrates include, but are not limited to, silicon, amorphous silicon, polycrystalline silicon, single crystal silicon, CdTe, copper indium selenide, copper indium sulfide, and gallium arsenide on gallium. Solar substrates can be doped or undoped. It should be understood that the term "microelectronic device" or "semiconductor device" is not meant to be limiting in any way and includes any substrate that will eventually become a microelectronic device or microelectronic assembly.
[0022] A "composite semiconductor device" or "composite microelectronic device" refers to a device having more than one material and / or layer and / or portions of a layer present on a non-conductive substrate. The material may include a high-K dielectric and / or a low-K dielectric and / or a barrier material and / or a capping material and / or a metal layer and / or other materials known to the skilled person.
[0023] As defined herein, "low-k dielectric material" corresponds to any material used as a dielectric material in a layered microelectronic device, wherein the material has a dielectric constant of less than about 3.5. Preferably, the low-k dielectric material includes low polarity materials such as silicon-containing organic polymers, silicon-containing hybrid organic / inorganic materials, organosilicate glass (OSG), TEOS, fluorinated silicate glass (FSG), silicon dioxide, and carbon-doped oxide (CDO) glass. It should be understood that the low-k dielectric material can have different densities and different porosities.
[0024] As defined herein, "high-k dielectric material" refers to a material having a higher dielectric constant than silicon oxide, and includes hafnium oxide.
[0025] "Substantially free" is defined herein as less than 0.001% by weight. "Substantially free" also includes 0.000% by weight. The term "free" means 0.000% by weight.
[0026] As used herein, "about" is intended to correspond to ±5% of the stated value.
[0027] In all such compositions wherein a particular component of the composition is discussed with reference to a weight percent range including a zero lower limit, it is understood that such components may or may not be present in various specific embodiments of the composition, and where such components are present, they may be present at a concentration as low as 0.001 weight percent based on the total weight of the composition in which such such components are present. Note that all component percentages are weight percents and are based on the total weight of the composition, i.e., 100%.
[0028] In a broad practice of this aspect, the etching solution of the present invention comprises, consists essentially of, or consists of: water; at least one alkaline ammonium compound selected from ammonium hydroxide, quaternary ammonium hydroxide, ammonium fluoride, and quaternary ammonium fluoride; at least one peroxide; at least one water-miscible organic solvent; at least one selected from C 4-12 nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; and optionally at least one chelating agent.
[0029] In some embodiments, the etching solution compositions disclosed herein are formulated to be substantially free or free of at least one of the following compounds: metal hydroxides, trace metal cations, silicon-containing compounds, chlorine-containing compounds, bromine-containing compounds, iodine-containing compounds, phosphorus-containing compounds, magnesium-containing compounds, and alkanolamines.
[0030] The composition of the present invention is suitable for use in a method for manufacturing a ring gate structure on an electronic device. Such methods are known in the art, such as the processes disclosed in U.S. Patent No. 6,617,209, U.S. Patent Application Publication No. 2017 / 0179248, U.S. Patent Application Publication No. 2017 / 0104062, U.S. Patent Application Publication No. 2017 / 0133462, and U.S. Patent Application Publication No. 2017 / 0040321, the disclosures of which are incorporated herein by reference.
[0031] The headings used herein are not intended to be limiting; rather, they are used for organizational purposes only.
[0032] The compositions disclosed herein exhibit excellent TiSiN removal in preference to hafnium oxide.
[0033] water
[0034] The etching compositions of the present invention are water-based and therefore contain water. In the present invention, water acts in a variety of ways, for example, dissolving one or more components of the composition, as a carrier of the components, as an auxiliary agent for removing residues, as a viscosity modifier for the composition, and as a diluent. Preferably, the water used in the cleaning composition is deionized (DI) water. The scope of water described in the next paragraph and elsewhere herein includes all water from any source in the composition.
[0035] It is believed that for most applications the weight percent of water in the composition will be present in a range with a starting point and an end point selected from the group consisting of: 0.5, 1, 5, 10, 15, 17, 20, 23, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 72, 74, 75, 76, 78, 80, 82, 84, 85, 86, 88, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 99.2, 99.3, 99.4, and 99.5. Examples of water ranges that can be used in the composition include, for example, about 40% to about 95% by weight or 50% to about 95% by weight of water; or about 70% to about 90% by weight, or about 70% to about 85% by weight, or about 75% to about 90% by weight, or about 75% to about 85% by weight of water. Other preferred embodiments of the present invention may include water in an amount to achieve the desired weight percentage of other ingredients. Other preferred embodiments of the present invention may include parts of the composition other than the amount of pure other ingredients.
