Electro-photonic assembly and assembly with electrochromic gel layer
By using an electroactive gel layer dispersed in a polymer matrix in the electro-optic assembly, the electrochemical and electro-optic properties of electrochromic materials in large-size electro-optic assemblies were solved, achieving feasibility for large-scale production and performance stability.
Patent Information
- Application Number
- CN202080024291.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-03-27
Smart Images

Figure CN113614629B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure generally relates to electro-optical assemblies and assemblies including electrochromic gel layers. More specifically, the present disclosure relates to electro-optical assemblies including anode or cathode gel layers on polymer substrates that can be assembled to form electro-optical assemblies. Background Art
[0002] Electro-optical assemblies incorporating electrochromic materials have been utilized in various devices to provide variability in color and transmittance when a voltage potential is applied. For example, an electro-optical assembly may be incorporated into a mirror to form an electrochromic mirror in which reflectivity may vary based on an applied voltage. In another example, an electro-optical assembly may be incorporated into a window to form an electrochromic window in which the transmission of light may vary based on an applied voltage. Conventional electro-optical assemblies are typically solution-based, wherein the electrochromic material is supplied to the chamber of the electro-optical assembly in the form of a solution. As the size of the electrochromic device increases, conventional solution-based electrochromic materials may not provide the desired electrochemical and electro-optical properties, or may not be suitable for large-scale manufacturing.
[0003] There is a need for materials and methods for forming electro-optical assemblies that address some of the challenges associated with solution-based electrochromic materials and provide opportunities for large-scale manufacturing. Summary of the invention
[0004] According to one aspect of the present disclosure, an electro-photonic assembly comprises a substrate web, a conductive layer disposed on the substrate web, and an electroactive gel layer disposed on the conductive layer, wherein the electroactive gel layer comprises an electroactive component dispersed in a polymer matrix, the electroactive gel layer has a certain thickness, and wherein the thickness variation of the electroactive gel layer accounts for less than about 20% of the average thickness of the electroactive gel layer.
[0005] According to one aspect of the present disclosure, an electro-optical assembly includes a cathode subassembly and an anode subassembly. The cathode subassembly includes a first substrate web, a first conductive layer disposed on the first substrate web, and a cathode gel layer disposed on the first conductive layer, wherein the cathode gel layer includes a cathode component dispersed in a polymer matrix, and the cathode gel layer has a certain thickness. The anode subassembly includes a second substrate web, a second conductive layer disposed on the second substrate web, and an anode gel layer disposed on the second conductive layer, wherein the anode gel layer includes an anode component dispersed in a polymer matrix, the anode gel layer has a certain thickness, and wherein at least one of the cathode component and the anode component is electro-optical, and the thickness of at least one of the cathode gel layer and the anode gel layer varies by less than about 20% of the average thickness of the corresponding gel layer.
[0006] These and other aspects, objects and features of the present disclosure will be understood and appreciated by those skilled in the art after studying the following specification, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] In the attached picture:
[0008] Figure 1 is a schematic cross-sectional view of an electro-optical assembly according to one aspect of the present disclosure;
[0009] Figure 2 According to one aspect of the present disclosure, Figure 1 A schematic cross-sectional view of a cathode subassembly and an anode subassembly of an electro-optical assembly;
[0010] Figure 3 is a flow chart illustrating a method of assembling an electro-optical assembly according to one aspect of the present disclosure;
[0011] Figure 4 is a schematic representation of a process for forming a conductive layer according to one aspect of the present disclosure;
[0012] Figure 5 is a schematic representation of a roll-to-roll process for forming an electro-photonic assembly according to one aspect of the present disclosure;
[0013] Figure 6 is a schematic representation of a process for applying an electrochromic gel composition according to one aspect of the present disclosure;
[0014] Fig. 7A is a top-down view of an electrochromic gel pattern according to one aspect of the present disclosure;
[0015] Figure 7B is a top-down view of an electrochromic gel pattern according to one aspect of the present disclosure;
[0016] Figure 7C is a top-down view of an electrochromic gel pattern according to one aspect of the present disclosure;
[0017] Figure 8 is an exploded view of an electrochromic device according to one aspect of the present disclosure;
[0018] Fig. 9 is a cross-sectional view of an electrochromic device according to one aspect of the present disclosure; and
[0019] Fig.10 is a cross-sectional view of an electrochromic device according to one aspect of the present disclosure. DETAILED DESCRIPTION
[0020] The presently presented aspects are primarily directed to combinations of method steps and apparatus components associated with electrochromic films for electro-optical elements and devices. Accordingly, apparatus components and method steps have been represented by conventional symbols in the accompanying drawings where appropriate, and only those specific details relevant to understanding aspects of the present disclosure are shown so as not to obscure the present disclosure with details that would be apparent to one of ordinary skill in the art having the benefit of the description herein. In addition, like numbers in the description and drawings represent like elements.
[0021] As used herein, the term "and / or" when used in a list of two or more items means that any one of the listed items may be taken alone, or any combination of two or more of the listed items may be taken. For example, if a composition is described as containing components A, B, and / or C, the composition may contain: A only; B only; C only; a combination of A and B; a combination of A and C; a combination of B and C; or a combination of A, B, and C.
[0022] In this document, for example, relational terms such as first and second, top and bottom are used only to distinguish one entity or action from another entity or action, and do not necessarily require or imply any actual such relationship or order between such entities or actions. The term "comprises" or any other variation thereof is intended to cover non-exclusive inclusions, so that a process, method, article, or device that includes a series of elements does not only include those elements, but may include other elements that are not explicitly listed or are not inherent to such process, method, article, or device. In the absence of more constraints, an element preceded by "including..." does not exclude the presence of additional identical elements in the process, method, article, or device that includes the element without more restrictions.
[0023] As used herein, "about" will be understood by one of ordinary skill in the art and will vary to some extent depending on the context in which it is used. If the use of this term is not clear to one of ordinary skill in the art, then "about" will mean up to plus or minus 10% of this particular term, given the context in which it is used.
[0024] The presently presented embodiments are primarily concerned with a combination of method steps and apparatus components associated with an electro-optical assembly formed from a pair of electro-optical assemblies. One of the electro-optical assemblies in the pair is formed from a substrate web such as a polymer web or a glass web, on which a conductive layer and an electroactive gel layer containing a cathode component are provided, while the other of the electro-optical assemblies in the pair is formed from a substrate web such as a polymer web or a glass web, on which a conductive layer and an electroactive gel layer containing an anode component are provided. Each of the electro-optical assemblies in the pair of electro-optical assemblies can be formed separately and merged together to form an electro-optical element having both a cathode component and an anode component. Each of the electro-optical assemblies in the pair of electro-optical assemblies can be formed from a substrate web from which a plurality of electro-optical assemblies can be cut. The electro-optical assemblies and methods disclosed herein that utilize a substrate web as a substrate can facilitate large-scale production of electro-optical assemblies and provide advantages in separately forming and / or storing cathode and anode electroactive gel layers.
[0025] Therefore, the device components and method steps have been represented by conventional symbols in the drawings where appropriate, and only those specific details relevant to understanding the embodiments of the present disclosure are shown so as not to obscure the present disclosure with details that are obvious to those of ordinary skill in the art who may benefit from this specification. In addition, the same numbers in the description and drawings represent the same elements.
[0026] Structure and materials
[0027] refer to Figure 1-2, an electro-optical assembly 10 according to aspects of the present disclosure is provided. The electro-optical assembly 10 includes a pair of electro-optical subassemblies in the form of a cathode subassembly 12 and an anode subassembly 14, wherein at least one of the electro-optical subassemblies includes an electrochromic component. The cathode subassembly 12 includes a first substrate 20 having a first surface 22 and a second surface 24. An optional first barrier layer 26 is disposed on the second surface 24 and between a first conductive layer 28 and the second surface 24. A cathode gel layer 30 including a cathode component dispersed in a polymer matrix is disposed on the first conductive layer 28. As used herein, the term "dispersed" when used to describe a specific component relative to a polymer matrix is used to mean that at least a portion of the molecules of the specific component are able to move within the polymer matrix (also referred to as being movable within the polymer matrix) and / or at least a portion of the molecules of the specific component are physically and / or chemically bonded or trapped within the polymer matrix so that their movement within the polymer matrix is restricted (also referred to as being immobile within the polymer matrix).
[0028] The anode subassembly 14 includes a second substrate 32 having a third surface 34 and a fourth surface 36. An optional second barrier layer 38 is disposed on the third surface 34 and between the second conductive layer 40 and the third surface 34. An anode gel layer 42 comprising an anode component dispersed in a polymer matrix is disposed on the second conductive layer 40. In some aspects, the anode component and the cathode component can exhibit electrochromic behavior and can therefore be alternatively referred to as chromophores or electrochromic molecules. In some aspects, the cathode component and the anode component are both electroactive, and at least one of them is electrochromic. It should be understood that, regardless of its ordinary meaning, the term "electroactive" is used herein to refer to a material that undergoes an oxidation state change when exposed to a specific potential difference. Regardless of its ordinary meaning, the term "electrochromic" is used herein to refer to a material that exhibits a change in extinction coefficient at one or more wavelengths when exposed to a specific potential difference. As described herein, an electrochromic component comprises a material whose color and / or opacity is affected by an electric current such that when an electric field is applied to the material, the color and / or opacity changes from a first phase to a second phase. In another aspect of the disclosure, the anode component and / or cathode component can be an electroactive component in the form of liquid crystal molecules or suspended particles. Non-limiting examples of electroactive and / or electrochromic components are described in the following: U.S. Patent No. 5,928,572, issued on July 27, 1999, and entitled “Electrochromic Layer And Devices Comprising Same”; U.S. Patent No. 5,998,617, issued on December 7, 1999, and entitled “Electrochromic Compounds”; U.S. Patent No. 6,020,987, issued on February 1, 2000, and entitled “Electrochromic Medium Capable Of Producing A Pre-selected Color”; U.S. Patent No. 6,020,987, issued on March 14, 2000, and entitled “Electrochromic Compounds”. No. 6,037,471, entitled “Electrochromic Compounds”, issued on October 31, 2000; No. 6,141,137, entitled “Electrochromic Media For Producing A Pre-selected Color”, issued on October 31, 2000; No. 6,241,916, entitled “Electrochromic System”, issued on June 5, 2001;U.S. Patent No. 6,193,912, issued on February 27, 2001, and entitled “Near Infrared-Absorbing Electrochromic Compounds And Devices Comprising Same”; U.S. Patent No. 6,249,369, issued on June 19, 2001, and entitled “Coupled Electrochromic Compounds With Photostable Dication Oxidation States”; U.S. Patent No. 6,249,369, issued on October 24, 2000, and entitled “Electrochromic Media With Concentration Enhanced Stability, Process For The Preparation Thereof and Use In Electrochromic Devices”; No. 6,137,620, entitled “Electrochromic Devices”; No. 6,519,072, issued on February 11, 2003 and entitled “Electrochromic Device”; and International Patent Application Serial No. PCT / US98 / 05570, entitled “Electrochromic Polymeric Solid Films, Manufacturing Electrochromic Devices Using Such Solid Films, And Processes For Making Such Solid Films And Devices”, published on October 1, 1998 as WO1998 / 042796; International Patent Application Serial No. PCT / EP98 / 03862, entitled “Electrochrome Polymer System”, published on January 21, 1999 as WO1999 / 02621;and International Patent Application Serial No. PCT / US98 / 05570, entitled “Electrochromic Polymeric Solid Films, Manufacturing Electrochromic Devices Using Such Solid Films, And Processes For Making Such Solid Films And Devices,” published on October 1, 1998 as WO1998 / 042796, all of which are incorporated herein by reference in their entirety. Non-limiting examples of cathode components according to the present disclosure include viologens, viologen derivatives, methyl viologens, octyl viologens, benzyl viologens, di-acrylate viologens, di-vinyl viologens, di-vinyl ether viologens, di-epoxy viologens, di-oxetane viologens, di-hydroxy viologens, 1,1'-dialkyl-2,2'-bipyridinium, ferrocenium, substituted ferrocenium, imides, N,N'-dialkylpyromellitic acid imides, N,N'-dimethyl-1,4,5,8-naphthalene diimide, and combinations thereof. Exemplary viologen derivatives are described in the following: U.S. Pat. Nos. 4,902,108, 6,188,505, 5,998,617, 9,964,828, and 6,710,906, the contents of which are incorporated herein by reference in their entirety. Non-limiting examples of anode components include metallocenes, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazines, substituted phenothiazines, substituted dithiazines, thianthrene, substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl-5,10-dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT), and combinations thereof. ;
[0029] The second surface 24 of the first substrate 20 and the third surface 34 of the second substrate 32 at least partially define a chamber 50 in which at least the cathode gel layer 30 and the anode gel layer 42 are disposed. A sealing member 52 may be disposed around the chamber 50 to protect the contents of the chamber 50 from oxygen and / or moisture. Figure 1Schematically illustrated as being located between the second surface 24 on the first substrate 20 and the third surface 34 of the second substrate 32, but other configurations of the sealing member 52 are possible and within the scope and spirit of the present disclosure. The sealing member 52 can be positioned around the perimeter of the device in a "C" shaped configuration, can be located remotely, or can be any number of other configurations that will vary depending on the end use of the electro-optical assembly 10. For simplicity, the sealing member 52 is referred to herein as being between the first substrate 20 and the second substrate 32, but such a configuration should be understood to be non-limiting to the present disclosure, and unless explicitly stated, an example or description of a device can be configured to have different variations of the sealing member 52.
