Polymer particles

By using hydrophilic oligomeric seed particles to prepare cross-linked hydrogel polymer particles in water-in-oil emulsions, the problems of high coefficient of variation and large polydispersity of monodisperse polymer particles are solved, achieving low coefficient of variation and suitable Polymer particles with high levels of cross-linking suitable for bioanalysis.

CN113637116BActive Publication Date: 2024-10-01LIFE TECH AS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110947391.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2015-07-20
Filing Date
2016-07-19
Publication Date
2024-10-01
Estimated Expiration
2036-07-19

AI Technical Summary

Technical Problem

Existing technologies have problems with high coefficient of variation and large polydispersity when preparing monodisperse polymer particles, and it is difficult to control porosity and size, which affects non-specific absorption and cross-linking levels for biological applications.

Method used

Cross-linked hydrogel polymer particles are prepared by emulsion polymerization using seed particles containing hydrophilic oligomers, using N,N-dimethylacrylamide, a stabilizer, a free radical initiator and a chain transfer agent to form a reaction mixture, Monodisperse seed particles are formed through thermal activation and are swollen and polymerized in a water-in-oil emulsion with controlled cross-linking levels to achieve low coefficient of variation and polydispersity.

Benefits of technology

Monodisperse polymer particles that achieve low coefficient of variation and polydispersity of less than 20% have suitable porosity and cross-linking levels and are suitable for bioanalysis and nucleic acid amplification, oligonucleotide sequencing and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113637116B_ABST
    Figure CN113637116B_ABST
Patent Text Reader

Abstract

The present invention relates to polymer particles. The present invention relates to monodisperse crosslinked hydrogel polymer particles, which include a polymer formed from (a) a hydrophilic vinyl monomer; and (b) a crosslinker including at least two vinyl groups. The present invention also relates to monodisperse seed particles having a Z-average diameter of 100 nm to 1500 nm, which include a plurality of non-crosslinked oligomers of poly-N,N-dimethylacrylamide. Methods of forming monodisperse crosslinked hydrogel polymer particles and monodisperse seed particles are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with application number 201680054042.0, application date July 19, 2016, priority date July 20, 2015, and invention name “Polymer Particles”.

[0002] The present invention relates to monodisperse polymer particles useful in bioanalysis and other applications, and seed particles for use in methods of preparing monodisperse polymer particles. The present invention also relates to methods for preparing such particles, as well as intermediates used in such methods and methods of using the particles, and other topics. Background Art

[0003] Emulsion polymerization can be used to form relatively monodisperse polymer particles of 50-1,000 nm. However, the formation of monodisperse polymer particles has a number of important limitations. First, all particles must be formed as part of the same batch and within a short time span relative to the polymerization time. Second, the growth conditions need to be controlled to ensure that the growth of the polymer particles is the same in all particles. Third, because the process requires monomer to be transferred from large storage droplets and swell into growing particles, the particles are either not cross-linked or have very low levels of cross-linking, because higher levels of cross-linking will prevent the particles from swelling.

[0004] Precipitation or dispersion polymerization can be used to produce larger particles of 0.5-10 microns. Precipitation polymerization is carried out in a solvent (e.g., alcohol) that dissolves the monomers but not the polymer. Monodispersity can be achieved when the polymer precipitates out of solution and particle formation occurs within a short time span. A relatively large amount of steric stabilizer is required to stabilize the particles after precipitation. The amount and type of stabilizer can change the size of the particles, and porous particles can be obtained by using high levels of cross-linking agents. However, the conditions in precipitation polymerization are difficult to control, for example, it is very difficult to control porosity, which is a result of how the pore structure is formed when the polymer precipitates out of solution. The difficulty of precipitation polymerization means that it is almost impossible to prepare porous particles with the same monomer composition and porosity in practice, and their size variation is very limited.

[0005] One way to solve some of these problems is to prepare cross-linked porous or solid monodisperse polymer particles by a two-stage method, which is called the Ugelstad method, named after the late Professor John Ugelstad, and is recorded in, for example, EP-B-3905 and US-A-4530956. An improved Ugelstad method is recorded in WO 00 / 61647. In the Ugelstad method, seed particles prepared by emulsion polymerization are converted into monodisperse particles in two steps by seed suspension polymerization. In the first step, the seed particles are swollen by preparing a fine (e.g., submicron) aqueous emulsion of a relatively low molecular weight water-insoluble substance and then adding an organic solvent (e.g., acetone) miscible with water to diffuse the water-insoluble substance into the seed particles. Conveniently, the water-insoluble substance is a heat-activated polymerization initiator. In the second step, the solvent is removed, the water-insoluble substance is locked in the seed particles, and the seed particles absorb a large amount of monomers and crosslinking agents. After initiation of polymerization, for example by activating the initiator by heating, larger polymer particles are produced. Thus, the Ugelstad process comprises the preparation of seed particles by emulsion polymerization and the expansion of the seed particles by suspension polymerization. The smallest monodisperse particles described in the aforementioned prior art have an average diameter of 1 μm.

[0006] In a simplified version of the Ugelstad process, the enhanced swelling capacity can be achieved simply by using oligomeric seed particles, for example where the oligomer weight average molecular weight corresponds to up to 50 monomer units (in the case of polystyrene a molecular weight of about 5000). This is described in US 4530956. In another version of the Ugelstad process described in WO2010 / 125170, oligomeric seed particles can be used to produce monodisperse particles with an average diameter in the submicron range.

[0007] The particles made by the Ugelstad method as described above and its variants are made from hydrophobic monomers such as styrene, which are usually used in oils (discontinuous phase) in aqueous (continuous phase) systems. Therefore, the resulting polymer particles are hydrophobic. When used for biological applications, hydrophobic particles suffer from the problem of non-specific absorption. This means that the hydrophobic polymer particles are usually surface modified to increase the hydrophilicity of the surface before being used for biological applications.

[0008] US 2014 / 0073715 describes a method for preparing monodisperse hydrophilic particles. The method uses monomers to which hydrophobic protective groups are added to the monomers that are polymerized to form the particles, and then the protective groups are removed. This method provides good results. However, the addition and removal of protective groups increases the complexity of the method and may limit the number of different types of monomers that can be used in the method.

[0009] It is apparent that known monodisperse polymer particles and methods of making such particles suffer from a number of limitations.Therefore, new monodisperse polymer particles and new methods of making them are needed.

[0010] It is an object of the present invention to provide monodisperse polymer particles having a low coefficient of variation (CV) and / or a low % polydispersity and a method for preparing monodisperse polymer particles. It is also an object of the present invention to provide seed particles suitable for making such monodisperse particles. Summary of the invention

[0011] The present invention is based, in part, on the recognition that seed particles comprising hydrophilic oligomers can be used in a new method for forming crosslinked monodisperse polymer particles.

[0012] According to a first aspect of the present invention, there are provided monodisperse cross-linked hydrogel polymer particles comprising a polymer formed from: (a) log P oct / wat a hydrophilic vinyl monomer having a (log P) of less than about 1; and (b) a cross-linking agent comprising at least two vinyl groups.

[0013] A second aspect of the present invention provides monodisperse seed particles having a Z-average diameter of 100 nm to 1500 nm, wherein each seed particle comprises a plurality of non-crosslinked oligomers of poly-N,N-dimethylacrylamide.

[0014] The third aspect of the present invention provides a method for forming monodisperse seed particles. The method comprises dissolving N,N-dimethylacrylamide, a stabilizer, a free radical initiator and a chain transfer agent in an organic solvent to form a reaction mixture; and heating the reaction mixture to activate the initiator; thereby forming monodisperse seed particles.

[0015] A fourth aspect includes the use of the seed particles of the present invention for forming monodisperse crosslinked hydrogel polymer particles. The monodisperse crosslinked hydrogel polymer particles may be crosslinked polyacrylamide particles. The seed particles may be the seed particles of the second aspect. The seed particles may be the seed particles obtainable or obtained by the method of the third aspect.

[0016] The fifth aspect provides a method for forming monodisperse cross-linked hydrogel polymer particles. The method includes forming a solution (a) of at least 2 weight percent of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution also comprising a cross-linking agent containing at least two vinyl groups; forming a solution (b) of a stabilizer in an organic solvent, wherein the organic solvent is immiscible with water, and wherein at least one of the solutions (a) and (b) comprises a free radical initiator; mixing solutions (a) and (b) to form an oil-in-water emulsion (c) and adding monodisperse seed particles to the emulsion; causing the monodisperse seed particles to form swollen particles in the emulsion; and polymerizing the swollen particles to form monodisperse cross-linked hydrogel polymer particles. The seed particles may be the seed particles of the second aspect. The seed particles may be seed particles obtainable or obtained by the method of the third aspect.

[0017] A sixth aspect provides a method for forming monodisperse cross-linked hydrogel polymer particles. The method comprises forming a solution (a) of at least 2 wt% of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution also comprising a chain transfer agent; forming a solution (b) of a stabilizer in an organic solvent, wherein the organic solvent is immiscible with water and wherein at least one of the solutions (a) and (b) comprises a free radical initiator; mixing solutions (a) and (b) to form an oil-in-water emulsion (c) and adding monodisperse seed particles to the emulsion; allowing the monodisperse seed particles to form swollen particles in the emulsion; polymerizing the swollen particles to form monodisperse polymer particles; forming in an organic solvent; A solution (d) of a stabilizer, wherein the organic solvent is immiscible with water; forming a solution (e) of at least 2 wt % of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution further comprising a crosslinker containing at least two vinyl groups, wherein at least one of the solution (d) and the solution (e) comprises a free radical initiator; mixing the solutions (d) and (e) to form a water-in-oil emulsion (f) and adding monodisperse polymer particles to the emulsion; causing the monodisperse polymer particles to form swollen polymer particles in the emulsion; and polymerizing the swollen polymer particles to form monodisperse crosslinked hydrogel polymer particles. The seed particles may be the seed particles of the second aspect. The seed particles may be seed particles obtainable or obtained by the method of the third aspect.

[0018] The seventh aspect comprises monodisperse cross-linked hydrogel polymer particles obtainable by the method of the fifth or sixth aspect. The monodisperse cross-linked hydrogel polymer particles may be obtained by the method of the fifth or sixth aspect.

[0019] An eighth aspect includes the use of monodisperse cross-linked hydrogel polymer particles in nucleic acid amplification and / or oligonucleotide sequencing. The nucleic acid amplification can be polymerase chain reaction (PCR) amplification or emulsion PCR amplification. The oligonucleotide sequencing can be based on chemical field effect transistor (chemFET) sequencing. The oligonucleotide sequencing can be based on ion sensitive field effect transistor (ISFET) sequencing.

[0020] A ninth aspect provides a method for nucleic acid amplification, which comprises performing a primer extension reaction on a polynucleotide (polynucleotide) hybridized to an oligonucleotide attached to a polymer particle of the present invention.

[0021] One embodiment of the present invention provides particles obtained by the method described in this specification.

[0022] One embodiment of the present invention provides particles having the characteristics of particles obtained by the method disclosed herein; although such particles can be obtained by the method described herein, they are characterized only by their properties and not by their manufacturing method. Therefore, the scope of protection of claims related to particles defined by their characteristics is determined only by the characteristics of the particles and not their actual manufacturing method.

[0023] The products, methods and uses of the present invention are not limited to the subject matter just mentioned, but are more fully described without limitation in the following description and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Embodiments of the present invention are further described below with reference to the accompanying drawings, in which:

[0025] Figure 1 is a schematic diagram of the single-stage swollen particle formation method of the present invention, including a representation of exemplary monomers.

[0026] Figure 2 is a schematic diagram of the single-stage particle formation method of the present invention.

[0027] Figure 3 is a schematic diagram of the two-stage swollen particle formation process of the present invention, including illustrations of exemplary monomers and chain transfer agents.

[0028] Figure 4 is a schematic diagram of the two-stage swollen particle formation method of the present invention.

[0029] Figure 5 The use of the particles of the invention in nucleotide sequencing and / or detection is described. DETAILED DESCRIPTION

[0030] Throughout the description and claims of this specification, the words "comprise" and "contain" and variations thereof mean "including but not limited to", and are not intended to (and do not) exclude other parts, additives, components, integers or steps. Throughout the description and claims of this specification, the singular encompasses the plural, unless the context requires otherwise. In particular, where the indefinite article is used, the recitation should be understood as contemplating both the plural and the singular, unless the context requires otherwise.

[0031] Features, integers, characteristics, compounds, chemical fragments or groups described in conjunction with a particular aspect, embodiment or example of the invention should be understood to be applicable to any other aspect, embodiment or example described herein unless incompatible therewith. All features disclosed in this specification (including any accompanying claims, abstract and drawings) and / or all steps of any method or process so disclosed may be combined in any combination, except where at least some of these features and / or steps are mutually exclusive. The present invention is not limited to the details of any embodiment disclosed herein. The present invention extends to any new feature or any new combination of the features disclosed in this specification (including any accompanying claims, abstract and drawings), or any new step or any new combination of the steps of any method or process so disclosed.

[0032] The reader's attention should be directed to all articles and documents related to the present application which are filed concurrently with or before the present specification and which are open to public inspection together with the present specification, and the contents of all these articles and documents are incorporated herein by reference.

[0033] All publications, patent applications, patents, and other references mentioned herein are incorporated by reference in their entirety. In the event of a conflict, the present specification, including definitions, will control.

[0034] In one embodiment, the present invention provides novel polymer particles, while another embodiment provides a method by which the novel particles can be prepared. One embodiment provides novel seed particles for use in the method of forming the polymer particles, and other embodiments provide methods of using the polymer particles obtainable by the method.

[0035] The polymer particle formation process involves a water-in-oil emulsion, ie, a discontinuous aqueous phase suspended in a continuous oil phase.

[0036] Thus, the polymer particle formation method described herein involves two different particles, namely Seed particles , which undergoes swelling and polymerization processes to form Polymer particles The terms "seed particles" and "polymer particles" are therefore used herein as follows:

[0037] Unless the context requires otherwise, "seed particles" mean particles obtainable by dispersion polymerisation and used as intermediates in the polymer particle formation process.

[0038] "Polymer particles" refers to particles that can be prepared from seed particles by suspension polymerization as described herein.

[0039] Reference to a "hydrogel" with respect to a polymer (e.g., a polymer particle) means a polymer gel in which the swelling agent is water. The hydrogel polymer can absorb at least 20% of its weight in water. The hydrogel polymer can absorb at least 45%, at least 65%, at least 85%, at least 100%, or at least 300% of its weight in water. For example, the hydrogel polymer can absorb at least 1000%, at least 1500%, or even at least 2000% of its weight in water.

[0040] Reference to "transparent" with respect to polymer particles (e.g., hydrogel polymer particles) means that the particles are porous and molecules of interest or other agents can easily diffuse through aqueous solutions in the pores of the particles. For example, the crosslinked hydrogel polymer particles of the present disclosure can be permeable to oligonucleotides and nucleic acid amplification and sequencing reagents, e.g., even when a polymerase is attached to the oligonucleotide, the oligonucleotide can be partially or completely located within the pores.

[0041] Unless otherwise indicated, the "average" diameter referred to in this specification refers to the mode diameter of the crosslinked polymer particles (e.g., crosslinked hydrogel polymer particles) or to the z-average diameter of the seed particles. The mode diameter can be measured by a disc centrifuge, such as a CPS disc centrifuge. The z-average diameter can be the z-average diameter measured by dynamic light scattering (also known as photon correlation spectroscopy). Further disclosed throughout are embodiments in which the average diameter is the mode diameter, such as the mode diameter determined by optical microscopy.

[0042] The term "monodisperse" means that for a plurality of particles (e.g., at least 100, more preferably at least 1000), the coefficient of variation (CV) or % polydispersity of the diameter of the particles is less than 20%, such as less than 15%, typically less than 10%, and optionally less than 8%, such as less than 5%.

[0043] The term "Mw" is the weight average molecular weight of a polymer. It is defined by the formula:

[0044]

[0045] Among them, M i is the molecular weight of a particular chain, and N iThe Mw of a polymer is the number of chains of that molecular weight. Mw can be measured using gel permeation chromatography (GPC) relative to a set of standard polymers with a specific eluent solvent system. For example, the Mw of an oligomer or polymer in a seed particle can be measured by GPC relative to a polystyrene standard using DMF with 0.01M LiBr as an eluent.

[0046] "Polydispersity" or "% polydispersity" referred to in this specification refers to the value of dynamic light scattering data derived from the "polydispersity index". The polydispersity index is a numerical value calculated by a simple 2-parameter fit to the relevant data (e.g., dynamic light scattering data), as defined in ISO standard documents 13321:1996E and ISO 22412:2008. The polydispersity index is dimensionless and is converted so that values ​​less than 0.05 are rarely seen except when using highly monodisperse standards. A polydispersity index value of the sample particles greater than 0.7 indicates that the sample has a very wide size distribution, e.g., the particles are not monodisperse.

[0047] As used herein, the terms "alkyl" and "C x -C y "Alkyl" (wherein x is at least 1 and less than 10, and y is a number greater than 10) includes straight or branched chain alkyl moieties having, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms. The term includes, for example, methyl, ethyl, propyl (n-propyl or isopropyl), butyl (n-butyl, sec-butyl or tert-butyl), pentyl, hexyl, and the like. In particular, alkyl may be "C 1 -C 6 "alkyl", i.e., an alkyl group having 1, 2, 3, 4, 5 or 6 carbon atoms; or "C 1 -C 4 The term "lower alkyl" includes alkyl groups having 1, 2, 3 or 4 carbon atoms. Where chemically possible, the alkyl group may be optionally substituted by 1 to 5 substituents independently selected in each case from the following: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)Ra 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 alkyl.

[0048] As used herein, the term "log P" refers to the octanol-water partition coefficient (log P) of a compound (e.g., a hydrophilic vinyl monomer). oct / wat ). The log P of a compound can be determined by any of a variety of methods. Specifically, for compounds used in the embodiments and other compounds disclosed herein, log P can be measured by the shake flask method, which is described in J. Sangster, "Octanol-water partition coefficients of simple organic compounds", J. Phys. Chem. Ref. Data, Vol. 18, No. 3, 1989, 1111-1227 (the entire text of which is incorporated herein by reference), Section 2.1, p. 1116. Log P can also be calculated from the structure of the compound using software, for example, log P can be calculated using software from CambridgeSoft Corp. Ultra 14.0 is used for calculation.

[0049] Polymer particles

[0050] The invention includes embodiments wherein the particles are polymeric and monodisperse. The invention includes embodiments wherein the particles are porous.

[0051] The population number of particles may be at least 100, such as at least 1000. For example, for measurement purposes, the population number of particles may be at least 100, such as at least 1000. For example, in some end-use applications, the population number of particles may conveniently be at least 100, such as at least 1000.

[0052] "Monodisperse" means that for a plurality of particles (e.g., at least 100, more preferably at least 1000), the coefficient of variation (CV) of the diameter of the particles is less than 20%, such as less than 15%, typically less than 10%, and optionally less than 8%, such as less than 5%. A particular class of polymer particles has a CV of less than 10%. CV is defined as 100 times (standard deviation) divided by the mean, where the "mean" is the average particle size and the standard deviation is the standard deviation of the particle size. The present invention also includes embodiments in which the "mean" is the z-average particle size or the mode particle size. The CV is preferably calculated based on the main mode. Therefore, some particles below or above the mode size can be discounted in the calculation, which can be, for example, based on about 90% of the total number of particles (i.e., detectable particles). This CV determination can be performed on a CPS disc centrifuge.

[0053] The polymer particles can be prepared by the polymer particle formation methods described later in the specification, for example, by using monodisperse seed particles as described herein.

[0054] Returning now to the polymer particles, this specification discloses crosslinked hydrogel polymer particles. The crosslinked hydrogel polymer particles are characterized in that when placed in an aqueous solution that is a good solvent for the polymer, the particles swell without dissolving. For example, water is a good solvent for hydrogel particles comprising acrylamide polymers. The hydrogel particles are hydrophilic and swell in water, and can be made with a variety of different porosities. The crosslinked hydrogel particles disclosed herein provide a combination of low nonspecific binding, monodispersity, and porosity, which provides many advantages when the particles are used for biological analysis.

[0055] The crosslinking level in the polymer particles prepared by the method can be expressed as the weight percentage (wt%) of the crosslinker monomer contained in the total monomers used for suspension polymerization. The weight % of the crosslinker monomer can be equal to the weight % of the crosslinker in the matrix polymer (i.e., the weight % of the crosslinker in the dry weight of the crosslinked polymer particles). Therefore, in the case where the monomers used for suspension polymerization are, for example, monofunctional acrylamide and difunctional acrylamide, the percentage of difunctional acrylamide (crosslinker monomer) is calculated as a weight percentage based on the total weight of difunctional acrylamide plus monofunctional acrylamide. Typical crosslinking levels include>1 wt% crosslinker, such as>2 wt% crosslinker, such as>5 wt% crosslinker. For example, the crosslinking level can be>10 wt% crosslinker, or>15 wt% crosslinker, such as>20 wt% crosslinker or>25 wt% crosslinker. The crosslinking level can also be, for example, 5-60 wt% crosslinker, such as 10-50 wt% crosslinker, such as 20-40 wt% crosslinker or 20-30 wt% crosslinker. The cross-linking level can also be 1-30 wt % cross-linking agent, such as 1-20 wt % cross-linking agent, such as 1-10 wt % cross-linking agent; or the cross-linking level can also be 2-30 wt % cross-linking agent, such as 2-20 wt % cross-linking agent, such as 2-10 wt % cross-linking agent: the cross-linking level is suitable for porous hydrogel particles, for example.

[0056] The degree of crosslinking may be >30 wt% crosslinker or >40 wt% crosslinker, for example in highly crosslinked particles. The crosslinking level may be 10-90 wt% crosslinker, 20-80 wt% crosslinker or 25-75 wt% crosslinker, for example 25-60 wt% crosslinker or 30-50 wt% crosslinker. In highly crosslinked particles, the crosslinking level may be up to 100 wt% crosslinker, for example a hydrophilic vinyl monomer may be the crosslinker.

