Polyvinylpyrrolidone as a dispersant for lithium-ion battery cathode production

By using a combination of solvents such as polyvinylpyrrolidone and N,N-dimethylpropionamide, the difficulty of dispersing nanoconductive agents in lithium-ion battery cathodes is solved, improving conductivity and production efficiency, reducing manufacturing costs and avoiding A bubble occurs.

CN113614959BActive Publication Date: 2024-10-25DOW GLOBAL TECHNOLOGIES LLC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN201980094497.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-04-26
Publication Date
2024-10-25
Estimated Expiration
2039-04-26

AI Technical Summary

Technical Problem

It is difficult to disperse nano-sized conductive agent particles in the cathode of lithium-ion batteries, which limits the conductivity improvement. Traditional methods require high doses of dispersants and are difficult to avoid foam generation.

Method used

Polyvinylpyrrolidone (PVP) is used as the dispersant, combined with N,N-dimethylpropionamide (DMPA) and other solvents to form a slurry to improve the dispersion of the conductive agent and the solubility of the adhesive polymer to avoid foam generation .

Benefits of technology

It achieves good dispersion of nano conductive agents, improves the conductivity and production efficiency of the cathode, reduces manufacturing costs, and avoids foam problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003272706630000021
    Figure BDA0003272706630000021
  • Figure BDA0003272706630000061
    Figure BDA0003272706630000061
  • Figure BDA0003272706630000071
    Figure BDA0003272706630000071
Patent Text Reader

Abstract

The method for manufacturing a lithium-ion battery cathode comprises the following steps: forming a slurry of an active material, a nano-sized conductive agent, a binder polymer, a solvent, and a dispersant. The solvent is essentially composed of one or more compounds of formula 1 and optionally one or more of N,N-dimethylacetoacetamide, N,N-diethylacetoacetamide, γ-valerolactone, and triethyl phosphate, and the dispersant comprises polyvinyl pyrrolidone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the production of lithium-ion batteries. On the one hand, the present invention relates to the production of cathodes for such batteries, and on the other hand, the present invention relates to materials for the production of such cathodes. Background Art

[0002] The significant growth of electric vehicles and portable electronic devices has increased the demand for rechargeable batteries (also called secondary batteries), especially various types of lithium-ion batteries. The modern trend of small size and light weight requires these rechargeable batteries to have not only high energy density, but also environmentally friendly. The requirement for eco-friendly environment applies not only to the battery products themselves, but also to the production methods for manufacturing them.

[0003] The cathode assembly of a lithium-ion battery is made by forming a slurry from an active material (e.g., lithium cobalt oxide, lithium iron phosphate, etc.) dissolved in a solvent and a binder polymer (e.g., polyvinylidene fluoride (PVDF)), coating the slurry on an aluminum foil, and drying the coated foil to remove the solvent. The conductivity of the cathode is always a goal of improvement, and for this purpose, lithium-ion battery manufacturers add conductive agents to the mixture. These agents (e.g., carbon black) form part of the slurry that is coated on the aluminum foil. In addition to having good conductivity, these conductive agents also have the characteristics of low gravity, stable structure, and good chemical resistance.

[0004] Generally speaking, the smaller the size of the conductive agent, the better the conductivity. It is well known that nano-sized particles have extremely high surface area and surface energy, but due to these characteristics, they tend to aggregate, or in other words, they are difficult to disperse. If the nano-sized conductive agent particles are not well dispersed in the cathode, then their improvement in cathode conductivity will be weakened.