[0036] Basic ammonium compounds
[0037] The etching compositions disclosed herein additionally comprise one or more alkaline ammonium compounds. The role of the alkaline ammonium compound is to help etch TiSiN. One or more alkaline ammonium compounds may be selected to provide the desired etching rate. Examples of these alkaline ammonium compounds include compounds such as ammonium hydroxide (NH4OH) and quaternary ammonium compounds and ammonium fluoride. Quaternary ammonium compounds include quaternary ammonium hydroxides, such as tetraalkylammonium hydroxides, and quaternary ammonium fluorides, such as tetraalkylammonium fluoride. Exemplary quaternary ammonium hydroxides (and tetraalkylammonium hydroxides) may be compounds having the formula [NR 1 R 2 R 3 R 4 ] + OH - Those compounds in which R 1 , R 2 , R 3 and R 4 Each is independently hydrogen, alkyl, hydroxyalkyl, and combinations thereof. Exemplary quaternary ammonium fluorides (and tetraalkylammonium fluorides) may be those having the formula [NR 1 R 2 R 3 R 4 ] + F - Those compounds in which R 1 , R 2 , R 3 and R 4Each independently is hydrogen, alkyl, fluoroalkyl and combinations thereof. As used herein, the term "alkyl" refers to a straight or branched hydrocarbon group of 1 to 20 carbon atoms or 1 to 8 carbon atoms or 1 to 4 carbon atoms. Examples of suitable alkyls include methyl, ethyl, propyl, isopropyl, butyl and tert-butyl. As used herein, the term "hydroxyalkyl" refers to a straight or branched hydrocarbon group containing a hydroxyl group with 1 to 20 carbon atoms or 1 to 8 carbon atoms or 1 to 4 carbon atoms. As used herein, the term "fluoroalkyl" refers to a straight or branched hydrocarbon group containing a fluorine group with 1 to 20 carbon atoms or 1 to 8 carbon atoms or 1 to 4 carbon atoms. Examples of suitable fluoroalkyls include fluoroethyl and fluoropropyl.
[0038] Examples of suitable quaternary ammonium hydroxides (and tetraalkylammonium hydroxides) include quaternary ammonium hydroxides in which all R groups are the same (but not all are H) or quaternary ammonium hydroxides in which not all R groups are the same, for example, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrabutylammonium hydroxide (TBAH), tetrapropylammonium hydroxide, trimethylethylammonium hydroxide, (2-hydroxyethyl)trimethylammonium hydroxide, (2-hydroxyethyl)triethylammonium hydroxide, (2-hydroxyethyl)tripropylammonium hydroxide, (1-hydroxypropyl)trimethylammonium hydroxide, ethyltrimethylammonium hydroxide, diethyldimethylammonium hydroxide, choline hydroxide, benzyltrimethylammonium hydroxide (Triton B), and mixtures thereof.
[0039] Examples of suitable fluorinated quaternary ammonium compounds include quaternary ammonium fluorides in which all R groups are the same (but not all are H) or quaternary ammonium fluorides in which not all R groups are the same, such as tetramethylammonium fluoride (TMAF), tetraethylammonium fluoride, tetrabutylammonium fluoride (TBAF), tetrapropylammonium fluoride, trimethylethylammonium fluoride, (2-hydroxyethyl)trimethylammonium fluoride, (2-hydroxyethyl)triethylammonium fluoride, (2-hydroxyethyl)tripropylammonium fluoride, (1-hydroxypropyl)trimethylammonium fluoride, ethyltrimethylammonium fluoride, diethyldimethylammonium fluoride and benzyltrimethylammonium fluoride.
[0040] In some embodiments, the etching compositions disclosed herein include ammonium hydroxide as the alkaline ammonium component. With respect to the concentration of the alkaline ammonium compound, in some embodiments, the amount of the total alkaline ammonium compound may be from about 3.7 to about 5.5 wt % or from about 3.7 to about 5.5 wt % or from about 3.7 to about 4.5 wt % (pure, i.e., without the presence of an aqueous solvent component) based on the total weight of the composition. In some embodiments, if ammonium fluoride or a quaternary ammonium fluoride is present in the composition, it may be from about 0.1 to about 2.0 wt % or from about 0.1 to about 1.8 wt % or from about 0.4 to about 1.5 wt %.
[0041] In other embodiments, if more than one basic ammonium compound is present in the composition (pure, i.e., without a water component), for most applications the total amount or the amount of each basic ammonium compound is included in a weight percent range having a starting point and an end point selected from the following group of numbers: 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4, 1.5, 1.8, 2, 2.5, 3, 3.7, 3.9, 4, 4.1, 4.5, 4.7, 5, 5.2, 5.5, 5.7, 6, 6.2, 6.5, 7, 7.5, 8, 9, 10, 11, 12, 13, 14, 15, 17, 18, 19, and 20. Other examples of ranges of basic ammonium compounds in the compositions disclosed herein can be from about 0.5% to about 20% by weight, or from about 1.0% to about 15% by weight, or from about 1.3% to about 15% by weight of the composition (pure). For example, if the basic ammonium compound is (or comprises) ammonium hydroxide (29% solution), if added at about 14% by weight of the etching formulation, then 4.06% of active ammonium hydroxide compound will be present in the etching formulation.
[0042] In some embodiments, ammonium hydroxide and ammonium fluoride may be used in the etching compositions of the present invention. In one embodiment, the ammonium hydroxide is present at about 4.0 wt % (pure) and the ammonium fluoride is present at about 0.4 to 1.2 wt % (pure).
[0043] peroxide
[0044] The composition disclosed herein includes a peroxide that also serves to etch TiSiN. The peroxide used in the composition may include, but is not limited to, hydrogen peroxide, ammonium persulfate, peracid, peroxybenzoic acid, and combinations thereof. For example, if the peroxide is a 30% hydrogen peroxide solution, the hydrogen peroxide may be used in the composition at a concentration of about 1 to about 80% by weight, preferably about 10 to about 30% by weight, and more preferably about 10 to about 20% by weight, and still more preferably about 14 to about 16% by weight.