[0030] One or both of cathode subassembly 12 and anode subassembly 14 may include additional layers, non-limiting examples of which include polarizers, anti-reflection layers, filters, resistive layers, UV light reflecting or absorbing layers, gas diffusion barriers, water vapor diffusion barriers, etc. In some examples, cathode gel layer 30 and / or anode gel layer 42 may include an ion conducting layer disposed thereon. The ion conducting layer may be configured to resist H + or Li + Ions with equal positive charges are conductive, but the conductivity of electrons is low in comparison.
[0031] The first substrate 20 and the second substrate 32 may be formed of the same or different materials. The first substrate 20 and / or the second substrate 32 may be formed of any suitable polymer material, glass material, or glass ceramic material. Non-limiting examples of suitable polymer materials for forming the first substrate 20 and / or the second substrate 32 include polyethylene (e.g., low density and / or high density), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone, acrylic polymer (e.g., poly(methyl methacrylate) (PMMA)), polymethacrylate, polyimide, polyamide (e.g., alicyclic diamine dodecanedioic acid polymer, such as polyurethane), polyimide, polyamide (e.g., ...imide, polyamide (e.g., polyurethane), polyimide, polyimide, polyamide (e.g., polyurethane), polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, polyimide, CX7323)), epoxy resin, cycloolefin polymer (COP) (e.g., Zeonor 1420R), cycloolefin copolymer (COC) (e.g., Topas 6013S-04 or Mitsui Apel), polymethylpentene, cellulose ester plastics (e.g., cellulose triacetate), transparent fluoropolymers, polyacrylonitrile, other polymer materials and / or combinations thereof. Non-limiting examples of suitable glass materials include borosilicate glass and soda-lime glass.
[0032] The first barrier layer 26 and the second barrier layer 38 may be formed of the same or different materials. The first barrier layer 26 and the second barrier layer 38 may be provided to protect the first substrate 20 and the second substrate 32 from interacting with the contents of the chamber 50, such as solvents, which may be harmful and / or may degrade the first substrate 20 and / or the second substrate 32, especially when the first substrate 20 and the second substrate 32 are made of polymer materials. In some aspects, the first barrier layer 26 and the second barrier layer 38 provide resistance to oxygen and / or water penetration. The first barrier layer 26 and the second barrier layer 38 may also be configured to reduce the degradation of the first conductive layer 28 and the second conductive layer 40 caused by the interaction with the contents of the chamber 50. In one aspect, the first barrier layer 26 and / or the second barrier layer 38 may be used in combination with the corresponding first conductive layer 28 and the second conductive layer 40 to form an insulator-metal-insulator (IMI) stack. The IMI stack may include a silver metal or silver metal alloy layer, a conductive layer 26, 40, and a polymer resin layer. The polymer resin layer may be selected from an acrylic polymer resin, a siloxane-based resin, polyethylene terephthalate (PET), a polyester resin, poly(methyl methacrylate) (PMMA), a polycarbonate resin, or a combination thereof. Exemplary IMI stacks for use as barrier layers 26 and 38 are disclosed in U.S. Provisional Patent Application No. 62 / 769,693, entitled “Plastic Coatings for Improved Solvent Resistance,” filed on November 20, 2018, and U.S. Provisional Patent Application No. 62 / 660,018, entitled “Plastic Coatings for Improved Solvent Resistance,” filed on April 19, 2018, the contents of which are incorporated herein by reference in their entirety.
[0033] In another example, the first barrier layer 26 and / or the second barrier layer 38 may comprise a polymer multilayer film. A polymer multilayer (PML) film is typically composed of alternating layers of cross-linked polymer layers and inorganic layers to form an optically transparent, flexible oxygen and water barrier that provides resistance to oxygen and water penetration into the chamber 50. An example of a commercially available PML barrier film is 3M TMA line of flexible transparent barrier (FTB) film products are provided. An exemplary process for forming a PML barrier layer comprises applying a first polymer to a polymer substrate by flash evaporation and vapor deposition of a monomer, followed by plasma, UV or electron beam curing. The first polymer layer can also be applied by printing, slot die coating or spraying, followed by UV or electron beam curing. The inorganic layer can then be applied under vacuum or ambient pressure using conventional sputtering, evaporation, atomic layer deposition, spraying and / or other deposition methods. The final polymer layer is applied on top of the inorganic layer using a flash evaporation method or other methods listed above. Optionally, another inorganic layer can be applied on top of the polymer layer. In one aspect, the PML structure or stack can be three layers, four layers or more. The polymer layer can include volatile monomers that can be cross-linked into a transparent polymer, examples of which include volatile monomers that can be obtained from Diacrylates such as SR833S, SR351, SR3238B and SR9003B, or other volatile monomers are available. Suitable inorganic layer materials include metal oxides, metal nitrides, aluminum oxide, silicon oxide, indium tin oxide, silicon nitride and combinations thereof. Other PMLs comprising alternative combinations of polymer layers and inorganic layers may also be used.
[0034] Examples of commercially available polymer substrates having barrier layers provided thereon include the FTB3-125 barrier film available from 3M, which 3M describes as a polyethylene terephthalate (PET) substrate having two vacuum deposited polymer layers and an inorganic oxide layer positioned between the two polymer layers. The FTB-125 product can be used to provide the first substrate 20 and / or the second substrate 32 to which the respective barrier layers 26, 38 have been applied. Commercially available IMI stacks suitable for use as the first substrate 20 and / or the second substrate 32 to which the respective barrier layers 26, 38 have been applied include silver-based IMI stacks commercially available from TDK Corporation, to which an additional transparent conductive oxide (TCO) layer such as indium tin oxide (ITO) has been applied to the exposed surface of the IMI stack.
[0035] The first conductive layer 28 and the second conductive layer 40 may be formed of the same or different materials. Depending on the end use of the electro-optical assembly 10, one or both of the first conductive layer 28 and the second conductive layer 40 may be transparent, and optionally one of the layers may be opaque. Non-limiting examples of suitable transparent materials for the first conductive layer 28 and / or the second conductive layer 40 include transparent conductive oxides (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide (for example, the metal may be any suitable metal or metal alloy such as silver, gold, palladium, silver alloy, gold alloy, palladium alloy, silver-gold alloy, and silver-palladium alloy), silver nanowire coatings, carbon nanotubes, graphene coatings, conductive nanorods, wire grids, and conductive polymers, examples of which include poly (3,4-ethylenedioxythiophene) (PEDOT). Suitable opaque materials for use as the conductive layer include metal coatings such as rhodium, chromium, nickel, silver, gold, and other metals, or mixtures of any two or more thereof. In one aspect, at least one layer can be deposited by atomic layer deposition (ALD) between the first conductive layer 28 and / or the second conductive layer 40 and the IMI stack barrier layer 26, 38. ALD deposited materials can include aluminum oxide, titanium dioxide, and AZO.
[0036] The cathode gel layer 30 comprises cathode components dispersed in a polymer gel matrix. The cathode gel layer 30 is formed as a free-standing (permanent) gel in which an electrochromic medium containing the cathode components is dispersed such as scattered and / or entrapped in the polymer matrix, and the free-standing (permanent) gel continues to behave similar to a solution. In one aspect, more than one cathode component may be included in the cathode gel layer 30. According to one aspect of the present disclosure, at least a portion of the cathode components dispersed within the polymer matrix is mobile within the polymer matrix. According to another aspect, at least a portion of the cathode components dispersed within the polymer matrix is immobile within the polymer matrix. For example, at least a portion of the cathode components dispersed within the polymer matrix may be chemically bonded to the polymer matrix and / or physically entrapped within the polymer matrix. In one example, at least a portion of the cathode components is functionalized such that the cathode components are capable of reacting with the polymer matrix so that the functionalized cathode components may be covalently bonded to the polymer matrix. Examples of cathode components chemically bonded or physically entrapped within the polymer matrix can be found in U.S. Patent No. 9,964,828, entitled "Electrochemical Energy Storage Devices," published on May 8, 2018, the entire content of which is incorporated herein by reference in its entirety. Non-limiting examples of suitable cathode components include viologens and metal oxides such as tungsten. Exemplary viologens include, but are not limited to, methyl viologen, octyl viologen, benzyl viologen, and polymeric viologen. In one aspect, the cathode component is octyl viologen. In some aspects, the cathode component may comprise crystalline or nanocrystalline tungsten oxide (WO x , where 2.6 < x < 3.4), vanadium oxide (V2O5), nickel oxide (NiO), ferrocenium, perovskite materials such as samarium nickelate (SmNiO3), or other metal oxides of the formula A y B z O x , where A and B are metals. The relative amounts of components A and B may vary such that y and z may each be any value from about 1 to about 20. For example, y and z may each be any value from about 1 to about 20, from about 1 to about 15, from about 1 to about 10, from about 1 to 5, or from about 1 to about 3. Present in the formula A y B z O xThe amount of oxygen in the metal oxide of can vary based at least in part on the oxidation state of metals A and B and their relative amounts in the film. According to one aspect, the value of x will nominally be at a level sufficient to achieve stoichiometry. For example, the value of x can be about 80% to about 120% of its stoichiometric value. In some instances, the value of x can be about 80% to about 120%, about 80% to about 110%, about 80% to about 100%, about 90% to about 120%, about 90% to about 110%, about 90% to about 100%, about 95% to about 120%, about 95% to about 110%, about 95% to about 105%, or about 90% to about 100% of the stoichiometric value. The concentration of the cathode component in the cathode gel layer 30 can be about 10 millimolar (mM) to about 200 mM.