[0005] In order to disperse and stabilize the nano-sized conductive agent in the cathode material of the slurry formulation, strong repulsion between the nano-sized conductive agent particles is required. The traditional method to achieve this is to use electrostatic mechanisms to change the density and type of surface charge on the particles. However, this method requires high dosage levels of dispersants. Summary of the invention

[0006] In one embodiment, the present disclosure provides a method for manufacturing a lithium ion battery cathode, the method comprising the steps of: forming a slurry of an active material, a nano-sized conductive agent, a binder polymer, a solvent, and a dispersant,

[0007] The solvent consists essentially of: one or more compounds of formula 1

[0008]

[0009] wherein R1 and R2 are hydrogen or C1-4 straight or branched alkyl or alkoxy, and R3 is C1-10 straight or branched alkyl or alkoxy, with the proviso that R1 and R2 are not both hydrogen; and optionally, one or more of N,N-dimethylacetoacetamide, N,N-diethylacetoacetamide, γ-valerolactone and triethyl phosphate; and the dispersant comprises polyvinylpyrrolidone.

[0010] In some embodiments, polyvinyl pyrrolidone ("PVP") is used as a dispersant in combination with a solvent of Formula 1 (and optionally in combination with one or more of N,N-dimethylacetoacetamide, N,N-diethylacetoacetamide, γ-valerolactone, and triethyl phosphate) and has several advantages. Specifically, PVP can advantageously dissolve quickly in the solvent and disperse the nano-sized conductive agent, thereby achieving good cathode coating, while advantageously avoiding the generation of foam. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 A block flow diagram is provided to illustrate a conventional production process for making lithium-ion batteries, wherein NMP is used as a solvent in forming cathode and anode slurries from active materials, conductive agents, binders, and dispersants.

[0012] Figure 2 is a collection of micrographs showing the appearance of SUPER P conductive carbon black in different dispersants. DETAILED DESCRIPTION

[0013] definition

[0014] For purposes of U.S. patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or their equivalent U.S. versions are so incorporated by reference), particularly with respect to the definitions of the present disclosure (to the extent not inconsistent with any definitions specifically provided in the present disclosure) and common knowledge in the art.

[0015] The numerical range disclosed herein includes all values ​​from the lower limit and the upper limit, and includes the lower limit and the upper limit. For a range containing an exact value (e.g., 1 to 7), any sub-range (e.g., 1 to 2; 2 to 6; 5 to 7; 3 to 7; 5 to 6; etc.) between any two exact values ​​is included.

[0016] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not the components, steps or procedures are specifically disclosed. For the avoidance of any doubt, all compositions claimed by using the term "comprising" may include any additional additives, adjuvants or compounds, whether in polymeric or other forms, unless stated to the contrary. In contrast, the term "consisting essentially of excludes any other components, steps or procedures from the scope of any subsequent enumeration, except those that are not essential to operability. The term "consisting of" excludes any components, steps or procedures that are not specifically depicted or listed. Unless otherwise stated, the term "or" refers to members listed individually and in any combination. The use of the singular encompasses the use of the plural, and vice versa.

[0017] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all test methods are current as of the filing date of this disclosure.

[0018] As used in the context of lithium-ion batteries, "active material" and similar terms mean either a source of lithium ions or a substance that receives and accepts lithium ions. In the case of the cathode of a lithium-ion battery cell, the active material is a source of lithium ions, such as lithium cobalt oxide, lithium manganese oxide, etc. In the case of the anode of a lithium-ion battery cell, the active material is an acceptor of lithium ions, such as graphite. The active material is typically in the form of very small particles ranging in diameter from 1000 nanometers to 100 micrometers.

[0019] "Alkoxy" refers to -OZ 1 Group, where Z is representative 1 The term "alkoxy" refers to alkyl, substituted alkyl, cycloalkyl, substituted cycloalkyl, heterocycloalkyl, substituted heterocycloalkyl, silyl and combinations thereof. Suitable alkoxy groups include, for example, methoxy, ethoxy, benzyloxy, tert-butoxy, etc. A related term is "aryloxy", where representative Z 1 Included are aryl, substituted aryl, heteroaryl, substituted heteroaryl, and combinations thereof. Examples of suitable aryloxy groups include phenoxy, substituted phenoxy, 2-pyridyloxy, 8-quinolyloxy, and the like.