[0057] As described above, when placed in a good solvent for the polymer, the cross-linked particles swell. The amount of swelling (e.g., measured as an increase in diameter) is related to the level of cross-linking. Particles with a higher degree of cross-linking generally swell less than particles made from similar but less cross-linked polymers. This property can be used to determine the relative level of cross-linking in a sample of polymer particles by comparing the sample of polymer particles to a series of standards known to have different levels of cross-linking.

[0058] The particles suitably comprise an addition polymer prepared by polymerising one or more ethylenically unsaturated monomers. The ethylenically unsaturated monomers may comprise a broadly vinyl group, -CR=CH 2 , where R is H or alkyl (e.g., where R is -CH 3 or -CH 2 CH 3The ethylenically unsaturated monomer may contain a vinyl group, -CH=CH 2 The monomer may be a hydrophilic vinyl monomer, for example a vinyl monomer having a log P value of less than about 1, for example a log P value of less than about 0.5. The hydrophilic vinyl monomer may include a broadly defined vinyl group, -CR=CH 2 , where R is H or alkyl (e.g., where R is -CH 3 or -CH 2 CH 3 The hydrophilic vinyl monomer may contain a vinyl group, -CH=CH 2 . The monomer may be a vinyl monomer having a log P of less than about 0.6. The monomer may be a vinyl monomer having a log P of less than about 0.5. For example, the monomer may be a vinyl monomer having a log P of less than about 0.3 or less than about 0.2, for example, the monomer may be a vinyl monomer having a log P of less than about 0.1. The monomer may be a vinyl monomer having a log P of less than about 0, for example, a vinyl monomer having a log P of less than about -0.2. The monomer may be a vinyl monomer having a log P of 0.5 to -2, for example, a vinyl monomer having a log P of 0 to -2, for example, a vinyl monomer having a log P of -0.2 to -2. In particular, the monomer may be a vinyl monomer further comprising a hydrophilic group, for example, an acrylamide monomer or an acrylate monomer.

[0059] The monomer used for the particles may be at least one compound of formula (I):

[0060]

[0061] in:

[0062] R 1 -H, -CH 3 or -CH 2 CH 3 ;

[0063] R 2 For-OR 3 or -N(R 4 )R 5 ;

[0064] R 3 -H, -C 1 -C 6 Alkyl or -C 1 -C 6 Alcohol; and

[0065] R 4 and R 5 are independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C6 Haloalkyl, -C 1 -C 6 alcohol.

[0066] When R 3 For -C 1 -C 6 Alkyl or -C 1 -C 6 In the case of alcohol, the alkyl group or alcohol may be substituted, where chemically possible, by 1 to 5 (e.g. 1, 2, 3 or 4) substituents, each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 For example, when R 3 For -C 1 -C 6 Alkyl or -C 1 -C 6 In the case of alcohol, where chemically possible, the alkyl group or alcohol may be selected from 1 to 5 (e.g. 1, 2, 3 or 4) groups, each independently selected from ORa or CO 2 R a substituted by a substituent, optionally wherein R a For H.

[0067] When R 4 and / or R 5 For -C 1 -C 6 Alkyl, -C 1 -C 6 Haloalkyl, -C 1 -C 6 alcohol, each of which may be independently substituted, where chemically possible, by 1 to 5 (e.g. 1, 2, 3 or 4) substituents, each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 For example, when R 4 and / or R 5 For -C 1 -C6 Alkyl, -C 1 -C 6 Haloalkyl, -C 1 -C 6 alcohol, each of which may be independently replaced, where chemically possible, by 1 to 5 (e.g. 1, 2, 3 or 4) selected in each case independently from OR a or CO 2 R a substituted by a substituent, optionally wherein R a For H.

[0068] R 1 Can be -H or -CH 3 For example, R 1 Can be -H.

[0069] R 2 Can be -OR 3 . R 2 Can be -N(R 4 )R 5 .

[0070] R 3 Can be -H. R 3 Can be -C 1 -C 6 Alkyl. For example, R 3 Can be -C 1 -C 6 alkyl, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where Ra For -H.R 3 Can be -C 1 -C 6 Alcohol. For example, R 3 Can be -C 1 -C 6 alcohol, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where R a is -H.

[0071] R 4 Can be -H or -C 1 -C 6 Alkyl. 4 Can be -C 1 -C 6 Alkyl. For example, R 4 Can be -C 1 -C 6 alkyl, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONRa R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where R a is -H.

[0072] R 5 Can be -H or -C 1 -C 6 Alkyl. 5 Can be -C 1 -C 6 Alkyl. For example, R 5 Can be -C 1 -C 6 alkyl, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where R a is -H.

[0073] For example, the log P value of the compound of formula (I) may be less than about 1, such as a log P of less than about 0.5. The log P of the compound of formula (I) may be less than about 0.6. The log P of the compound of formula (I) may be less than about 0.5. For example, the log P of the compound of formula (I) may be less than about 0.3 or less than about 0.2, such as a log P of the compound of formula (I) may be less than about 0.1. The log P of the compound of formula (I) may be less than about 0, such as a log P of less than about -0.2. The log P of the compound of formula (I) may be from 0.5 to -2, such as a log P of 0 to -2, such as a log P of -0.2 to -2.

[0074] The monomer may contain at least one primary amide group (-C(O)NH 2 )'s hydrophilic vinyl monomer.

[0075] In particular, acrylamide monomers and / or acrylate monomers may be mentioned. Suitable monomers include acrylamide (prop-2-enamide), N-(hydroxymethyl)acrylamide, N-hydroxyethylacrylamide, N-[tris(hydroxymethyl)methyl]acrylamide, 3-acrylamidopropionic acid, methacrylamide, N-(2-hydroxyethyl)methacrylamide, N-(3-aminopropyl)methacrylamide, hydroxypropylacrylamide, N,N-dimethylacrylamide, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, acrylic acid; and other acrylamide monomers, acrylic acid monomers, methacrylamide monomers or methacrylic acid monomers having a log P value of less than about 1 (e.g., a log P value of less than about 0.5).

[0076] The monomer may comprise a mixture of monomers. For example, the monomer may comprise at least one monomer as defined above and at least one compatible functional monomer. The corresponding functional monomer is a hydrophilic vinyl monomer as defined herein, comprising a carboxylic acid (—COOH), a primary amine or a secondary amine.

[0077] In highly crosslinked particles, the monomer may be or include a crosslinker, for example as defined elsewhere herein.For example, the monomer may be or include at least one compound of formula (IIa) or (IIb).

[0078] Functional monomers can be vinyl monomers having a log P value less than about 1, such as vinyl monomers having a log P value less than about 0.5, which contain carboxylic acid or primary amines. Functional monomers can be vinyl monomers having a log P value less than about 0.6. Functional monomers can be vinyl monomers having a log P value less than about 0.5. For example, functional monomers can be vinyl monomers having a log P value less than about 0.3 or less than about 0.2, such as functional monomers can be vinyl monomers having a log P value less than about 0.1. Functional monomers can be vinyl monomers having a log P value less than about 0, such as vinyl monomers having a log P value less than about -0.2. Functional monomers can be vinyl monomers having a log P value of 0.5 to -2, such as vinyl monomers having a log P value of 0 to -2, such as vinyl monomers having a log P value of -0.2 to -2. Functional monomers can be compounds of formula (I) containing carboxylic acid or primary amines. Functional monomers can be acrylamide monomers containing carboxylic acid or primary amines. Suitable functional monomers include 3-acrylamidopropionic acid, 4-acrylamidobutyric acid, 5-acrylamidovaleric acid, N-(3-aminopropyl)methacrylamide and acrylic acid.

[0079] In the presence of at least one functional monomer, the amount of the functional monomer can be from about 0.1 to about 100 mol%, such as from about 0.2 to about 50 mol%, such as from about 0.5 to about 40 mol% or from about 1 to about 30 mol% (e.g., from about 2 to about 20 mol%). The amount of the functional monomer can be from about 0.1 to about 10 weight%, such as from about 0.2 to about 5 weight%, such as from about 0.5 to about 2 weight%. The weight % can refer to the weight percentage of the functional monomer contained in the total monomers used in the polymerization process. The total monomers can, for example, include hydrophilic vinyl monomers, crosslinking agents and functional monomers that are not the at least one functional monomer.

[0080] Crosslinking can be achieved by introducing a polyvinyl group comprising at least two (e.g., two) vinyl groups (—CH═CH 2 ) as a crosslinking agent for the comonomer. The crosslinking agent may be at least one compound of formula (IIa) or (IIb):

[0081]

[0082] Where R 6 Selected from -C 1 -C 6 Alkyl-, -C 1 -C 6 Heteroalkyl, -C 1 -C 6 Cycloalkyl-, -C 1 -C 6 Hydroxyalkyl-, -C 1 -C 6 Ether-, containing 2 to 100 C2 -C 3 Polyethers of ether units;

[0083] R 7 and R 8 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Heteroalkyl, -C 3 -C 6 Cycloalkyl, -C 1 -C 6 Hydroxyalkyl or -C 1 -C 6 ether;

[0084] R 9 -N(R 11 )C(O)CH=CH 2 ;

[0085] R 10 Selected from -H and -N(R 12 )C(O)CH=CH 2 ;as well as

[0086] R 11 and R 12 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Heteroalkyl, -C 3 -C 6 Cycloalkyl, -C 1 -C 6 Hydroxyalkyl or -C 1 -C 6 ether.

[0087] The cross-linking agent may be at least one compound of formula (IIa). The cross-linking agent may be at least one compound of formula (IIb).

[0088] Where chemically possible, R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be independently substituted by 1 to 5 substituents each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR aS(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a In each case, independently selected from: H, C 1 -C 4 Alkyl and C 1 -C 4 Alkenyl.

[0089] R 6 Selected from -C 1 -C 6 Alkyl-, -C 1 -C 6 Heteroalkyl-, -C 1 -C 6 Cycloalkyl-, -C 1 -C 6 Hydroxyalkyl- and -C 1 -C 6 Ether-. R 6 Can be selected from -C 1 -C 6 Alkyl- and -C 1 -C 6 Hydroxyalkyl-. 6 Can be -C 1 -C 6 Alkyl-, such as -CH 2 -、-(CH 2 ) 2-、-(CH 2 ) 3 -or-(CH 2 ) 4 -, for example -(CH 2 ) 2 -. R 6 Can be -C 1 -C 6 Hydroxyalkyl-, such as -C(OH)H-, -(C(OH)H) 2 -、-(C(OH)H) 3 -or-(C(OH)H) 4 -, for example -(C(OH)H) 2 -.

[0090] R 6 Can be -C 1 -C 6 Heteroalkyl-, optionally wherein the heteroatom is an amine (eg, a tertiary amine). For example, C(O)R a Replaced-C 1 -C 6 Heteroalkyl, optionally wherein the heteroatom is an amine, such as R 6 Can be -CH 2 CH 2 N(C(O)CH=CH 2 )CH 2 CH 2 -.

[0091] When R 6 When it is a polyether, the polyether may be linear or branched. 6 It can contain 2 to 100 C 2 -C 3 Polyethers of ether units, for example containing 2 to 50 C 2 -C 3 Polyether of ether units. 6 It can contain 2 to 100 C 2 Polyethers of ether units, for example containing 2 to 50 C 2 For example, R 6 It can be -(CH 2 ) r (OCH 2 CH 2 ) n O(CH 2 ) s , wherein r and s are each independently 2 or 3 (e.g., 2); and n is an integer from 1 to 100 (e.g., 1 to 50 or 1 to 25; e.g., 5 to 50 or 5 to 25). Without wishing to be bound by any theory, it is believed that a crosslinking agent comprising a polyether (e.g., wherein R6 The crosslinking agent (e.g., polyether) has excellent solubility in the aqueous phase. This means that, while such crosslinking agents can be used to provide particles with low crosslinking levels (e.g., 1-20 wt. % crosslinking agent, or 1-10 wt. % crosslinking agent), such crosslinking agents comprising polyethers are particularly suitable for providing particles comprising relatively high crosslinking levels, such as >20 wt. % crosslinking agent, >25 wt. % crosslinking agent, or >30 wt. % crosslinking agent. For example, the crosslinking level may be 10-90 wt. % crosslinking agent, 20-80 wt. % crosslinking agent, or 25-75 wt. % crosslinking agent, such as 25-60 wt. % crosslinking agent, or 30-50 wt. % crosslinking agent.

[0092] R 7 and / or R 8 and / or R 11 and / or R 12 It can be H. For example, R 7 and / or R 8 It can be H. For example, R 11 and / or R 12 Can be H.

[0093] The log P value of the compound of formula (II) may be less than about 1, for example, a log P of less than about 0.5. The log P of the compound of formula (II) may be less than about 0.6. The log P of the compound of formula (II) may be less than about 0.5. For example, the log P of the compound of formula (II) may be less than about 0.3 or less than about 0.2, for example, the log P of the compound of formula (II) may be less than about 0.1. The log P of the compound of formula (II) may be less than about 0, for example, a log P of less than about -0.2. The log P of the compound of formula (II) may be from 0.5 to -2, for example, a log P of 0 to -2, for example, a log P of -0.2 to -2.

[0094] Exemplary crosslinking agents for use in the particles of the present invention include N,N'-(1,2-dihydroxyethylene)bisacrylamide, N,N'-methylenebis(acrylamide), N,N'-ethylenebis(acrylamide), piperazine diacrylamide, glycerol 1,3-diglycerolate diacrylate, N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl)) diacrylamide, polyethylene glycol diacrylamide (MW≤2000), 4-arm PEG-acrylamide (MW≤2000), N,N-bis(2-acrylamidoethyl)acrylamide. Exemplary crosslinking agents N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide, polyethylene glycol diacrylamide (MW≤2000) and 4-arm PEG-acrylamide (MW≤2000), (particularly N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide) are particularly suitable for highly crosslinked particles and mechanically more stable particles, such as particles with a crosslinking level of at least 20% by weight of the crosslinker (e.g., a crosslinking level of at least 30% by weight of the crosslinker). One embodiment of the present invention includes the use of a combination of crosslinkers. As specific monomers, mention may be made of acrylamide (prop-2-enamide), with N,N'-(1,2-dihydroxybisacrylamide) being a suitable crosslinker. As specific monomers, mention may be made of methylol acrylamide, of which N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide is a suitable crosslinking agent. As specific monomers, mention may be made of ethylol acrylamide, of which N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide is a suitable crosslinking agent.

[0095] The crosslinking agent may be a compound that does not contain a primary amine, a secondary amine, a hydroxyl group or a carboxylic acid. The crosslinking agent may be a compound of formula (IIa) or formula (IIb) that does not contain a primary amine, a secondary amine, a hydroxyl group or a carboxylic acid.

[0096] Table 1 lists a number of exemplary monomers and crosslinkers that can be used. Table 2 lists a number of other monomers. The log P values ​​of the monomers listed in Tables 1 and 2 were calculated using software from CambridgeSoft Corp. Ultra 14.0. In some particles of embodiments of the present invention, monomers of Table 2 are not used, for example, due to the log P values ​​of the monomers. In addition, the monomers methyl acrylate and methacrylic acid of Table 2 can be conventionally used in the Ugelstad process, so these monomers and other monomers with higher log P values ​​may be less preferred for use in the particles of the present invention, which can be prepared using the polymer particle formation methods described herein.

[0097] Table 1: Exemplary Monomers and Crosslinkers

[0098]

[0099]

[0100]

[0101]

[0102]

[0103]

[0104] The level of crosslinking in the crosslinked hydrogel polymer particles can be expressed as the weight percent (wt%) of the crosslinker monomer contained in the total monomers used for polymerization. Typical crosslinking levels include >1 wt% crosslinker, such as >2 wt% crosslinker, such as >5 wt% crosslinker. For example, the crosslinking level can be >10 wt% crosslinker, or >15 wt% crosslinker, such as >20 wt% crosslinker (e.g. >30 wt% crosslinker or >40 wt% crosslinker). The crosslinking level can also be 1-60 wt% crosslinker, such as 5-30 wt% crosslinker. For example, the crosslinking level can be 5-60 wt% crosslinker, such as 10-50 wt% crosslinker. The crosslinking level can also be, for example, 15-40 wt% crosslinker, such as 20-40 wt% crosslinker, such as 20-30 wt% crosslinker. The crosslinking level may be 10-90% by weight of the crosslinking agent, 20-80% by weight of the crosslinking agent or 25-75% by weight of the crosslinking agent, such as 25-60% by weight of the crosslinking agent or 30-50% by weight of the crosslinking agent; for example in highly crosslinked particles. The crosslinking level may also be 1-30% by weight of the crosslinking agent, such as 1-20% by weight of the crosslinking agent, such as 1-10% by weight of the crosslinking agent. The crosslinking level may also be 2-30% by weight of the crosslinking agent, such as 2-20% by weight of the crosslinking agent, such as 2-10% by weight of the crosslinking agent. In highly crosslinked particles, the crosslinking level may be up to 100% by weight of the crosslinking agent, for example a hydrophilic vinyl monomer may be the crosslinking agent.

[0105] In one embodiment, where the particles have a diameter of at least 1 μm, the average diameter of the particles may be at least 500 nm, such as at least 600 nm, optionally at least 800 nm.

[0106] In one embodiment, where the particles have a diameter of no more than 2 μm, the average diameter of the particles may be no more than 10 μm, such as no more than 5 μm, optionally no more than 3 μm.

[0107] In one embodiment, the present invention comprises a class of polymer particles having an average diameter of 0.5 μm to 10 μm, such as 0.8 μm to 5 μm.

[0108] The size and size distribution of the polymer particles can be determined as described below under the heading "Analytical Methods".

[0109] The present disclosure includes porous polymer particles having a porosity of at least 5%, such as at least 10%.The present disclosure includes porous particles having a porosity of 20% to 95%, particularly 30% to 90%, such as 40% to 90%, such as 50% to 80%.

[0110] Since the density of acrylamide and acrylate polymers is about 1.3 g / mL, and the density of water is about 1 g / mL, the porosity can be calculated after determining the density of the hydrogel polymer particles. The porous polymer particles can be permeable to solvated molecules, for example, the porous polymer particles can be permeable to oligonucleotides and nucleic acid amplification reagents and sequencing reagents (e.g., primers, nucleotides, and polymerase).

[0111] In one embodiment, the particle comprises a functional group. The functional group can be selected from a hydroxyl, a carboxylic acid (-COOH), a primary amine or a secondary amine. In one embodiment, the functional group is provided by a hydrophilic vinyl monomer (e.g., a compound of formula (I)) rather than a cross-linking agent (e.g., a compound of formula (IIa) or formula (IIb)). The functional group can be enhanced to promote binding to a target analyte (e.g., an oligonucleotide) or a target receptor. An exemplary method for enhancing the functional group of the particle of the present invention is described herein in the section related to "use of the particle".

[0112] In one embodiment, the particle comprises one or more oligonucleotides connected to the particle. The oligonucleotide can be connected to the particle by a linker. For example, each (or a portion of) particle can include multiple oligonucleotides connected to the particle. For each single particle, multiple oligonucleotides can be identical. For example, the first particle can include multiple oligonucleotides with a first sequence connected to the first particle, and the second particle can include multiple oligonucleotides with a second sequence connected to the second particle. In the embodiment where the particle of the present invention is porous, the oligonucleotide can be connected to the outer surface of the particle, or connected in a hole, or connected on the entire particle matrix. The hole can have enough sizes to make the particle permeable to oligonucleotides, related molecules and other reagents, so that the oligonucleotide can be partially or completely located in the hole, even when the polymerase is connected to the oligonucleotide.

[0113] The particles of the invention can be stable (i.e., resistant to polymer degradation) over a typical temperature range of aqueous solutions. The monodisperse crosslinked hydrogel polymer particles can be stable at temperatures up to about 100° C. For example, the monodisperse crosslinked hydrogel polymer particles can be stable over a temperature range of about 0° C. to about 100° C.

[0114] Seed particles

[0115] Polymer particles can be prepared by a polymer particle formation method starting from a specific seed particle. Applicants have determined that seed particles commonly used in other methods, such as polystyrene seed particles, are incompatible with the method of the present invention. Therefore, the present invention provides seed particles suitable for use in the polymer particle formation method of the present invention.

[0116] In one embodiment, the seed particles are monodisperse. The seed particles comprise a plurality of non-crosslinked oligomers of poly-N,N-dimethylacrylamide and have a z-average diameter of 100 nm to 1,500 nm. Each seed particle may comprise more than 1×10 5 (For example, more than 1×10 6 ) non-crosslinked oligomers of poly-N,N-dimethylacrylamide, for example, each seed particle may contain more than 5×10 6 A non-crosslinked oligomer of poly N,N-dimethylacrylamide.

[0117] The z-average diameter of the seed particles may be 150 nm to 1,300 nm. For example, the z-average diameter of the seed particles may be 300 nm to 1,100 nm.

[0118] The weight average molecular weight (Mw) of the oligomers is from about 2,000 Da to about 100,000 Da when measured by GPC relative to polystyrene standards. In addition to or in the alternative to the recited Mw ranges, the polymer of each oligomer may contain from about 30 to 2,000 (e.g., from about 60 to about 1,000 or from about 80 to about 500) monomer units.

[0119] The seed particle oligomer may have an Mw of less than 100,000 Da, optionally less than 50,000 Da, further optionally less than 40,000 Da, for example less than 30,000 Da. The Mw may be greater than 4,000 Da, optionally greater than 5,000 Da, further optionally greater than 6,000 Da, such as greater than 8,000 Da, for example greater than 10,000 Da. For example, the Mw may be 5,000 Da to 70,000 Da, such as 6,000 Da to 60,000 Da, such as 7,000 Da to 50,000 Da or 8,000 Da to 40,000 Da.

[0120] Without wishing to be bound by any theory, it is believed that the Mw of the oligomer of the seed particles is an important feature of the seed particles. For example, it may be necessary to have a seed particle oligomer Mw within the range to provide seed particles that form monodisperse polymer particles during the particle formation method described herein. If the seed particle polymer has a higher molecular weight, for example because a chain transfer agent is not used in the seed particle formation process (e.g., for monodisperse microspheres of M. Babic and D. Horak, Macromolecular Reaction Engineering, 2007, 1, 86-94), then the particles are not suitable for use in the method of the present invention, for example, because the particles produced by this method may not be monodisperse, for example, the CV may be greater than 20%.