[0037] The anode gel layer 42 comprises an anode component dispersed in a polymer gel matrix. The anode gel layer 42 is formed as an independent (permanent) gel, wherein the electrochromic medium comprising the anode component is dispersed such as dispersed and / or entrapped in the polymer matrix, and the independent (permanent) gel continues to behave similarly to a solution. In one aspect, more than one anode component may be included in the anode gel layer 42. According to one aspect of the present disclosure, at least a portion of the anode component dispersed in the polymer matrix is movable in the polymer matrix. According to another aspect, at least a portion of the anode component dispersed in the polymer matrix is immobile in the polymer matrix. For example, at least a portion of the anode component dispersed in the polymer matrix can be chemically bonded to the polymer matrix and / or physically entrapped in the polymer matrix. In one example, at least a portion of the anode component is functionalized so that the anode component can react with the polymer matrix so that the functionalized anode component can be covalently bonded to the polymer matrix. Examples of anode components chemically bonded or physically entrapped within a polymer matrix can be found in U.S. Patent No. 9,964,828, entitled “Electrochemical Energy Storage Devices,” published on May 8, 2018, the entire contents of which are incorporated herein by reference in their entirety. Non-limiting examples of suitable anode components include metallocenes, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazines, substituted phenazines, and substituted phenothiazines, including substituted dithiazines, thianthrene and substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl-5,10-dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, and bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT). In one aspect, the anode component comprises 5,10-dihydro-5,10-dimethylphenazine. In another aspect, the anode component comprises a combination of 5,10-dihydro-5,10-dimethylphenazine and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine, 5,10-triethylammoniumpropylphenazine. The total concentration of the anode component can be from about 10 mM to about 130 mM.
[0038] The cathode gel layer 30 and the anode gel layer 42 may be formed as separate gels comprising at least one solvent and a cross-linked polymer matrix. As described in more detail below, because each of the cathode subassembly 12 and the anode subassembly 14 is formed separately on their respective substrates, the cathode gel layer 30 and the anode gel layer 42 are preferably formed to have sufficient rigidity to maintain their shape (thickness and length and width dimensions) during processing until the subassemblies 12, 14 are assembled to form the electro-optical assembly 10. In one aspect, the cathode gel composition and the anode gel composition are configured such that the shape change between the initially deposited gel composition and the final cured gel layer is less than about 30%, less than about 20%, or less than about 10%.
[0039] The cathode gel layer 30 and the anode gel layer 42 can have the same or different thicknesses. In one aspect, the thicknesses of the cathode gel layer 30 and the anode gel layer 42 can be in the range of about 20 micrometers (μm) to about 500 μm, about 20 μm to about 400 μm, about 20 μm to about 300 μm, about 20 μm to about 200 μm, about 20 μm to about 100 μm, about 20 μm to about 50 μm, about 50 μm to about 500 μm, about 50 μm to about 400 μm, about 50 μm to about 3 ...20 μm to about 500 μm, about 20 μm to about 100 μm, about 20 μm to about 50 μm, about 20 μm to about 500 μm, about 20 μm to about 400 μm, about 20 μm to about 300 μm, about 20 μm to about 300 μm, about 20 μm to about 300 μm, about 20 μm to about 300 μm, about 20 μm to about 300 μm, about 20 μm to about 300 μm, about 20 μm to about 300 μm, about 20 μ In the range of about 200μm, about 50μm to about 100μm, about 100μm to about 500μm, about 100μm to about 400μm, about 100μm to about 300μm, about 100μm to about 200μm, about 200μm to about 500μm, about 200μm to about 400μm, about 200μm to about 300μm, about 300μm to about 500μm, about 300μm to about 400μm, or about 400μm to about 500μm.
[0040] In some aspects of the present disclosure, the cathode gel layer 30 and / or the anode gel layer 42 may have a predetermined thickness variation. For example, the thickness of the cathode gel layer 30 and / or the anode gel layer 42 may be determined by a maximum measured thickness Th. MAX , minimum measurement thickness Th MIN , average thickness Th AVG and is defined as (Th MAX -Th MIN ) is characterized by a thickness variation. In some aspects, the cathode gel layer 30 and / or the anode gel layer 42 can be configured such that the thickness variation of the layer is less than the average thickness Th of the corresponding layer. AVG For example, the cathode gel layer 30 and / or the anode gel layer 42 may be configured such that the thickness variation of the layer is less than the average thickness Th AVGThe cathode gel layer 30 and / or the anode gel layer 42 may be configured to satisfy the desired thickness variation over the entire area or a portion of the area of the corresponding layer. For example, the cathode gel layer 30 and / or the anode gel layer 42 may be configured such that the layer has a desired thickness variation over greater than about 50% of the layer area, greater than about 65% of the layer area, greater than about 75% of the layer area, greater than about 85% of the layer area, or greater than about 95% of the layer area.
[0041] In one aspect, the polymer matrix forming the cathode gel layer 30 and / or the anode gel layer 42 is formed by crosslinking polymer chains, wherein the polymer chains are formed by polymerization of at least one monomer. Non-limiting examples of suitable monomers include methyl methacrylate, methyl acrylate, isocyanatoethyl methacrylate, 2-isocyanatoethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 3-hydroxypropyl methacrylate, glycidyl methacrylate, 4-vinylphenol, acetoacetoxy methacrylate, and acetoacetoxy acrylate. The at least one monomer may be prepolymerized and dispersed and / or dissolved in a suitable solvent system before the solution is applied to the substrate or after the solution is deposited on the substrate, so that polymerization and crosslinking are both performed on the substrate.
[0042] In one aspect, hydroxyethyl methacrylate (HEMA) can be combined with methyl methacrylate (MA) to form a copolymer. On the other hand, hydroxyethyl methacrylate (HEMA) can be combined with methyl methacrylate (MMA) to form a copolymer. The molar ratio of HEMA to MMA is about 1:3 to about 1:50, and a preferred ratio is about 1:10. In one aspect, the cross-linking agent for the prepolymer with hydroxyl (or any reactive group with active hydrogen, such as mercaptan, hydroxyl, acetoacetyl, urea, melamine, carbamate, etc.) is an isocyanate, isothiocyanate, etc., with a functionality greater than one. In one aspect, the molar ratio of the isocyanate cross-linking agent to the hydroxyl in the catalyzed polymer or copolymer is about 0.5:1 to about 10:1. In exemplary aspects, 2-hydroxyethyl methacrylate and methyl acrylate are randomly polymerized to form a polymer matrix. In one aspect, 2-isocyanatoethyl methacrylate (IEMA) can be combined with MMA in a ratio of about 1:3 to about 1:50, and a preferred ratio is about 1:20. Isocyanate containing groups can crosslink with any compound containing a reactive hydrogen such as hydroxyl, thiol, acetoacetyl, urea, melamine or urethane.
[0043] In one aspect, the polymer matrix of the cathode gel layer 30 and / or the anode gel layer 42 can include materials that are prepolymerized before the layers are deposited on the respective substrates and crosslinked after deposition, or the materials can be simultaneously polymerized and crosslinked after the layers are deposited on the substrates. In one aspect, the polymer matrix of the cathode gel layer 30 and / or the anode gel layer 42 includes a polyol having a hydroxyl functionality of at least two, i.e., a polymer molecule having at least two hydroxyl groups that can react with other functional groups such as isocyanate groups, metal alkoxide groups, or ketone groups. Examples of metal alkoxides include tetramethyl orthosilicate or tetraethyl orthosilicate or titanium (IV) isopropoxide. In the polymer matrix, the polyol is crosslinked by molecules of a bridging compound, which in turn has at least two functional groups that can react with the reactive hydroxyl groups of the polyol, examples of which include materials including thiol functional groups.
[0044] On the other hand, the polymer matrix of the cathode gel layer 30 and / or the anode gel layer 42 can be formed by crosslinking two copolymers. For example, HEMA / MMA can be combined with IEMA / MMA, and the hydroxyl groups of HEMA will self-react with the isocyanate groups of IEMA to form an open polymer structure.
[0045] In some aspects, the amount of polymer matrix in cathode gel layer 30 and / or anode gel layer 42 is about 5 weight percent (wt.%) to about 50 wt.%, about 5 wt.% to about 20 wt.%, or about 20 wt.% to about 50 wt.%. The properties of the materials and methods used to form the gel layers can be selected to provide each of the cathode gel layer 30 and the anode gel layer 42 with desired gel properties (e.g., gel thickness and gel rigidity), while also providing a gel layer that allows sufficient ion mobility within the gel layer to provide the desired electrochromic properties.
[0046] The cathode gel layer 30 and the anode gel layer 42 can be formed using the same or different solvents. In one aspect, the cathode gel layer 30 and the anode gel layer 42 are all formed using propylene carbonate as a solvent. Other non-limiting examples of suitable solvents include cyclic esters, such as propylene carbonate, isobutylene carbonate, γ-butyrolactone, γ-valerolactone, any two or more of propylene carbonate, isobutylene carbonate, γ-butyrolactone and γ-valerolactone are any homogeneous mixtures of liquid at room temperature, and any one or more of propylene carbonate, isobutylene carbonate, γ-butyrolactone and γ-valerolactone and ethylene carbonate are any homogeneous mixtures of liquid at room temperature. Other co-solvents may be included in the cathode gel layer 30 and / or the anode gel layer 42 to assist the gel coating process, and the non-limiting examples of the co-solvents include acetonitrile and 3-methoxypropionitrile. Co-solvents may promote the surface tension of the regulating fluid and / or increase the solubility limit of the cathode gel layer 30 and / or the anode gel layer 42 as needed.
[0047] Characteristics such as the amount of polymer matrix, degree of crosslinking, crosslinking rate, type of crosslinking agent and type of polymer can be selected to provide desired gel characteristics for the cathode gel layer 30 and the anode gel layer 42 formed. For example, the rigidity of the independent gel layer 30 and / or 42 can be changed by changing the polymer molecular weight, polymer weight percentage and / or the crosslinking density of the polymer matrix. In one aspect, the gel rigidity usually increases with the increase of polymer concentration (weight percentage), the increase of crosslinking density and / or to some extent with the increase of molecular weight. In one aspect, the crosslinking rate of any polymer described herein can ultimately be controlled in part by selecting a reactive crosslinking material. For example, in some aspects, the reaction rate can be increased by using aromatic isocyanates or aromatic alcohols or both. In other aspects, the reaction rate can be reduced, for example, by using sterically hindered isocyanates or sterically hindered alcohols or both.
[0048] The polymer matrix forming the cathode gel layer 30 and the anode gel layer 42 may be the same or different. One or both of the cathode gel layer 30 and the anode gel layer 42 may include additional components, non-limiting examples of which include ultraviolet (UV) stabilizers, thickeners, stabilizers, current-carrying electrolytes, surfactants, rheology modifiers, etc. In some aspects, the cathode gel layer 30 and / or the anode gel layer 42 are formed from a composition including a thickener to provide a gel layer with a desired thickness. Non-limiting examples of suitable thickeners include colloidal silica and acrylic fibers.