[0045] In some embodiments, the peroxide (based on the pure substance) comprises a weight percent within a range having a starting point and an endpoint selected from the group consisting of: 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 2.5, 3, 3.5, 3.8, 3.9, 4, 4.3, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 22, 25, 28, 30, and 30.
[0046] In other embodiments, the peroxide is present in the composition at about 0.5 wt % to about 30 wt %, or about 1 wt % to about 10 wt %, or about 2 wt % to about 8 wt % (pure). In one embodiment, the peroxide is present at about 4.5 wt % (pure).
[0047] Water miscible organic solvents
[0048] The etching composition of the present invention optionally contains a water-miscible organic solvent. Examples of water-miscible organic solvents that can be used are ethylene glycol, propylene glycol, 1,4-butanediol, tripropylene glycol methyl ether, propylene glycol propyl ether, diethylene glycol n-butyl ether (BDG) (e.g., available under the trade name DB is commercially available), dipropylene glycol methyl ether (DPM) hexyloxypropylamine, poly (ethylene oxide) diamine, dimethyl sulfoxide (DMSO), tetrahydrofurfuryl alcohol, glycerol, alcohols, sulfolane, sulfoxides or mixtures thereof. Preferred solvents are alcohols, diols or mixtures thereof. The most preferred solvents are sulfolane and polyols, including diols, such as ethylene glycol and propylene glycol, and triols, such as glycerol.
[0049] It is believed that for most applications, the amount of water-miscible organic solvent in the composition, if used, can be within a range having a starting point and an end point selected from the following weight percentage list: 0.5, 1, 3, 5, 7, 10, 12, 13, 14, 15, 20, 25, 29, 30, 33, 35, 40, 44, 50, 59.5. Examples of such solvent ranges include about 0.5% to about 59.5% by weight of the composition; or about 5% to about 50% by weight; or about 1% to about 40% by weight; or about 0.5% to about 30% by weight; or about 1% to about 30% by weight; or about 5% to about 30% by weight; or about 5% to about 15% by weight; or about 7% to about 10% by weight, or about 10% by weight.
[0050] Nitrogen-containing compounds (Hafnium oxide corrosion inhibitors)
[0051] The etching composition of the present invention comprises at least one selected from C 4-12 Nitrogen-Containing Compounds of Alkylamines, Polyalkyleneimines and Polyamines Preferably, the at least one nitrogen-containing compound is present in the composition at about 0.1 wt % to about 10 wt % (pure).
[0052] Suitable C 4-12 Examples of the alkylamines include hexylamine, octylamine, decylamine, and dodecylamine.
[0053] Preferably, the polyalkyleneimine is polyethyleneimine (PEI). Any PEI may be used, but preferably homopolymeric polyethyleneimine is used. The PEI may be branched or linear, but preferably is branched.
[0054] Although it has been found that the PEI used can have any formula weight to achieve efficacy, preferably the PEI has a lower formula weight (FW). In one embodiment, the PEI has a FW between 100 and 50,000, between 400 and 25,000, between 800 and 10,000, or between 1000 and 3000.
[0055] In one embodiment, the polyalkylene imine comprises polyethylene imine (PEI) and preferably PEI accounts for about 0.1 to about 10 weight % of the composition, preferably less than 5.0 weight %, preferably less than 2.5 weight %, preferably less than 1.5 weight %, preferably less than 1.0 weight %, or less than 0.8 weight % or less than 0.5 weight % of the composition. Preferably, the molecular weight of PEI is between 100 and 2500, preferably between 200 and 1500, and most preferably between 400 and 1200.
[0056] In a preferred embodiment, the molecular weight of the polyalkylene imine is between 100 and 2500, between 200 and 1500, between 400 and 1200 or between 700 and 900. A molecular weight of 800 is particularly suitable. The molecular weight is suitably determined by light scattering techniques known in the art.
[0057] Polyethyleneimine is commercially available, for example from BASF 800.
[0058] Examples of the polyamine include pentamethyldiethylenetriamine (PMDETA), triethylenediamine (TEDA), triethylenetetramine (TETA), tetramethylethylenediamine (TMEDA), and diethylenetriamine (DETA).
[0059] The at least one nitrogen-containing compound is primarily used to protect the hafnium oxide from corrosion or etching.
[0060] In some embodiments, two or more nitrogen-containing compounds are used in the etching compositions of the present invention. In some embodiments, two or more polyamines, two or more C 4-12 In an optional embodiment, polyamine, C alkylamine or two or more polyalkylene imines can be used in the etching composition of the present invention. 4-12 A mixture of at least two of an alkylamine and a polyalkyleneimine. For example, in some embodiments, a mixture of PMDETA and octylamine can be used. In an alternative embodiment, a mixture of PMDETA and PEI can be used in the composition of the present invention.
[0061] It is believed that for most applications, the composition selected from C 4-10The total amount of at least one nitrogen-containing compound of alkylamines, polyalkyleneimines, and polyamines can be in a range having a starting point and an endpoint selected from the following weight percent list: 0.01, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, 1.0, 1.25, 1.3, 1.5, 2, 2.5, 2.75, 3.0, 3.25, 3.5, 3.75, 4.0, 4.25, 4.50, 4.75, 5, 6, 7, 8, 9, and 10. Examples of such ranges of the at least one nitrogen-containing compound include from about 0.01 wt % to about 4.0 wt % of the composition; or from about 0.10 wt % to about 3.0 wt %; or from about 0.10 wt % to about 2 wt %; or from about 0.3 wt % to about 1 wt %; or from about 0.10 wt % to about 6 wt %; or from about 0.3 wt % to about 2 wt %.