[0020] "Alkyl" refers to a saturated straight chain, cyclic or branched hydrocarbon group. Non-limiting examples of suitable alkyl groups include, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, isobutyl (or 2-methylpropyl), etc. In one embodiment, the alkyl group has 1 to 20 carbon atoms.

[0021] "Anode" and similar terms as used in the context of lithium-ion batteries mean the negative electrode in a discharge cycle. The anode is the electrode within the battery where oxidation occurs during discharge, ie, electrons are released and flow out of the battery.

[0022] "Battery" and similar terms mean a collection of battery cells or battery cell assemblies ready for use. A battery typically contains a suitable housing, electrical interconnects, and may contain electronics to control and protect the battery cells from failure (e.g., fire, thermal runaway, explosion, loss of charge, etc.). The simplest battery is a single battery cell. Batteries can be primary (i.e., non-rechargeable) or secondary (i.e., rechargeable).

[0023] As used in the context of lithium-ion batteries, "binder polymer" and similar terms mean a polymer that holds active material particles together within the electrodes of a lithium-ion battery to maintain a strong connection between the electrodes and the contacts. The binder polymer is generally inert to materials with which it comes into contact in a lithium-ion battery during discharge, charge, and storage.

[0024] "Cathode" and similar terms as used in the context of lithium-ion batteries mean the positive electrode in the discharge cycle. The lithium in a lithium-ion battery is in the cathode. The cathode is the electrode where reduction occurs within the battery during discharge.

[0025] "Battery" and similar terms mean the basic electrochemical unit comprising electrodes, separator, and electrolyte.

[0026] "Conductive agent" and similar terms as used in the context of lithium-ion batteries mean a substance that facilitates the flow of ions between the electrodes of a battery cell. Carbon-based compounds and materials such as acetylene black, carbon nanotubes, carbon-based polymers, etc. are typical conductive agents used in lithium-ion batteries.

[0027] "Dispersant" and similar terms mean a substance added to a suspension, usually a colloidal one, to improve particle separation and prevent settling or agglomeration. Dispersants are usually composed of one or more surfactants.

[0028] "Electrolyte" and similar terms as used in the context of lithium-ion batteries means the substance that carries positively charged lithium ions from the anode to the cathode, and vice versa, through the separator.

[0029] "Lithium-ion battery" and similar terms mean a rechargeable, i.e., secondary, battery in which lithium ions move from the negative electrode to the positive electrode during discharge and return to the negative electrode during charging. Lithium-ion batteries use intercalated lithium compounds as an electrode material, as opposed to metallic lithium used in non-rechargeable lithium batteries (also called primary batteries). An electrolyte that allows ions to move and two electrodes are the constituent components of a lithium-ion battery cell.

[0030] "Nano" means one billionth (10 -9 ). "Nano-sized particles" and similar terms mean the size of a particle (e.g., diameter, length / width / depth, etc.) typically measured in parts per billion. Nano-sized particles include particles that are smaller or larger than parts per billion, for example, particles up to one millionth and down to one pico in size.

[0031] "Separator" and similar terms as used in the context of lithium-ion batteries mean a porous film that physically separates the anode and cathode. The primary function of the separator is to prevent physical contact between the anode and cathode while facilitating the transport of lithium ions within the battery cell. The separator is typically a simple plastic film, such as polyethylene or polypropylene, or a ceramic, with pores designed to allow lithium ions to pass through.

[0032] "Solvent" and like terms mean a substance that is capable of dissolving another substance (ie, a solute) so as to form a substantially uniformly dispersed mixture (ie, a solution) at the molecular or ionic size level.

