A high-brightness silver film, reflective sheet and backlight module
By setting a UV pre-coating on a PET base film, adjusting the refractive index and thickness with UV-cured acrylic resin, and combining a silver plating layer and a protective layer, the problem of limited improvement in reflectivity of the silver plating film was solved, and a significant effect of enhancing reflectivity was achieved.
Patent Information
- Application Number
- CN202111108998.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-09-22
AI Technical Summary
In existing technologies, the improvement in reflectivity of silver-coated films is limited, making it difficult to meet higher optical performance requirements.
By setting a UV pre-coating on a PET base film, using UV-cured acrylic resin, adjusting its refractive index and thickness, and combining it with a silver plating layer and a protective layer, the optical performance is optimized to improve reflectivity.
It significantly improves the reflectivity of the silver coating, exceeding existing technologies and the company's previous patents, with an increase of over 5.73%, optimizing light source incidence and reducing reflection loss.
Smart Images

Figure CN113625378B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optical films, and in particular to a high-brightness silver film, a reflective sheet and a backlight module. Background Art
[0002] Optical reflective film has the function of reflecting the light source of the light guide plate in the LCD backlight module. Common specifications on the market include white reflective film, mainly products of Japanese companies Mitsubishi and Toray Industries, Ltd., and similar products of Chinese companies such as Nan Ya, Changhong, and Changyang Products; or reflective film in the form of multi-layer stacked extrusion, represented by 3M's ESR. The former is mostly used for large LCD screens, while the latter is common in small and medium-sized display products, from mobile phones to tablets and laptops. Guangzhi Optoelectronics Company uses silver reflective film, mainly focusing on the backlight modules of mobile phones and tablets with LCD screens, and has a considerable product share in the domestic reflective film market.
[0003] Our company's published patent application (publication number CN111679508A) describes the use of coating stacking to increase reflective brightness and makes adjustments to the process. Another patent application (publication number CN112015005A) describes a structure that uses two layers of metal film reflection to enhance reflective efficiency. The above patent application (publication number CN111679508A) discloses the use of three layers of PET functional film stacking to optimize optical benefits and also increases the reflective brightness to a maximum efficiency of 3.05%.
[0004] In order to further increase the reflective brightness, this proposal considers focusing the research on the UV pre-coating of the PET optical film, by changing the optical properties of the PET base film (including the UV pre-coating) to further improve the reflective brightness of the silver-coated film. Summary of the invention
[0005] In order to solve the problems raised in the above background technology, the present invention provides a high brightness silver film and a reflective sheet for a mobile phone backlight module to further improve the reflective brightness of the silver-plated film.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a high-brightness silver film, comprising: a first PET layer; a first pre-coating layer, arranged on the first PET layer; a UV pre-coating layer, arranged on the first pre-coating layer; a silver-plated layer, arranged on the UV pre-coating layer; a protective layer, arranged on the silver-plated film; the thickness of the silver-plated layer is 90 to 120 nm, the UV pre-coating layer is an acrylic resin cured by UV light, the refractive index of the UV pre-coating layer is 1.483 to 1.562, and the thickness of the UV pre-coating layer is 1.5-2.5 μm.
[0007] Among them, the first pre-coating layer is mainly composed of water-based acrylic resin, and its formula includes the following components by mass: 15% propylene glycol methyl ether, 5% butyl acrylate, 8% butyl methacrylate, 25% methyl methacrylate, 10% methacrylic acid ~ 5% styrene, 2% initiator Tx21S, 2% dimethylethanolamine, and the rest is 28% ethanol.
[0008] As an optimal embodiment of the high-brightness silver film of the present invention, the thickness of the silver-plated layer is 90 nm, the thickness of the UV pre-coating layer is 2.5 μm, and the refractive index of the UV pre-coating layer is 1.524.
[0009] As an optimal embodiment of the high-brightness silver film of the present invention, the thickness of the silver-plated layer is 120 nm, the thickness of the UV pre-coating layer is 1.5 μm, and the refractive index of the UV pre-coating layer is 1.483 or 1.524.
[0010] As an optimal embodiment of the high-brightness silver film of the present invention, the thickness of the silver-plated layer is 120 nm, the thickness of the UV pre-coating layer is 2.5 μm, and the refractive index of the UV pre-coating layer is 1.524 or 1.547.
[0011] A high-brightness reflective sheet comprises the above-mentioned high-brightness silver film, wherein an aluminized film is bonded to the surface of the protective layer of the high-brightness silver film via a bonding layer, wherein the aluminized film comprises a second PET layer and an aluminized layer arranged on the second PET layer, and wherein the aluminized layer is arranged between the bonding layer and the second PET layer.