[0049] Non-limiting examples of polymers and solvent systems that can be used to form the cathode gel layer 30 and the anode gel layer 42 in the present disclosure are disclosed in U.S. Pat. Nos. 5,888,431; 7,001,540; 5,940,201; 6,635,194 and 5,928,572; and U.S. Patent Application Publication Nos. 2015 / 0346573 and 2019 / 0048159, the contents of which are incorporated herein by reference in their entirety.
[0050] The sealing member 52 can be any suitable structure for sealing the perimeter of the electro-optical assembly 10 to isolate the contents of the chamber 50 from ambient oxygen and / or moisture. In one aspect, the sealing member 52 can be a heat-sealing film attached to the first substrate 20 and the second substrate 32 at the edges of the first substrate 20 and the second substrate 32 around the perimeter of the electro-optical assembly 10. In one aspect, the sealing member covers the edge of the first surface 22 of the first substrate 20 and extends to the edge of the fourth surface 36 of the second substrate 32. The sealing member 52 can be configured to provide a barrier to isolate the contents of the chamber 50 from moisture and / or oxygen. Suitable heat-sealing films are typically multilayers consisting of an inner sealant layer, an intermediate core layer, and an outer barrier layer, which may or may not include an aluminum foil layer. The film can be applied using a heat sealer to attach the film to the edge of the electro-optical assembly 10. An example of a heat-sealing film without a foil layer includes Toray's CBS2, and an example of a metallized heat seal film is Toray's PWXS. Additionally, a pressure sensitive adhesive may be added to the inner sealant layer to adhere the film at room temperature and / or to improve adhesion during heat sealing. An example of a pressure sensitive adhesive for this purpose is 8142KCL.
[0051] In some aspects, the sealing member 52 can be applied as a liquid layer around the periphery of the cathode gel layer 30 and the anode gel layer 42, and heat, ultraviolet light, or a combination thereof can be applied to cure the liquid layer and form the sealing member 52. Non-limiting examples of suitable liquid layer materials include silicone, epoxy resin, acrylic resin, hot melt material, and polyurethane. On the other hand, a preformed layer such as a pressure-sensitive adhesive layer (e.g., acrylic resin) can be used to form the sealing member 52. In these examples, the sealing member 52 can optionally extend between the first conductive layer 28 and the second conductive layer 40, or have a generally C-shaped cross-sectional profile.
[0052] refer to Figure 2, each of the cathode subassembly 12 and the anode subassembly 14 is separately formed on a first substrate web 60 and a second substrate web 62, respectively, and is merged together to form the electro-optical assembly 10. Although aspects of the present disclosure are discussed with respect to exemplary embodiments in which the first substrate web 60 and the second substrate web 62 are formed of a polymer material and are therefore referred to as the first polymer web 60 and the second polymer web 62, respectively, as discussed in more detail below, the first substrate web 60 and / or the second substrate web 62 can be formed of a glass material and be referred to as the first glass web and the second glass web. In one aspect, the separately formed cathode subassembly 12 and the anode subassembly 14 can be laminated together using heat, pressure, and / or vacuum. On the other hand, the separately formed cathode subassembly 12 and the anode subassembly 14 can be assembled by coupling the first substrate 20 and the second substrate 32 using a seal 52 and / or any adhesive or bonding layer. As discussed in more detail below, a plurality of cathode subassemblies 12 and a plurality of anode subassemblies 14 can be formed from respective first and second polymer webs 60, 62, respectively, such that a plurality of electro-optical assemblies 10 can be formed from and separable from the assembled first and second polymer webs 60, 62. The first polymer web 60 comprises at least a first substrate 20 and an optional first barrier layer 26 and / or a first conductive layer 28. The second polymer web 62 comprises at least a second substrate 32 and an optional second barrier layer 38 and / or a second conductive layer 40.
[0053] As used herein, a web refers to a continuous piece of material having a certain width and length, so that a component or multiple components (i.e., one, two, or more) can be formed from a single piece provided in a stack or roll. The length and / or width of the substrate web can be selected to accommodate the formation of a single component or multiple components in either or both of the length and width directions. The web can have a flat cross-sectional profile in all directions; alternatively, the cross-sectional profile of the web in at least one direction can deviate from a flat surface.
[0054] The polymer webs 60 and 62 form at least the first substrate 20 and the second substrate 32, respectively, and are therefore made of the same types of materials listed above as being suitable for forming the first substrate 20 and the second substrate 32. Non-limiting examples of suitable polymer materials for forming the first polymer web 60 and / or the second polymer web 62 include polyethylene (e.g., low density and / or high density), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone, acrylic polymers (e.g., poly(methyl methacrylate) (PMMA)), polymethacrylates, polyimides, polyamides (e.g., cycloaliphatic diamine dodecanedioic acid polymers such as poly(methylene methacrylate) (PMMA)), polyimides, polyamides (e.g., poly(methylene methacrylate) (PMMA)), ...amides) (e.g., poly(methylene methacrylate) (PMMA)), polyamides (e.g., polyamides) (e.g., poly(methylene methacrylate) (PMMA)), polyamides (e.g., polyamides) (e.g., polyamides) (e.g., polyamides) (e.g., polyamides) ( CX7323)), epoxy resin, cyclic olefin polymer (COP) (e.g., Zeonor 1420R), cyclic olefin copolymer (COC) (e.g., Topas 6013S-04 or Mitsui Apel), polymethylpentene, cellulose ester plastics (e.g., cellulose triacetate), transparent fluoropolymers, polyacrylonitrile, other polymer materials and / or combinations thereof. In one aspect, when the first substrate 20 and the second substrate 32 are made of glass, the corresponding first substrate web 60 and the second substrate web 62 are made of glass instead of a polymer material and can be referred to as a first glass web 60 and a second glass web 62. Non-limiting examples of suitable glass materials include borosilicate glass and soda-lime glass.
[0055] method
[0056] Reference now Figure 3-7C , methods for forming an electro-optical cathode subassembly and an anode subassembly and a method for forming an electro-optical assembly from a pair of cathode subassemblies and anode subassemblies according to aspects of the present disclosure are provided. Figure 3, a method 300 for forming an electro-optical assembly 10 from a cathode subassembly 12 and an anode subassembly 14 is provided. The method 300 may be a continuous process, or may consist of a plurality of separate processing steps, between which intermediate products are stored under appropriate conditions (e.g., in a clean room, under vacuum, in an oxygen-free environment, etc.). In general, the method 300 may be considered to include three process stages: a substrate web forming process 302, a subassembly forming process 304, an electro-optical assembly forming process 306, and optionally an electrochromic device forming process 308. The substrate web forming process 302 and the subassembly forming process 304 may be used to form each of the cathode subassembly 12 and the anode subassembly 14, which are combined in the electro-optical assembly forming process 306 to form the electro-optical assembly 10. The cathode subassembly 12 and the anode subassembly 14 may be formed continuously or simultaneously according to the processes 302 and 304. Cathode subassembly 12 and anode subassembly 14 may be formed at the same or different locations as where electro-optical assembly 10 is formed in process 306. In one aspect, each of processes 302, 304, and 306 may be performed immediately following a previous process in a generally continuous process of forming cathode subassembly 12 and anode subassembly 14 and electro-optical assembly 10. In another aspect, a product formed using one or more of processes 302 and / or 304 may be stored for a predetermined period of time before being processed according to the next process stage 304 and / or 306. In one aspect, all of processes 302, 304, and 306 of method 300 are performed in the same facility; alternatively, one or more of processes 302, 304, and / or 306 may be performed in a facility different from the other processes. It should be understood that for illustrative purposes, a specific order of steps is disclosed according to method 300 and the three process stages 302, 304 and 306 of method 300, and without departing from the spirit of the present disclosure, the specific steps of method 300 and any of the three process stages 302, 304 and 306 of method 300 may be performed in a different order or in a different combination.
[0057] Still refer to Figure 3, the substrate web forming process 302 includes the steps of providing a polymer web at 310 and forming a conductive layer on the polymer web at 312. As discussed above, each of the cathode subassembly 12 and the anode subassembly 14 is formed on polymer webs 60 and 62, respectively, which form a portion of the corresponding substrates 20 and 32. The polymer webs 60 and 62 can be provided in the form of individual sheets or rolls for storage and / or processing, and can include any of the materials described above for forming the first substrate 20 and the second substrate 32. Although steps 310 and 312 are discussed in the context of forming the cathode subassembly 12, it should be understood that steps 310 and 312 can be used in a similar manner to form the anode subassembly 14 using the same or different materials as the cathode subassembly 12 as discussed above.
[0058] The polymer web 60 at 310 may include one or more barrier layers 26, or step 310 may include a process for applying one or more barrier layers 26 to the polymer web 60. Although method 300 is described in the context of providing a barrier layer 26, it should be understood that the barrier layer 26 can be skipped, or the element can be incorporated into the body of the polymer web 60 as needed to provide barrier properties. When the barrier layer 26 is disposed on the polymer web 60, the barrier layer 26 can be laminated to the polymer web 60, adhered to the polymer web 60, or formed integrally with the polymer web 60, such as by a co-extrusion process. The barrier layer 26 can be a single layer or multiple layers. In one aspect, the polymer web 60 having one or more barrier layers 26 formed thereon can be purchased from a supplier. One such example is a PET web to which a multilayer polymer / oxide / polymer barrier layer has been applied, an example of which includes a flexible transparent barrier film sold by 3M under the trade name FTB3-125 barrier film. The FTB-125 barrier film is described by 3M as a PET substrate having two vacuum deposited polymer layers with an inorganic oxide layer positioned between the two polymer layers. The "125" in the trade name of the 3M material refers to the thickness of the substrate, in this case 125 μm. However, it should be understood that alternative FTB3 products having different thicknesses may also be used. In another aspect, as part of the substrate web forming process 302, one or more barrier layers 26 may be coextruded or laminated with the polymer web 60.
[0059] In one aspect, the polymer web 60 can be provided with a removable interlayer (also referred to as a release liner) disposed over the surface on which the conductive layer 28 is to be formed to protect the surface until the conductive layer 28 is deposited. When the polymer web 60 includes one or more barrier layers 26, the interlayer can be disposed over the exposed surface of the outermost barrier layer 26. When the polymer web 60 does not include a barrier layer 26 or before applying the barrier layer 26, the polymer web 60 can be disposed within the interlayer to protect the barrier layer 26 and / or the surface on which the conductive layer 28 is to be deposited. The interlayer can be applied to the surface of the polymer web 60 or formed integrally with the polymer web 60 to provide a peelable clean substrate. For example, the polymer resin forming the polymer web 60 and the polymer resin forming the interlayer can be co-extruded to form a substrate, and the co-extruded interlayer can be peeled off from the substrate to expose the surface of the polymer web 60 below.
[0060] In one aspect, when barrier layer 26 is used, an interlayer can be applied over the outer surface of barrier layer 26 under vacuum to minimize the deposition of debris and / or degradation of the exposed outer surface of barrier layer 26, and optionally, the interlayer can be applied as a process continuous with the process of forming barrier layer 26 on web 60. Optionally, the outer surface of barrier layer 26 can be subjected to a cleaning process such as plasma treatment prior to applying the interlayer. When the interlayer is present, process 302 can include a step of removing the interlayer prior to forming conductive layer 28. Alternatively, when barrier layer 26 and conductive layer 28 are formed in a continuous process, an interlayer may not be necessary.