[0033] Production method of lithium-ion battery

[0034] Figure 1 A flow chart showing a conventional production method for a lithium-ion battery is shown, wherein NMP is used as a solvent. NMP is used as a solvent to dissolve a binder polymer such as polyvinylidene fluoride (PVDF), which is then used to form a slurry of active materials, conductive agents, dispersants, and other additives. Conductive agents include, but are not limited to, carbon black, carbon nanotubes, graphene, nanographite, and / or fullerenes. Active materials include, but are not limited to: lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium cobalt manganese nickel oxide (LiNiMnCoO2 or NMC), lithium iron phosphate (LiFePO4), lithium aluminum cobalt nickel oxide (LiNiCoAlO2), and lithium titanate (Li4Ti5O 12 ). The slurry is then coated onto a foil, typically aluminum for the cathode and copper for the anode, and the coated foil is then dried.

[0035] During the drying process (typically in an oven), the NMP evaporates without residue, and the dried foil comprises a film with a thickness of 50 to 200 microns and contains a solid component, which is a dried slurry including a binder polymer, active materials, conductive agents, dispersants, and other additives. The dried foil is then rolled in a calender to solidify it and then collected on a reel. Finally, the cathode and anode films are combined into an electrode stack and the battery cell is completed by adding an electrolyte.

[0036] Conductive agent

[0037] Any nano-sized conductive agent can be used in the practice of the disclosed embodiments. Typically, the conductive agent is nano-sized carbon black, such as acetylene black, carbon nanotubes, carbon nanofibers, graphene, nanographite, etc. In some embodiments, the nano-sized conductive agent has an average particle size of 1.2 microns or less. In some embodiments, the nano-sized conductive agent has an average particle size of 1.0 microns or less. Available from TIMCAL TM Graphite and Carbon's SUPER P conductive carbon black is an example of a commercially available conductive agent that can be used in practicing embodiments of the present disclosure. SUPER P conductive carbon black has an average particle size of about 1 micron.

[0038] Dispersants

[0039] The dispersant used in practicing the embodiments of the present disclosure is polyvinyl pyrrolidone, which has the structure:

[0040]

[0041] Wherein n is 100 to 10,000. In some embodiments, n in the above structure is 300 to 3,000. The dispersant can be, for example, a single PVP species having one molecular weight, or a mixture of PVPs having different molecular weights. In some embodiments, the PVP has a molecular weight of 3,000 to 400,000, in other embodiments, a molecular weight of 10,000 to 200,000, and in other embodiments, a molecular weight of 30,000 to 60,000. Non-limiting examples of commercially available PVPs include PVP K-15, PVP K-30, PVP K-60, and other PVPs available from various suppliers. In some embodiments in which the solvent used in the slurry is DMPA, the amount of PVP in the slurry can be 0.01 to 5 wt %, or 0.1 to 2 wt %, or 0.3 to 1 wt % (each based on the total weight of the slurry).

[0042] The dispersant may consist solely of PVP (preferred), or it may include PVP and one or more other dispersants, such as polyethylene glycol, and other nonionic and anionic surfactants. In the case of mixing with one or more other dispersants, PVP typically includes at least 50wt% or 55wt% or 60wt% or 65wt% or 70wt% or 75wt% of the dispersant mixture. In some embodiments where other dispersants are used with PVP, the mixture of dispersants does not contain ethyl cellulose. In some embodiments where other dispersants are used with PVP, the mixture of dispersants includes less than 1wt% ethyl cellulose, or less than 0.1wt% ethyl cellulose, or less than 0.01wt% ethyl cellulose (each by weight of the dispersant mixture).

[0043] Solvents

[0044] The solvents used in the practice of the disclosed embodiments are Figure 1 An alternative solvent for NMP in the lithium-ion battery production method shown. This solvent consists of or is essentially composed of: one or more compounds of formula 1, and optionally one or more of N,N-dimethylacetoacetamide, N,N-diethylacetoacetamide, γ-valerolactone and triethyl phosphate. In one embodiment, the solvent consists of only one of any compounds of formula 1. In one embodiment, the solvent consists of N,N-dimethylpropionamide (DMPA). In those embodiments in which the solvent consists of formula 1 or consists of two or more compounds of formula 1 or consists of a compound of formula 1 and one or more of N,N-dimethylacetoacetamide, N,N-diethylacetoacetamide, γ-valerolactone and triethyl phosphate, the amount of any one compound in the mixture may vary in the range of 1 to 99 weight percent (wt%) or 10 to 90 wt% or 20 to 80 wt% or 30 to 70 wt% or 40 to 60 wt% of the weight of the mixture. In one embodiment, each solvent in the solvent mixture is present in an amount of 20 wt %, or 15 wt %, or 10 wt %, or 5 wt %, or 3 wt %, or 1 wt % of each other solvent in the mixture.