[0062] Chelating agent (optional)
[0063] The etching composition of the present invention may optionally contain at least one chelating agent. The one or more chelating agents may be aminophosphonic acids, aminocarboxylic acids, organic acids, preferably with multiple functional groups, and other known chelating agents. These include, for example, ethylenediaminetetraacetic acid (EDTA), butylene diaminetetraacetic acid, (1,2-cyclohexanediamine)tetraacetic acid (CyDTA), diethylenetriaminepentaacetic acid (DETPA), ethylenediaminetetrapropionic acid, (hydroxyethyl)ethylenediaminetriacetic acid (HEDTA), N,N,N',N'-ethylenediaminetetra(methylenephosphonic) acid (EDTMP), triethylenetetraaminehexaacetic acid (TTHA), 1,3-diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid (DHPTA), methyliminodiacetic acid, propylenediaminetetraacetic acid, nitrotriacetic acid (NTA), citric acid, tartaric acid, gluconic acid, sugar acid, glyceric acid, oxalic acid, phthalic acid, maleic acid, mandelic acid, malonic acid, lactic acid, salicylic acid, propyl gallate, pyrogallol, 8-hydroxyquinoline and cysteine. In some embodiments, the chelating agent is selected from ethylenediaminetetraacetic acid (EDTA), butanediaminetetraacetic acid, (1,2-cyclohexanediamine)tetraacetic acid (CyDTA), diethylenetriaminepentaacetic acid (DETPA), ethylenediaminetetrapropionic acid, (hydroxyethyl)ethylenediaminetriacetic acid (HEDTA), N,N,N',N'-ethylenediaminetetra(methylenephosphonic) acid (EDTMP), triethylenetetraaminehexaacetic acid (TTHA) and 1,3-diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid (DHPTA). Preferred chelating agents are aminocarboxylic acids, such as EDTA, CyDTA, DEPTA and HEDTA. In some embodiments, aminophosphonic acids such as EDTMP can be used. In some embodiments, a mixture of chelating agents is used.
[0064] It is believed that for most applications, the total amount of the at least one chelating agent in the composition can be within a range having starting and ending points selected from the following weight percentage list: 0, 0.01, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, 1.0, 1.25, 1.3, 1.5, 2, 2.5, 2.75, 3.0, 3.25, 3.5, 3.75, 4.0, 4.25, 4.50, 4.75, 5, and 6. Examples of such ranges of at least one chelating agent include from about 0.01% to about 4.0% by weight of the composition; or from about 0.10% to about 3.0% by weight; or from about 0.10% to about 2% by weight; or from about 0.3% to about 1% by weight; or from about 0.10% to about 6% by weight; or from about 0.3% to about 2% by weight.
[0065] Surfactant (optional)
[0066] The etching composition of the present invention optionally comprises at least one surfactant. The role of the surfactant is to protect silicon oxide from etching. The surfactant used for the composition described herein includes, but is not limited to, amphoteric salts, cationic surfactants, anionic surfactants, zwitterionic surfactants, nonionic surfactants and combinations thereof, including, but not limited to, bis(2-ethylhexyl)phosphate, perfluoroheptanoic acid, perfluorodecanoic acid, trifluoromethanesulfonic acid, phosphonoacetic acid, dodecenylsuccinic acid, dioctadecyl hydrogen phosphate, octadecyl dihydrogen phosphate, dodecylamine, dodecenylsuccinic acid monodiethanolamide (dodecenylsuccinic acid monodiethanolamide), lauric acid, palmitic acid, oleic acid, linalool acid, 12-hydroxystearic acid and dodecyl phosphate.
[0067] Contemplated nonionic surfactants include, but are not limited to, polyoxyethylene lauryl ether (Emalmin NL-100 (Sanyo), Brij 30, Brij 98, Brij 35), dodecenyl succinic acid monodiethanolamide (DSDA, Sanyo), ethylenediaminetetra(ethoxylate-block-propoxylate)tetraol (Tetronic 90R4), polyethylene glycol (e.g., PEG 400), polypropylene glycol, polyethylene glycol or polypropylene glycol ether, block copolymers based on ethylene oxide and propylene oxide (Newpole PE-68 (Sanyo), Pluronic L31, Pluronic 31R1, Pluronic L61, Pluronic F-127), polyoxypropylene sucrose ether (SN008S, Sanyo), tert-octylphenoxypolyethoxyethanol (Triton X100), 10-ethoxy-9,9-dimethyldecan-1-amine ( CF-32), polyoxyethylene (9) nonylphenyl ether, branched (IGEPAL CO-250), polyoxyethylene (40) nonylphenyl ether, branched (IGEPAL CO-890), polyoxyethylene sorbitan hexaoleate, polyoxyethylene sorbitan tetraoleate, polyethylene glycol sorbitan monooleate (Tween 80), sorbitan monooleate (Span 80), a combination of Tween 80 and Span 80, alcohol alkoxylates (e.g., Plurafac RA-20), alkyl-polyglycosides, ethyl perfluorobutyrate, 1,1,3,3,5,5-hexamethyl-1,5-bis[2-(5-norbornene-2-yl)ethyl]trisiloxane, monomeric octadecylsilane derivatives, such as SIS6952.0 (Siliclad, Gelest), siloxane-modified polysilazanes such as PP1-SG10 Siliclad Glide 10 (Gelest), silicone-polyether copolymers such as Silwet L-77 (Setre Chemical Company), Silwet ECO Spreader (Momentive), and ethoxylated fluorosurfactants ( FSO-100, FSN-100).