[0061] Still refer to Figure 3 At step 312 , a conductive layer 28 may be formed over the exposed surface of the barrier layer 26 on the polymer web 60 using any suitable process. Figure 4An exemplary roll-to-roll sputtering process 400 for forming a conductive layer 28 according to one aspect of the present disclosure is shown. A polymer web 60 having a barrier layer 26 deposited thereon may be provided to a processing drum 402 configured to expose the polymer web 60 to a sputtering source 404 for depositing a conductive layer on the polymer web 60. The polymer web 60 may be provided on an unwinder 406, which optionally includes an interlayer remover 408 to remove an interlayer 410 from the polymer web 60 if present. The processing drum 402 moves the polymer web 60 from the unwinder 406 past the sputtering source 404 so that the outermost surface of the barrier layer 26 is exposed to the sputtering source 404 for depositing the conductive layer 28 onto the barrier layer 26. The properties of the material and the control parameters of the sputtering source 404 will vary depending on the material being deposited to form the conductive layer 28. Although only a single sputtering source 404 is shown, aspects of the present disclosure may include more than one sputtering source, optionally located in separate chambers, to deposit the material used to form the conductive layer 28. Optionally, the polymer web 60 may be degassed prior to depositing the conductive layer 28 on the polymer web 60 to prevent water and / or oxygen from affecting the conductive material during deposition. The degassing process may include heating the polymer web roll or sheet under vacuum, or storing the polymer web roll or sheet in an inert atmosphere at an elevated temperature.
[0062] The polymer web 60 with the barrier layer 26 and the conductive layer 28 deposited thereon forms a substrate web 60', which can be wound into a roll on a rewinder 412 for storage or further processing. Optionally, step 412 can include applying an interlayer to the exposed surface of the conductive layer 28 (not shown) to protect the exposed surface from debris and / or degradation between processing steps. The application of the interlayer can be performed under vacuum and can be a continuous process with the roll-to-roll sputtering process 400 or a separate process step.
[0063] Although aspects of step 312 of forming conductive layer 28 on polymer web 60 to form substrate web 60' are described in the context of a roll-to-roll process utilizing sputtering to deposit conductive material, other forms and processes may be utilized within the scope of the present disclosure. For example, polymer web 60 may be provided in individual sheets rather than in a roll to provide individual sheets of substrate web 60'. In other aspects, the conductive material may be deposited using processes other than sputtering, examples of which include chemical vapor deposition (CVD) and physical vapor deposition (PVD).
[0064] Reference again Figure 3The subassembly forming process 304 includes applying an electrochromic gel to the substrate web 60' at 314 and then curing the electrochromic gel to form an electro-optical subassembly at 316. A cathode electrochromic gel is applied to form cathode subassembly 12, and an anodic electrochromic gel is applied to form anode subassembly 14.
[0065] Figure 5 An exemplary roll-to-roll process 500 for forming an electro-optical subassembly according to one aspect of the present disclosure is shown, the electro-optical subassembly comprising a cathode subassembly 12 and / or an anode subassembly 14. Although aspects of forming the electro-optical subassembly at 304 are discussed in the context of forming the cathode subassembly 12, it should be understood that the anode subassembly 14 may be formed in a similar manner using materials suitable for forming an anode gel, as described above. Still referring to Figure 5 , a web substrate 60' formed according to the substrate web forming process 302 described above can be provided on a substrate roll 502. The web substrate 60' can be unwound from the substrate roll 502 so that the conductive layer 28 is exposed for application of the gel composition at the coating station 504. When the conductive layer 28 is covered by an interlayer, the process 500 can include an interlayer removal station (not shown) to remove the interlayer before the web substrate 60' passes through the coating station 504. Optionally, the removal of the interlayer and / or the entire roll-to-roll process 500 can be performed in a clean room to minimize debris, static electricity, etc. Optionally, before the web substrate 60' passes through the coating station 504, the exposed surface of the conductive layer 28 can be treated to remove impurities and / or defects, non-limiting examples of which include heat treatment or plasma treatment.
[0066] refer to Figure 5 and 6, the coating station 504 can be configured to apply an electroactive gel composition comprising at least one electroactive component dispersed in a polymer matrix and a solvent, and optional additives, as discussed above with respect to forming the cathode gel layer 30 and the anode gel layer 42. When forming the cathode subassembly 12, the electroactive gel composition will be a cathode gel composition comprising at least one cathode component. When forming the anode subassembly 14, the electroactive gel composition will be an anode gel composition comprising at least one anode component. The coating station 504 can be any suitable type of equipment for applying one or more layers of the gel composition to the substrate web 60', such as a slot die for extrusion, a laminating system, a screen printing system, a drawdown bar, a Meyer rod (rod coating), gravure printing, sol-gel process, spin coating, die casting, dip coating, or inkjet printing. In addition, it should be understood that the shape of the component and / or the thickness of the gel layer can be defined by depositing the layer according to one or more of the methods listed above (or other suitable methods) with the aid of a template placed on the substrate. The template can be removed before or after the gel is cured. Figure 6 An exemplary coating station 504 in the form of a screen printing system 600 according to one aspect of the present disclosure is shown. The screen printing system may include a rotating screen 602 including a dispenser 604 and a squeegee 606 and an impression cylinder 608 for printing the cathode gel composition 30' onto the exposed surface of the conductive layer 28. The screen printing system 600 is configured to apply the cathode gel composition 30' at a desired thickness and temperature based on the desired properties of the cathode gel layer 30 to be formed.
[0067] In one aspect, the cathode and anode gel compositions are configured to be suitable for deposition using a desired type of equipment. For example, when a screen printing system is used, it may be advantageous to form cathode and anode gel compositions having a viscosity suitable for the screen printing equipment. In one aspect, the cathode and anode gel compositions are screen printing compositions having a minimum viscosity of about 1200 centipoise (cP) and / or a minimum solids content of about 20%. The cathode and anode gel compositions may be modified by adjusting the solids content and / or adding suitable additives to provide cathode and anode gel compositions having desired properties. The cathode and gel compositions may include prepolymerized polymers dispersed and / or dissolved in a solvent, and / or polymerization may be initiated after the gel composition is applied to the substrate web 60'.
[0068] Optionally, substrate web 60 ′ may be provided with a mask to facilitate deposition and / or maintain the deposited cathode and / or anode gel compositions in a desired shape corresponding to the desired final shape of cathode gel layer 30 and / or gel layer 42 .
[0069] Reference again Figure 5 , the substrate web 60' having the cathode gel composition 30' applied thereon is then conveyed to a curing station 506 to cure the cathode gel composition 30' so as to form a cathode layer 30 on the substrate web 60', thereby forming a cathode subassembly web 60". The nature of the curing station 506 will depend on the components of the cathode gel composition 30'. For example, the curing station 506 can be a thermal curing station, an electron beam curing station, and / or an ultraviolet light curing station, depending on whether the polymer material in the cathode gel composition 30' is thermally cross-linkable and / or cross-linkable when exposed to ultraviolet light. The parameters of the curing station 506, such as time, temperature, ultraviolet light exposure, etc., can be set based on the characteristics of the applied cathode gel composition 30', the Non-limiting examples of properties include polymeric materials, solvents, additives, thickness of the cathode gel composition layer, desired degree of gelation, and desired thickness of the cured cathode gel layer. In one aspect, the curing process is implemented in a hypoxic or oxygen-free environment. In one aspect, the curing process is implemented under nitrogen and / or in the presence of filtered air. Optionally, the method may include a leveling step prior to curing. The leveling step may include exposing the deposited gel layer to a holding period during which surface irregularities in the thickness of the layer may be allowed to dissipate by flowing or otherwise. The holding period may be implemented at a temperature above the deposition temperature of the gel layer but below the curing temperature of the gel layer so as to promote leveling of the layer, such as by increasing the leveling rate.
[0070] Cathode gel layer 30 can be formed by the deposition of a single layer of cathode gel composition, or by the deposition of multiple sublayers of one or more cathode gel compositions. In one aspect, cathode gel layer 30 can be formed by continuously depositing two or more cathode gel sublayers. Each deposited sublayer can have the same or different compositions. In one aspect, the curing step occurs after all sublayers are deposited. Optionally, one or more sublayers in the sublayer can be cured before depositing the next sublayer. Anode gel layer 42 can be formed in a similar manner using a suitable anode gel composition.
[0071] After the curing station 506, the cathode subassembly web 60" formed thereon can be wound onto a cathode subassembly roll 508. Optionally, an interlayer 510 can be applied to the exposed surface of the cathode gel layer 30 before the cathode subassembly web 60" is wound onto the cathode subassembly roll 508. The cathode subassembly web 60" can be stored for future use or used immediately in further processing steps. Although the formation of the cathode subassembly web 60" is described in the context of a roll-to-roll process, it should be understood that the cathode subassembly can be formed in a similar manner using separate sheets of the web 60'. In addition to utilizing components suitable for forming the anode gel composition, the formation of the anode sub-assembly web can be carried out in any of the roll-to-roll or separate sheet processes described with respect to the formation of the cathode sub-assembly web 60". For example, the parameters of the anode gel composition application and curing process can differ from those described for the cathode gel composition based on characteristics such as the components of the anode gel composition, the thickness of the anode gel composition layer, the desired degree of gelation, and the desired thickness of the cured anode gel layer. In one aspect, the cathode and anode sub-assembly webs can be formed simultaneously on a parallel system and further processed in a continuous process. In another aspect, one or both of the cathode and anode sub-assembly webs can be formed and stored prior to additional processing.
[0072] In this manner, steps 314 and 316 of the subassembly forming process 304 can be repeated for both the cathode subassembly web formation and the anode subassembly web formation. Forming the cathode subassembly 12 and the anode subassembly 14 in separate processes on separate webs allows for selection of materials and processing conditions based on the individual characteristics of each of the cathode subassembly 12 and the anode subassembly 14. For example, because each of the cathode subassembly 12 and the anode subassembly 14 is cured separately, the curing parameters at 316 can be set based on the materials from which each separate subassembly is formed, thereby allowing the conditions of each of the cathode subassembly 12 and the anode subassembly 14 to be adjusted or optimized independently. In addition, forming the cathode subassembly 12 and the anode subassembly 14 separately allows each of the cathode gel layer 30 and the anode gel layer 42 to be stored separately until they are sealed in the electro-optical assembly 10. One or both of the cathode gel layer 30 and / or the anode gel layer 42 may contain components that may be sensitive to moisture, oxygen, and / or light. For some materials, this sensitivity may increase when the cathode component and the anode component are in contact with each other. Forming the cathode subassembly 12 and the anode subassembly 14 separately may help protect sensitive components from damage / degradation until the subassemblies 12, 14 are sealed together.
[0073] According to one aspect of the present disclosure, the electrochromic gel composition applied at step 314 can be applied as a continuous layer across at least a portion of the width of the substrate web. According to another aspect of the present disclosure, the electrochromic gel composition applied at step 314 is applied to the substrate web 60' in a pattern based on the shape of the part to be formed.