[0045] In one embodiment, the solvent used in the practice of the present invention consists of a compound of Formula 1. In one embodiment, the solvent used according to the embodiments of the present disclosure consists of two or more compounds of Formula 1

[0046]

[0047] wherein R1 and R2 are hydrogen or C1-4 straight or branched chain alkyl or alkoxy, and R3 is C1-10 straight or branched chain alkyl or alkoxy, provided that R1 and R2 are not both hydrogen.

[0048] In one embodiment, the solvent comprising the compound of formula 1 is one or more of: N,N-dimethylpropionamide (DMPA); 3-methoxy-N,N-dimethylpropionamide (M3DMPA); N,N-dimethylbutanamide; N,N-dimethylvaleramide; N,N-diethylpropionamide; N,N-dipropylpropionamide; N,N-dibutylpropionamide; N,N-dimethylethylpropionamide; 3-butoxy-N-methylpropionamide; and N,N-diethylacetamide (DEAC). In one embodiment, the compound of formula 1 is DMPA.

[0049] In some embodiments, the solvent used in the practice of the present invention includes at least one additional compound in addition to the solvent according to Formula 1. Examples of solvents that can be mixed with the solvent according to Formula 1 include N,N-dimethylacetoacetamide (DMAA), N,N-diethylacetoacetamide (DEAA), γ-valerolactone, triethyl phosphate (TEP), and mixtures thereof.

[0050] Each solvent used in the practice of the present invention is a known compound that is liquid under ambient conditions (23° C. and atmospheric pressure) and is generally commercially available. To form a mixture of two or more solvents (e.g., two or more solvents of Formula 1; or a solvent of Formula 1 and one or more of DMAA, DEAA, and TEP), the solvents can be simply mixed with each other using conventional mixing equipment and standard mixing protocols. The individual solvents can be added to each other in any order (including simultaneously).

[0051] In one embodiment, the solvent is intended to replace NMP in a process for producing a lithium ion battery. Thus, it is useful in the process (e.g., Figure 1 Typically, the method comprises the following steps: dissolving the binder polymer with a solvent, and then forming a slurry from the dissolved binder, active material, conductive agent and dispersant. The slurry is then applied to a foil and the foil is dried, during which the solvent is removed by evaporation.

[0052] Compared with NMP, the solvent used in the practice of the embodiments of the present disclosure can dissolve the binder polymer faster, which can then improve the production efficiency of the battery. Compared with the binder polymer solution based on NMP, the binder polymer solution based on the solvent used in the embodiments of the present disclosure also shows a lower viscosity, which in turn also improves the production efficiency of the battery. In addition, compared with NMP, some solvents used in the embodiments of the present disclosure have a lower boiling point and a higher evaporation rate, which means that they can evaporate faster and leave less residue with lower energy consumption. Since NMP is typically recycled, the solvent disclosed herein is easier to recycle due to its lower boiling point and higher evaporation rate, thereby saving the overall cost of the battery production method.

[0053] In one embodiment, the present disclosure provides a method for manufacturing a cathode for a lithium ion battery, wherein one or more compounds of Formula 1 (or a compound of Formula 1 and one or more solvents used as a binder polymer, and polyvinyl pyrrolidone is a dispersant for a nano-sized conductive agent. This combination of solvent and dispersant results in good conductive agent dispersion, strong dissolving power for PVDF, shorter dissolution time and lower viscosity. These benefits bring value to lithium ion battery manufacturers due to increased production efficiency and reduced manufacturing costs.