[0121] The seed particles may have characteristics of seed particles formed according to the method for forming seed particles disclosed herein. For example, the seed particles may have characteristics of seed particles formed by free radical initiated polymerization of N,N-dimethylacrylamide in an organic solvent in the presence of a stabilizer and a chain transfer agent.

[0122] Preparation of seed pellets

[0123] Polymer particles can be prepared starting from specific seed particles by the methods described herein. The present invention thus provides a method for preparing monodisperse seed particles.

[0124] The monodisperse seed particles may be prepared by a method comprising dissolving N,N-dimethylacrylamide, a stabilizer, a free radical initiator, and a chain transfer agent in an organic solvent to form a reaction mixture; and heating the reaction mixture to activate the initiator, thereby forming the monodisperse seed particles.

[0125] In this process, once the reaction mixture is formed in a suitable container, the reaction mixture is typically mixed, for example with a stirrer during the heating step.

[0126] Preferably, the polymerization reaction occurs in a reaction mixture containing a minimum amount of oxygen. Therefore, the reaction mixture can be purged of oxygen before the reaction mixture is heated. The purging can include spraying with a chemically inert gas. The inert gas can be nitrogen or a rare gas (e.g., helium, neon, argon, krypton or xenon). For example, the inert gas can be argon, helium or nitrogen, such as argon or nitrogen.

[0127] The method can be considered as reverse precipitation polymerization, wherein the hydrophilic seed particles are precipitated from an organic solvent. Stabilizers can prevent the aggregation of seed particles and help to form monodisperse seed particles. The selection of suitable stabilizers depends on the ability of the stabilizer to dissolve in an organic solvent. Stabilizers can be block copolymers of styrene and polyolefins, such as triblock copolymers based on styrene and ethylene / butylene, such as linear triblock copolymers composed of styrene and ethylene / butylene. Stabilizers can be triblock copolymers composed of a poly(ethylene-to-butylene) midblock and a polystyrene outer block. Exemplary stabilizers include Kraton A1535H, Kraton G1650M, Kraton G1652M or Kraton G1657M, or a combination thereof.

[0128] The free radical initiator can be a peroxide initiator or an azo initiator, such as a peroxide initiator or an azo initiator that decomposes at an elevated temperature. Exemplary free radical initiators include 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dibenzoyl peroxide, and the like. The free radical initiator can be 2,2'-azobis(2-methylpropionitrile). The temperature to which the reaction mixture can be heated depends on the temperature at which the free radical initiator is activated. Heating the reaction mixture to activate the initiator can include heating the reaction mixture to a temperature of at least 40°C, such as heating to a temperature of at least 50°C, such as heating to a temperature of at least 60°C, or, for example, heating to a temperature of at least 70°C. For example, when the free radical initiator is 2,2'-azobis(2-methylpropionitrile), the reaction mixture can be heated to a temperature of at least 50°C or a temperature of at least 60°C.

[0129] By making chain termination with the free radical reaction of the growing polymer chain and transferring the lone electron to the free radical species derived from the chain transfer agent, the addition of the chain transfer agent reduces the molecular weight of the polymer of the seed particles. Then the free radical species derived from the chain transfer agent can react with the monomer and form free radicals by the monomer, and then it can react with another monomer and start to form a new polymer chain. The chain transfer agent can be a mercaptan or a haloalkane. For example, the chain transfer agent can be selected from mercaptan (for example 1-octyl mercaptan, hexanethiol, 6-mercapto-1-hexanol, benzyl mercaptan), alkyl mercaptan (for example 1-octyl mercaptan, hexanethiol), carbon tetrachloride and bromotrichloromethane. For example, the chain transfer agent can be 1-octyl mercaptan. The total addition amount of the chain transfer agent can be 1mol / 10mol monomer to 1mol / 300mol monomer, for example 1mol / 20mol monomer to 1mol / 100mol monomer, for example about 1mol chain transfer agent / 30mol monomer. The timing of addition of the chain transfer agent is important for obtaining monodisperse seed particles: the chain transfer agent should be present in the reaction mixture before polymerization initiation (i.e., before activation of the free radical initiator). This finding is surprising because for seed particles used in conventional Ugelstad processes (e.g., polystyrene seed particles), the chain transfer agent should be added (if added) after the start of particle formation, as taught in WO 2010 / 125170, which is incorporated herein by reference.

[0130] The organic solvent may comprise a mixture of an alkane component and an aromatic compound component. The organic solvent may comprise a single component, such as an alkane component or an aromatic compound component. The alkane component may be or include hexane, heptane or octane. The aromatic compound component may be or include C 1 -C 10 Alkyl substituted phenyl or C 1 -C 8 Dialkyl-substituted phenyl, such as C 1 -C 4 When the organic solvent comprises a single component and the component is an aromatic compound component, the aromatic compound component may be C 4 -C 12 Alkyl substituted phenyl or C 2 -C 8 The phenyl of dialkyl substitution. The alkane component can be heptane and the aromatic compound component can be toluene. The alkane component and the aromatic compound component can exist with a weight ratio of the alkane component: the aromatic compound component of about 0.5:1 to about 20:1, for example, the weight ratio of the alkane component: the aromatic compound component can be about 1:1 to about 15:1, for example, about 1:1 to about 10:1.

[0131] The reaction mixture may include: N,N-dimethylacrylamide in an amount of about 2 wt % to about 5 wt %; a stabilizer in an amount of about 1 wt % to about 5 wt %; a free radical initiator in an amount of about 0.01 wt % to about 4 wt % (e.g., about 0.05 wt % to about 0.25 wt %); and a chain transfer agent in an amount of about 0.05 wt % to about 0.25 wt %.

[0132] The monodisperse seed particles may then be subjected to a particle formation process, such as described below:

[0133] Preparation of particles

[0134] The present invention provides a method for forming monodisperse crosslinked hydrogel polymer particles. The Ugelstad method cannot be used to directly form such particles, for example because the Ugelstad method requires that the particles be formed in the oil phase of an oil-in-water emulsion, while the hydrogel polymer particles and the corresponding hydrophilic monomers should be preferentially soluble in water. Applicants have solved this problem by providing the method of the present disclosure, which provides a particle formation method using an oil (continuous phase)-water (discontinuous phase) system. It is believed that this represents the first such method for forming monodisperse crosslinked polymer particles.

[0135] In one embodiment, the present invention provides a method for forming monodisperse crosslinked hydrogel polymer particles. The method includes forming a solution (a) of at least 2 weight percent of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution also comprising a crosslinker containing at least two vinyl groups; forming a solution (b) of a stabilizer in an organic solvent, wherein the organic solvent is immiscible with water, and wherein at least one of the solutions (a) and (b) comprises a free radical initiator; mixing solutions (a) and (b) to form an oil-in-water emulsion (c) and adding monodisperse seed particles to the emulsion; allowing the monodisperse seed particles to form swollen particles in the emulsion; and polymerizing the swollen particles to form monodisperse crosslinked hydrogel polymer particles. As described below, the method can be considered a single-stage method because it includes a single swelling step and a single polymerization step.

[0136] Solution (a) can be formed by first forming a solution of at least 2 weight percent of a hydrophilic vinyl monomer in aqueous solution and then adding a crosslinker; the crosslinker can be added before the hydrophilic vinyl monomer; or the hydrophilic vinyl monomer and the crosslinker can be added to the solution at about the same time. Similarly, the stabilizer and free radical initiator can be added to solution (b) at about the same time or sequentially.

[0137] In the context of the present disclosure, an organic solvent is considered immiscible with water if the organic solvent and water separate into two separate phases when at least 5 weight percent water is mixed with the organic solvent.

[0138] The method involves swelling seed particles with an aqueous discontinuous phase in an oil continuous phase. Figure 1 (illustrated with specific monomers) and Figure 2 (More generally) A schematic diagram of the process is provided, which can be considered a single-stage process since it comprises a single swelling step and a single polymerization step. Figure 1 and Figure 2 The method shown in is conveniently divided into two steps, swelling of monodisperse seed particles 100 to form swollen particles 110, and polymerization of monomers in the swollen seed particles to form crosslinked hydrogel polymer particles 120. Prior to the first step, a water-in-oil emulsion is formed. The water-in-oil emulsion is formed by mixing an aqueous solution comprising an exemplary monomer acrylamide 101 and an exemplary crosslinker 1,2-dihydroxybisacrylamide 102 with an oil phase comprising a steric stabilizer, wherein the emulsion is formed when the aqueous phase and the oil phase are agitated (e.g., by stirring). If (very) highly crosslinked particles are desired, the monomers may also be replaced by a crosslinker, such that the only monomer present in the water-in-oil emulsion is the crosslinking monomer (i.e., the crosslinker, such as 1,2-dihydroxybisacrylamide 102). The water-in-oil emulsion typically also contains an initiator that can be added to the oil phase. An initiator is a compound that initiates polymerization of the monomers and the crosslinker when activated. The monodisperse seed particles 100 comprise non-crosslinked oligomers of poly-N,N-dimethylacrylamide 131 and are considered "activated seed particles." Seed particles 100 can be prepared as described elsewhere in this application. In the first step, monodisperse seed particles 100 are added to a water-in-oil emulsion, and the emulsion is stirred for a period of time (e.g., at least 30 minutes or at least 1 hour, typically 4-48 hours). During this period of time, monomers 101 and crosslinking agents 102 diffuse into the activated seed particles 100 to form swollen seed particles 110. The swollen seed particles 110 contain at least a mixture of monomers 101, crosslinking agents 102, and polymers from the activated seed particles 100. The swollen seed particles 110 may also contain other components, such as one or more pore-forming agents, which can enter the particles if contained in a water-in-oil emulsion. For example, in the method shown, water is also present in the swollen seed particles 110, and the water can be considered as a pore-forming agent. The second step includes the polymerization of monomers 101 and crosslinking agents 102 to form crosslinked hydrogel polymer particles 120. In the second step, polymerization is initiated by activating an initiator, such as by heating the emulsion.

[0139] Providing activated seed particles is a key feature of a successful Ugelstad process. Activation of the seed particles is usually provided by adding an organic compound with very low solubility as an emulsion to produce entropy activated seed particles. However, the applicant has surprisingly determined that this additional activation step is not necessary in the process, for example where the seed particles comprise oligomers of poly-N,N-dimethylacrylamide.

[0140] Swelling is critical for embodiments of the particle formation method. In this method, monomers and (when present) porogens need to have limited solubility in the continuous phase. If the monomers and porogens have too high solubility in the continuous phase, the solubility will not help drive the monomers (and optional porogens) into the seeds and form swollen particles. On the other hand, if the solubility of the monomers (and optional porogens) in the continuous phase is insufficient, the diffusion through the continuous phase can be ignored, so the monomers cannot transfer mass to the seeds, hindering the formation of swollen particles. The time to complete swelling, that is, until all monomers (and optional porogens) are co-located on the seed particles, will be highly dependent on factors such as temperature, solubility and viscosity, and will therefore vary with the system. Therefore, the typical time scale of the step of allowing monodisperse seed particles to form swollen particles will vary between 30 minutes and 48 hours. For example, in one embodiment of the method, the step of allowing monodisperse seed particles to swell can be carried out for at least 30 minutes, such as at least 1 hour. The step of allowing the monodisperse seed particles to swell may be carried out for at least 4 hours, at least 8 hours or at least 12 hours. The upper limit of the swelling time is not believed to be critical, for example it is believed that swelling times of several days, such as 3 days or 2 days, may be used.

[0141] The step of allowing the monodisperse seed particles to form swollen particles may include mixing the emulsion, for example, mixing the emulsion for substantially all of the swelling time. The step of allowing the monodisperse seed particles to form swollen particles may be performed at a temperature of about 10°C to about 60°C, for example, at a temperature of about 10°C to about 40°C, at a temperature of about 15°C to about 30°C. For example, mixing may be performed at a temperature of about 10°C to about 60°C, for example, at a temperature of about 10°C to about 40°C, for example, at a temperature of about 15°C to about 30°C.

[0142] Solution (a) comprises at least 2 wt % of a hydrophilic vinyl monomer in an aqueous solution. The aqueous solution may be water. The aqueous solution may comprise water and up to 50 wt % (e.g. up to 30 wt % or up to 25 wt %, e.g. up to 20 wt %, optionally up to 10 wt %) of a water-miscible organic solvent. The water-miscible organic solvent may be C 1 -C 4 Alcohol, such as ethanol or methanol, such as methanol. The water-miscible organic solvent may be C 2 -C 4 Nitriles, such as acetonitrile.

[0143] The hydrophilic vinyl monomer may contain a broad vinyl group, -CR=CH 2 , where R is alkyl (e.g., where R is -CH 3 or -CH2 CH 3 The hydrophilic vinyl monomer may contain a vinyl group, -CH=CH 2 . The hydrophilic vinyl monomer may be a vinyl monomer having a log P value of less than about 1, for example, a log P of less than about 0.5. The monomer may be a vinyl monomer having a log P of less than about 0.6. The monomer may be a vinyl monomer having a log P of less than about 0.5. For example, the monomer may be a vinyl monomer having a log P of less than about 0.3 or less than about 0.2, for example, the monomer may be a vinyl monomer having a log P of less than about 0.1. The monomer may be a vinyl monomer having a log P of less than about 0, for example, a vinyl monomer having a log P of less than about -0.2. The monomer may be a vinyl monomer having a log P of 0.5 to -2, for example, a log P of 0 to -2, for example, a vinyl monomer having a log P of -0.2 to -2. In particular, the monomer may be a vinyl monomer further comprising a hydrophilic group, for example, an acrylamide monomer or an acrylate monomer.

[0144] The monomer used in the method may be at least one compound of formula (I) wherein R 1 Yes -H, -CH 3 or -CH 2 CH 3 ; R 2 Yes-OR 3 or -N(R 4 )R 5 ;;R 3 Yes -H, -C 1 -C 6 Alkyl or -C 1 -C 6 alcohol; and R 4 and R 5 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Haloalkyl, -C 1 -C 6 alcohol.

[0145] When R 3 For -C 1 -C 6 Alkyl or -C 1 -C 6 In the case of alcohol, the alkyl group or alcohol may be substituted, where chemically possible, by 1 to 5 (e.g. 1, 2, 3 or 4) substituents, each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R aNR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 For example, when R 3 For -C 1 -C 6 Alkyl or -C 1 -C 6 In the case of alcohol, where chemically possible, the alkyl group or alcohol may be selected from 1 to 5 (e.g. 1, 2, 3 or 4) groups, each independently selected from OR a or CO 2 R a substituted by a substituent, optionally wherein R a For H.

[0146] When R 4 and / or R 5 For -C 1 -C 6 Alkyl, -C 1 -C 6 Haloalkyl, -C 1 -C 6alcohol, each of which may be independently substituted, where chemically possible, by 1 to 5 (e.g. 1, 2, 3 or 4) substituents, each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 For example, when R 4 and / or R 5 For -C 1 -C 6 Alkyl, -C 1 -C 6 Haloalkyl, -C 1 -C 6 alcohol, each of which may be independently replaced, where chemically possible, by 1 to 5 (e.g. 1, 2, 3 or 4) selected in each case independently from OR a or CO 2 R a substituted by a substituent, optionally wherein R a For H.

[0147] R 1 Can be -H or -CH 3 For example, R 1 Can be -H.

[0148] R 2 Can be -OR 3 . R 2 Can be -N(R 4 )R 5 .

[0149] R 3 Can be -H. R 3 Can be -C 1 -C 6 Alkyl. For example, R 3 Can be -C 1 -C 6 alkyl, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where R a For -H.R 3 Can be -C 1 -C 6 Alcohol. For example, R 3 Can be -C 1 -C 6 alcohol, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a Ra NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where R a is -H.

[0150] R 4 Can be -H or -C 1 -C 6 Alkyl. 4 Can be -C 1 -C 6 Alkyl. For example, R 4 Can be -C 1 -C 6 alkyl, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4Alkyl, for example, where R a is -H.

[0151] R 5 Can be -H or -C 1 -C 6 Alkyl. 5 Can be -C 1 -C 6 Alkyl. For example, R 5 Can be -C 1 -C 6 alkyl, which is substituted by 1 or 2 substituents, each independently selected from the group consisting of oxo, halogen, cyano, NR a R a NR a CONR a R a NR a CO 2 R a , OR a ;CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 Alkyl, for example, where R a is -H.

[0152] The log P value of the compound of formula (I) may be less than about 1, for example, the log P is less than about 0.5. The log P of the compound of formula (I) may be less than about 0.6. The log P of the compound of formula (I) may be less than about 0.5. For example, the log P of the compound of formula (I) may be less than about 0.3 or less than about 0.2, for example, the log P of the compound of formula (I) may be less than about 0.1. The log P of the compound of formula (I) may be less than about 0, for example, the log P is less than about -0.2. The log P of the compound of formula (I) may be from 0.5 to -2, for example, the log P is from 0 to -2, for example, the log P is from -0.2 to -2.

[0153] The monomer may contain at least one primary amide group (-C(O)NH 2)'s hydrophilic vinyl monomer.

[0154] In particular, acrylamide monomers and / or acrylic acid monomers may be mentioned. Suitable monomers include acrylamide (prop-2-enamide), N-(hydroxymethyl)acrylamide, N-hydroxyethylacrylamide, N-[tris(hydroxymethyl)methyl]acrylamide, 3-acrylamidopropionic acid, methacrylamide, N-(2-hydroxyethyl)methacrylamide, N-(3-aminopropyl)methacrylamide, hydroxypropylacrylamide, N,N-dimethylacrylamide, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, acrylic acid; and other acrylamide monomers, acrylic acid monomers, methacrylamide monomers or methacrylic acid monomers having a log P value of less than about 1 (e.g., a log P value of less than about 0.5).

[0155] Solution (a) may contain no more than 60% by weight of hydrophilic vinyl monomers. For example, solution (a) may contain no more than 55% by weight or 50% by weight of hydrophilic vinyl monomers. For example, solution (a) may contain no more than 45% by weight or 40% by weight of hydrophilic vinyl monomers; for example, solution (a) may contain no more than 30% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 2% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 5% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 8% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 2% by weight (e.g., 5% by weight) of hydrophilic vinyl monomers and no more than 60% by weight of hydrophilic vinyl monomers, for example, solution (a) may contain at least 8% by weight of hydrophilic vinyl monomers and no more than 60% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 50 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain at least 8 wt % of hydrophilic vinyl monomer and no more than 50 wt % of hydrophilic vinyl monomer. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 45 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain at least 8 wt % of hydrophilic vinyl monomer and no more than 45 wt % of hydrophilic vinyl monomer. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 30 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain at least 8 wt % of vinyl monomer and no more than 30 wt % of hydrophilic vinyl monomer. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 15 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain about 10 wt % of hydrophilic vinyl monomer.

[0156] The hydrophilic vinyl monomer may comprise a mixture of monomers. For example, the monomer may comprise at least one monomer as defined above and at least one compatible functional monomer. The corresponding functional monomer is a hydrophilic vinyl monomer as defined herein, comprising a carboxylic acid (-COOH), a primary amine or a secondary amine. The functional monomer may be a vinyl monomer having a log P value less than about 1 (e.g., log P less than about 0.5), comprising a carboxylic acid or a primary amine. The functional monomer may be a vinyl monomer having a log P value less than about 0.6. The functional monomer may be a vinyl monomer having a log P value less than about 0.5. For example, the functional monomer may be a vinyl monomer having a log P value less than about 0.3 or less than about 0.2, for example, the functional monomer may be a vinyl monomer having a log P value less than about 0.1. The functional monomer may be a vinyl monomer having a log P value less than about 0, for example, a log P value less than about -0.2. The functional monomer may be a vinyl monomer having a log P value of 0.5 to -2, for example, a log P value of 0 to -2, for example, a log P value of -0.2 to -2. The functional monomer may be a compound of formula (I) comprising a carboxylic acid or a primary amine. The functional monomer may be an acrylamide monomer containing a carboxylic acid or a primary amine. Suitable functional monomers include 3-acrylamidopropionic acid, 4-acrylamidobutyric acid, 5-acrylamidopentanoic acid, N-(3-aminopropyl)methacrylamide and acrylic acid.

[0157] In the presence of at least one functional monomer, the amount of the functional monomer can be from about 0.1 to about 100 mol%, such as from about 0.2 to about 50 mol%, such as from about 0.5 to about 40 mol% or from about 1 to about 30 mol% (e.g., from about 2 to about 20 mol%). The amount of the functional monomer can be from about 0.1 to about 10 mol%, such as from about 0.2 to about 5 mol%, such as from about 0.5 to about 2 mol%. Mol% can refer to the molar percentage of the functional monomer in the total hydrophilic vinyl monomers contained in solution (a) (i.e., a solution containing at least 2 wt% of the hydrophilic vinyl monomer in water).

[0158] In highly crosslinked particles, the monomer may be or include a crosslinking agent. For example, the monomer may be or include at least one compound of formula (IIa) or formula (IIb).

[0159] The crosslinking agent used in the method may contain at least two (e.g., 2) vinyl groups (—CH═CH 2 ). The cross-linking agent used in the method may be at least one compound of formula (IIa) or formula (IIb), wherein R 6 Selected from -C 1 -C 6 Alkyl-, -C 1 -C 6 Heteroalkyl-, -C 1 -C 6Cycloalkyl-, -C 1 -C 6 Hydroxyalkyl-, -C 1 -C 6 Ether - or containing 2 to 100 C 2 -C 3 ether units; and R 7 and R 8 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Heteroalkyl, -C 3 -C 6 Cycloalkyl, -C 1 -C 6 Hydroxyalkyl or -C 1 -C 6 Ether; R 9 -N(R 11 )C(O)CH=CH 2 ; R 10 Selected from -H and -N(R 12 )C(O)CH=CH 2 ; and R 11 and R 12 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Heteroalkyl, -C 3 -C 6 Cycloalkyl, -C 1 -C 6 Hydroxyalkyl or -C 1 -C 6 ether.

[0160] The crosslinking agent may be at least one compound of formula (IIa). The crosslinking agent may be at least one compound of formula (IIb).

[0161] Where chemically possible, R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be independently substituted by 1 to 5 substituents each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 Ra NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a In each case, independently selected from: H, C 1 -C 4 Alkyl and C 1 -C 4 Alkenyl.