[0012] More specifically, the bonding layer is UV-PSA or polyurethane glue.
[0013] More specifically, the thickness of the first PET layer is 25 μm, and the thickness of the second PET layer is 50 μm.
[0014] More specifically, the thickness of the aluminum plating layer is 45 nm.
[0015] A backlight film group comprises a back plate, a light source, a light guide plate and a high-brightness reflective sheet arranged in sequence, wherein the high-brightness reflective sheet is the high-brightness reflective sheet mentioned above.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention can further enhance the silver reflection brightness by improving the UV pre-coating layer and changing the optical properties of the PET base film (including the UV pre-coating layer), which is not only higher than the reflection brightness of the existing optical commodity film, but also higher than the brightness of the CN11679508A reflection film previously applied for by the company. Compared with the prior art, the UV pre-coating layer with an optical refractive index design effect is used to optimize the light source incident and reduce the reflection loss caused by the incident light source colliding with the silver film, that is, the reflection brightness is relatively effectively improved. In the research range of this design scheme (1.483-1.562), it is found that in a range lower than the optical refractive index of the PET film (1.56), when the silver film thickness is 120nm, the thickness and refractive index of the UV acrylic resin pre-coating layer are 2.5μm and 1.524 respectively, which can reach 5.73% higher than the currently commercially available product GF-80D3, and the effect is remarkable. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the seventh embodiment of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0018] Figure 1 It is a schematic structural diagram of the high brightness silver film of the present invention;
[0019] Figure 2 It is a schematic structural diagram of the high brightness reflector of the present invention. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] See also Figure 1-2, Embodiment 1 of the high brightness reflective sheet comprises: a first PET layer 100; a first pre-coating layer 200, arranged on the first PET layer 100; a UV pre-coating layer 300, arranged on the first pre-coating layer 200, and a silver-plated layer 400, arranged on the UV pre-coating layer 300; a protective layer 500, arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film comprises a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer is 120nm, the thickness of the UV pre-coating layer is 1.5μm, and the refractive index of the UV pre-coating layer is 1.483.
[0022] Embodiment 2 of the high brightness reflective sheet includes: a first PET layer 100; a first pre-coating layer 200, which is arranged on the first PET layer 100; a UV pre-coating layer 300, which is arranged on the first pre-coating layer 200, and a silver-plated layer 400, which is arranged on the UV pre-coating layer 300; a protective layer 500, which is arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film includes a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer is 120nm, the thickness of the UV pre-coating layer is 1.5μm, and the refractive index of the UV pre-coating layer is 1.524.
[0023] Embodiment 3 of the high brightness reflective sheet comprises: a first PET layer 100; a first pre-coating layer 200, arranged on the first PET layer 100; a UV pre-coating layer 300, arranged on the first pre-coating layer 200, and a silver-plated layer 400, arranged on the UV pre-coating layer 300; a protective layer 500, arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film comprises a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer is 120nm, the thickness of the UV pre-coating layer is 2.5μm, and the refractive index of the UV pre-coating layer is 1.524.
[0024] Embodiment 4 of the high brightness reflective sheet includes: a first PET layer 100; a first pre-coating layer 200, which is arranged on the first PET layer 100; a UV pre-coating layer 300, which is arranged on the first pre-coating layer 200, and a silver-plated layer 400, which is arranged on the UV pre-coating layer 300; a protective layer 500, which is arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film includes a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer is 120nm, the thickness of the UV pre-coating layer is 2.5μm, and the refractive index of the UV pre-coating layer is 1.547.
[0025] Embodiment 5 of the high brightness reflective sheet comprises: a first PET layer 100; a first pre-coating layer 200, arranged on the first PET layer 100; a UV pre-coating layer 300, arranged on the first pre-coating layer 200, and a silver-plated layer 400, arranged on the UV pre-coating layer 300; a protective layer 500, arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film comprises a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer is 90nm, the thickness of the UV pre-coating layer is 1.5μm, and the refractive index of the UV pre-coating layer is 1.483.
[0026] Embodiment 6 of the high brightness reflective sheet comprises: a first PET layer 100; a first pre-coating layer 200, arranged on the first PET layer 100; a UV pre-coating layer 300, arranged on the first pre-coating layer 200, and a silver-plated layer 400, arranged on the UV pre-coating layer 300; a protective layer 500, arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film comprises a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer is 90nm, the thickness of the UV pre-coating layer is 1.5μm, and the refractive index of the UV pre-coating layer is 1.524.