[0054] By way of example and not limitation, some embodiments of the present disclosure will now be described in detail in the following examples.

[0055] Examples

[0056] Material

[0057] The solvents were N-methyl-2-pyrrolidone (NMP) (Sinopharm Group, 99%) and N,N-dimethylpropionamide (DMPA) (Xingxin, 98%). All solvent samples were treated with 4A dehydrated molecular sieves (from Sigma-Aldrich) for more than 2 days to remove water.

[0058] Nano-sized conductive agents are available from TIMCAL TM Graphite and Carbon's SUPER P conductive carbon black.

[0059] The dispersant was ETHOCEL from Dow Chemical Company TM Std. 100 ethyl cellulose and PVP K-30 polyvinylpyrrolidone (PVP) from Sinopharm Chemical Reagent Co., Ltd. The dispersion was dehydrated in a 60°C oven for at least two hours before use.

[0060] The binder was Kynar 761A polyvinylidene fluoride (PVDF) from Arkema Group. The PVDF was dehydrated in an oven at 80°C for at least two hours before use.

[0061] The cathode material was lithium iron phosphate (LiFePO4 or LFP) from AVIC Lithium Battery Co., Ltd. The cathode material was dehydrated in an oven at 80°C for more than 2 hours before use.

[0062] Example 1

[0063] In this example, the time to dissolve a dispersant in a DMPA solvent is measured. 0.2 grams of the specified dispersant and 19.8 grams of DMPA are added to a vial, and the vial is then sealed with a cap. The vial is secured in a SPEEDMIX TMDAC 150.1FVZ-k mixer and mixed at 2000rpm. During the mixing process, the mixer was stopped every 2 minutes to cool and determine whether all dispersants were dissolved. The time when all dispersants in the vial were dissolved was recorded. The different samples and results are shown in Table 1.

[0064] Table 1

[0065] sample Composition Dissolution time (minutes) Comparative Example A 1wt.% ethyl cellulose in DMPA 28 Comparative Example B 2wt.% ethyl cellulose in DMPA 52 Comparative Example C 3wt.% ethylcellulose in DMPA 66 Example 1 of the present invention 1wt.% PVP in DMPA 4 Example 2 of the present invention 2wt.% PVP in DMPA 6 Example 3 of the present invention 3wt.% PVP in DMPA 8

[0066] Foaming of these solutions is not desirable. After mixing, Comparative Example A and Inventive Example 1 were manually shaken for 30 seconds to evaluate foaming. Comparative Example A produced a stable foam (less than 1 cm in height) that lasted for more than 30 minutes. In contrast, Inventive Example 1 did not produce foam bubbles even after vigorous shaking.

[0067] Example 2

[0068] In this example, the dispersing properties of two dispersants were evaluated. A specified amount of conductive agent (Super P conductive carbon black) was weighed in a vial. A solvent in which the specified dispersant was dissolved was added. The vial was sealed with a cap and placed in a SPEEDMIX TM Mixing was performed in a DAC 150.1FVZ-k mixer at 3000 rpm for 3 minutes, and then repeated for another 3 minutes. After mixing, the conductive agent dispersion was poured on a glass slide to observe whether the conductive agent particles were agglomerated or dispersed. The appearance of the solution was observed using a LEICA DM2500 M microscope and micrographs were taken. Figure 2 The appearance of the conductive agent in two different concentrations of the dispersant is shown. Figure 2 As shown, the dispersibility of the conductive agent in DMPA is better when PVP is used as a dispersant than when ethyl cellulose is used as a dispersant.

[0069] Example 3

[0070] For this example, cathode slurry performance and coating performance were evaluated. Table 2 below shows the different cathode slurry formulations that were prepared. Each slurry formulation was prepared as follows.