[0162] R 6 Selected from -C 1 -C 6 Alkyl-, -C 1 -C 6 Heteroalkyl-, -C 1 -C 6 Cycloalkyl-, -C 1 -C 6 Hydroxyalkyl- and -C 1 -C 6 Ether-. R 6 Can be selected from -C 1 -C 6 Alkyl- and -C 1 -C 6 Hydroxyalkyl-. 6 Can be -C 1 -C 6 Alkyl-, such as -CH 2 -、-(CH 2 ) 2 -、-(CH 2 )3 -or-(CH 2 ) 4 -, for example -(CH 2 ) 2 -. R 6 Can be -C 1 -C 6 Hydroxyalkyl-, such as -C(OH)H-, -(C(OH)H) 2 -、-(C(OH)H) 3 -or-(C(OH)H) 4 -, for example -(C(OH)H) 2 -.

[0163] R 6 Can be -C 1 -C 6 Heteroalkyl-, optionally wherein the heteroatom is an amine (eg, a tertiary amine). For example, C(O)R a Replaced-C 1 -C 6 Heteroalkyl, optionally wherein the heteroatom is an amine, such as R 6 Can be -CH 2 CH 2 N(C(O)CH=CH 2 )CH 2 CH 2 -.

[0164] When R 6 When it is a polyether, the polyether may be linear or branched. 6 It can contain 2 to 100 C 2 -C 3 Polyethers of ether units, for example containing 2 to 50 C 2 -C 3 Polyether of ether units. 6 It can contain 2 to 100 C 2 Polyethers of ether units, for example containing 2 to 50 C 2 For example, R 6 It can be -(CH 2 ) r (OCH 2 CH 2 ) n O(CH 2 ) s , wherein r and s are each independently 2 or 3 (e.g., 2); and n is an integer from 1 to 100 (e.g., 5 to 50 or 5 to 25). Without wishing to be bound by any theory, it is believed that a crosslinking agent comprising a polyether (e.g., wherein R 6The crosslinking agent (e.g., polyether) has excellent solubility in the aqueous phase. This means that, while such crosslinking agents can be used to provide particles with low crosslinking levels (e.g., 1-20 wt% crosslinking agent, or 1-10 wt% crosslinking agent), such crosslinking agents comprising polyethers are particularly suitable for providing particles comprising relatively high crosslinking levels, such as >20 wt% crosslinking agent, >25 wt% crosslinking agent, or >30 wt% crosslinking agent. For example, the crosslinking level may be 10-90 wt% crosslinking agent, 20-80 wt% crosslinking agent, or 25-75 wt% crosslinking agent, such as 25-60 wt% crosslinking agent, or 30-50 wt% crosslinking agent.

[0165] R 7 and / or R 8 and / or R 11 and / or R 12 It can be H. For example, R 7 and / or R 8 It can be H. For example, R 11 and / or R 12 Can be H.

[0166] The log P value of the compound of formula (II) may be less than about 1, for example, a log P of less than about 0.5. The log P of the compound of formula (II) may be less than about 0.6. The log P of the compound of formula (II) may be less than about 0.5. For example, the log P of the compound of formula (II) may be less than about 0.3 or less than about 0.2, for example, the log P of the compound of formula (II) may be less than about 0.1. The log P of the compound of formula (II) may be less than about 0, for example, a log P of less than about -0.2. The log P of the compound of formula (II) may be from 0.5 to -2, for example, a log P of 0 to -2, for example, a log P of -0.2 to -2.

[0167] Exemplary cross-linking agents used in embodiments of the method include N,N'-(1,2-dihydroxyethylene)bisacrylamide, N,N'-methylenebis(acrylamide), N,N'-ethylenebis(acrylamide), piperazine diacrylamide, glycerol 1,3-diglyceryl diacrylate, N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl)) diacrylamide, polyethylene glycol diacrylamide (MW≤2000), 4-arm PEG-acrylamide (MW≤2000), and N,N-bis(2-acrylamidoethyl)acrylamide. Exemplary crosslinking agents N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide, polyethylene glycol diacrylamide (MW≤2000), and 4-arm PEG-acrylamide (MW≤2000) (e.g., N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide) are particularly suitable for use in highly crosslinked particles and mechanically more stable particles, i.e., particles having a crosslinking level of at least 20% by weight of the crosslinker (e.g., a crosslinking level of at least 30% by weight of the crosslinker). Embodiments may also include the use of a combination of crosslinking agents.

[0168] The crosslinking agent may be a compound that does not contain a primary amine, a secondary amine, a hydroxyl group or a carboxylic acid. The crosslinking agent may be a compound of formula (IIa) or formula (IIb) that does not contain a primary amine, a secondary amine, a hydroxyl group or a carboxylic acid.

[0169] The level of crosslinking in the crosslinked hydrogel polymer particles formed by the method can be expressed as the weight percentage (wt%) of the crosslinker monomer contained in the total monomers used for polymerization. Typical crosslinking levels include >5 wt% crosslinker, such as >10 wt% crosslinker, or >15 wt% crosslinker, such as >20 wt% crosslinker. The crosslinking level can also be, for example, 5-60 wt% crosslinker, such as 10-50 wt% crosslinker. The crosslinking level can also be, for example, 15-40 wt% crosslinker, such as 20-40 wt% crosslinker, such as 20-30 wt% crosslinker. Therefore, solution (a) can contain an amount of crosslinker in wt% corresponding to 5-60% of the amount of hydrophilic vinyl monomer, such as 10-50% of the amount of hydrophilic vinyl monomer. Thus, solution (a) may comprise an amount of crosslinker in wt% corresponding to, for example, 15-40% of the amount of hydrophilic vinyl monomer, such as 20-40% of the amount of hydrophilic vinyl monomer, such as 20-30% of the amount of hydrophilic vinyl monomer.

[0170] For example, in highly crosslinked particles, the crosslinking level may be >30 wt% crosslinker or >40 wt% crosslinker (e.g. >50 wt% crosslinker). The crosslinking level may be 10-90 wt% crosslinker, 20-80 wt% crosslinker or 25-75 wt% crosslinker, for example 25-60 wt% crosslinker or 30-50 wt% crosslinker. In highly crosslinked particles, the crosslinking level may be up to 100 wt% crosslinker, for example a hydrophilic vinyl monomer may be the crosslinker, for example the hydrophilic vinyl monomer and the crosslinker may be the same compound. Thus, solution (a) may contain an amount of crosslinker in wt% corresponding to 20-80 %, for example 25-60 % of the amount of the hydrophilic vinyl monomer.

[0171] As specific hydrophilic vinyl monomers, mention may be made of acrylamide (prop-2-enamide), of which 1,2-dihydroxybisacrylamide is a suitable crosslinking agent. As specific hydrophilic vinyl monomers, mention may be made of methylol acrylamide, of which N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide is a suitable crosslinking agent. As specific hydrophilic vinyl monomers, mention may be made of hydroxyethyl acrylamide, of which N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide is a suitable crosslinking agent.

[0172] Stabilizer can be or include nonionic surfactant, for example nonionic polymer surfactant.Nonionic surfactant can include at least one oligomeric surfactant.For example, nonionic surfactant can include oligomeric surfactant.Nonionic polymer or oligomeric surfactant can include at least one polyoxyethylene group or at least one polyoxypropylene group.Nonionic polymer surfactant can include at least one polyoxyethylene group.Nonionic oligomeric surfactant can include at least one polyoxyethylene group or at least one polyoxypropylene group.Stabilizer can be selected from or include hypermer 2296, Abil WE09, Abil EM90 and sorbitan monooleate (Span 80).

[0173] Polymerization can include activating a free radical initiator. The free radical initiator is typically activated by heating to form free radicals that initiate polymerization, however other activation methods, such as radiation, can also be used. Activating the free radical initiator can include heating an emulsion containing swollen particles. Heating typically includes heating the emulsion to a temperature above the temperature of the step that allows the monodisperse seed particles to form swollen particles. Heating can include heating to a temperature of at least 40° C., such as heating to a temperature of at least 50° C., such as a temperature of at least 60° C. or a temperature of at least 70° C.

[0174] The free radical initiator can be or include a peroxide initiator or an azo initiator. For example, the free radical initiator can be a peroxide initiator. For example, the free radical initiator can be an azo initiator. An exemplary free radical initiator is 2,2'-azobis-2,4-dimethylvaleronitrile. An exemplary free radical initiator is 2,2'-azobis(2-methylbutyronitrile). The free radical initiator can be present in solution (a). The free radical initiator can be present in solution (b). The free radical initiator can be present in the emulsion in an amount of about 0.1% by weight to about 1.5% by weight. For example, the free radical initiator can be present in the emulsion in an amount of about 0.6% by weight to about 1.2% by weight; for example, the free radical initiator can be present in the emulsion in an amount of about 0.8% in the emulsion.

[0175] The organic solvent used in the method for forming monodisperse crosslinked hydrogel polymer particles may contain (or consist of) at least one aliphatic hydrocarbon, aliphatic carbonate, aliphatic ester, aliphatic ether, aromatic hydrocarbon or silicone, or a combination thereof. For example, the organic solvent may contain (or consist of) at least two of aliphatic hydrocarbons, aliphatic carbonates, aliphatic esters, aliphatic ethers, aromatic hydrocarbons and silicones; or the organic solvent may contain (or consist of) at least three of aliphatic hydrocarbons, aliphatic carbonates, aliphatic esters, aliphatic ethers, aromatic hydrocarbons and silicones. The organic solvent may contain (or consist of) a mixture of heptane and toluene. The organic solvent may contain (or consist of) a mixture of aliphatic hydrocarbons. The organic solvent may contain (or consist of) bis(2-ethylhexyl) carbonate. The organic solvent may contain (or consist of) bis(2-ethylhexyl) carbonate, aliphatic hydrocarbons and aromatic hydrocarbons. The organic solvent may contain (or consist of) bis(2-ethylhexyl) adipate.

[0176] The monodisperse seed particles added to the water-in-oil emulsion (c) may have the characteristics of monodisperse seed particles formed according to the method for preparing monodisperse seed particles disclosed herein. The monodisperse seed particles added to the water-in-oil emulsion (c) may be monodisperse seed particles formed according to the method for preparing monodisperse seed particles disclosed herein. The monodisperse seed particles may be monodisperse seed particles of the present disclosure, such as monodisperse seed particles of the present invention.

[0177] In one embodiment, the present invention provides a method for forming monodisperse crosslinked hydrogel polymer particles. The method comprises forming a solution (a) of at least 2 wt. % of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution also comprising a chain transfer agent; forming a solution (b) of a stabilizer in an organic solvent, wherein the organic solvent is immiscible with water and wherein at least one of the solutions (a) and (b) comprises a free radical initiator; mixing solutions (a) and (b) to form a water-in-oil emulsion (c) and adding monodisperse seed particles to the emulsion; allowing the monodisperse seed particles to form swollen particles in the emulsion; polymerizing the swollen particles to form monodisperse polymer particles; forming a monodisperse crosslinked hydrogel polymer particle in an organic solvent; and forming a stabilizer solution (d), wherein the organic solvent is immiscible with water; forming a solution (e) of at least 2 wt% of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution also comprising a crosslinker containing at least two vinyl groups, wherein at least one of the solution (d) and the solution (e) comprises a free radical initiator; mixing the solutions (d) and (e) to form a water-in-oil emulsion (f) and adding monodisperse polymer particles to the emulsion; allowing the monodisperse polymer particles to form swollen polymer particles in the emulsion; and polymerizing the swollen polymer particles to form monodisperse crosslinked hydrogel polymer particles. As described below, the method can be considered a two-stage method because it includes a first swelling step and a first polymerization step, followed by a second swelling step and a second polymerization step. Compared to the single-stage method, the two-stage method can provide large monodisperse crosslinked hydrogel crosslinked polymer particles.

[0178] Similar to the one-stage process, the two-stage process involves swelling the seed particles with an aqueous discontinuous phase in an oil continuous phase. Figure 3 (illustrated with specific monomers) and Figure 4 (More generally) A schematic diagram of this process is provided, which can be considered a two-stage process as it includes two swelling steps and two polymerization steps. Figure 3 and 4The method shown in is conveniently divided into four steps: swelling of monodisperse seed particles 100 with monomers 103 and chain transfer agents 105 to form swollen (monodisperse) seed particles 110; polymerization of the monomers in the swollen seed particles to form (uncrosslinked) hydrophilic polymer particles 130; swelling of the hydrophilic polymer particles with monomers 103 and crosslinking agents 102 to form swollen hydrophilic polymer particles 140; and polymerization of the monomers in the hydrogel polymer particles to form crosslinked hydrogel polymer particles 150. Prior to the first step, a water-in-oil emulsion is formed. The water-in-oil emulsion is formed by mixing a monomer (e.g., hydroxymethyl acrylamide 103) and a chain transfer agent (e.g., 1-thioglycerol 105) with an oil phase containing a steric stabilizer, wherein the emulsion is formed when the aqueous phase and the oil phase are agitated (e.g., by stirring). The water-in-oil emulsion also typically contains an initiator, which may have been added to the oil phase and / or the aqueous phase. An initiator is a compound that initiates polymerization of the monomers when activated. The monodisperse seed particles 100 comprise non-crosslinked oligomers of poly-N,N-dimethylacrylamide 131 and are considered “activated seed particles.” The seed particles 100 can be prepared as described elsewhere in this application.

[0179] In the first step, monodisperse seed particles 100 are added to a water-in-oil emulsion, and the emulsion is stirred for a period of time (e.g., at least 30 minutes or at least 1 hour, typically 4-48 hours). During this period of time, monomers 103 and chain transfer agents 105 diffuse into the activated seed particles 100 to form swollen seed particles 110. The swollen seed particles 110 contain at least a mixture of monomers 103, chain transfer agents 105, and polymers from the activated seed particles 100. The swollen seed particles 110 may also contain other components, such as one or more porogens, which may enter the particles if they are contained in the water-in-oil emulsion. For example, in the method shown, water is also present in the swollen seed particles 110, and the water can be considered as a porogen. The second step includes the polymerization of the polymerized monomers 103 to form (uncrosslinked) hydrophilic polymer particles 130. In the second step, polymerization is initiated by activating an initiator, such as by heating the emulsion. The presence of chain transfer agent 105 makes the polymers of polyhydroxymethyl acrylamide 132 (e.g., oligomers) in the hydrogel polymer particles relatively short. These relatively short polymers combined with the lack of crosslinking means that the hydrophilic polymer particles 130 can act as larger "activated seed particles" suitable for another round of swelling and polymerization. The hydrophilic polymer particles contain non-crosslinked, relatively short polymers of the polymer of polyhydroxymethyl acrylamide 132 and non-crosslinked oligomers of poly N,N-dimethyl acrylamide 131 (usually in a smaller proportion).

[0180] Prior to the third step, a water-in-oil emulsion is formed. The water-in-oil emulsion is formed by mixing a monomer (e.g., hydroxymethyl acrylamide 103) and a crosslinker (e.g., 1,2-dihydroxybisacrylamide 102) with an oil phase containing a steric stabilizer. If (very) highly crosslinked particles are desired, the monomer may also be replaced by a crosslinker so that the only monomer present in the water-in-oil emulsion is the crosslinking monomer (i.e., the crosslinker). The water-in-oil emulsion typically also contains an initiator that can be added to the oil phase or the water phase. An initiator is a compound that initiates polymerization of the monomer and the crosslinker when activated. In the third step (second round of swelling), hydrophilic polymer particles 130 are added to the water-in-oil emulsion, and the emulsion is stirred for a period of time (e.g., at least 30 minutes or at least 1 hour, typically 4-48 hours). During this period of time, the monomer 103 and the crosslinker 102 diffuse into the hydrophilic polymer particles 130 to form swollen hydrogel polymer particles 140. The swollen hydrophilic polymer particles 140 include a mixture of at least monomers 103, crosslinkers 102, and polymers from the hydrophilic polymer particles 130. The swollen hydrogel polymer particles 140 may also include other components, such as one or more pore formers, which may enter the particles if contained in a water-in-oil emulsion. For example, in the method shown, water is also present in the swollen seed particles 110, and this water can be considered a pore former. The fourth step includes polymerization of the monomers 103 and the crosslinkers 102 to form crosslinked hydrogel polymer particles 104. In the fourth step, polymerization is initiated by activating the initiator, such as by heating the emulsion.

[0181] Monomer, chain transfer agent, free radical initiator, stabilizer, crosslinking agent, organic solvent and optional porogen can each be as defined elsewhere herein. Monomer can be or include hydroxymethyl acrylamide or hydroxyethyl acrylamide. Chain transfer agent can be or include 1-thioglycerol. Free radical initiator can be or include azobismethylvaleronitrile, such as 2,2'-azobis(2-methylbutyronitrile) (AMBN). Stabilizer can be or include Hypermer 2296, Abil WE09 and Abil EM90. Crosslinking agent can be 1,2-dihydroxybisacrylamide or N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide.

[0182] Solution (a) may contain no more than 60% by weight of hydrophilic vinyl monomers. For example, solution (a) may contain no more than 55% by weight or 50% by weight of hydrophilic vinyl monomers. For example, solution (a) may contain no more than 45% by weight or 40% by weight of hydrophilic vinyl monomers; for example, solution (a) may contain no more than 30% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 2% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 5% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 8% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 2% by weight (e.g., 5% by weight) of hydrophilic vinyl monomers and no more than 60% by weight of hydrophilic vinyl monomers, for example, solution (a) may contain at least 8% by weight of hydrophilic vinyl monomers and no more than 60% by weight of hydrophilic vinyl monomers. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 50 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain at least 8 wt % of hydrophilic vinyl monomer and no more than 50 wt % of hydrophilic vinyl monomer. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 45 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain at least 8 wt % of hydrophilic vinyl monomer and no more than 45 wt % of hydrophilic vinyl monomer. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 30 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain at least 8 wt % of vinyl monomer and no more than 30 wt % of hydrophilic vinyl monomer. Solution (a) may contain at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 15 wt % of hydrophilic vinyl monomer, for example, solution (a) may contain about 10 wt % of hydrophilic vinyl monomer.

[0183] Solution (e) may contain no more than 60% by weight of hydrophilic vinyl monomers. For example, solution (e) may contain no more than 55% by weight or 50% by weight of hydrophilic vinyl monomers. For example, solution (e) may contain no more than 45% by weight or 40% by weight of hydrophilic vinyl monomers; for example, solution (e) may contain no more than 30% by weight of hydrophilic vinyl monomers. Solution (e) may contain at least 2% by weight of hydrophilic vinyl monomers. Solution (e) may contain at least 5% by weight of hydrophilic vinyl monomers. Solution (e) may contain at least 8% by weight of hydrophilic vinyl monomers. Solution (e) may contain at least 2% by weight (e.g., 5% by weight) of hydrophilic vinyl monomers and no more than 60% by weight of hydrophilic vinyl monomers, for example, solution (e) may contain at least 8% by weight of hydrophilic vinyl monomers and no more than 60% by weight of hydrophilic vinyl monomers. Solution (e) may include at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 50 wt % of hydrophilic vinyl monomer, for example, solution (e) may include at least 8 wt % of hydrophilic vinyl monomer and no more than 50 wt % of hydrophilic vinyl monomer. Solution (e) may include at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 45 wt % of hydrophilic vinyl monomer, for example, solution (e) may include at least 8 wt % of hydrophilic vinyl monomer and no more than 45 wt % of hydrophilic vinyl monomer. Solution (e) may include at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 30 wt % of hydrophilic vinyl monomer, for example, solution (e) may include at least 8 wt % of vinyl monomer and no more than 30 wt % of hydrophilic vinyl monomer. Solution (e) may include at least 2 wt % (e.g. 5 wt %) of hydrophilic vinyl monomer and no more than 15 wt % of hydrophilic vinyl monomer, for example, solution (e) may include about 10 wt % of hydrophilic vinyl monomer.

[0184] In highly crosslinked particles, the hydrophilic vinyl monomer of solution (e) may be or include a crosslinking agent. For example, the monomer may be or include at least one compound of formula (IIa) or (IIb).

[0185] The level of crosslinking in the crosslinked hydrogel polymer particles formed by the method can be expressed as the weight percentage (wt%) of the crosslinker monomer contained in the total monomers used for polymerization (i.e., in the second polymerization step). The wt% of the crosslinker monomer can be equal to the wt% of the crosslinker in the matrix polymer (i.e., the wt% of the crosslinker in the dry weight of the crosslinked polymer particles). Typical crosslinking levels include >5 wt% crosslinker, such as >10 wt% crosslinker, or >15 wt% crosslinker, such as >20 wt% crosslinker (e.g., >30 wt% crosslinker). The crosslinking level can also be, for example, 5-60 wt% crosslinker, such as 10-50 wt% crosslinker. The crosslinking level can also be, for example, 15-40 wt% crosslinker, such as 20-40 wt% crosslinker, such as 20-30 wt% crosslinker. The crosslinking level may be 20-80 wt% crosslinker or 25-75 wt% crosslinker, such as 25-60 wt% crosslinker or 30-50 wt% crosslinker; for example in high density particles. Thus, solution (e) may contain an amount of crosslinker in wt% corresponding to 5-60 wt% of the amount of hydrophilic ethylenic monomer, such as 10-50 wt% of the amount of hydrophilic vinyl monomer. Thus, solution (e) may contain an amount of crosslinker in wt% corresponding to, for example, 15-40 wt% of the amount of hydrophilic vinyl monomer, such as 20-40 wt% of the amount of hydrophilic vinyl monomer, such as 20-30 wt% of the amount of hydrophilic vinyl monomer.

[0186] For example, in highly crosslinked particles, the crosslinking level may be >30 wt% crosslinker or >40 wt% crosslinker (e.g. >50 wt% crosslinker). The crosslinking level may be 10-90 wt% crosslinker, 20-80 wt% crosslinker or 25-75 wt% crosslinker, e.g. 25-60 wt% crosslinker or 30-50 wt% crosslinker. In highly crosslinked particles, the crosslinking level may be up to 100 wt% crosslinker, e.g. the hydrophilic vinyl monomer in solution (e) may be the crosslinker, e.g. the hydrophilic vinyl monomer and the crosslinker may be the same compound. Solution (e) may contain an amount of crosslinker in wt% corresponding to 20-80 %, e.g. 25-60 % of the amount of the hydrophilic vinyl monomer.