[0068] Cationic surfactants contemplated include, but are not limited to, hexadecyltrimethylammonium bromide (CTAB), heptadecafluorooctanesulfonic acid, tetraethylammonium, stearyltrimethylammonium chloride (Econol TMS-28, Sanyo), 4-(4-diethylaminophenylazo)-1-(4-nitrobenzyl)pyridinium bromide, hexadecylpyridinium chloride monohydrate, benzalkonium chloride, benzethonium chloride, benzyldimethyldodecylammonium chloride, benzyldimethylhexadecylammonium chloride, hexadecyltrimethylammonium bromide, dimethyldi-octadecylammonium chloride, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium p-toluenesulfonate, didodecyldimethylammonium bromide, di(hydrogenated tallow)dimethylammonium chloride, tetraheptylammonium bromide, tetra(decyl)ammonium bromide, 336 and oxphenium bromide, guanidine hydrochloride (C (NH2) 3Cl) or trifluoromethanesulfonate, such as tetrabutylammonium trifluoromethanesulfonate, dimethyldi-octadecyl ammonium chloride, dimethyldi-hexadecyl ammonium bromide and di(hydrogenated tallow)dimethylammonium chloride (e.g., Arquad 2HT-75, Akzo Nobel). In some embodiments, cationic surfactants are preferred, for example, bromide-containing surfactants, such as 1-hexadecyltrimethylammonium bromide.
[0069] Contemplated anionic surfactants include, but are not limited to, ammonium polyacrylate (e.g., DARVAN 821A), modified aqueous polyacrylic acid (e.g., SOKALAN CP10S), phosphate polyether esters (e.g., TRITON H-55), decylphosphonic acid, dodecylphosphonic acid (DDPA), tetradecylphosphonic acid, hexadecylphosphonic acid, octadecylphosphonic acid, dodecylbenzenesulfonic acid, poly(acrylic acid sodium salt), sodium polyoxyethylene lauryl ether, sodium dihexylsulfosuccinate, sodium dicyclohexylsulfosuccinate, sodium 7-ethyl-2-methyl-4-undecyl sulfate (Tergitol 4), SODOSIL RM02, and phosphate fluorosurfactants such as Zonyl FSJ and UR.
[0070] Zwitterionic surfactants include, but are not limited to, acetylenic diols or modified acetylenic diols (e.g. 504), cocamidopropyl betaine, ethylene oxide alkylamine (AOA-8, Sanyo), N,N-dimethyl dodecylamine N-oxide, sodium cocamidopropionate (LebonApl-D, Sanyo), 3-(N,N-dimethyl myristyl ammonium) propane sulfonate and (3-(4-heptyl) phenyl-3-hydroxypropyl) dimethyl ammonium propane sulfonate. Preferably, at least one surfactant comprises dodecylbenzene sulfonic acid, dodecylphosphonic acid, dodecyl phosphate, TRITON X-100, SOKALANCP10S, PEG 400 and PLURONIC F-127.
[0071] When present, the amount of surfactant can be in the range of about 0.001% to about 5% by weight, or 0.001% to about 1% by weight, or about 0.01% to about 1% by weight, or about 0.1% to about 1% by weight, based on the total weight of the composition. Alternatively, it is believed that for some applications, if present, one or more surfactants will account for about 0.1% to about 15% by weight of the composition; or about 0.1% to about 10% by weight of the composition, or about 0.5% to about 5% by weight, or about 0.05% to about 2% by weight, or about 0.5% to about 5% by weight. In an optional embodiment, based on the total weight of the composition, the weight percentage of the surfactant in the composition can be in any range having a starting point and an end point selected from the following: 0.001, 0.01, 0.05, 0.1, 0.5, 1, 2, 4, 5, 8, 10 and 15.
[0072] In some embodiments, the compositions of the present invention will be free or substantially free of any or all of the above-listed surfactants in any combination, or any of the above-listed types of surfactants in any combination.
[0073] Other optional ingredients
[0074] The etching composition of the present invention may also include one or more of the following additives: chemical modifiers, dyes, biocides and other additives. The additives may be added to such an extent that the performance of the composition is not adversely affected. Additives such as dyes, biocides, etc. may be included in the cleaning composition in conventional amounts, for example, in a total amount of up to about 5% by weight of the composition. In some embodiments, the composition of the present invention will be free of or substantially free of any or all of the additives listed above.