[0074] refer to Figures 7A-7C , showing exemplary patterns for applying electrochromic gel formers to substrate webs. Figures 7A-7C As shown, cathode gel layer 30 can be applied to substrate web 60' so that each cathode subassembly 12 has a predetermined shape. In one aspect, the predetermined shape can correspond to the final component shape of electro-optical assembly 10. The size and orientation of the cathode subassembly pattern can be based on the final component size and the size of substrate web 60". Forming the electrochromic gel layer in a pattern on the substrate web can reduce the waste of material forming cathode gel layer 30 and anode gel layer 42. As discussed above, screen printing is an exemplary method for applying the electrochromic gel composition, and the application can be controlled to print the gel composition under a tolerance suitable for forming the pattern of cathode subassembly 12 and / or anode subassembly 14. Optionally, one or more additional elements of cathode subassembly 12 and / or anode subassembly 14, such as first and second barrier layers 26 and 38 and / or first and second conductive layers 28 and 40, respectively, can also be applied in a pattern to reduce the waste of these components.
[0075] Reference again Figure 3 , the cathode subassembly web and the anode subassembly web formed in process 304 are combined to form the electro-optical assembly 10 according to the electro-optical assembly forming process 306. In step 318, the cathode subassembly web and the anode subassembly web are assembled together to form the electro-optical subassembly web. In one aspect, the assembly step 318 can be a lamination step, and the lamination step includes applying heat and / or pressure to assemble the cathode subassembly 12 and the anode subassembly 14 together. On the other hand, the assembly step 318 includes merging the cathode subassembly 12 and the anode subassembly 14 together using one or more adhesive layers, a tie layer and / or a sealing layer. Optionally, the assembly step 318 is performed in an inert atmosphere (e.g., under nitrogen) or under vacuum. When one or both of the cathode subassembly web and / or the anode subassembly web formed in process 304 include an interlayer, the interlayer is removed before the assembly step of 318.
[0076] When cathode subassembly 12 and anode subassembly 14 are patterned on their respective substrate webs, assembling step 318 may include an alignment step by which the patterns of cathode subassembly 12 and anode subassembly 14 are aligned such that at least a portion of cathode subassembly 12 overlaps at least a portion of anode subassembly 14. In some aspects, cathode subassembly 12 and anode subassembly 14 may be aligned such that at least one edge of cathode subassembly 12 and at least one edge of anode subassembly 14 are offset from one another. In some aspects, one of cathode subassembly 12 or anode subassembly 14 has at least one dimension that is larger than a corresponding dimension of the other of cathode subassembly 12 or anode subassembly 14 such that at least one pair of subassembly edges are offset.
[0077] In one aspect, the assembly forming process 306 may include an optional degassing step to remove air trapped in one or both of the cathode gel layer 30 and the anode gel layer 42 in the form of bubbles. During assembly such as by lamination, bubbles are trapped between the cathode gel layer 30 and the anode gel layer 42. In some aspects, a vacuum is applied after lamination to laterally draw bubbles along the interface between the cathode gel layer 30 and the anode gel layer 42, thereby removing bubbles from the system. In one aspect, the cathode gel layer 30 and the anode gel layer 42 are formed so that they have sufficient rigidity and / or solid content to facilitate the movement of bubbles at the interface between the cathode gel layer 30 and the anode gel layer 42 and to facilitate the removal of bubbles from the system. The degree of polymer reaction and / or crosslinking density may be adjusted to provide sufficient rigidity suitable for the degassing step. On the other hand, by laminating the cathode gel layer 30 and the anode gel layer 42 in a vacuum-sealed chamber below atmospheric pressure, the formation of bubbles may be minimized or eliminated.
[0078] In step 320, one or more seals, power buses, etc. can be applied to the aligned cathode subassemblies 12 and anode subassemblies 14. All or some parts of step 320 can occur before, after, or simultaneously with the assembly step 318. In some aspects, before applying heat and / or pressure to laminate the subassemblies at 318, a power bus and at least a seal 52 are provided between the cathode subassembly 12 and the anode subassembly 14. In step 322, shaped parts can be cut from the aligned cathode and anode subassembly webs to form each electro-optical assembly 10. Laser or other suitable methods can be used to cut the shaped parts. Step 322 can occur before or after laminating the aligned cathode and anode subassembly webs. After cutting the electro-optical assembly 10 from the aligned cathode and anode subassembly webs, additional seals can be optionally applied. In step 30, the electro-optical assembly 10 can be stored for future use, or optionally further processed with additional components to form an electrochromic device.
[0079] Some or all of the steps of method 300 may be performed in an inert atmosphere and / or under vacuum. In one aspect, one or more of substrate web forming process 302, subassembly forming process 304, and electro-optical assembly forming process 306 may be formed in a continuous process maintained under an inert atmosphere or vacuum. On the other hand, one or more of substrate web forming process 302, subassembly forming process 304, and electro-optical assembly forming process 306 may be performed separately in an inert atmosphere or under vacuum, and care may be taken to maintain an inert atmosphere or vacuum during storage and / or transition between processes 302, 304, and 306 or between individual steps of each process 302, 304, and 306.
[0080] The electro-optical assemblies of the present disclosure may be used in a variety of devices to provide electrochromic features to the devices, non-limiting examples of which include interior and exterior mirror assemblies, skylights, architectural windows, vehicle windows, aircraft windows, and the like.
[0081] refer to Figure 8, an exemplary electrochromic device incorporating the electro-optical assembly 10 is shown in the form of a skylight 700. The skylight 700 includes a first glass plate 702 and a second glass plate 704, the electro-optical assembly 10, and one or more additional layers 706, 708, 710, and 712, non-limiting examples of which include solar control films, structural support layers, laminate layers, filter layers, and the like. Non-limiting examples of laminate layer materials include ethylene-vinyl acetate (EVA), polyurethane, and polyvinyl butyral (PVB). The electro-optical assembly 10 may include an electrical connector 720 that is electrically coupled to the first conductive layer 28 and the second conductive layer 40 through the power bus of the electro-optical assembly 10. The electrical connector 720 may be configured to be electrically coupled to an additional electrical connector 722 of the skylight 700 so that an electrical potential may be applied across the first conductive layer 28 and the second conductive layer 40 by an external power source (not shown). The skylight 700 may include a primary seal 730 that seals the inner layers 706 - 712 and the electro-optical assembly 10 between the glass panels 702 , 704 .
[0082] Fig. 9 A cross-sectional schematic diagram showing an example of a configuration of a skylight 700 according to one aspect of the present disclosure is shown. Fig. 9 In an exemplary configuration of the sunroof 700, the seal 52 is in the form of a tape sealant that forms a perimeter seal around the electro-optical assembly 10 and around an electrical connector 720 that extends into the electro-optical assembly 10 and electrically couples the first and second conductive surfaces. The electrical connector 720 is electrically coupled to an additional electrical connector 722 that extends beyond the main seal 730 of the sunroof 700 for connection to an external power source (not shown).
[0083] Fig.10 An alternative skylight configuration 700' is shown that is similar to skylight 700, but has some differences, such as differences in electrical connectors. Thus, similar components are used with Figure 8 and 9 The same reference numerals as in the figure are used to mark the same reference numerals as in the figure. Fig.10 The skylight 700' includes an electro-optical assembly 10', which is similar to the electro-optical assembly 10 described herein, except that the seal 52' is a multilayer assembly including a conductive component 720', a dielectric layer, and an oxygen-resistant pressure-sensitive adhesive layer, and the conductive component can be in the form of a conductive metal strip (e.g., copper). The skylight electrical connector 722' is in the form of a conductive epoxy resin, which is provided to electrically couple the conductive component 720' of the seal 52' to an external power source (not shown). The device may include one or more additional components not shown. For example, one or more additional components may be provided to electrically connect the conductive component 720' to the electrical connector 722'.
[0084] The following examples describe various features and advantages provided by the present disclosure and are in no way intended to limit aspects of the present disclosure and the appended claims.
[0085] Examples
[0086] According to aspects of the present disclosure suitable for forming cathode subassembly 12 and anode subassembly 14, Tables 1 and 2 below show exemplary compositions for forming cathode gel layers and anode gel layers, respectively. The "matrix copolymer" used to form the polymer matrix in the cathode and anode gel layer compositions is a random polymerization of 2-hydroxyethyl methacrylate and methyl acrylate in a 1:10 molar ratio. A 22 wt.% stock solution of the resulting copolymer was prepared in propylene carbonate solvent and used to form the cathode gel layer and anode gel layer, respectively, according to Tables 1 and 2 below.
[0087] Table 1: Cathode gel layer composition
[0088]
[0089]
[0090] Table 2: Anode gel layer composition
[0091]
[0092] The present disclosure encompasses the following non-limiting aspects. To the extent not yet described, any one of the features of the following aspects may be combined in part or in whole with the features of any one or more other aspects of the present disclosure to form further aspects, even if such combination is not explicitly described.
[0093] According to a first aspect of the present disclosure, an electro-photonic assembly comprises a substrate web, a conductive layer disposed on the substrate web, and an electroactive gel layer disposed on the conductive layer, wherein the electroactive gel layer comprises an electroactive component dispersed in a polymer matrix, the electroactive gel layer has a certain thickness, and wherein the thickness variation of the electroactive gel layer accounts for less than about 20% of the average thickness of the electroactive gel layer.
[0094] According to the first aspect of the present disclosure, the electro-photonic assembly further comprises a release liner disposed over the electroactive gel layer.
[0095] In accordance with the first aspect or any intervening aspects, the electroactive gel layer is patterned on the conductive layer.
[0096] According to the first aspect or any intervening aspects, the electroactive component comprises an anode component or a cathode component.
[0097] According to the first aspect or any intervening aspects, the electroactive component comprises: at least one electrochromic cathode component, the at least one cathode component comprising a viologen, a metal oxide, a methyl viologen, an octyl viologen, a benzyl viologen, a polymeric viologen, a ferrocenium, a tungsten oxide, a vanadium oxide, a nickel oxide, a perovskite, a samarium nickelate and a y B z O x A material of a metal oxide wherein A and B are metals, y is 1≤y≤20, z is 1≤z≤20, and x is about 80% to about 120% of the stoichiometry; or at least one electrochromic anode component, the at least one anode component comprising a metallocene, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazines, substituted phenothiazines, substituted dithiazines, thianthrene, substituted thianthrene , di-tert-butyl-diethylferrocene, 5,10-dimethyl-5,10-dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT) and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine.
[0098] According to the first aspect or any intervening aspects, the substrate web is a polymer web, and the polymer web comprises a material selected from the following: polyethylene polymer, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone polymer, acrylic polymer, poly(methyl methacrylate) (PMMA), polymethacrylate polymer, polyimide polymer, polyamide polymer, alicyclic diamine dodecanedioic acid polymer, epoxy polymer, cycloolefin polymer, cycloolefin copolymer (COC), polymethylpentene polymer, cellulose ester polymer, cellulose triacetate, transparent fluorine-containing polymer, polyacrylonitrile polymer and combinations thereof.
[0099] According to the first aspect or any intervening aspect, the substrate web is a glass web comprising a material selected from borosilicate glass and soda-lime glass.
[0100] In accordance with the first aspect or any intervening aspects, the electro-photonic assembly further comprises at least one barrier layer disposed between the substrate web and the conductive layer, wherein the at least one barrier layer is resistant to at least one of oxygen and water.