[0027] Embodiment 7 of the high brightness reflective sheet comprises: a first PET layer 100; a first pre-coating layer 200, arranged on the first PET layer 100; a UV pre-coating layer 300, arranged on the first pre-coating layer 200, and a silver-plated layer 400, arranged on the UV pre-coating layer 300; a protective layer 500, arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film comprises a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer 400 is 90nm, the thickness of the UV pre-coating layer 300 is 2.5μm, and the refractive index of the UV pre-coating layer 300 is 1.524.
[0028] Embodiment 8 of the high brightness reflective sheet comprises: a first PET layer 100; a first pre-coating layer 200, arranged on the first PET layer 100; a UV pre-coating layer 300, arranged on the first pre-coating layer 200, and a silver-plated layer 400, arranged on the UV pre-coating layer 300; a protective layer 500, arranged on the silver-plated layer 400; an aluminum-plated film is bonded to the surface of the protective layer 500 through a bonding layer 600, and the aluminum-plated film comprises a second PET layer 800 and an aluminum-plated layer 700 arranged on the second PET layer 800, and the aluminum-plated layer 700 is arranged between the bonding layer 600 and the second PET layer 800; the UV pre-coating layer 300 is an acrylic resin cured by UV light, the thickness of the silver-plated layer 400 is 90nm, the thickness of the UV pre-coating layer 300 is 2.5μm, and the refractive index of the UV pre-coating layer 300 is 1.527.
[0029] In the above-mentioned embodiments 1 to 8, the first pre-coating layer 200 is a pre-coating layer connected to the first PET layer 100, and is mainly composed of a commercial water-based acrylic resin material, and its formula is 15% propylene glycol methyl ether, 5% butyl acrylate, 8% butyl methacrylate, 25% methyl methacrylate, 10% methacrylic acid-5% styrene, 2% initiator Tx21S, 2% dimethylethanolamine, and the rest is 28% ethanol. In the process, the above-mentioned pre-coating layer and ethanol are adjusted in a ratio of 1:3, and the viscosity is 120cps. The micro-concave coating machine speed is 180m / m, the baking temperature is 110°C, and the thickness is 0.5-1.0μm.
[0030] Among them, the acrylic resin formulas of four UV pre-coatings with different refractive indices (1.483, 1.524, 1.547, 1.562) are as follows:
[0031] Chemical name Monomer type Refractive Index 1.483 1.524 1.547 1.562 Tripropylene glycol diacrylate TPGDA 1.448 21 Tetrahydropyran acrylate THFA 1.458 26 6 Ethoxylated (10) bisphenol A diacrylate BPA(10EO)DA 1.515 27 27 27 10 Polyethylene glycol (600) diacrylate PEG(600)DA 1.468 10 10 o-Phenylphenethoxyethyl acrylate OPPEOA 1.576 10 27 48 52 2-Phenoxyethyl acrylate PHEA 1.515 2 26 21 18 p-Phenyl Methacrylate BPMA 1.601 16 1-Hydroxycyclohexylphenyl ketone 184 3 3 3 3 (2,4,6-Trimethylbenzoyl)diphenylphosphine oxide TPO 1 1 1 1
[0032] Formula table description: For the UV pre-coating layer with a refractive index of 1.483 (UV light-cured acrylic resin), its composition ratio is: 21% (mass fraction) of tripropylene glycol diacrylate, 26% of tetrahydrofuran acrylate, 27% of ethoxylated (10) bisphenol A diacrylate, 10% of polyethylene glycol (600) diacrylate, 10% of o-phenylphenethoxyethyl acrylate, 2% of 2-phenoxyethyl acrylate, 3% of 1-hydroxycyclohexyl phenyl ketone, and 1% of (2,4,6-trimethylbenzoyl) diphenylphosphine oxide. The formulas of UV pre-coating layers with other refractive indices are inferred from the above table and are not described in detail here.
[0033] The protective layer 500 is Covestro Dispercoll U58 water-based polyurethane resin glue with a solid content of 50%, mixed with ethyl ester at a ratio of 1:1.2, and coated at a temperature of 110°C, a coating machine speed of 37 m / min, and a coating thickness of approximately 2-3 μm.
[0034] Among them, the bonding layer adopts UV-PSA glue (UV curing pressure sensitive adhesive) or Shanghai Guanbao 1860's polyurethane glue.