[0187] The free radical initiator may be present in each or at least one emulsion in an amount of about 0.1 wt % to about 1.5 wt %. For example, the free radical initiator may be present in each or at least one emulsion in an amount of about 0.6 wt % to about 1.2 wt %; for example, the free radical initiator may be present in each or at least one emulsion in an amount of about 0.8 wt % in each or at least one emulsion.

[0188] By making chain termination with the free radical reaction of the growing polymer chain and transferring the lone electron to the free radical species derived from the chain transfer agent, the interpolation of the chain transfer agent reduces the molecular weight of the polymer of the seed particles.Then the free radical species derived from the chain transfer agent can react with the monomer and form free radicals by the monomer, and then it can react with another monomer and start to form a new polymer chain.The chain transfer agent can be a mercaptan or a haloalkane.For example, the chain transfer agent can be selected from mercaptan (for example 1-thioglycerol, 1-octyl mercaptan, hexyl mercaptan, 6-mercapto-1-hexanol, benzyl mercaptan), alkyl mercaptan (for example 1-octyl mercaptan, hexyl mercaptan) and thiopolyol.For example, the chain transfer agent can be or include 1-thioglycerol.The total addition of the chain transfer agent can be 1mol / 10mol monomer to 1mol / 300mol monomer, for example 1mol / 20mol monomer to 1mol / 100mol monomer, for example about 1mol chain transfer agent / 30mol monomer.

[0189] The monodisperse cross-linked hydrogel polymer particles formed according to the method of the present invention may be porous. For example, the porosity of the monodisperse cross-linked hydrogel polymer particles formed may be at least 5%, such as at least 10%. The present disclosure includes porous monodisperse cross-linked hydrogel polymer particles having a porosity of 20% to 95%, particularly 30% to 90%, such as 40% to 90%, such as 50% to 80%. The porous monodisperse cross-linked hydrogel polymer particles formed may be permeable to solvated molecules, for example, the porous monodisperse cross-linked hydrogel polymer particles may be permeable to oligonucleotides and nucleic acid amplification reagents and sequencing reagents (e.g., primers, nucleotides, and polymerases).

[0190] The monodisperse crosslinked hydrogel polymer particles formed according to the method of the present invention may have a mode diameter of 0.5 μm to 10 μm, for example 0.5 μm to 5 μm. The mode diameter of the monodisperse crosslinked hydrogel polymer particles formed may be at least 500 nm, for example at least 600 nm, optionally at least 800 nm, such as in the case of particles with a diameter of at least 1 μm. The mode diameter of the monodisperse crosslinked hydrogel polymer particles formed according to the method of the present invention may not exceed 10 μm, for example not exceed 5 μm, optionally not exceed 3 μm, such as in the case of particles with a diameter of not more than 2 μm. The size and size distribution of the monodisperse crosslinked hydrogel polymer particles formed according to the method of the present invention may be determined as described below under the heading "Analytical Methods".

[0191] The monodisperse crosslinked hydrogel polymer particles formed according to the method of the present invention may have a CV of less than 20%, such as less than 15%. For example, the particles may have a CV of less than 10%, such as a CV of less than 8%, such as a CV of less than 5%.

[0192] The monodisperse cross-linked hydrogel polymer particles formed according to the method of the present invention may include functional groups. The functional groups may be selected from hydroxyl, carboxylic acid (-COOH), primary amine or secondary amine. In one embodiment, the functional groups are provided by hydrophilic vinyl monomers (e.g., compounds of formula (I)) rather than cross-linking agents (e.g., compounds of formula (IIa) or formula (IIb)). The functional groups may be enhanced to promote binding to target analytes (e.g., oligonucleotides) or target receptors. Exemplary methods for enhancing the functional groups of particles are described herein in the section related to "Use of Particles".

[0193] The monodisperse cross-linked hydrogel polymer particles formed according to the method of the present invention may include oligonucleotides connected to the particles. Oligonucleotides may be connected to the monodisperse cross-linked hydrogel polymer particles by a connector. For example, each (or a portion) monodisperse hydrogel polymer particle may include multiple oligonucleotides connected to the particles. For each single cross-linked hydrogel polymer particle, multiple oligonucleotides may be identical. For example, the first cross-linked hydrogel polymer particle may include multiple oligonucleotides with a first sequence connected to the first particle, and the second cross-linked hydrogel polymer particle may include multiple oligonucleotides with a second sequence connected to the second cross-linked hydrogel polymer particle. In the case where the monodisperse cross-linked hydrogel polymer particles are porous, the oligonucleotides may be connected to the outer surface of the particle, or connected in the hole. The hole may have enough size to make the particle permeable to the oligonucleotide, so that the oligonucleotide may be partially or completely located in the hole, even when the polymerase is connected to the oligonucleotide.

[0194] The monodisperse crosslinked hydrogel polymer particles formed according to the methods of the present invention can be stable (i.e., resistant to polymer degradation) over a typical temperature range of aqueous solutions. The monodisperse crosslinked hydrogel polymer particles formed can be stable at temperatures up to about 100° C. For example, the monodisperse crosslinked hydrogel polymer particles formed can be stable over a temperature range of about 0° C. to about 100° C.

[0195] One embodiment of the present invention provides a particle obtained by the preparation method described herein or a particle having the characteristics of a particle obtained by the preparation method described herein.

[0196] The polymer particle formation method described herein can be processed to be highly repeatable and scalable. Therefore, the present invention can achieve consistency between batches and within batches, which is a prerequisite for industrial applications. The present invention can also produce, for example, pilot scale batches, for example, at least 300g and kilogram scale industrial batches.

[0197] The polymer particle formation methods described herein can be performed consistently without the problems associated with emulsion polymerization that may occur in practice, such as agglomeration of particles and product variation.

[0198] Uses of granules

[0199] The particles can be used in many applications, for example, polynucleotide sequencing, polynucleotide sequencing, information storage, color imaging, bioprocessing, diagnostic microbiology, biosensors, and drug delivery.

[0200] The polymer particles can be activated to facilitate conjugation with target analytes such as polynucleotides. In addition to the methods described below, suitable activation and bioconjugation methods are described in GT Hermanson, Bioconjugate Techniques, 2013 (3rd edition), Academic Press, the contents of which are incorporated herein by reference in their entirety.

[0201] For example, the functional group on the polymer particles can be enhanced to allow binding to the target analyte or analyte receptor. In a specific example, the functional group of the polymer particles can be modified with a reagent that can convert the functional group into a reactive part that can undergo nucleophilic or electrophilic substitution. For example, the hydroxyl on the polymer particles can be activated by replacing at least a portion of the hydroxyl with a sulfonate group or chlorine. Exemplary sulfonate groups can be derived from tresyl, mesyl, tosyl or toluenesulfonyl chloride, or any combination thereof. Sulfonate can play the role of allowing nucleophilic reagents to replace sulfonate. Sulfonate can further provide a chlorinated group with the released chlorine reaction, which can be used in the process of conjugated particles. In another example, when the polymer particles include an amine group or a carboxylic acid group (for example, from a functional monomer), the amine group or the carboxylic acid group can be activated.

[0202] For example, a target analyte or analyte receptor can be bound to a polymer particle by nucleophilic substitution with a sulfonate group or other activated group. In a specific example, a target analyte receptor terminated with a nucleophile such as an amine or thiol can undergo nucleophilic substitution to replace the sulfonic acid group on the surface of the polymer particle. As a result of activation, a conjugated particle can be formed.

[0203] In another example, the sulfonated particles can be further reacted with a monofunctional or polyfunctional mononucleophilic or polynucleophilic reagent that can form a link to the particle while retaining the nucleophilic activity of an oligonucleotide containing an electrophilic group (such as maleimide). In addition, residual nucleophilic activity can be converted to electrophilic activity by linking with a reagent containing a polyelectrophic group that is subsequently linked to an oligonucleotide containing a nucleophilic group.

[0204] In another example, during polymerization, monomers containing functional groups (functional monomers) can be included in the monomer mixture. Functional monomers can include, for example, acrylamides containing carboxylic acid, ester, halogen or other amine reactive groups. The ester group can be hydrolyzed before reacting with the amine oligonucleotide.

[0205] Other activation chemistries include combining multiple steps to convert specific functional groups to adapt to specific desired connections. For example, sulfonate-modified hydroxyls can be converted into nucleophilic groups by several methods. In one example, the reaction of sulfonate with azide anion produces azide-substituted hydrophilic polymers. The azide can be directly used to conjugate to acetylene-substituted biomolecules by "CLICK" chemistry that can be carried out with or without copper catalysis. Optionally, azide can be converted into amines by, for example, hydrogen catalytic reduction or reduction with organic phosphine. Then the resulting amine can be converted into electrophilic groups with a variety of reagents such as diisocyanates, bis-NHS esters, cyanuric chloride or their combinations. In one example, diisocyanates are used to generate urea connections between polymers and connectors, which generate residual isocyanate groups, which can react with amino-substituted biomolecules and generate urea connections between connectors and biomolecules. In another example, bis-NHS esters are used to generate amide bonds between polymers and connectors, and residual NHS ester groups can react with amino-substituted biomolecules and generate amide bonds between connectors and biomolecules. In another example, cyanuric chloride is used to create an amino-triazine linkage between the polymer and the linker, and one of the two residual chloro-triazine groups can react with an amino-substituted biomolecule to create an amino-triazine linkage between the linker and the biomolecule. Other nucleophilic groups can be incorporated into the particle through sulfonate activation. For example, reaction of the sulfonated particle with a thiobenzoate anion and subsequent hydrolysis of the thiobenzoate will incorporate sulfhydryl groups into the particle, which can then react with a maleimide-substituted biomolecule to create a sulfo-succinimide linkage to the biomolecule. Sulfhydryl groups can also react with bromoacetyl groups.

[0206] The covalent attachment of biomolecules to refractory or polymeric substrates can be produced using an electrophilic moiety on the substrate coupled to a nucleophilic moiety on the biomolecule or a nucleophilic attachment on the substrate coupled to an electrophilic attachment on the biomolecule. Due to the hydrophilic nature of the most common biomolecules of interest, the solvents selected for these attachments are water or water containing some water-soluble organic solvents so that the biomolecules are dispersed on the substrate. In particular, polynucleotides are usually attached to substrates in aqueous systems due to their polyanionic nature. Because water competes with nucleophiles for electrophiles by hydrolyzing electrophiles into inactive moieties for conjugation, aqueous systems usually result in low yields of coupled products, wherein the yield is based on the electrophilic moiety of the attachment. When a high yield of electrophilic moieties of a reaction conjugate is desired, a high concentration of nucleophiles is required to drive the reaction and mitigate hydrolysis, resulting in inefficient utilization of nucleophiles. In the case of polynucleic acids, the metal counterions of the phosphates can be replaced with lipophilic counterions to help solubilize the biomolecules in polar non-reactive non-aqueous solvents. These solvents can include amides or ureas such as formamide, N,N-dimethylformamide, acetamide, N,N-dimethylacetamide, hexamethylphosphoramide, pyrrolidone, N-methylpyrrolidone, N,N,N',N'-tetramethylurea, N,N'-dimethyl-N,N'-trimethyleneurea, or a combination thereof; carbonates such as dimethyl carbonate, propylene carbonate, or a combination thereof; ethers such as tetrahydrofuran; sulfoxides and sulfones such as dimethyl sulfoxide, dimethyl sulfone, or a combination thereof; hindered alcohols such as tert-butyl alcohol; or a combination thereof. The lipophilic cation can include tetraalkylammonium or tetraarylammonium cations such as tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, tetrapentylammonium, tetrahexylammonium, tetraheptylammonium, tetraoctylammonium and mixtures of alkyl and aryl groups thereof, tetraarylphosphonium cations such as tetraphenylphosphonium, tetraalkylarsenic or tetraarylarsenic such as tetraphenylarsenic, and trialkylsulfonium cations such as trimethylsulfonium, or a combination thereof. The conversion of polynucleic acids into organic solvent-soluble materials by the exchange of metal cations with lipophilic cations can be performed by a variety of standard cation exchange techniques.

[0207] The polymer particles can be activated to promote conjugation with target analytes such as polynucleotides. For example, the functional groups on the cross-linked hydrogel polymer particles can be enhanced to allow binding to target analytes or analyte receptors. In a specific example, the functional groups of the polymer can be modified with reagents that can convert hydrophilic polymer functional groups into reactive moieties that can undergo nucleophilic or electrophilic substitution. In particular, where the polymer particles have carboxyl functional groups, they can be activated to promote conjugation, such as conjugation with biomolecules, such as nucleic acids.

[0208] In the embodiment that particle is formed with the comonomer that comprises hydroxyl, the hydroxyl group on the hydrophilic particle can be activated by replacing at least a portion of hydroxyl group with sulfonate group or chlorine.Exemplary sulfonate group can be derived from tresyl, methylsulfonyl, toluenesulfonyl or toluenesulfonyl chloride, or its arbitrary combination.Sulfonate can play the effect that allows nucleophilic reagent to replace sulfonate.Sulfonate can further provide chlorinated group with the chlorine reaction of release, and it can be used in the process of conjugated particle.In another example, the amine group on the hydrophilic polymer can be activated.

[0209] For example, a target analyte or analyte receptor can be bound to a hydrophilic polymer by nucleophilic substitution with a sulfonate group. In a specific example, a target analyte receptor terminated with a nucleophilic agent such as an amine or thiol can be nucleophilically substituted to replace the sulfonic acid group on the surface of the hydrophilic polymer. As a result of activation, conjugated particles can be formed.

[0210] In another example, where the particles are formed from monomers containing amines, the nucleophilic amino groups can be modified with difunctional di-electrophilic moieties (eg, diisocyanates or bis-NHS esters) to produce hydrophilic particles reactive toward nucleophiles.

[0211] When conjugated to a polynucleotide, the polymer particle may comprise at least 7×10 4 / μm 3 The density of polynucleotides is referred to as nucleotide density. For example, the nucleotide density can be at least 10 5 / μm 3 , such as at least 10 6 / μm 3 , at least 5×10 6 / μm 3 , at least 8×10 6 / μm 3 , at least 1×10 7 / μm 3 Or even at least 3×10 7 / μm 3 In another example, the nucleotide density may be no greater than 10 15 / μm 3 .

[0212] Such polymer particles can be used in a variety of separation techniques and analytical techniques. In particular, polymer particles can be used to bind polynucleotides. Such bound polynucleotides can be used to separate polynucleotides from solutions or can be used in analytical techniques, such as sequencing. Figure 5In the specific example shown, such polymer particles can be used as carriers of polynucleotides in sequencing techniques. For example, the particles can use fluorescent sequencing techniques to immobilize polynucleotides for sequencing. In another example, the polymer particles can use ion sensing techniques to immobilize multiple copies of polynucleotides for sequencing.

[0213] Typically, the polymer particles can be treated to contain biomolecules, including nucleosides, nucleotides, nucleic acids (oligonucleotides and polynucleotides), polypeptides, sugars, polysaccharides, lipids or derivatives or analogs thereof. For example, the polymer particles can be bound or attached to the biomolecule. The end or any internal portion of the biomolecule can be bound or attached to the polymer particles. The polymer particles can be bound or attached to the biomolecule using a connection chemistry. The connection chemistry includes covalent bonds or non-covalent bonds, including ionic bonds, hydrogen bonds, affinity bonds, dipole-dipole bonds, van der Waals bonds and hydrophobic bonds. Linking chemistries include affinity between binding partners, such as affinity between: an avidin portion and a biotin portion; an antigenic epitope and an antibody or immunoreactive fragment thereof; an antibody and a hapten; a digoxigen portion and an anti-digoxigenin antibody; a fluorescein portion and an anti-fluorescein antibody; an operator and a repressor; a nuclease and a nucleotide; a lectin and a polysaccharide; a steroid and a steroid binding protein; an active compound and an active compound receptor; a hormone and a hormone receptor; an enzyme and a substrate; an immunoglobulin and protein A; or an oligonucleotide or polynucleotide and its corresponding complement.

[0214] like Figure 5 As shown, a plurality of polymer particles 204 (e.g., monodisperse cross-linked hydrogel polymer particles of the present disclosure) can be placed in a solution together with a plurality of polynucleotides 202. The plurality of particles 204 can be activated or prepared to bind to the polynucleotides 202. For example, the particles 204 can include oligonucleotides that are complementary to a portion of the polynucleotides 202.

[0215] In a specific embodiment, polymer particles and polynucleotides carry out polymerase chain reaction (PCR) amplification.For example, dispersed phase droplet 206 or 208 is formed as a part of emulsion, and can include particles or polynucleotides.In an example, polynucleotide 202 and hydrophilic particles 204 are provided with low concentration and ratio relative to each other, so that single polynucleotide 202 may be located in the same dispersed phase droplet with single polymer particles 204.Other droplets, such as droplet 208, can include single polymer particles and do not include polynucleotides.Each droplet 206 or 208 can include enzymes, nucleotides, salts or other components that are enough to promote the replication of polynucleotides.Or, amplification techniques can be used, such as recombinase polymerase amplification (RPA) with or without emulsion.

[0216] In one aspect, the present invention provides use of the cross-linked hydrogel polymer particles of the present invention in nucleic acid amplification.

[0217] In an embodiment, the method for nucleic acid amplification comprises: performing a primer extension reaction on a polynucleotide hybridized to an oligonucleotide attached to a polymer particle. In an embodiment, the polymer particle is a monodisperse cross-linked hydrogel polymer particle of the present disclosure. In an embodiment, the method for nucleic acid amplification comprises: (a) providing a polymer particle attached to a single-stranded oligonucleotide (e.g., a primer oligonucleotide); (b) providing a single-stranded template polynucleotide; (c) hybridizing the single-stranded oligonucleotide with the single-stranded template polynucleotide; (d) contacting the single-stranded template polynucleotide with a polymerase and at least one nucleotide under conditions suitable for the polymerase to catalyze the polymerization of at least one nucleotide to the single-stranded oligonucleotide, thereby producing an extended single-stranded oligonucleotide. In an embodiment, the method further comprises: (e) removing (e.g., denaturing) the single-stranded template polynucleotide from the extended single-stranded oligonucleotide so that the single-stranded oligonucleotide remains attached to the polymer particle; (f) hybridizing the remaining single-stranded oligonucleotide with a second single-stranded template polynucleotide; and (g) contacting the second single-stranded template polynucleotide with a second polymerase and a second at least one nucleotide under conditions suitable for the second polymerase to catalyze the polymerization of the second at least one nucleotide onto the single-stranded oligonucleotide, thereby producing a subsequent extended single-stranded oligonucleotide. In an embodiment, steps (e), (f), and (g) may be repeated at least once. In an embodiment, the polymerase and the second polymerase comprise a thermostable polymerase. In an embodiment, conditions suitable for nucleotide polymerization comprise performing a nucleotide polymerization step (e.g., step (d) or (g)) at an elevated temperature. In an embodiment, conditions suitable for nucleotide polymerization comprise performing a nucleotide polymerization step (e.g., step (d) or (g)) at alternating temperatures (e.g., elevated temperature and relatively low temperature). In an embodiment, the alternating temperatures are in the range of 60-95°C. In embodiments, the temperature cycle can be from about 10 seconds to about 5 minutes, or about 10 minutes, or about 15 minutes or longer. In embodiments, the method for nucleic acid amplification can produce one or more polymer particles, each polymer particle is connected to a plurality of template polynucleotides, and the plurality of template polynucleotides include a sequence supplemented to a single strand template polynucleotide or to a second single strand template polynucleotide. In embodiments, each polymer particle can be connected to a plurality of single strand oligonucleotides (e.g., capture oligonucleotides). In embodiments, step (b), (c), (d), (e), (f) or (g) can be carried out with a plurality of single strand polynucleotides. In embodiments, at least a portion of a single strand oligonucleotide includes a nucleotide sequence supplemented to at least a portion of a single strand polynucleotide (or partially supplemented). In embodiments, the method for nucleic acid amplification (as described above) can be carried out in an aqueous solution in an oil phase (e.g., dispersed phase droplets).

[0218] After PCR, a particle is formed, such as particle 210, which may include multiple copies 214 of polymer particles 212 and polynucleotides. For clarity, most polynucleotides 214 are shown on the outer surface of particle 210. However, as also shown, polynucleotides may extend in particle 210 (or be located therein). For example, hydrogels and hydrophilic particles may have a low concentration of polymer relative to water, and may therefore be relatively porous. It may include polynucleotide fragments in the inside of particle 210 and on the entire particle 210, and polynucleotides may be located in pores and other openings. In particular, particle 210 may allow for the diffusion of enzymes, nucleotides, primers and reaction products for monitoring reactions. Polynucleotides with high numbers per particle produce better signals.

[0219] In embodiments, the polymer particles from the demulsification process can be collected and cleaned in preparation for sequencing. The collection can be carried out by contacting the biotin moiety (e.g., a polynucleotide template for an amplification connected to the polymer particles) with the avidin moiety and separating from the polymer particles lacking the biotinylated template. The collected polymer particles carrying the double-stranded template polynucleotide can be denatured to produce a single-stranded template polynucleotide for sequencing. The denaturation step can include treatment with an alkali (e.g., NaOH), formamide, or pyrrolidone.

[0220] Sequencing can be performed by detecting nucleotide addition. Nucleotide addition can be detected using methods such as fluorescence emission methods or ion detection methods. For example, a group of fluorescently labeled nucleotides can be provided to system 216 and can migrate to well 218. Excitation energy can also be provided to well 218. When nucleotides are captured by polymerase and added to the end of the extension primer, the label of the nucleotide can fluoresce, indicating which type of nucleotides have been added. These and other sequencing methods described herein can be combined with methods for nucleic acid amplification. For example, in the method for nucleic acid amplification described with steps (a)-(g), the method can include a step (h) of sequencing by detecting nucleotide addition.

[0221] In an alternative example, solutions including a single type of nucleotide may be fed sequentially. In response to the addition of nucleotides, the pH in the local environment of well 218 may change. This pH change may be detected by an ion-sensitive field effect transistor (ISFET). Thus, the change in pH may be used to generate a signal indicating the order of nucleotides complementary to the polynucleotide of particle 210.