[0075] Examples of some embodiments of the present invention will include from about 10% to about 95% by weight, or from about 70% to about 90% by weight, or from about 75% to about 85% by weight of water; from about 0.5% to about 50% by weight, or from about 1% to about 20% by weight, or from 1% to about 15% by weight, or from about 1% to about 10% by weight of at least one basic ammonium compound (pure); from about 0.5% to about 30% by weight, or from about 0.5% to about 20% by weight, or from about 1% to about 15%, or about 1.5% to about 10% by weight of at least one peroxide (pure); about 1% to about 60% by weight, or about 2% to about 30% by weight, or about 5% to about 15% by weight of a water-miscible solvent; about 0.10% to about 10% by weight, or about 0.01% to about 5.0% by weight, or about 0.1% to about 2% by weight, or about 0.1% to about 1.5% by weight, or about 0.40% to about 0.60% by weight of at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; and optionally from about 0.10% to about 10% by weight, or from about 0.01% to about 5.0% by weight, or from about 0.1% to about 2% by weight, or from about 0.1% to about 1.5% by weight of at least one chelating agent.
[0076] In one embodiment, the etching solution is suitable for selectively removing TiSiN relative to hafnium oxide from a microelectronic device, the etching solution consisting essentially of or consisting of: from about 0.5% to about 50% by weight, or from about 1% to about 20% by weight, or 1% to about 15% by weight, or about 1% to about 10% by weight of at least one basic ammonium compound (pure); from about 0.5% to about 30% by weight, or from about 0.5% to about 20% by weight, or 1% to about 10% by weight of at least one basic ammonium compound (pure); 5%, or about 1.5% to about 10% by weight of at least one peroxide (pure); about 1% to about 60% by weight, or about 2% to about 30% by weight, or about 5% to about 15% by weight of a water-miscible solvent; and about 0.10% to about 10% by weight, or about 0.01% to about 5.0% by weight, or about 0.1% to about 2% by weight, or about 0.1% to about 1.5% by weight, or about 0.40% to about 0.80% by weight of at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines, and optionally from about 0.10% to about 10% by weight, or from about 0.01% to about 5.0% by weight, or from about 0.1% to about 2% by weight, or from about 0.1% to about 1.5% by weight of at least one chelating agent, with the remainder being water.
[0077] In another embodiment, an etching solution suitable for selectively removing TiSiN relative to hafnium oxide from a microelectronic device is provided, comprising, consisting essentially of, or consisting of: about 3.7 to about 4.5 weight percent or 3.8 to about 5.6 weight percent (pure) of at least one alkaline ammonium compound selected from ammonium hydroxide, quaternary ammonium hydroxide, ammonium fluoride, and quaternary ammonium fluoride; about 3.9 to about 4.5 weight percent (pure) of at least one peroxide; about 10 to about 15 weight percent or about 7 to about 12 weight percent of a water-miscible organic solvent; about 0.4 to about 0.6 weight percent or about 0.5 to about 1.6 weight percent of at least one selected from C 4-12 nitrogen-containing compounds of alkylamines, polyalkyleneimines, and polyamines; water; and optionally from about 0.4 to about 0.6 weight percent or from about 0.5 to about 1.6 weight percent of a chelating agent.
[0078] In another embodiment, an etching solution suitable for selectively removing polysilicon relative to silicon oxide from a microelectronic device is provided, comprising, consisting essentially of, or consisting of: about 4.1% by weight ammonium hydroxide (pure); about 4.3% hydrogen peroxide (pure); about 0.4 to about 1.2% by weight ammonium fluoride (pure); about 10% water-miscible organic solvent; about 0.30 to about 0.8% or about 0.2 to about 1% of at least one selected from C 4-12nitrogen-containing compounds of alkylamines, polyalkyleneimines, and polyamines; water; and optionally from about 0.30 to about 0.8% or from about 0.2 to about 1% of at least one chelating agent.
[0079] The etching solution compositions of the present invention are typically prepared by mixing the components together in a container at room temperature until all solids are dissolved in the water-based medium.
[0080] method
[0081] In another aspect, a method for selectively increasing the etch rate of TiSiN relative to hafnium oxide in a composite semiconductor device comprising TiSiN and hafnium oxide is provided, the method comprising the steps of: contacting the composite semiconductor device comprising TiSiN and hafnium oxide with an aqueous composition, wherein the composition comprises: water; at least one alkaline ammonium compound selected from ammonium hydroxide, quaternary ammonium hydroxide, ammonium fluoride and quaternary ammonium fluoride; at least one peroxide; a water-miscible organic solvent; at least one selected from C 4-12 A nitrogen-containing compound of an alkylamine, polyalkyleneimine, and polyamine, and optionally at least one chelating agent; and rinsing the composite semiconductor device after at least partially removing the TiSiN, wherein the etch selectivity of the TiSiN relative to hafnium oxide is greater than 30.
[0082] An additional drying step may also be included in the process. "At least partially removed" means at least 50% of the material is removed, preferably at least 80% is removed. Most preferably, 100% is removed using the composition developed in the present invention.
[0083] The contacting step can be performed by any suitable means, such as dipping, spraying or by a single wafer process. The temperature of the composition during the contacting step is preferably about 25 to 100° C., and more preferably about 40 to 75° C. In some embodiments, the contacting step is performed at a temperature of about 60° C. or higher. In other embodiments, the contacting step is performed at a temperature of about 40° C. or higher. In other embodiments, the contacting step is performed at a temperature of about 40° C. to about 80° C. The contacting time may be about 1 to 60 minutes.