[0035]
[0036]
[0037] The thickness of the silver coating is 90nm or 120nm, the coating power is 6.7KW, and the machine speed is 80m / min. The thickness of the aluminum coating is 45nm, the coating power is 12.6KW, and the machine speed is 300m / min. The above embodiments 1 to 8 are tested:
[0038] Test equipment: LB-8601 brightness box, using the high brightness reflector of the above embodiments 1 to 8 with a size of 118x65mm and a known reflector as a standard value (the reflector is a reflector GF-80D3 that the applicant has commercially sold) to compare the brightness increase, wherein the test voltage of the test backlight module is 19V, the current is 0.04A, and the brightness increase = (brightness value - standard value) / standard value, as shown in the following table:
[0039] Description: The brightness value of the existing Guangzhi commercial film GF-80D3 is 8515 (standard value), and the brightness value of the patent applied for by our company (publication number CN111679508A) is 8863 (standard value). The above data show that the performance of the two conditions of 1.524 and 1.547 is better than that of CN111679508A, and is also higher than the current Guangzhi commercial film GF-80D3 by 5.73% and 5.38% (the thickness of the silver coating is 120nm). It can be seen from the above that this solution has greater superiority than the existing technology and further improves the reflective brightness of the reflective sheet.
[0040] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high brightness silver film, It is characterized in that include: First PET layer; A first pre-coating layer, disposed on the first PET layer; UV pre-coating layer, arranged in the first pre-coating layer; Silver coating, set on UV pre-coating; A protective layer, disposed on the silver-plated film; The thickness of the silver-plated layer is 90-120 nm, the UV pre-coating layer is an acrylic resin cured by UV light, the refractive index of the UV pre-coating layer is 1.483-1.562, and the thickness of the UV pre-coating layer is 1.5-2.5 μm; The first pre-coating layer is mainly composed of water-based acrylic resin, and its formula includes the following components by mass: 15% propylene glycol methyl ether, 5% butyl acrylate, 8% butyl methacrylate, 25% methyl methacrylate, 10% methacrylic acid ~ 5% styrene, 2% initiator Tx21S, 2% dimethylethanolamine, and the rest is 28% ethanol; The UV light-cured acrylic resin comprises the following components in parts by weight: 0-21% of tripropylene glycol diacrylate, 0-26% of tetrahydrofuran acrylate, 10%-27% of ethoxylated (10) bisphenol A diacrylate, 0-10% of polyethylene glycol (600) diacrylate, 10%-52% of o-phenylphenethoxyethyl acrylate, 2%-26% of 2-phenoxyethyl acrylate, 3% of 1-hydroxycyclohexyl phenyl ketone, and 1% of (2,4,6-trimethylbenzoyl) diphenyl phosphine oxide.
2. The high brightness silver film according to claim 1, characterized in that: The thickness of the silver-plated layer is 90 nm, the thickness of the UV pre-coating layer is 2.5 μm, and the refractive index of the UV pre-coating layer is 1.
524.
3. The high brightness silver film according to claim 1, characterized in that: The thickness of the silver-plated layer is 120 nm, the thickness of the UV pre-coating layer is 1.5 μm, and the refractive index of the UV pre-coating layer is 1.483 or 1.
524.
4. The high brightness silver film according to claim 1, characterized in that: The thickness of the silver-plated layer is 120 nm, the thickness of the UV pre-coating layer is 2.5 μm, and the refractive index of the UV pre-coating layer is 1.524 or 1.
547.
5. A high brightness reflective sheet, characterized in that: It comprises the high-brightness silver film according to any one of claims 1 to 4, wherein the protective layer surface of the high-brightness silver film is bonded with an aluminum-plated film via a bonding layer, the aluminum-plated film comprises a second PET layer and an aluminum-plated layer arranged on the second PET layer, and the aluminum-plated layer is arranged between the bonding layer and the second PET layer.
6. The high brightness reflector according to claim 5, characterized in that: The laminating layer is UV-PSA or polyurethane glue.
7. The high brightness reflector according to claim 6, characterized in that: The thickness of the first PET layer is 25 μm, and the thickness of the second PET layer is 50 μm.
8. The high brightness reflector according to claim 7, characterized in that: The thickness of the aluminum plating layer is 45 nm.
9. A backlight film assembly, comprising a back plate, a light source, a light guide plate, and a high-brightness reflective sheet arranged in sequence, wherein the high-brightness reflective sheet is the high-brightness reflective sheet according to any one of claims 5 to 8.
Citation Information
Patent Citations
High-luminance reflector plate and backlight module
CN111679508A
Reflector plate and backlight module
CN112015005A
Light reflecting film and backlight unit for liquid crystal display device
CN107783209A
Polarizer, display screen and display module
CN213544871U
High-brightness silver film with enhanced brightness
CN216083162U