[0101] According to the first aspect or any intervening aspects, the at least one barrier layer comprises a polymer-inorganic layer-polymer stack or an insulator-metal-insulator (IMI) stack.
[0102] According to the first aspect or any intervening aspects, the conductive layer comprises at least one material selected from the following: transparent conductive oxide (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide, metal oxide / metal alloy / metal oxide, insulator-metal-insulator (IMI) stack, silver nanowire coating, carbon nanotubes, graphene coating, conductive nanorods, wire grids, conductive polymers and poly (3,4-ethylenedioxythiophene) (PEDOT).
[0103] According to the first aspect or any intervening aspects, the electroactive component is covalently bonded to the polymer matrix.
[0104] According to a second aspect of the present disclosure, an electro-optical assembly includes a cathode subassembly and an anode subassembly. The cathode subassembly includes a first substrate web, a first conductive layer disposed on the first substrate web, and a cathode gel layer disposed on the first conductive layer, wherein the cathode gel layer includes a cathode component dispersed in a polymer matrix, and the cathode gel layer has a certain thickness. The anode subassembly includes a second substrate web, a second conductive layer disposed on the second substrate web, and an anode gel layer disposed on the second conductive layer, wherein the anode gel layer includes an anode component dispersed in a polymer matrix, and the anode gel layer has a certain thickness. At least one of the cathode component and the anode component is electro-optical, and the thickness variation of at least one of the cathode gel layer and the anode gel layer accounts for less than about 20% of the average thickness of the corresponding gel layer.
[0105] According to a second aspect of the present disclosure, the cathode gel layer forms a pattern on the first conductive layer, and the anode gel layer forms a pattern on the second conductive layer.
[0106] According to the second aspect or any intervening aspects, the cathode component comprises at least one material selected from the group consisting of viologen, metal oxide, methyl viologen, octyl viologen, benzyl viologen, polymeric viologen, ferrocenium, tungsten oxide, vanadium oxide, nickel oxide, perovskite, samarium nickelate and a material of formula A y B z O x A metal oxide wherein A and B are metals, y is 1≤y≤20, z is 1≤z≤20, and x is about 80% to about 120% of the stoichiometric amount.
[0107] According to the second aspect or any intervening aspects, the anode component comprises at least one material selected from the group consisting of metallocenes, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazines, substituted phenothiazines, substituted dithiazines, thianthrene and substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl- 5,10-dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT) and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine.
[0108] According to the second aspect or any intervening aspects, the first substrate web, the second substrate web or both comprise a polymer material selected from the group consisting of polyethylene polymers, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone polymers, acrylic polymers, poly(methyl methacrylate) (PMMA), polymethacrylate polymers, polyimide polymers, polyamide polymers, alicyclic diamine dodecanedioic acid polymers, epoxy polymers, cycloolefin polymers, cycloolefin copolymers (COC), polymethylpentene polymers, cellulose ester polymers, cellulose triacetate, transparent fluoropolymers, polyacrylonitrile polymers and combinations thereof.
[0109] According to the second aspect or any intervening aspect, the electro-optical assembly further comprises: at least one first barrier layer disposed between the first substrate web and the first conductive layer; and at least one second barrier layer disposed between the second substrate web and the second conductive layer. The at least one first barrier layer and the at least one second barrier layer are resistant to at least one of oxygen and water.
[0110] According to the second aspect or any intervening aspects, the at least one first barrier layer, the at least one second barrier layer, or both comprise a polymer-inorganic layer-polymer stack or an insulator-metal-insulator (IMI) stack.
[0111] According to the second aspect or any intervening aspects, the first conductive layer, the second conductive layer or both include at least one material selected from the following: transparent conductive oxide (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide, metal oxide / metal alloy / metal oxide, insulator-metal-insulator (IMI) stack, silver nanowire coating, carbon nanotubes, graphene coating, conductive nanorods, wire grids, conductive polymers and poly (3,4-ethylenedioxythiophene) (PEDOT).
[0112] In accordance with the second aspect or any intervening aspect, the first substrate web, the second substrate web, or both, comprises a glass material selected from borosilicate glass and soda-lime glass.
[0113] According to a third aspect of the present disclosure, a method for forming an electro-photonic assembly is provided. The method comprises applying an electroactive gel composition on the conductive layer, wherein the electroactive gel composition comprises an electroactive component dispersed in a polymer matrix. The electroactive gel composition is cured to form an electroactive gel layer on the conductive layer.
[0114] According to the third aspect or any intervening aspect, applying the electroactive gel composition comprises applying the electroactive gel in a pattern on the conductive layer.
[0115] In accordance with the third aspect or any intervening aspect, the polymer web further comprises at least one barrier layer disposed between the polymer web and the conductive layer, wherein the at least one barrier layer is resistant to at least one of oxygen and water.
[0116] According to the third aspect or any intervening aspect, the at least one barrier layer comprises a polymer-inorganic layer-polymer stack or an insulator-metal-insulator (IMI) stack.
[0117] According to the third aspect or any intervening aspect, the method further comprises applying a release liner over the electroactive gel layer.
[0118] According to the third aspect or any intervening aspect, the electroactive component comprises an anode component or a cathode component.
[0119] According to the third aspect or any intervening aspect, the electrochromic component comprises at least one electrochromic cathode component, wherein the at least one cathode component comprises a viologen, a metal oxide, a methyl viologen, an octyl viologen, a benzyl viologen, a polymeric viologen, a ferrocenium, a tungsten oxide, a vanadium oxide, a nickel oxide, a perovskite, a samarium nickelate and a y B z O x A material of a metal oxide, wherein A and B are metals, y is 1≤y≤20, z is 1≤z≤20, and x is about 80% to about 120% of the stoichiometric amount; or the electrochromic component comprises at least one electrochromic anode component, the at least one anode component comprising a metallocene, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazines, substituted phenothiazines, substituted dithiazines, thianthracene, substituted Materials of substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl-5,10-dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT) and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine.
[0120] According to the third aspect or any intervening aspect, the substrate web is a polymer web, and the polymer web comprises a material selected from the following: polyethylene polymer, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone polymer, acrylic polymer, poly(methyl methacrylate) (PMMA), polymethacrylate polymer, polyimide polymer, polyamide polymer, alicyclic diamine dodecanedioic acid polymer, epoxy polymer, cycloolefin polymer, cycloolefin copolymer (COC), polymethylpentene polymer, cellulose ester polymer, cellulose triacetate, transparent fluorine-containing polymer, polyacrylonitrile polymer and combinations thereof.
[0121] In accordance with the third aspect or any intervening aspect, the substrate web is a glass web comprising a material selected from the group consisting of borosilicate glass and soda-lime glass.
[0122] According to the third aspect or any intervening aspect, the conductive layer comprises at least one material selected from the following: transparent conductive oxide (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide, metal oxide / metal alloy / metal oxide, insulator-metal-insulator (IMI) stack, silver nanowire coating, carbon nanotubes, graphene coating, conductive nanorods, wire grids, conductive polymers and poly (3,4-ethylenedioxythiophene) (PEDOT).
[0123] According to the third aspect or any intervening aspects, curing the electroactive gel composition comprises at least one of heating the electroactive gel composition and exposing the electroactive gel composition to ultraviolet light.
[0124] According to the third aspect or any intervening aspect, the substrate web further comprises a release liner disposed over the conductive layer, wherein the method further comprises removing the release liner prior to applying the electroactive gel composition on the conductive layer.
[0125] In accordance with the third aspect or any intervening aspect, providing a substrate web comprises unrolling a roll of the substrate web.
[0126] According to the third aspect or any intervening aspect, the electroactive gel composition is applied by one of the following: screen printing process, extrusion process, lamination process, gravure printing process, rod coating process, doctor bar process, sol-gel process, spin coating process, die casting process, dip coating process and inkjet printing process.
[0127] According to a fourth aspect of the present disclosure, a method for forming an electro-optical assembly is provided. The method includes providing a cathode subassembly and an anode subassembly. The cathode subassembly includes a first substrate web, a first conductive layer disposed on the first substrate web, and a cathode gel layer disposed on the first conductive layer, wherein the cathode gel layer includes a cathode component dispersed in a polymer matrix, and the cathode gel layer has a certain thickness. The anode subassembly includes a second substrate web, a second conductive layer disposed on the second substrate web, and an anode gel layer disposed on the second conductive layer, wherein the anode gel layer includes an anode component dispersed in a polymer matrix, and the anode gel layer has a certain thickness. The cathode subassembly and the anode subassembly are assembled together to form an electro-optical subassembly web. A shaped part corresponding to the shape of the electro-optical assembly is cut from the electro-optical subassembly web. At least one of the cathode component or the anode component is electro-optical, and the thickness variation of at least one of the cathode gel layer and the anode gel layer accounts for less than about 20% of the average thickness of the corresponding gel layer.
[0128] According to the fourth aspect, the first substrate web comprises at least one first barrier layer disposed between the first substrate web and the first conductive layer, and the second substrate web comprises at least one second barrier layer disposed between the second substrate web and the second conductive layer. The at least one first barrier layer and the at least one second barrier layer are resistant to at least one of oxygen and water.
[0129] According to the fourth aspect or any intervening aspect, the at least one first barrier layer, the at least one second barrier layer, or both comprise a polymer-inorganic layer-polymer stack or an insulator-metal-insulator (IMI) stack.
[0130] According to the fourth aspect or any intervening aspect, the cathode gel layer and the anode gel layer each include a release liner. The method further comprises removing the release liner from the cathode gel layer and removing the release liner from the anode gel layer before the step of assembling the cathode subassembly and the anode subassembly.
[0131] According to the fourth aspect or any intervening aspect, the cathode gel layer is present in a pattern corresponding to the shaped part, and the anode gel layer is present in a pattern corresponding to the shaped part. The method further comprises aligning the cathode gel layer pattern with the anode gel layer pattern before the step of assembling the cathode subassembly and the anode subassembly. The step of cutting the shaped part from the electro-optical subassembly web comprises cutting the aligned cathode gel layer pattern and the anode gel layer pattern.
[0132] In accordance with the fourth aspect or any intervening aspect, the method further comprises applying a power bus to a portion of the electro-optical assembly web from which the shaped component is cut, simultaneously with or after the step of assembling the cathode subassembly and the anode subassembly.
[0133] According to the fourth aspect or any intervening aspect, the cathode subassembly is provided as a first roll and the anode subassembly is provided as a second roll.
[0134] According to the fourth aspect or any intervening aspects, the cathode component comprises at least one material selected from the group consisting of viologen, metal oxide, methyl viologen, octyl viologen, benzyl viologen, polymeric viologen, ferrocenium, tungsten oxide, vanadium oxide, nickel oxide, perovskite, samarium nickelate and a material of formula A y B z O x A metal oxide wherein A and B are metals, y is 1≤y≤20, z is 1≤z≤20, and x is about 80% to about 120% of the stoichiometric amount.
[0135] According to the fourth aspect or any intervening aspect, the anode component comprises at least one material selected from the group consisting of metallocenes, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazines, substituted phenothiazines, substituted dithiazines, thianthrene and substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl- 5,10-dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT) and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine.