[0222] In particular, the sequencing system can include one or more wells disposed on an entire sensor plate of an ion sensor, such as a field effect transistor (FET). In embodiments, the system includes one or more polymer particles loaded into a well disposed on a sensor plate of an ion sensor, such as a FET, or one or more polymer particles loaded into a plurality of wells disposed on a sensor plate of an ion sensor, such as a FET. In embodiments, the FET can be a chemFET or an ISFET. "ChemFETs" or chemical field effect transistors include types of field effect transistors that act as chemical sensors. A chemFET has a structural analogue of a MOSFET transistor, in which the charge on the gate electrode is applied chemically. "ISFETs" or ion sensitive field effect transistors can be used to measure ion concentrations in a solution; when the ion concentration (such as H + ) changes, the current through the transistor changes accordingly.

[0223] Back to Figure 5 In one example, the wells 218 of the well array can be operably connected to a measuring device. For example, for a fluorescence emission method, the wells 218 can be operably coupled to a light detection device. In the case of ion detection, the lower surface of the wells 218 can be disposed on the entire sensor plate of an ion sensor such as a field effect transistor (e.g., chemFET).

[0224] An exemplary system involving sequencing by detecting ionic byproducts of nucleotide incorporation is the Ion Torrent PGM TM or Proton TM Sequencer (Life Technologies), which is an ion-based sequencing system that sequences nucleic acid templates by detecting hydrogen ions produced as a byproduct of nucleotide binding. Typically, hydrogen ions are released as a byproduct of nucleotide binding produced during template-dependent nucleic acid synthesis by a polymerase. IonTorrent PGM TM or Proton TM The sequencer detects nucleotide incorporation by detecting the hydrogen ion byproduct of nucleotide incorporation. Ion Torrent PGM TM or Proton TM The sequencer may include a plurality of template polynucleotides to be sequenced, each template being placed in a corresponding sequencing reaction well in the array. The wells of the array may each be coupled to at least one ion sensor, which may detect H + The ion sensor includes a field effect transistor (FET) coupled to an ion-sensitive detection layer, which can sense H +The presence of ions or a change in solution pH. The ion sensor can provide an output signal indicative of nucleotide binding, which can be expressed as a voltage change whose magnitude is proportional to the H in the corresponding pore or reaction chamber. + Different nucleotide types can flow into the reaction chamber continuously and can be bound to the extension primer (or polymerization site) by the polymerase in an order determined by the template sequence. Each nucleotide binding can be accompanied by a H + The release of ions, accompanied by changes in local pH. + The release of ions can be recorded by the sensor's FET, which generates a signal indicating that nucleotide binding has occurred. Nucleotides that are not bound during a particular nucleotide flow may not generate a signal. The amplitude of the signal from the FET can also be related to the number of nucleotides of a particular type in the nucleic acid molecule that binds the extension, thereby allowing the resolution of homopolymer regions. Therefore, during the sequencer run, multiple nucleotides flow into the reaction chamber, and the binding monitoring across multiple holes or reaction chambers can allow the instrument to resolve the sequences of many nucleic acid templates at the same time.

[0225] Another sequencing system is Applied Biosystems' SOLiD TM Sequencing system (sequencing by oligonucleotide ligation and detection) that uses step-by-step cyclic ligation for high-throughput DNA sequencing. In this bead-based system, beads (i.e., polymer particles) loaded with DNA templates undergo sequential ligation and cleavage reactions using 4-color fluorescently labeled octamer probes. These probes are continuously transmitted and used to query dinucleotide positions on the DNA chain. It is hoped that higher bead density can be supported to promote the increase in the number of bead events per instrument run and the improvement of probe chemistry, thereby improving sequencing fidelity.

[0226] Sequencing by oligonucleotide ligation and detection involves attaching a nucleic acid target to cross-linked polymer particles (beads) followed by immobilization of multiple particles to a surface. Each nucleic acid-bead conjugate contains a unique DNA sequence, and this type of sequencing technology is disclosed in International Publication No. WO 2006 / 084132 A2 (incorporated herein by reference).

[0227] The method of linking beads to a support uses a flat glass microscope slide that is irreversibly coated with streptavidin. The beads carrying the nucleic acid are contacted with biotinylated nucleotides (e.g., obtained by the action of biotinylated dNTP's and terminal deoxytransferase on a DNA target after linking to the beads). The biotinylated beads are incubated with the streptavidin-coated slide so that the beads are fixed to the slide through the interaction of streptavidin with biotin. Kinetically, this is a very efficient linking scheme, and movement of beads on the slide is sometimes observed under the conditions required for DNA sequencing. When the beads are present on the slide at high density (e.g., up to 100,000 beads / mm 2 ) and are queried multiple times (e.g., up to 25 times), any significant bead motion can prevent strong identification of a specific bead in subsequent scans within a dense bead population.

[0228] Thus, US 2009 / 0099027 (equivalent to WO 2009 / 026546, both of which are incorporated herein by reference) describes a covalent system for bead immobilization that reduces the movement of beads during sequencing and other forms of genetic analysis. The method comprises: reacting a nucleophilic group on a substrate surface with a molecule comprising a plurality of electrophilic groups, thereby providing one or more free electrophilic groups on the substrate surface; and reacting a nucleophilic group on a particle material surface with the one or more free electrophilic groups on a substrate surface to covalently link the particle material to the substrate.

[0229] US 2009 / 0099027 describes the modification of nucleophilic (more particularly amino-functional) surfaces with multifunctional electrophiles. For example, the electrophilic surface of a silicate glass microscope slide can be easily converted into a nucleophilic surface by reacting the surface groups with (aminopropyl)trialkoxysilanes.

[0230] DNA target nucleic acids that have been covalently attached to cross-linked polymer beads can be modified after attachment to the beads by aminoalkyl dNTP's and terminal deoxytransferase acting on the DNA target. The nucleophilic amino groups on the DNA target can then react with the residual electrophilic groups on the support surface to form multiple stable covalent bonds between the beads and the glass surface.

[0231] It has been found that stable covalent bonds can be formed between surfaces containing electrophilic groups and particles containing nucleophilic groups. Additionally, beads containing nucleophilic amino groups from the action of amino-dNTP's and terminal deoxytransferases on DNA targets can be immobilized on modified surfaces under alkaline conditions. For example, surfaces containing amino groups that have been activated with benzene 1,4-diisothiocyanate can be used to immobilize beads with nucleophilic groups. Additionally, the covalent attachment appears to be quite stable and no bead movement has been observed.

[0232] Surface-immobilized beads can be used in methods for analyzing nucleic acid sequences based on repeated cycles of double-stranded extension along a single-stranded template by ligation. This type of sequencing method is disclosed in U.S. Pat. Nos. 5,750,341; 5,969,119; and 6,306,597 B1 and International Publication No. WO 2006 / 084132 A2. Each of these publications is incorporated herein by reference in its entirety. In addition, the techniques described in the aforementioned publications can be used to analyze (e.g., sequence) nucleic acid templates that are attached to particles attached to a carrier as described herein. Immobilized beads can be used in sequencing methods that do not necessarily employ a ligation step, such as sequencing using labeled nucleotides with removable blocking groups that prevent polynucleotide chain extension (e.g., U.S. Pat. Nos. 6,664,079; 6,232,465; and 7,057,026, each of which is incorporated herein by reference in its entirety). Immobilized beads can be used in a variety of techniques in which the signal on the beads is repeatedly detected through multiple cycles.

[0233] The beads for SOLiD sequencing can be monodisperse cross-linked hydrogel particles of the present disclosure. Therefore, one embodiment includes using the monodisperse particles in the method and product disclosed in the publication mentioned in the previous paragraph, and the applicant of the present application believes that all these uses, methods and products fall into the present invention, and reserves the right to claim. Submicron particles are used in SOLiD sequencing to enable particles of greater density to be connected to glass surfaces (such as glass panels or microscope slides). Also included in one embodiment is a method for implementing SOLiD sequencing, which uses monodisperse particles of the present disclosure, such as wherein the monodisperse submicron of the present disclosure is coupled to nucleic acid targets and fixed on the surface, such as glass surfaces. The immobilization method is not important, and can be covalent or non-covalent, and the example of non-covalent coupling is to be combined by streptavidin / avidin-biotin. Covalent coupling can be, for example, as described in US 2009 / 0099027 and WO2009026546, but any other technology suitable for covalent coupling can be used. Thus, included in one embodiment is a method of forming a product (article of manufacture) comprising coupling the monodisperse submicron particles of the present disclosure to a nucleic acid, and optionally further comprising immobilizing the resulting nucleic acid-loaded particles on a surface, such as a glass surface. The nucleic acid can be used as a target in sequencing, such as using SOLiD sequencing.

[0234] For example, a method is provided, comprising:

[0235] (a) hybridizing a first initializing oligonucleotide probe to a target polynucleotide to form a probe-target duplex, wherein the oligonucleotide probe has an extendable probe end, wherein the target polynucleotide is attached to a polymer particle, the polymer particle is a member of a polymer population as disclosed herein, and wherein the particle is covalently attached to a surface of a solid support;

[0236] (b) ligating a first end of an extension oligonucleotide probe to the extendable probe end, thereby forming an extension duplex containing the extension oligonucleotide probe, wherein the extension oligonucleotide probe comprises a cleavage site and a detectable label;

[0237] (c) identifying one or more nucleotides in the target polynucleotide by detecting the label attached to the just-attached extended oligonucleotide probe;

[0238] (d) cleaving the just-ligated extended oligonucleotide probe at the cleavage site to generate an extendable probe end, wherein the cleavage removes a portion of the just-ligated extended oligonucleotide probe that includes the label from the probe-target duplex; and

[0239] (e) Repeating steps (b), (c) and (d) until the nucleotide sequence in the target polynucleotide is determined.

[0240] Also provided is a method for sequencing a nucleic acid, comprising:

[0241] (a) hybridizing a primer to a target polynucleotide to form a primer-target duplex, wherein the target polynucleotide is attached at the 5' end to a polymer particle, the polymer particle being a member of a polymer particle population as disclosed herein, and wherein the polymer particle is covalently attached to the surface of a support;

[0242] (b) contacting the primer-target duplex with a polymerase and one or more different nucleotide analogs to bind the nucleotide analogs to the 3' end of the primer, thereby forming an extended primer chain, wherein the bound nucleotide analogs terminate the polymerase reaction, and wherein each of the one or more nucleotide analogs comprises (i) a base selected from adenine, guanine, cytosine, thymine and uracil and analogs thereof; (ii) a unique tag attached to the base or its analog via a cleavable linker; (iii) a deoxyribose sugar; and (iv) a cleavable chemical group that blocks the -OH group at the 3'-position of the deoxyribose sugar;

[0243] (c) washing the support surface to remove any unbound nucleotide analogs;

[0244] (d) detecting the unique label attached to the just-bound nucleotide analog, thereby identifying the just-bound nucleotide analog;

[0245] (e) optionally, permanently capping any unreacted -OH groups on the extended primer strand;

[0246] (f) cleaving the cleavable linker between the just-bound nucleotide analog and the unique tag;

[0247] (g) cleaving the chemical group that blocks the -OH group at the 3'-position of the deoxyribose of the nucleotide analog just bound, thereby unblocking the -OH group;

[0248] (h) washing the support surface to remove the cleavage compound;

[0249] (i) Repeat steps (b)-(h).

[0250] The polymer particles of the present disclosure can be used in any nucleic acid sequencing method involving polymer particles. One embodiment includes particles of the present disclosure coupled to nucleic acids and methods for sequencing nucleic acids, which include coupling nucleic acids to a population of particles of the present disclosure. The nucleic acids can be DNA or RNA.

[0251] The present disclosure includes products (e.g., articles) comprising a plurality of monodisperse particles of the present disclosure, which are coupled to a substrate, such as a glass surface, for example, by streptavidin-biotin connection, avidin-biotin connection, or by covalent bonds, such as described in US 2009 / 0099027 and WO2009 / 026546. The particles can be coupled to the substrate by nucleic acids. The present disclosure includes the use of monodisperse submicron particles of the present disclosure to manufacture such products. One embodiment includes connecting the monodisperse submicron particles of the present disclosure to a substrate using the connection chemistry described in US 2009 / 0099027 and WO2009 / 026546, and the applicant reserves the right to claim methods using such chemistry and its products. Therefore, this specification includes the disclosures of US2009 / 0099027 and WO2009026546 by reference.

[0252] Thus, embodiments include methods in which the functionalized monodisperse polymer particles of the present disclosure undergo one or more further reactions to obtain the desired products. Other embodiments include the use of these products in applications.

[0253] In view of the consistency of quality and properties that the particles of the present disclosure may have, they can be used in methods including the implementation of processes related to conjugated substances, such as substances selected from markers, biomolecules and biostructures, such as biomolecules such as amino acids, sugars, nucleotides and nucleosides and polymers made by condensing two or more such monomers together, such as polypeptides, proteins, polysaccharides, oligonucleotides and nucleic acids. As markers, dyes such as fluorescent dyes, quenchers, enzymes and semiconductor nanocrystals can be mentioned. Embodiments of the present invention include such uses as well as:

[0254] (i) a conjugate comprising a population of particles of the present disclosure, at least a portion of which is coupled to a conjugated substance, such as those just described

[0255] (ii) a method comprising coupling at least a portion of the particle population of the present disclosure to a substance, such as those just described

[0256] (iii) A method comprising coupling at least a portion of a population of particles of the present disclosure to a substrate.

[0257] The present invention includes the following embodiments:

[0258] 1. Monodisperse cross-linked hydrogel polymer particles comprising a polymer formed from:

[0259] (a)log P oct / wat A hydrophilic vinyl monomer having a (log P) of less than about 1;

[0260] as well as

[0261] (b) A cross-linking agent comprising at least two vinyl groups.

[0262] 2. The polymer particles of claim 1, wherein the hydrophilic vinyl monomer has a log P of less than about 0.6, optionally wherein the log P is less than about 0.3, further optionally wherein the log P is less than about 0.

[0263] 3. The polymer particle of item 1 or item 2, wherein the hydrophilic vinyl monomer has a log P of 0.5 to -2, optionally wherein the log P is 0 to -2.

[0264] 4. The polymer particles of any one of the preceding items, wherein the hydrophilic vinyl monomer is an acrylamide monomer and / or an acrylate monomer.

[0265] 5. The polymer particle of any of the preceding items, wherein the hydrophilic vinyl monomer comprises at least one compound of formula (I):

[0266]

[0267] in:

[0268] R 1 -H, -CH 3 or -CH 2 CH 3 ;

[0269] R 2 For-OR 3 or -N(R 4 )R 5 ;

[0270] R 3 -H, -C 1 -C 6 Alkyl or -C 1 -C 6 Alcohol; and

[0271] R 4 and R 5 are independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Haloalkyl, -C 1 -C 6 alcohol,

[0272] Where chemically possible, R 3 and / or R 4 and / or R 5 are optionally substituted independently by 1 to 5 substituents selected independently in each case from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 Ra C(O)R a ,CONR a R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a is independently selected from: H and C 1 -C 4 alkyl.

[0273] 6. The polymer particles of item 5, wherein R 1 -H or -CH 3 , optionally wherein R 1 is -H.

[0274] 7. The polymer particles of item 5 or item 6, wherein R 2 For-OR 3 .

[0275] 8. The polymer particles according to any one of items 5 to 7, wherein R 3 is -H.

[0276] 9. The polymer particles according to any one of items 5 to 8, wherein R 4 -H or -C 1 -C 6 Alkyl, optionally wherein R 4 is -H.

[0277] 10. The polymer particles of any one of items 5 to 9, wherein R 5 Can be -H or -C 1 -C 6 Alkyl, optionally wherein R 5 is -H.

[0278] 11. The polymer particle of any of the preceding items, wherein the hydrophilic vinyl monomer is selected from or comprises at least one acrylamide monomer, acrylic acid monomer, methacrylamide monomer or methacrylic acid monomer.

[0279] 12. The polymer particles of any of the preceding items, wherein the hydrophilic vinyl monomer is selected from or includes acrylamide, hydroxymethyl acrylamide, hydroxyethyl acrylamide, [tris(hydroxymethyl)methyl] acrylamide, 3-acrylamidopropionic acid, methacrylamide, 2-hydroxyethyl methacrylamide, (3-aminopropyl) methacrylamide, or 2-hydroxyethyl acrylate; optionally wherein the hydrophilic vinyl monomer is selected from or includes at least one of acrylamide (prop-2-enamide), hydroxymethyl acrylamide, hydroxyethyl acrylamide, trishydroxymethyl methacrylamide, 2-hydroxyethyl methacrylate and acrylic acid.

[0280] 13. The polymer particle of any of the preceding items, wherein the hydrophilic vinyl monomer comprises a primary amide group (-C(O)NH 2 ).

[0281] 14. The polymer particle of any preceding item, wherein the crosslinker is a difunctional, trifunctional or tetrafunctional acrylamide, optionally wherein the crosslinker is a difunctional acrylamide.

[0282] 15. The polymer particle of any of the preceding items, wherein the crosslinking agent comprises at least one compound of formula (IIa) or (IIb):

[0283]

[0284] Where R 6 Selected from -C 1 -C 6 Alkyl-, -C 1 -C 6 Heteroalkyl, -C 1 -C 6 Cycloalkyl-, -C 1 -C 6 Hydroxyalkyl-, -C 1 -C 6 Ether - or containing 2 to 100 C 2 -C 3 Polyethers of ether units;

[0285] R 7 and R 8 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Heteroalkyl, -C 3 -C 6 Cycloalkyl, -C 1 -C 6 Hydroxyalkyl or -C 1 -C 6 ether;

[0286] R 9 -N(R 11 )C(O)CH=CH 2 ;

[0287] R 10 Selected from -H and -N(R 12 )C(O)CH=CH 2 ;as well as

[0288] R 11 and R 12 Each independently selected from -H, -C 1 -C 6 Alkyl, -C 1 -C 6 Heteroalkyl, -C 3 -C 6 Cycloalkyl, -C 1 -C 6 Hydroxyalkyl or -C 1 -C 6 ether;

[0289] Optionally wherein, where chemically possible, R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 One or more of the following are independently substituted by 1 to 5 substituents, each independently selected from the following: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O) 2 R a NR a CONR a R a NR a CO 2 R a , OR a SR a 、S(O)R a 、S(O) 2 OR a 、S(O) 2 R a 、S(O) 2 NR a R a , CO 2 R a C(O)R a ,CONRa R a , C 1 -C 4 -alkyl, C 2 -C 4 -Alkenyl, C 2 -C 4 -Alkynyl, C 1 -C 4 haloalkyl; wherein R a In each case, independently selected from: H, C 1 -C 4 Alkyl and C 1 -C 4 Alkenyl.

[0290] 16. The compound of item 15, wherein R 6 Selected from -C 1 -C 6 Alkyl-, -C 1 -C 6 Hydroxyalkyl- and containing 2 to 100 C 2 -C 3 ether units, optionally wherein R 6 Selected from -C 1 -C 6 Alkyl- and -C 1 -C 6 Hydroxyalkyl-, further optionally wherein R 6 For -C 1 -C 6 Hydroxyalkyl-.

[0291] 17. The compound of item 15 or item 16, wherein R 6 Selected from -CH 2 -、-(CH 2 ) 2 -、-(CH 2 ) 3 -or-(CH 2 ) 4 -, optionally wherein R 6 For -(CH 2 ) 2 -.

[0292] 18. The compound of any one of items 15 to 17, wherein R 6 Selected from -C(OH)H-, -(C(OH)H) 2 -、-(C(OH)H) 3 -or-(C(OH)H) 4 -, optionally wherein R 6 -(C(OH)H) 2 -.

[0293] 19. The compound of item 15 or item 16, wherein R 6 for (CH 2 ) r (OCH 2 CH 2 ) n O(CH 2 ) s , wherein r and s are each independently 2 or 3, and n is an integer from 1 to 100.

[0294] 20. The compound of item 19, wherein r and s are each 2 and n is an integer from 1 to 50.

[0295] 21. The polymer particle of any one of items 15 to 20, wherein R 7 and / or R 8 For H.

[0296] 22. The polymer particle of any of the preceding items, wherein the crosslinking agent has a log P value of less than about 1, optionally a log P value of less than about 0.5, further optionally a log P value of less than about 0.

[0297] 23. The polymer particles of any of the preceding items, wherein the crosslinker is or includes N,N'-(1,2-dihydroxyethylene)bisacrylamide, N,N'-methylenebis(acrylamide), N,N'-ethylenebis(acrylamide), glycerol 1,3-diglyceride diacrylate, piperazine diacrylamide, N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide, polyethylene glycol diacrylamide (MW≤2000), 4-arm PEG-acrylamide (MW≤2000) and / or N,N-bis(2-acrylamidoethyl)acrylamide.

[0298] 24. The polymer particle of any preceding clause, wherein the crosslinker is or comprises 1,2-dihydroxybisacrylamide.

[0299] 25. The polymer particle of any of the preceding items, wherein the crosslinker is or comprises N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide, polyethylene glycol diacrylamide (MW≤2000) and 4-arm PEG-acrylamide (MW≤2000), optionally wherein the crosslinker is or comprises N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide.

[0300] 26. The polymer particle of any preceding clause, wherein the crosslinker does not comprise a primary amine, a secondary amine, a hydroxyl group or a carboxylic acid.

[0301] 27. The polymer particle of any of the preceding items, wherein the crosslinking level is 1-60 wt% crosslinker, optionally 1-30 wt% crosslinker; or wherein the crosslinking level is 10-90 wt% crosslinker, optionally 25-60 wt% crosslinker.

[0302] 28. The polymer particles of any one of items 1 to 3, wherein the hydrophilic vinyl monomer is a cross-linking agent as defined in any one of items 14 to 26.

[0303] 29. The polymer particle of any preceding item, wherein the polymer particle is porous.

[0304] 30. The polymer particles of any of the preceding items, wherein the polymer particles have an average diameter of from 0.5 μm to 10 μm, optionally from 0.5 μm to 5 μm.

[0305] 31. The polymer particle of any preceding item, wherein the coefficient of variation (CV) is less than 20%, optionally wherein the CV is less than 15%.

[0306] 32. The polymer particle of any preceding item, wherein the particle comprises an oligonucleotide attached to the particle.

[0307] 33. The polymer particle of any preceding item, wherein each said particle comprises a plurality of oligonucleotides attached to said particle, optionally wherein said plurality of oligonucleotides are identical for each individual particle.