[0084] The compositions of the present invention surprisingly exhibit excellent etch selectivity of TiSiN relative to hafnium oxide when used on substrates comprising TiSiN and hafnium oxide, for example in the fabrication of p-type microelectronic devices. The term "selectivity" is generally used to refer to the ratio of the etching rates of two materials. In some embodiments, the compositions according to the present invention exhibit a wet etch selectivity of TiSiN / hafnium oxide of >10. In other embodiments, the etch rate selectivity of TiSiN / hafnium oxide is >30. In other embodiments, the etch rate selectivity of TiSiN / hafnium oxide is >100. In other embodiments, the etch rate selectivity of TiSiN / hafnium oxide is >500. In other embodiments, the etch rate selectivity of TiSiN / hafnium oxide is >1000. In other embodiments, the etch rate selectivity of TiSiN / hafnium oxide is >3000. In other embodiments, the etch rate selectivity of TiSiN / hafnium oxide is >5000.
[0085] The contacting step is followed by an optional rinsing step. The rinsing step can be performed in any suitable manner, for example, by rinsing the substrate with deionized water by immersion or spraying techniques. In a preferred embodiment, a mixture of deionized water and an organic solvent (e.g., isopropanol) can be used for the rinsing step.
[0086] The contacting step and optional rinsing step are followed by an optional drying step, which is performed by any suitable means, for example, isopropyl alcohol (IPA) vapor drying, heating, or by centripetal force.
[0087] Features and advantages are more fully illustrated by the illustrative embodiments discussed below. Example
[0088] General Procedure for Preparing Cleaning Compositions
[0089] All compositions that are the subject of this example were prepared by mixing the components in a 250 mL beaker with a 1 / 2" Teflon-coated stir bar. Typically, the first material added to the beaker was deionized (DI) water, followed by the other ingredients in no particular order.
[0090] Processing conditions
[0091] Etching tests were conducted using 100 g of the etching composition in a 250 ml beaker with a 1 / 2" round Teflon stirring bar set at 400 rpm. The etching composition was heated on a hot plate to a temperature of about 40 to 60°C. The coupons were immersed in the composition for about 10 minutes with stirring.
[0092] The segments were then rinsed in a deionized water bath or spray for 3 minutes and subsequently dried using filtered nitrogen. The etch rates were measured for TiSiN wafers at 40°C to 60°C for 2 minutes and for HfO2 wafers for 10 minutes. TiSiN and HfO2 etch rates were measured by ellipsometer (SCIFilmTek SE2000). The etch rates were calculated by dividing the thickness difference before and after treatment by the immersion time. The typical starting layer thickness of TiSiN is The initial thickness of the hafnium oxide layer is
[0093] The temperature of the etching solution when used can be appropriately determined according to the etching conditions or the material of the substrate used.
[0094] The treatment time when the etching treatment is performed using the TiSiN etching solution disclosed herein, i.e., the time required to etch TiSiN, is generally in the range of about 0.1 to about 10 minutes, preferably 0.2 to 8 minutes and more preferably 0.3 to 5 minutes, and can be appropriately determined according to the etching conditions or the material of the substrate used.
[0095] The formulations evaluated below demonstrate that the hafnium oxide etch rate can be suppressed by adding an oxide inhibitor to the alkaline formulation. Once the inhibitor is added, the TiSiN / hafnium oxide etch rate selectivity can be maintained.
[0096] For comparison purposes, the following data provides a performance baseline for prior art SC1 etch performance.
[0097] Table 1: HfO2 etching rate in SC1 (NH4OH / H2O2 / DIW=1:1:5)
[0098] SC1 TiSiN <![CDATA[HfO2]]> <![CDATA[TiSiN / HfO2]]> 50℃ 25.1 0.3 83.8 55℃ 36.0 0.5 71.9 60℃ 48.0 0.8 60.1
[0099] Unit: A / min
[0100] In addition to the e / r of HfO2 on blanket wafers, XPS was used to examine the loss of HfO2 when treated with SC1. The HfO2 samples were treated with SC1 at 60°C for 10 minutes, and then XPS analysis was performed to examine the HfO2 loss by monitoring the Hf intensity.
[0101] Potential candidates for HfO2 protection have been screened as listed in Table 2. It was found that molecules with amine functional groups provided the best HfO2 protection. XPS results also supported better protection of HfO2 by adding PMDETA to SC1.
[0102] Table 2. Studies on HfO2 corrosion inhibition
[0103]
[0104]
[0105] in 485, 607 is a nonionic surfactant. 10 is an anionic surfactant, CTAB is a cationic surfactant, and 800 is a nitrogen-containing polymer; and H2O2 is a 30% aqueous solution.
[0106] The results are displayed graphically in Figure 1 middle.
[0107] For TiSiN patterning, SC1 gave an acceptable TiSiN etch rate of 20-30 angstroms / min at 50°C. However, after removing the bulk TiSiN film, some Si residues were found on the HfO2 surface. It is desirable to improve the Si removal capability of SC1.
[0108] In terms of redox reaction, Si in TiSiN is oxidized to SiO2 in the presence of hydrogen peroxide. Increasing the SiO2 etching rate of SC1 may help minimize the Si residue in the intermixed layer.
[0109] The solvent effect and the increase in SiO2 etching rate of the SiO2 etchant were examined. The results are shown in Table 3.
[0110] Table 3. Effect of solvent on TiSiN and TEOS etch rates.