[0136] According to the fourth aspect or any intervening aspect, the first substrate web, the second substrate web or both include a polymer material selected from the following: polyethylene polymers, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone polymers, acrylic polymers, poly(methyl methacrylate) (PMMA), polymethacrylate polymers, polyimide polymers, polyamide polymers, alicyclic diamine dodecanedioic acid polymers, epoxy polymers, cycloolefin polymers, cycloolefin copolymers (COC), polymethylpentene polymers, cellulose ester polymers, cellulose triacetate, transparent fluorinated polymers, polyacrylonitrile polymers and combinations thereof.
[0137] According to the fourth aspect or any intervening aspects, the first conductive layer, the second conductive layer or both include at least one material selected from the following: transparent conductive oxide (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide, metal oxide / metal alloy / metal oxide, insulator-metal-insulator (IMI) stack, silver nanowire coating, carbon nanotubes, graphene coating, conductive nanorods, wire grids, conductive polymers and poly (3,4-ethylenedioxythiophene) (PEDOT).
[0138] Modifications of the present disclosure will occur to those skilled in the art and to those who formulate or use the concepts disclosed herein. It should therefore be understood that the embodiments shown in the drawings and described above are for illustrative purposes only and are not intended to limit the scope of the present disclosure, which is defined by the following claims interpreted in accordance with the principles of patent law including the doctrine of equivalents.
[0139] It should be understood by those of ordinary skill in the art that the described concepts and the construction of other components are not limited to any particular materials. Unless otherwise described herein, other exemplary embodiments of the concepts disclosed herein may be formed of a variety of materials.
[0140] For purposes of this disclosure, the term "coupled" (in all of its forms, couple, coupling, coupled, etc.) generally refers to the joining of two (electrical or mechanical) components directly or indirectly to one another. Such joining may be fixed in nature or removable in nature. Such joining may be achieved by the two (electrical or mechanical) components and any additional intermediate members that are integrally formed as a single unitary body with each other or with the two components. Unless otherwise specified, such joining may be permanent in nature or may be removable or releasable in nature.
[0141] It is also important to note that the construction and arrangement of the elements of the present disclosure as shown in the exemplary embodiments are only illustrative. Although only several embodiments are described in detail in the present disclosure, it will be easily understood by those skilled in the art who review the present disclosure that many modifications are possible (e.g., the size, size, structure, shape and ratio of various elements, parameter values, installation arrangements, use of materials, colors, orientations, etc.), without substantially departing from the novel teachings and advantages of the narrated subject matter. For example, the elements shown as being integrally formed can be composed of multiple parts, or the elements shown as multiple parts can be integrally formed, the operation of the interface can be reversed or otherwise changed, the length or width of the connector or other elements of the structure and / or member or system can be changed, and the nature or quantity of the adjustment position provided between the elements can be changed. It should be noted that the elements and / or assemblies of the system can be constructed with any color, texture and combination in various colors, textures and combinations by various materials providing sufficient strength or durability. Therefore, all such modifications are intended to be included in the scope of the present invention's innovation. Without departing from the spirit of the present disclosure, other substitutions, modifications, changes and omissions can be made in the design, operating conditions and arrangement of the desired and other exemplary embodiments.
[0142] It should be understood that any described process or steps within a described process can be combined with other disclosed processes or steps to form structures within the scope of the present disclosure. The exemplary structures and processes disclosed herein are for illustrative purposes and should not be construed as limiting.
[0143] It will also be understood that changes and modifications may be made to the structures and methods described above without departing from the concepts of the present disclosure and further, it will be understood that such concepts are intended to be covered by the appended claims unless such claims, by their language, expressly state otherwise.
Claims
1. An electro-optical assembly comprising: a substrate web; a conductive layer disposed on the substrate web; as well as an electroactive gel layer disposed on the conductive layer, wherein the electroactive gel layer comprises an electroactive component dispersed in a polymer matrix, the electroactive gel layer comprises a certain thickness, and wherein the thickness variation of the electroactive gel layer accounts for less than 20% of the average thickness of the electroactive gel layer, The electroactive components include: At least one cathode component of the electrochromic device, the at least one cathode component comprising a material selected from the group consisting of viologen, metal oxide, methyl viologen, octyl viologen, benzyl viologen, polymeric viologen, ferrocenium, tungsten oxide, vanadium oxide, nickel oxide, perovskite, samarium nickelate, and a material having the formula A y B z O x wherein A and B are metals, y is 1 ≤ y ≤ 20, z is 1 ≤ z ≤ 20, and x is 80% to 120% of the stoichiometric amount; or At least one anode component of an electrochromic device, the at least one anode component comprising a material selected from the group consisting of metallocene, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazine, substituted phenothiazine, substituted dithiazine, thianthrene, substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl-5,1 0-Dihydrophenazine (DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT), and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine.
2. The electro-optical assembly of claim 1, further comprising: A release liner is disposed over the electroactive gel layer.
3. An electro-photonic assembly according to claim 1 or claim 2, wherein the electroactive gel layer is patterned on the conductive layer.
4. An electro-photonic assembly according to claim 1 or 2, wherein the electroactive component comprises an anode component or a cathode component.
5. The electro-photonic assembly of claim 1 or 2, wherein the substrate web is a polymer web comprising a material selected from the group consisting of polyethylene polymers, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone polymers, acrylic polymers, poly(methyl methacrylate) (PMMA), polymethacrylate polymers, polyimide polymers, polyamide polymers, alicyclic diamine dodecanedioic acid polymers, epoxy polymers, cycloolefin polymers, cycloolefin copolymers (COC), polymethylpentene polymers, cellulose ester polymers, cellulose triacetate, transparent fluoropolymers, polyacrylonitrile polymers, and combinations thereof.
6. An electro-photonic assembly according to claim 1 or 2, wherein the substrate web is a glass web comprising a material selected from the group consisting of borosilicate glass and soda-lime glass.
7. The electro-optical assembly according to claim 1 or 2, further comprising: at least one barrier layer disposed between the substrate web and the conductive layer, Wherein the at least one barrier layer is resistant to at least one of oxygen and water. 8 . The electro-photonic assembly of claim 7 , wherein the at least one blocking layer comprises a polymer-inorganic layer-polymer stack or an insulator-metal-insulator (IMI) stack.
9. An electro-photonic assembly according to claim 1 or 2, wherein the conductive layer comprises at least one material selected from the group consisting of transparent conductive oxides (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide, metal oxide / metal alloy / metal oxide, insulator-metal-insulator (IMI) stacks, silver nanowire coatings, carbon nanotubes, graphene coatings, conductive nanorods, wire grids, conductive polymers, and poly(3,4-ethylenedioxythiophene) (PEDOT).
10. An electro-photonic assembly according to claim 1 or 2, wherein the electroactive component is covalently bonded to the polymer matrix.
11. An electro-optical assembly comprising: A cathode subassembly, the cathode subassembly comprising: a first substrate web; a first conductive layer disposed on the first substrate web; and a cathode gel layer disposed on the first conductive layer, wherein the cathode gel layer comprises a cathode component dispersed in a polymer matrix, the cathode gel layer comprising a thickness; and An anode sub-assembly, the anode sub-assembly comprising: a second substrate web; a second conductive layer disposed on the second substrate web; and an anode gel layer disposed on the second conductive layer, wherein the anode gel layer comprises an anode component dispersed in a polymer matrix, the anode gel layer comprises a certain thickness, and wherein at least one of the cathode component and the anode component is electro-optical, and the thickness of at least one of the cathode gel layer and the anode gel layer varies by less than 20% of the average thickness of the corresponding gel layer, The cathode component comprises at least one material selected from the group consisting of viologen, metal oxide, methyl viologen, octyl viologen, benzyl viologen, polymeric viologen, ferrocenium, tungsten oxide, vanadium oxide, nickel oxide, perovskite, samarium nickelate and a y B z O x A metal oxide wherein A and B are metals, y is 1 ≤ y ≤ 20, z is 1 ≤ z ≤ 20, and x is 80% to 120% of the stoichiometric amount, and The anode component includes at least one material selected from the group consisting of metallocenes, 5,10-dihydrophenazine, phenothiazine, phenoxazine, carbazole, triphenodioxazine, triphenodithiazine, ferrocene, substituted ferrocene, substituted ferrocenyl salts, phenazine, substituted phenazines, substituted phenothiazines, substituted dithiazines, thianthrene, and substituted thianthrene, di-tert-butyl-diethylferrocene, 5,10-dimethyl-5,10-dihydrophenazine ( The following are some of the most common phenazine compounds: DMP), bis(triethylaminopropyl)dihydrophenazine bis(tetrafluoroborate), 3,7,10-trimethylphenothiazine, 2,3,7,8-tetramethoxy-thianthrene, 10-methylphenothiazine, tetramethylphenazine (TMP), 5,10-triethylammoniumpropylphenazine, bis(butyltriethylammonium)-p-methoxytriphenodithiazine (TPDT), and 5,10-dineopentyl-5,10-dihydro-2,7-diisobutylphenazine.
12. The electro-optical assembly of claim 11, wherein the cathode gel layer is patterned on the first conductive layer and the anode gel layer is patterned on the second conductive layer.
13. An electro-optical assembly according to claim 11 or 12, wherein the first substrate web, the second substrate web or both comprise a polymer material selected from the group consisting of polyethylene polymers, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, polysulfone polymers, acrylic polymers, poly(methyl methacrylate) (PMMA), polymethacrylate polymers, polyimide polymers, polyamide polymers, alicyclic diamine dodecanedioic acid polymers, epoxy polymers, cycloolefin polymers, cycloolefin copolymers (COC), polymethylpentene polymers, cellulose ester polymers, cellulose triacetate, transparent fluoropolymers, polyacrylonitrile polymers, and combinations thereof.
14. An electro-optical assembly according to claim 11 or 12, wherein the first substrate web, the second substrate web, or both, comprises a glass material selected from borosilicate glass and soda-lime glass.
15. The electro-optical assembly according to claim 11 or 12, further comprising: at least one first barrier layer disposed between the first substrate web and the first conductive layer; as well as at least one second barrier layer disposed between the second substrate web and the second conductive layer, Wherein the at least one first barrier layer and the at least one second barrier layer are resistant to at least one of oxygen and water.
16. The electro-optical assembly of claim 15, wherein the at least one first barrier layer, the at least one second barrier layer, or both comprise a polymer-inorganic layer-polymer stack or an insulator-metal-insulator (IMI) stack.
17. An electro-optical assembly according to claim 11 or 12, wherein the first conductive layer, the second conductive layer or both comprise at least one material selected from the group consisting of transparent conductive oxides (TCO), fluorine-doped tin oxide (F:SnO2), aluminum-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), doped zinc oxide, indium zinc oxide, metal oxide / metal / metal oxide, metal oxide / metal alloy / metal oxide, insulator-metal-insulator (IMI) stacks, silver nanowire coatings, carbon nanotubes, graphene coatings, conductive nanorods, wire grids, conductive polymers, and poly(3,4-ethylenedioxythiophene) (PEDOT).
Citation Information
Patent Citations
Electrochemical energy storage devices
US20150346573A1
Electro-optical device having a transparent ion exchange membrane
US20190048159A1
Single-compartment, self-erasing, solution-phase electrochromic devices, solutions for use therein, and uses thereof
US4902108A
Electrochromic layer and devices comprising same
US5888431A
Electrochromic layer and devices comprising same
US5928572A