[0308] 34. Monodisperse seed particles having a Z-average diameter of 100 nm to 1500 nm, wherein each seed particle comprises a plurality of non-crosslinked oligomers of poly-N,N-dimethylacrylamide.

[0309] 35. The seed particle of claim 34, wherein the weight average molecular weight (Mw) of the oligomer is from 2,000 Da to 100,000 Da.

[0310] 36. The seed particle of item 34 or 35, wherein the Mw of the oligomer is 5,000Da to 70,000Da; optionally 6,000Da to 40,000Da; further optionally 7,000Da to 50,000Da or 8,000Da to 40,000Da.

[0311] 37. The seed particle of any one of items 34 to 36, wherein the particle has the characteristics of a seed particle formed by free radical initiated polymerization of N,N-dimethylacrylamide in an organic solvent in the presence of a stabilizer and a chain transfer agent.

[0312] 38. Use of the seed particles of any one of items 34 to 37 for forming monodisperse cross-linked hydrogel polymer particles, optionally wherein the monodisperse cross-linked hydrogel polymer particles are cross-linked polyacrylamide particles.

[0313] 39. The use of item 38, wherein the monodisperse cross-linked hydrogel polymer particles are further defined as in any one of items 1 to 33.

[0314] 40. A method of forming monodisperse seed particles, comprising:

[0315] dissolving N,N-dimethylacrylamide, a stabilizer, a free radical initiator, and a chain transfer agent in an organic solvent to form a reaction mixture; and

[0316] The reaction mixture is heated to activate the initiator.

[0317] Thus, monodisperse seed particles are formed.

[0318] 41. The method of claim 40, wherein the stabilizer is a block copolymer of styrene and a polyolefin, optionally wherein the stabilizer is a triblock copolymer consisting of a poly(ethylene-co-butylene) midblock and polystyrene outer blocks.

[0319] 42. The method of claim 40 or claim 41, wherein the stabilizer is selected from or includes Kraton A1535H, Kraton G1650M, Kraton G1652M or Kraton G1657M.

[0320] 43. The method of any one of items 40 to 42, wherein the free radical initiator is a peroxide initiator or an azo initiator.

[0321] 44. The method of any one of items 40 to 43, wherein the free radical initiator is selected from 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dibenzoyl peroxide, optionally wherein the free radical initiator is 2,2'-azobis(2-methylpropionitrile).

[0322] 45. The method of any one of items 40 to 44, wherein heating the reaction mixture to activate the initiator comprises heating to at least 40°C, optionally heating to at least 50°C, further optionally heating to at least 60°C.

[0323] 46. ​​The process of any one of items 40 to 45, wherein the chain transfer agent is a mercaptan or a haloalkane, optionally wherein the chain transfer agent is an alkyl mercaptan.

[0324] 47. The process of any one of items 40 to 46, wherein the chain transfer agent is selected from 1-octanethiol, hexanethiol, 6-mercapto-1-hexanol, benzyl mercaptan, carbon tetrachloride and bromotrichloromethane.

[0325] 48. The process of any one of items 40 to 47, wherein the chain transfer agent is 1-octanethiol.

[0326] 49. The process of any one of items 40 to 48, wherein the organic solvent comprises a mixture of an alkane component and an aromatic component.

[0327] 50. The method of claim 49, wherein the alkane component and the aromatic component are present in a weight ratio of alkane component:aromatic component of about 0.5:1 to about 20:1, optionally wherein the weight ratio of alkane component:aromatic component is about 1:1 to about 10:1.

[0328] 51. The process of claim 49 or claim 50, wherein the alkane component is heptane and the aromatic component is toluene.

[0329] 52. The method of any one of items 40 to 51, wherein the reaction mixture comprises:

[0330] N,N-dimethylacrylamide in an amount from about 2 wt % to about 5 wt %;

[0331] a stabilizer in an amount from about 1 wt % to about 5 wt %;

[0332] a free radical initiator in an amount from about 0.01 wt % to about 4 wt %; and

[0333] Chain transfer agents are present in amounts ranging from about 0.05 wt % to about 0.25 wt %.

[0334] 53. The method of claim 52, wherein the weight % of the N,N-dimethylacrylamide is greater than the weight % of the stabilizer.

[0335] 54. The method of any one of items 40 to 53, wherein the reaction mixture is purged of oxygen prior to heating the reaction mixture.

[0336] 55. The method of claim 54, wherein the oxygen removal comprises sparging with a chemically inert gas, optionally wherein the chemically inert gas is selected from argon, helium or nitrogen.

[0337] 56. A method of forming monodisperse cross-linked hydrogel polymer particles comprising:

[0338] forming a solution (a) of at least 2 wt. % of a hydrophilic vinyl monomer in aqueous solution, the solution further comprising a crosslinking agent having at least two vinyl groups;

[0339] forming a solution (b) of a stabilizer in an organic solvent, wherein the organic solvent is immiscible with water and wherein at least one of the solution (a) and the solution (b) comprises a free radical initiator; mixing the solutions (a) and (b) to form a water-in-oil emulsion (c) and adding monodisperse seed particles to the emulsion;

[0340] causing monodisperse seed particles to form swollen particles in an emulsion; and

[0341] The swollen particles are polymerized to form monodisperse cross-linked hydrogel polymer particles.

[0342] 57. The method of item 56, wherein the hydrophilic vinyl monomer is further defined as in any one of items 1 to 13 or 28.

[0343] 58. The method of item 56 or 57, wherein the cross-linking agent is further defined as in any one of items 14 to 26.

[0344] 59. The method of any one of items 56 to 58, wherein the stabilizer is a nonionic surfactant, optionally wherein the nonionic surfactant is a nonionic polymeric surfactant.

[0345] 60. The method of claim 59, wherein the nonionic polymeric surfactant comprises at least one polyoxyethylene group or at least one polyoxypropylene group.

[0346] 61. The method of claim 59 or 60, wherein the stabilizer comprises at least one polyoxyethylene group.

[0347] 62. The method of any one of items 59 to 61, wherein the nonionic polymeric surfactant is an oligomeric surfactant.

[0348] 63. The method of any one of items 56 to 62, wherein the stabilizer is selected from hypermer 2296, Abil EM90 and sorbitan monooleate.

[0349] 64. The method of any one of items 56 to 63, wherein the free radical initiator is a peroxide initiator or an azo initiator.

[0350] 65. The method of any one of items 56 to 64, wherein the free radical initiator is 2,2'-azobis-2,4-dimethylvaleronitrile.

[0351] 66. The method of any one of items 56 to 65, wherein the organic solvent comprises at least one of an aliphatic hydrocarbon, an aliphatic carbonate, an aliphatic ester, an aliphatic ether, an aromatic hydrocarbon or a silicone, or a combination thereof.

[0352] 67. The process of any one of items 56 to 66, wherein the organic solvent comprises a mixture of heptane and toluene; a mixture of aliphatic hydrocarbons; bis(2-ethylhexyl) carbonate, optionally mixed with aliphatic and aromatic hydrocarbons; or bis(2-ethylhexyl) adipate.

[0353] 68. The method of any one of items 56 to 67, wherein the monodisperse seed particles have the characteristics of monodisperse seed particles formed according to the method of any one of items 40 to 55.

[0354] 69. The method of any one of items 56 to 67, wherein the monodisperse seed particles are formed according to the method of any one of items 40 to 55.

[0355] 70. The process of any one of items 56 to 69, wherein solution (a) comprises not more than 60% by weight of the hydrophilic vinyl monomer.

[0356] 71. The method of any one of items 56 to 70, wherein solution (a) comprises at least 2 weight percent of hydrophilic vinyl monomers and no more than 60 weight percent of hydrophilic vinyl monomers, optionally wherein solution (a) comprises at least 5 weight percent of hydrophilic vinyl monomers and no more than 45 weight percent of hydrophilic vinyl monomers.

[0357] 72. The process of any one of items 56 to 71, wherein solution (a) comprises about 10% by weight of the hydrophilic vinyl monomer.

[0358] 73. The method of any one of items 56 to 72, wherein the initiator is present in the emulsion in an amount of about 0.1 wt % to about 1.5 wt %, optionally wherein the initiator is present in the emulsion in an amount of about 0.6 wt % to about 1.2 wt %, further optionally wherein the initiator is present in the emulsion in an amount of about 0.8 wt %.

[0359] 74. The method of any one of items 56 to 72, wherein the polymerization comprises activating the free radical initiator.

[0360] 75. The method of claim 74, wherein activating the free radical initiator comprises heating the emulsion comprising the swollen particles, optionally wherein the heating comprises heating to a temperature of at least 40°C.

[0361] 76. The method of any one of items 56 to 75, wherein the step of allowing the monodisperse seed particles to form swollen particles is carried out for at least 30 minutes, optionally at least 1 hour.

[0362] 77. The method of any one of items 56 to 76, wherein the step of forming the monodisperse seed particles into swollen particles comprises mixing the emulsion, optionally wherein the mixing is carried out at a temperature not exceeding 30°C, optionally wherein the mixing is carried out at a temperature of about 15°C to about 25°C.

[0363] 78. A method of forming monodisperse cross-linked hydrogel polymer particles comprising:

[0364] forming a solution (a) of at least 2 weight percent of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution further comprising a chain transfer agent;

[0365] forming a solution (b) of the stabilizer in an organic solvent, wherein the organic solvent is immiscible with water, and wherein at least one of the solution (a) and the solution (b) comprises a free radical initiator;

[0366] mixing solutions (a) and (b) to form a water-in-oil emulsion (c) and adding monodisperse seed particles to the emulsion;

[0367] causing monodisperse seed particles to form swollen particles in an emulsion;

[0368] polymerizing the swollen particles to form monodisperse polymer particles;

[0369] forming a solution (d) of the stabilizer in an organic solvent, wherein the organic solvent is immiscible with water;

[0370] forming a solution (e) of at least 2 wt. % of a hydrophilic vinyl monomer in an aqueous solution, the aqueous solution further comprising a crosslinker containing at least two vinyl groups, wherein at least one of the solution (d) and the solution (e) comprises a free radical initiator;

[0371] mixing solutions (d) and (e) to form a water-in-oil emulsion (f) and adding monodisperse polymer particles to the emulsion;

[0372] causing monodisperse polymer particles to form swollen polymer particles in the emulsion; and

[0373] The swollen polymer particles are polymerized to form monodisperse cross-linked hydrogel polymer particles.

[0374] 79. The method of item 78, wherein the hydrophilic vinyl monomer of solution (a) is further defined as in any one of items 1 to 13.

[0375] 80. The method of item 78 or item 79, wherein the hydrophilic vinyl monomer of solution (e) is further defined as in any one of items 1 to 13 or 28; optionally wherein the hydrophilic vinyl monomers of solution (a) and solution (e) are the same.

[0376] 81. The method of any one of items 78 to 80, wherein the cross-linking agent is further defined as in any one of items 14 to 26.

[0377] 82. The method of any one of items 78 to 82, wherein each stabilizer is a nonionic surfactant, optionally wherein each nonionic surfactant is a nonionic polymeric surfactant.

[0378] 83. The method of claim 82, wherein the nonionic polymer surfactant comprises at least one polyoxyethylene group or at least one polyoxypropylene group.

[0379] 84. The method of claim 82 or 83, wherein each stabilizer comprises at least one polyoxyethylene group.

[0380] 85. The method of any one of items 82 to 84, wherein each nonionic polymeric surfactant is an oligomeric surfactant.

[0381] 86. The method of any one of items 78 to 85, wherein each stabilizer is selected from Hypermer 2296, Abil WE09 or AMBN and Abil EM90.

[0382] 87. The process of any one of items 78 to 86, wherein the chain transfer agent is selected from a mercaptan or a haloalkane, optionally wherein the chain transfer agent is a thiopolyol.

[0383] 88. The method of any one of items 78 to 87, wherein the chain transfer agent is selected from 1-thioglycerol, 1-octanethiol, hexanethiol, 6-mercapto-1-hexanol, benzyl mercaptan, carbon tetrachloride and bromotrichloromethane; optionally wherein the chain transfer agent is 1-thioglycerol.

[0384] 89. The method of any one of items 78 to 88, wherein the free radical initiator is a peroxide initiator or an azo initiator.

[0385] 90. The method of any one of items 78 to 89, wherein the free radical initiator is 2,2'-azobis-2,4-dimethylvaleronitrile and / or 2,2'-azobis(2-methylbutyronitrile) (AMBN).

[0386] 91. The method of any one of items 78 to 90, wherein the organic solvent comprises at least one of an aliphatic hydrocarbon, an aliphatic carbonate, an aliphatic ester, an aliphatic ether, an aromatic hydrocarbon or a silicone, or a combination thereof.

[0387] 92. The process of any one of items 78 to 91, wherein the organic solvent comprises a mixture of heptane and toluene; a mixture of aliphatic hydrocarbons; bis(2-ethylhexyl) carbonate, optionally mixed with aliphatic and aromatic hydrocarbons; or bis(2-ethylhexyl) adipate.

[0388] 93. The method of any one of items 78 to 92, wherein the monodisperse seed particles have the characteristics of monodisperse seed particles formed according to the method of any one of items 40 to 55.

[0389] 94. The method of any one of items 78 to 92, wherein the monodisperse seed particles are formed according to the method of any one of items 40 to 55.

[0390] 95. The process of any one of items 78 to 94, wherein solution (a) and / or solution (e) comprises not more than 60% by weight of a hydrophilic vinyl monomer.

[0391] 96. The method of any one of items 78 to 95, wherein solution (a) and / or solution (e) comprises at least 2 weight percent of hydrophilic vinyl monomers and no more than 60 weight percent of hydrophilic vinyl monomers, optionally wherein solution (a) and / or solution (e) comprises at least 5 weight percent of hydrophilic vinyl monomers and no more than 45 weight percent of hydrophilic vinyl monomers.

[0392] 97. The process of any one of items 78 to 96, wherein solution (a) and / or solution (e) comprises about 10% by weight of a hydrophilic vinyl monomer.

[0393] 98. The method of any one of items 78 to 97, wherein the initiator is present in the emulsion in an amount of about 0.1 wt % to about 1.5 wt %, optionally wherein the initiator is present in the emulsion in an amount of about 0.6 wt % to about 1.2 wt %, and further optionally wherein the initiator is present in the emulsion in an amount of about 0.8 wt %.

[0394] 99. The method of any one of items 78 to 98, wherein each polymerization comprises activating the free radical initiator.

[0395] 100. The method of claim 99, wherein activating the free radical initiator comprises heating the emulsion comprising the swollen particles, optionally wherein the heating comprises heating to a temperature of at least 40°C.

[0396] 101. The method of any one of items 78 to 100, wherein the step of allowing the monodisperse seed particles to form swollen particles is carried out for at least 30 minutes, optionally at least 1 hour.

[0397] 102. The method of any one of items 78 to 101, wherein the step of forming the monodisperse seed particles into swollen particles comprises mixing the emulsion, optionally wherein the mixing is carried out at a temperature not exceeding 30°C, optionally wherein the mixing is carried out at a temperature of about 15°C to about 25°C.

[0398] 103. The method of any one of items 56 to 102, wherein the monodisperse cross-linked hydrogel polymer particles formed are porous.

[0399] 104. The method of any one of items 56 to 103, wherein the monodisperse cross-linked hydrogel polymer particles formed have a mode diameter of 0.5 μm to 10 μm or 1 μm to 10 μm, optionally with a mode diameter of 0.5 μm to 5 μm or 1 μm to 5 μm.

[0400] 105. The method of any one of items 56 to 104, wherein the coefficient of variation (CV) of the monodisperse cross-linked hydrogel polymer particles formed is less than 20%, optionally wherein the CV is less than 15%.

[0401] 106. The method of any one of items 56 to 105, wherein the monodisperse cross-linked hydrogel polymer particles formed comprise functional groups, optionally wherein the functional groups are selected from hydroxyl, carboxylic acid (—COOH), primary amine or secondary amine.

[0402] 107. The method of claim 106, further comprising attaching one or more oligonucleotides to the monodisperse cross-linked hydrogel polymer particles.

[0403] 108. Monodisperse seed particles obtainable by the method of any one of items 40 to 55.

[0404] 109. Monodisperse cross-linked hydrogel polymer particles obtainable by the method of any one of items 56 to 107.

[0405] 110. Use of the monodisperse cross-linked hydrogel polymer particles of any one of items 1 to 33 or item 109 in nucleic acid amplification.

[0406] 111. The use of claim 110, wherein the nucleic acid amplification comprises amplifying the oligonucleotide into a plurality of oligonucleotides, optionally wherein at least a portion of the plurality of oligonucleotides is attached to at least one of the monodisperse cross-linked hydrogel polymer particles.

[0407] 112. The use of item 110 or 111, wherein the nucleic acid amplification comprises polymerase chain reaction (PCR) amplification or emulsion PCR amplification.

[0408] 113. Use of the monodisperse cross-linked hydrogel polymer particles of any one of items 1 to 33 or item 109 in oligonucleotide sequencing.

[0409] 114. The use of item 113, wherein the oligonucleotide sequencing comprises chemical field effect transistor (chemFET)-based sequencing or ion sensitive field effect transistor (ISFET)-based sequencing.

[0410] 115. The use of any one of items 110 to 114, wherein the monodisperse cross-linked hydrogel polymer particles are stable in a temperature range of about 10°C to about 100°C.

[0411] 116. The use of any one of items 110 to 115, wherein the particles are porous and permeable to oligonucleotides and nucleic acid amplification and sequencing reagents.

[0412] 117. A method for nucleic acid amplification, comprising performing a primer extension reaction on a polynucleotide hybridized to an oligonucleotide attached to a polymer particle, wherein the polymer particle is a monodisperse cross-linked hydrogel polymer particle of any one of items 1 to 33 or item 109.

[0413] 118. The method of claim 117, wherein the method comprises:

[0414] (a) providing a polymer particle attached to a single-stranded oligonucleotide;

[0415] (b) providing a single-stranded template polynucleotide;

[0416] (c) hybridizing the single-stranded oligonucleotide to the single-stranded template polynucleotide; and

[0417] (d) contacting the single-stranded template polynucleotide with a polymerase and at least one nucleotide under conditions suitable for the polymerase to catalyze the polymerization of the at least one nucleotide to the single-stranded oligonucleotide, thereby producing an extended single-stranded oligonucleotide.

[0418] 119. The method of claim 118, wherein the method further comprises:

[0419] (e) removing (e.g., denaturing) the single-stranded template polynucleotide from the extended single-stranded oligonucleotide such that the single-stranded oligonucleotide remains attached to the polymer particle;

[0420] (f) hybridizing the remaining single-stranded oligonucleotide to a second single-stranded template polynucleotide; and

[0421] (g) contacting the second single-stranded template polynucleotide with a second polymerase and the second at least one nucleotide under conditions suitable for the second polymerase to catalyze polymerization of the second at least one nucleotide into the single-stranded oligonucleotide, thereby producing a subsequent extended single-stranded oligonucleotide.

[0422] 120. The method of any one of items 117 to 119, further comprising:

[0423] (h) Sequencing by detecting nucleotide additions.

[0424] 121. The method of claim 120, wherein detecting nucleotide addition comprises detecting fluorescent emission from the added fluorescent nucleotide or detecting a pH change in the local environment of the polymer particle.

[0425] 122. The method of claim 121, wherein detecting nucleotide addition comprises detecting a pH change in the local environment of the polymer particle using an ion sensor, optionally wherein the ion sensor is a field effect transistor (FET), further optionally wherein the ion sensor is a chemical field effect transistor (ChemFET) or an ion sensitive field effect transistor (ISFET).

[0426] Analytical methods

[0427] Molecular weight measurement

[0428] The weight average molecular weight (Mw) of the oligomer in the seed particles can be determined by the measurement performed using gel permeation chromatography (GPC). In GPC, a series of polymer particle standards are run and used to generate a calibration curve. The Mw of the oligomer can be measured by GPC relative to polystyrene standards using DMF containing 0.01M LiBr as an eluent. Since these Mw values ​​are calculated relative to the standards (polystyrene) of the polymers of the polymers different from the seed particles, the calculated Mw represents a relative value rather than an absolute value. Therefore, the measurement result is repeatable, but actual Mw can not be provided.

[0429] A summary of the GPC method used in the examples provided herein is as follows. The following experimental conditions were used:

[0430] Eluent: DMF containing 0.01M LiBr

[0431] Pre-column: PSS GRAM, 10μm, Guard ID 8.0mm×50mm

[0432] Column: PSS GRAM, 10μm, linear M ID 8.0mm×300mm PSS GRAM, 10μm, linear M ID 8.0mm×300mm

[0433] Temperature: 70℃

[0434] Pump: PSS SECurity 1260HPLC pump

[0435] Flow rate: 1.0mL / min

[0436] Injection system: PSS SECurity 1260 autosampler

[0437] Injection volume: 50 μL

[0438] Sample concentration: 3.0g / L

[0439] Detector: PSS SECurity 1260 Refractive Index Detector (RID)

[0440] Chromatography data system: PSS WinGPC UniChrom version 8.2

[0441] Polystyrene standards with different molecular weights were measured under the above experimental conditions to obtain a calibration curve. The samples were then run. The Mw of the samples was then calculated based on the PS calibration curve.

[0442] Size and size distribution

[0443] The size distribution of a sample can be measured using disc centrifugation, such as the CPS Disc Centrifugation System on a Disc Centrifuge Model DC20000 using the protocol provided by the instrument manufacturer. TM Accurate results require calibration with standards of similar density to the sample being analyzed, and can therefore only be used if suitable polymer standards are available, such as a set of dense polystyrene particle standards comprising primarily polystyrene for the particles of the present disclosure. In cases where the sample being measured has an unknown density, such as for porous particles, the measurements obtained by CPS disk centrifugation are reproducible but cannot provide the actual diameter.

[0444] CPS Disc Centrifugation used in the examples provided herein TM An overview is given below, in which three different experimental approaches are used, with the appropriate method being selected based on, for example, the size and porosity of the particles to be analyzed.