[0111]
[0112]
[0113] From Table 3, it can be seen that the addition of 10% organic co-solvents such as sulfolane and BDG helps to increase the etch rates of both TiSiN and TEOS compared to the DIW solvent system.
[0114] As shown in Table 4, the TEOS etch rate can be further increased by adding NH4F.
[0115] Table 4. Effect of NH4F on TiSiN and TEOS etching rates
[0116]
[0117] Table 5. Effect of temperature on formulation 524O
[0118] 524O TiSiN TEOS <![CDATA[HfO2]]> 50℃ 39.1 2.7 0.01 55℃ 47.3 3.4 0.02 60℃ 56.8 4.7 0.08
[0119] TiSiN and TEOS etch rates can be increased by increasing the temperature as shown in Table 5, while keeping the HfO2 etch rate low.
[0120] A double layer (TiSiN on HfO2) sample was used to examine whether the TEOS etch rate is a good indicator for removing Si residues on the HfO2 surface. For comparison, the TiSiN layer was etched by 524O and SC1. XPS was then performed to examine the Si signal on the HfO2 surface. Figure 2 It can be seen that the Si signal is significantly reduced after treatment with 524O compared to SC1.
[0121] XPS analysis shows that the oxide etch rate is a good indicator for the removal of Si residues in the intermixed layer.
[0122] The foregoing description is primarily for illustrative purposes. Although the present invention has been shown and described with respect to its exemplary embodiments, it will be appreciated by those skilled in the art that the foregoing and various other changes, omissions and additions may be made in form and detail without departing from the spirit and scope of the present invention.
Claims
1. An etching solution suitable for selectively removing TiSiN relative to hafnium oxide from microelectronic devices, comprising: composition: water; From about 3.7 to about 4.5 weight percent pure ammonium hydroxide; from about 3.9 to about 4.5 weight percent of pure at least one peroxide; a water-miscible organic solvent; and At least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; Wherein "about" is intended to correspond to ±5% of the stated value.
2. The etching solution of claim 1, wherein the water-miscible organic solvent is selected from the group consisting of sulfolane, dimethyl sulfoxide, and propylene glycol; and the at least one peroxide is hydrogen peroxide.
3. The etching solution of claim 2, wherein the at least one nitrogen-containing compound is selected from the group consisting of pentamethyldiethylenetriamine, triethylenediamine, triethylenetetramine, tetramethylethylenediamine and diethylenetriamine.
4. The etching solution of claim 2, wherein the at least one nitrogen-containing compound is octylamine.
5. The etching solution of claim 2, wherein the at least one nitrogen-containing compound is the polyalkylene imine.
6. The etching solution of claim 5, wherein the polyalkylene imine is polyethylene imine.
7. The etching solution of claim 2, wherein the at least one nitrogen-containing compound is pentamethyldiethylenetriamine.
8. The etching solution of any one of the preceding claims, further comprising a surfactant.
9. A method for selectively increasing the etching rate of TiSiN relative to hafnium oxide in a composite semiconductor device comprising TiSiN and hafnium oxide, the method The following steps are involved: contacting the composite semiconductor device comprising TiSiN and hafnium oxide with an etching solution as claimed in any one of claims 1 to 8; and The composite semiconductor device is rinsed after at least partially removing the TiSiN, wherein an etch selectivity of the TiSiN relative to hafnium oxide is greater than 30.
10. The method of claim 9, further comprising the step of drying the semiconductor device.
11. The method of claim 9 or 10, wherein the etching selectivity of TiSiN to hafnium oxide is greater than 500.
12. The method of claim 9 or 10, wherein the etch selectivity of TiSiN to hafnium oxide is greater than 1,000.
13. The method of claim 9 or 10, wherein the contacting step is performed at a temperature of about 60°C or higher, wherein "about" is intended to correspond to ±5% of the stated value.
14. An etching solution suitable for selectively removing TiSiN relative to hafnium oxide from microelectronic devices, comprising: composition: From about 3.7 to about 4.5 weight percent pure ammonium hydroxide; from about 3.9 to about 4.5 weight percent of pure at least one peroxide; from about 10 to about 15 weight percent of a water-miscible organic solvent; About 0.4 to about 1% by weight of at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; and water; Wherein "about" is intended to correspond to ±5% of the stated value.
15. The etching solution of claim 14, wherein The at least one peroxide is hydrogen peroxide; The water miscible organic solvent is selected from sulfolane, propylene glycol and dimethyl sulfoxide; and The at least one nitrogen-containing compound is selected from octylamine, pentamethyldiethylenetriamine and polyethyleneimine.
16. An etching solution suitable for selectively removing TiSiN relative to hafnium oxide from microelectronic devices, comprising: composition: about 4.1% by weight of pure ammonium hydroxide; about 4.3% by weight pure hydrogen peroxide; From about 0.4 to about 1.2 weight percent pure ammonium fluoride; about 10% by weight of a water-miscible organic solvent; About 0.30 to about 1% by weight of at least one selected from C 4-12 Nitrogen-containing compounds of alkylamines, polyalkyleneimines and polyamines; and water; Wherein "about" is intended to correspond to ±5% of the stated value.
17. The etching solution of claim 16, wherein The water-miscible organic solvent is selected from sulfolane, propylene glycol and dimethyl sulfoxide; and The at least one nitrogen-containing compound is selected from octylamine, pentamethyldiethylenetriamine and polyethyleneimine.