[0071] First, prepare a high concentration PVDF solution. Transfer PVDF to a 3-neck flask and fill with solvent according to the desired concentration. After purging with high-quality N2 for 10 minutes, heat the oil bath to 60°C and start mixing at 60rpm. After all solid or gel-like substances are completely dissolved, stop the equipment and transfer the solution to a clean, dry glass bottle for use.

[0072] According to the procedure described in Example 2, four different conductive agent dispersions were prepared using dispersants and solvents.

[0073] Next, cathode slurry was prepared by using conductive agent dispersion, cathode material, PVDF solution and solvent. The components in the amounts specified for cathode slurry in Table 2 were added to a vial. The vial was sealed with a cap and placed in a SPEEDMIX TM Mix at 3000 rpm for 18 minutes in a DAC 150-1FVZ-k mixer. During this step, the mixer was stopped every 3 minutes for cooling. The viscosity of each cathode slurry was measured at 25°C using the #63 spindle on a Brookfield DV1MLVTJ0 viscometer according to ASTM D562-2001. The viscosity is shown in Table 2.

[0074] Next, a 20 cm x 30 cm aluminum foil sample was cleaned with ethanol and dried to serve as a substrate for the cathode slurry. Each cathode slurry was applied to the Al foil substrate using a manual scraping blade with a gap of 150 microns. After applying scraping, the wet coating was moved to a ventilated drying oven. The drying temperature started at 50 ° C and was maintained at this temperature for 30 minutes. Then, the temperature was increased by 10 ° C and maintained at this temperature for 30 minutes. These temperature increases continued until a temperature of 100 ° C was reached.

[0075] The coating surface morphology was characterized with high resolution to determine whether the conductive agent was well dispersed. For each cathode slurry formulation, the slurry was applied to four film samples. On each coated film sample, the resistance at three locations was tested using a 4-probe tester to evaluate the resistance. A total of twelve data points were collected and the average resistance is reported in Table 2. In addition, the adhesion of two points on four different samples of each cathode slurry formulation was tested. Adhesion was measured according to ASTM D-3359. These results are shown in Table 2.

[0076] Table 2

[0077]

[0078] As seen in the above examples, the combination of PVP and DMPA as dispersants is a solvent that provides good carbon black dispersion, good slurry viscosity, desirable cathode resistance, and desirable adhesion. In addition, PVP dissolves much faster in the solvent relative to the ethylcellulose dispersant while also avoiding foaming. This is beneficial for the manufacture of lithium-ion batteries.

Claims

1. A method for manufacturing a lithium ion battery cathode, the method comprising the following steps: forming a slurry of active material, nano-sized conductive agent, binder polymer, solvent and dispersant, The solvent is N,N-dimethylpropionamide (DMPA); and The dispersant is polyvinyl pyrrolidone. 2 . The method according to claim 1 , wherein the nano-sized conductive agent is carbon black, carbon nanotubes, graphene or nanographite.

3. The method of claim 1, wherein the binder polymer is polyvinylidene fluoride (PVDF). The method of claim 2 , wherein the binder polymer is polyvinylidene fluoride (PVDF).

5. The method according to any one of claims 1 to 4, wherein the active material is lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel manganese cobalt oxide (LiNiMnCoO2), lithium iron phosphate (LiFePO4), lithium nickel cobalt aluminum oxide (LiNiCoAlO2) and lithium titanate (Li4Ti5O 12 ) 6. A cathode produced by the method according to any one of claims 1 to 5.

7. A lithium ion battery comprising the cathode according to claim 6.

Citation Information

Patent Citations

  • Method for preparation of electrode slurry

    CN101207193A

  • Electrode assembly and secondary battery having the same

    CN101604767A

  • Conductive agent dispersion liquid, electrode slurry, electrode, battery, and preparation methods thereof

    CN101752548A

  • Negative electrode material and preparation method thereof, negative electrode plate and lithium ion battery

    CN107946561A

  • Anode material of lithium battery