[0445] CPS Method 1 (e.g. Examples 32, 33): Disc centrifugation analysis was performed on a CPS DC20000 from CPS Instruments at a disc speed of 7500 rpm and a gradient of 3-7 wt% sucrose in 1.5 g / L SDS (aq). The gradient was made using an Auto Gradient pump from CPS Instruments and the volume of the injected gradient was 16-17 mL. Prior to injection, the sample was centrifuged in MilliQ-H 2The method used for analysis had the following settings: maximum diameter 4.0 μm, minimum diameter 0.2 μm, particle density 1.032 g / mL, particle refractive index 1.4, particle absorption 0, particle non-sphericity 1, calibration standard diameter 1.069 μm, calibration standard density 1.052, standard half-with 0.15 μm, liquid density 1.016 g / mL, liquid refractive index 1.343.

[0446] The reported size is the diameter of the absorption peak, and the CV is determined by setting boundaries around the main peak.

[0447] CPS Method 2 (e.g. Examples 8, 9, 16-30): Disc centrifugation analysis was performed on a CPS DC20000 from CPS Instruments at a disc speed of 7500 rpm and a gradient of 3-7 wt% sucrose in 1.5 g / L SDS (aq). The gradient was made using an Auto Gradient pump from a CPS instrument and the volume of the injected gradient was 16-17 mL. The method used for the analysis had the following settings: maximum diameter 6.0 μm, minimum diameter 0.05 μm, particle density 1.032 g / mL, particle refractive index 1.032, particle absorption 0, particle non-sphericity 1, calibration standard diameter 0.486 μm, calibration standard density 1.052, standard half value 0.15 μm, liquid density 1.016 g / mL, liquid refractive index 1.343.

[0448] The reported sizes are the absorption peak diameters, and the CVs are determined by setting boundaries around the major peaks.

[0449] CPS Method 3 (e.g. Examples 34-47): Disc centrifugation analysis was performed on a CPS DC20000 from CPS Instruments at a disc speed of 10000 rpm and a gradient of 8-24 wt% sucrose in 1.5 g / L SDS (aq). The gradient was made using an Auto Gradient pump from CPS Instruments and the volume of the injected gradient was 16-17 mL. Prior to injection, the sample was centrifuged in MilliQ-H 2 The particle size was 400 μm and the particle size was diluted to about 0.01 wt % in 2% O. The method used for the analysis had the following settings: maximum diameter 4.0 μm, minimum diameter 0.1 μm, particle density 1.6 g / mL, particle refractive index 1.592, particle absorption 0.2, particle non-sphericity 1, calibration standard diameter 1.098, calibration standard density 1.6, standard half value 0.2 μm, liquid density 1.06 g / mL, liquid refractive index 1.355.

[0450] The reported size is the diameter of the absorption peak, and the CV is determined by setting boundaries around the main peak.

[0451] Photon correlation spectroscopy (PCS) can be used to obtain the hydrodynamic diameter of particles in z-average form. The measurement is independent of particle density and is based on the Brownian motion of small particles. PCS measurements of nanoparticles can be obtained, for example, with the Malvern Zetasizer Nano-ZS, Model ZEN3600. Further details and methods can be found in the Malvern Zetasizer Nano series manual (incorporated herein in its entirety by reference).

[0452] Another technique that can be used to determine the size and size distribution of particles is optical microscopy. A population of beads can be prepared by placing an aqueous solution containing beads on a microscope slide, then capturing an image of the beads at a suitable magnification (e.g., 100× or higher), and analyzing the size of the beads using image analysis software.

[0453] A summary of the optical microscopy methods used in the examples provided herein is as follows. TM Spacer sandwiched between cover glass and Secure-Seal TM The microscopy samples were prepared between the hybridization chamber gaskets. The formed cavity was filled with 8 μL of beads diluted with 150 mM NaCl, then centrifuged for a short time and connected to a microscope slide. Then a 100X lens was used to perform phase contrast optical microscopy on an Olympus 1X81 inverted microscope. Multiple images were automatically collected using the Matlab-based macro of μManager. Out-of-focus images were collected as background and deducted from the phase contrast images. The background-deducted images were then thresholded using the Otsu method to identify individual beads for size analysis. Green fluorescent polystyrene beads with standard sizes were used to calibrate the measured bead size by fluorescence microscopy. A series of Alexa 488-labeled hydrogel beads were then used to calibrate the relative size (contrast size) and the fluorescent size.

[0454] Optical microscopy is the preferred method for measuring the size of particles because it provides a measurement that is independent of particle density. Disc centrifugation analysis is the preferred method for measuring the size distribution (CV) of particles because optical microscopy is based on image analysis and the presence of artifacts in the image can result in artificially high CVs.

[0455] Example

[0456] Synthesis of seed particles

[0457] Example 1

[0458] 5.0 g of distilled N,N-dimethylacrylamide, 4.0 g of Kraton G1650, 0.20 g of 2,2'-azobis(2-methylpropionitrile), 108.0 g of heptane, 27.1 g of toluene and 0.21 mL of 1-octanethiol were loaded into a 250 mL three-necked round bottom flask equipped with a mechanical paddle stirrer and a condenser. Once all materials were dissolved, the reaction mixture was purged with Ar(g) for 10 min. The reactants were then heated to 70 ° C using an oil bath and heated for 8 hours while stirring at 400 rpm. The resulting dispersion was analyzed by dynamic light scattering to give a z-average diameter of 521 nm.

[0459] Example 2

[0460] A 500 mL three-necked round bottom flask equipped with a mechanical and paddle stirrer and a condenser was charged with 10.1 g of distilled N,N-dimethylacrylamide, 8.0 g of Kraton G1650, 0.40 g of 2,2'-azobis(2-methylpropionitrile), 216.0 g of heptane, 54.1 g of toluene and 0.85 mL of 1-octanethiol. Once all materials were dissolved, the reaction mixture was purged with Ar(g) for 10 min. The reactants were then heated to 70 ° C using an oil bath and heated for 8 hours while stirring at 360 rpm. The resulting dispersion was analyzed by dynamic light scattering to obtain a z-average diameter of 733 nm. The particles present in the dispersion were also analyzed by GPC to obtain an Mw of 8,410.

[0461] Example 3

[0462] A 2L jacketed round bottom flask equipped with a mechanical anchor stirrer and a condenser was charged with 36.6g of distilled N,N-dimethylacrylamide, 27.7g of Kraton G1650, 1.4g of 2,2'-azobis(2-methylpropionitrile), 747.2g of heptane, 186.9g of toluene and 2.56g of 1-octanethiol. Once all materials were dissolved, the reaction mixture was purged with Ar(g) for 30min. The reactants were then heated to 71°C using a temperature-controlled water bath connected to the reactor and heated for 15h while stirring at 350rpm. During the first 2.5h of heating, a low flow of Ar(g) was maintained. The resulting dispersion was analyzed by dynamic light scattering to obtain a z-average diameter of 1035nm. The particles present in the dispersion were also analyzed by GPC to obtain a Mw of 10,300.

[0463] Example 4

[0464] The process was carried out as in Example 1, but the reaction mixture was heated and stirred at 350 rpm overnight. The resulting dispersion was analyzed by dynamic light scattering to give a z-average diameter of 387 nm. The particles present in the dispersion were also analyzed by GPC to give a Mw of 22,400.

[0465] Example 5 (Comparative Example)

[0466] The process was carried out as in Example 4, but without the addition of 1-octanethiol, i.e. the reaction mixture did not contain any 1-octanethiol. The resulting dispersion was analyzed by dynamic light scattering to give a z-average diameter of 238 nm. The particles present in the dispersion were also analyzed by GPC to give a Mw of 403,000.

[0467] Example 6

[0468] The process was carried out as in Example 4. The resulting dispersion was analyzed by dynamic light scattering and gave a z-average diameter of 358 nm. The particles present in the dispersion were also analyzed by GPC and gave a Mw of 21,200.

[0469] Synthesis of polymer particles from low molecular weight seed particles

[0470] Example 7

[0471] A 100 mL batch of micron-sized acrylamide particles was formed in heptane / toluene using 0.8 wt% initiator.

[0472] Solution 1 (10 wt% acrylamide (AAm) stock solution): 50 g acrylamide monomer and 450 g water were mixed until a clear and homogeneous solution was formed.

[0473] Solution 2 (stabilizer): 10 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 70 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a homogeneous solution was obtained. 0.8 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring.

[0474] Solution 3 (monomer phase): 0.5 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 20 g of solution 1 (10 wt% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0475] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed using an Ultraturrax for 1 minute and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, solution 4 was transferred to a 100 mL reactor with a stirrer and 8.1 g of a suspension of seed particles of Example 2 (about 7 wt.% dry content—hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen overnight (~16 h) at room temperature under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0476] Example 8

[0477] 10 mL batches of micron-sized acrylamide particles formed in heptane / toluene using 0.5 wt% initiator.

[0478] Solution 1 (10 wt% acrylamide (AAm) stock solution): 50 g acrylamide monomer and 450 g water were mixed until a clear and homogeneous solution was formed.

[0479] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a homogeneous solution was obtained. 0.05 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring.

[0480] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0481] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content—hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at room temperature overnight (~16 h) under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0482] Redispersion and analysis: 300 μL polymer emulsion, 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50) were added to 2mL eppendorf tubes. The tube was vortexed and centrifuged. The supernatant was removed and the sediment was washed three times with 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50). Subsequently, a wash was performed in methanol / deionized water mixture (50:50) and two washes were performed in deionized water, and the sediment was then resuspended in 200 μL deionized water. The product was analyzed using optical microscopy and disc centrifugation. Microscopy was performed by diluting the redispersed product 20 times in 150mM NaCl solution, and image statistics were collected from 28 images to obtain a mode diameter of 2.3 μm. The relative disc centrifuge diameter using CPS Method 2 was determined to be 2.8 μm with a CV = 3.0% (main peak).

[0483] Example 9

[0484] 10 mL batches of micron-sized acrylamide particles in heptane / toluene using alternative stabilizers.

[0485] Solution 1 (10 wt% acrylamide (AAm) stock solution): 50 g acrylamide monomer and 450 g water were mixed until a clear and homogeneous solution was formed.

[0486] Solution 2 (stabilizer): 1 g of Abil EM 90 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a uniform solution was obtained. 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring.

[0487] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0488] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content—hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at room temperature overnight (~16 h) under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0489] Redispersion and Analysis: 300 μL of polymerized emulsion was added to a 2 mL eppendorf tube, the tube was filled to the 2 mL mark with toluene and centrifuged. After removing the supernatant, the precipitate was redispersed in toluene and centrifuged. In addition, two washes were performed with toluene, followed by two washes with deionized water. Finally, the precipitate was redispersed in deionized water to a total volume of 2 mL, and the product was analyzed using optical microscopy and disk centrifugation. Microscopy image statistics were collected from 10 images, resulting in a mode diameter of 2.6 μm. The relative disk centrifugation diameter using CPS method 2 was determined to be 3.3 μm with a CV = 3.9%.

[0490] Example 10

[0491] 10 mL batches of micron-sized acrylamide particles swollen in a non-polar solvent at elevated temperature were used.

[0492] Solution 1 (10 wt% acrylamide (AArm) stock solution): 50 g acrylamide monomer and 450 g water were mixed until a clear and homogeneous solution was formed.

[0493] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a homogeneous solution was obtained.

[0494] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0495] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content - hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at 50° C. overnight (~16 h) under gentle stirring / rotation. After swelling, 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring. Solution 4 was polymerized at 50° C. under stirring for 7 h.

[0496] Embodiment 11

[0497] 10 mL batches of micron-sized acrylamide particles formed in heptane / toluene using higher acrylamide content.

[0498] Solution 1 (40 wt% acrylamide (AAm) stock solution): 200 g acrylamide monomer and 300 g water were mixed until a clear and homogeneous solution was formed.

[0499] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a homogeneous solution was obtained.

[0500] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0501] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content - hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at 50°C overnight (~16 h) under gentle stirring / rotation. After swelling, 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring. Solution 4 was polymerized at 50°C under stirring for 7 h.

[0502] Example 12

[0503] A 10 mL batch of micron-sized acrylamide particles formed in a Linpar 10-13.

[0504] Solution 1 (10 wt% acrylamide (AAm) stock solution): 50 g acrylamide monomer and 450 g water were mixed until a clear and homogeneous solution was formed.

[0505] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of Linpar 10-13 (hereinafter referred to as solvent). The stabilizer solution was stirred until a homogeneous solution was obtained.

[0506] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0507] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of PDMAAm particles (about 7 wt% dry content - hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at 50° C. overnight (~16 h) under gentle stirring / rotation. After swelling, 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring. Solution 4 was polymerized at 50° C. under stirring for 7 h.

[0508] Example 13

[0509] 10 mL batches of micron-sized hydroxymethyl acrylamide particles formed in heptane / toluene.

[0510] Solution 1 (10 wt% N-methylolacrylamide (HMAAm) stock solution): 50 g of methylolacrylamide monomer and 450 g of water were mixed until a clear and homogeneous solution was formed.

[0511] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a homogeneous solution was obtained.

[0512] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% HMAAm stock solution). The solution was then heated to ~40°C to facilitate mixing. 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring.

[0513] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content—hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at room temperature overnight (~16 h) under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0514] Embodiment 14

[0515] 10 mL batches of micron-sized TRIS acrylamide particles formed in heptane / toluene.

[0516] Solution 1 (10 wt% TRIS acrylamide (TRIS) stock solution): 50 g of TRIS acrylamide monomer and 450 g of water were mixed until a clear and homogeneous solution was formed.

[0517] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). The stabilizer solution was stirred until a uniform solution was obtained. Under gentle stirring, 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution.

[0518] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% TRIS stock solution). The solution was then heated to ~40°C to facilitate mixing.

[0519] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content—hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at room temperature overnight (~16 h) under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0520] Embodiment 15

[0521] 10 mL batches of micron-sized hydroxyethyl methacrylate particles formed in heptane / toluene.

[0522] Solution 1 (10 wt% hydroxyethyl methacrylate (HEMA) stock solution): 50 g of hydroxyethyl methacrylate monomer and 450 g of water were mixed until a clear and homogeneous solution was formed.

[0523] Solution 2 (stabilizer): Weigh 1 g of Hypermer 2296 (stabilizer) and then add 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). Stir the stabilizer solution until a homogeneous solution is obtained.

[0524] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt % HEMA stock solution). The solution was then heated to ~40°C to facilitate mixing. 0.01 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring.

[0525] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of a suspension of seed particles from Example 2 (about 7 wt% dry content—hereinafter referred to as seeds) was added to the emulsion and the emulsion containing the seeds was swollen at room temperature overnight (~16 h) under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0526] Example 16 (Comparative Example)

[0527] 10 mL batch of acrylamide product formed in heptane / toluene in the absence of seed particles.

[0528] Solution 1 (10 wt% acrylamide (AAm) stock solution): 50 g acrylamide monomer and 450 g water were mixed until a clear and homogeneous solution was formed.

[0529] Solution 2 (stabilizer): 1 g of Hypermer 2296 (stabilizer) was weighed, followed by the addition of 7 g of a 1:1 (volume ratio) heptane:toluene (hereinafter referred to as solvent or H / T) mixture. The stabilizer solution was stirred until a homogeneous solution was obtained.

[0530] Solution 3 (monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (crosslinker, hereinafter referred to as DHEBA) was added to 2 g of solution 1 (10 wt% AAm stock solution). The solution was then heated to ~40°C to facilitate mixing. 0.08 g of azobisdimethylvaleronitrile (free radical initiator from Wako Chemicals, hereinafter referred to as V-65) was added to the solution under gentle stirring.

[0531] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed using an Ultraturrax for 1 minute and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, the emulsion was allowed to swell overnight (~16 h) at room temperature under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. under stirring for 7 h.

[0532] Redispersion and analysis: 300 μL polymer emulsion, 300 μL toluene and 1200 μL deionized water were added to 2mL eppendorf tubes. The tubes were vortexed and centrifuged. The supernatant was removed and the precipitate was washed twice with 300 μL toluene and deionized water (added to the 2mL line). Subsequently, two washes were carried out in deionized water and the precipitate was resuspended in 200 μL deionized water at last. The product was analyzed using optical microscopy and disc centrifugation. Microscopy was performed by diluting the redispersed product 10 times in 150mM NaCl solution and collecting image statistics from 25 images. The wide distribution makes it difficult to use microscopy to determine the true value of the size. The relative disc centrifugation diameter using CPS method 2 was determined to be 1.4 μm with a CV=30%.

[0533] Embodiment 17

[0534] Solution 1 (monomer phase): 0.9 g N,N'-(1,2-dihydroxyethylene)bisacrylamide (DHEBA) and 39 g H 2O. The mixture was heated to -40°C with stirring until all the DHEBA was dissolved, followed by the addition of 4.4 g of acrylamide (AAm).

[0535] Solution 2 (stabilizer): 0.8 g 2,2'-azobis(2-methylpropionitrile) (AIBN), 9 g Span 80, 33 g toluene, and 33 g heptane were added to a 250 mL Duran flask and shaken until all dissolved.

[0536] Solution 3 (emulsion): 20 g of solution 1 was added to solution 2 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 3 and 5 g of the seed particles of Example 4) were charged into a three-necked round-bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred at 100 rpm and 22° C. overnight. The flask was finally purged with Ar(g) for 10 min and then heated to 70° C. while stirring at 50 rpm for 7 h.

[0537] Redispersion and analysis: 300 μL of polymerized emulsion was added to a 2 mL eppendorf tube and the tube was filled with 1-methyl-2-pyrrolidone (NMP). The tube was vortexed and centrifuged. The supernatant was removed and the precipitate was washed twice with NMP, twice with deionized water, and finally the precipitate was resuspended in 150 μL deionized water. The product was analyzed using optical microscopy and disk centrifugation. Microscopy was performed by diluting the redispersed sample 100 times in 150 mM NaCl (aq), resulting in a mode diameter of 1.3 μm. Characterization was performed by disk centrifugation using CPS method 2, resulting in a diameter of 1.5 μm with a CV = 6.5% (main peak).

[0538] Embodiment 18

[0539] Solution 1 (monomer phase): as in Example 17.

[0540] Solution 2 (stabilizer): 0.8 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 9 g Hypermer 2296, 64 g dodecane were added to a 250 mL Duran flask and shaken until all dissolved.

[0541] Solution 3 (emulsion): As in Example 17, but polymerized for 24 h.

[0542] Redispersion and analysis: 300 μL polymer emulsion, 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50) were added to 2mL eppendorf tubes. The tube was vortexed and centrifuged. The supernatant was removed and the sediment was washed three times with 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50). Subsequently, a wash was carried out in methanol / deionized water mixture (50:50) and two washes were carried out in deionized water, and finally the sediment was resuspended in 100 μL deionized water. The product was analyzed using optical microscopy and disc centrifugation. Microscopy was carried out by diluting the redispersed sample 100 times for microscopy in 150mM NaCl (aq), and a mode diameter of 1.0 μm was obtained. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.4 μm with a CV = 5.2% (main peak).

[0543] Embodiment 19

[0544] Solution 1 (monomer phase): as in Example 17.

[0545] Solution 2 (stabilizer): 0.8 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 9 g Abil WE09, 13 g mineral oil and 52 g diethylhexyl carbonate (Tegosoft DEC) were added separately to a 250 mL Duran flask and shaken until all dissolved.

[0546] Solution 3 (emulsion): as in Example 17.

[0547] Redispersion and analysis: As in Example 18, but final redispersion in 50 μL and dilution 30-fold in 150 mM NaCl (aq) for microscopy gave a mode diameter of 1.0 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.7 μm with CV = 6.4% (main peak).

[0548] Embodiment 20

[0549] Solution 1 (monomer phase): as in Example 17, except that AAm was replaced by hydroxyethylacrylamide (HEAAm).

[0550] Solution 2 (stabilizer): as in Example 19.

[0551] Solution 3 (emulsion): as in Example 17.

[0552] Redispersion and analysis: As in Example 18, but final redispersion in 50 μL and dilution 30-fold in 150 mM NaCl (aq) for microscopy gave a mode diameter of 1.0 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.7 μm with CV = 6.4% (main peak).

[0553] Embodiment 21

[0554] Solution 1 (monomer phase): 0.95 g N,N'-(1,2-dihydroxyethylene)bisacrylamide (DHEBA) and 18 g H 2 O. The mixture was heated to -40°C with stirring until all the DHEBA was dissolved, followed by the addition of 4.8 g of acrylamide (AAm).

[0555] Solution 2 (stabilizer): as in Example 19.

[0556] Solution 3 (emulsion): as in Example 17.

[0557] Redispersion and analysis: As in Example 18, but finally redispersed in 50 μL and diluted 30-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.3 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 2.5 μm with CV = 5.6% (main peak).

[0558] Embodiment 22

[0559] Solution 1 (monomer phase): as in Example 17.

[0560] Solution 2 (stabilizer): as in Example 19.

[0561] Solution 3 (emulsion): As Example 17, but using 21 g of solution 1 and 4 g of seed particles of Example 6.

[0562] Redispersion and analysis: As in Example 17. Microscopy The redispersed product was used for microscopy by diluting 200 times in 150 mM NaCl (aq) giving a mode diameter of 1.2 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 2.0 μm with CV = 5.7% (main peak).

[0563] Embodiment 23

[0564] Solution 1 (monomer phase): as in Example 17, except that AAm was replaced by 2.5 g AAm and 0.03 g 3-acrylamidopropionic acid (AAmPA).

[0565] Solution 2 (stabilizer): as in Example 19.

[0566] Solution 3 (emulsion): as in Example 22.

[0567] Redispersion and analysis: As in Example 17, but finally redispersed in 150 μL and diluted 200-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.3 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.7 μm with CV = 8.0% (main peak).

[0568] Reaction of carboxylic acid groups: 50 μL of the redispersed beads were added to a 2 mL eppendorf tube, washed twice with NMP, and then redispersed in 100 μL NMP. As a first step, 40 μL of a 100 mM solution of N,N,N',N'-tetramethyl-O-(N-succinimidyl)uronium tetrafluoroborate in NMP was added and the tube was placed in a thermomixer at 1000 rpm for 1 hour. In a second step, 20 μL of Alexafluor 488 cadaverine (1 mg in 250 μL NMP) was added and the tube was placed in a thermomixer at 1000 rpm for 1 hour. The beads were washed three times with NMP and heated with H 2 The beads were then redispersed in 1000 mL of 150 mM NaCl (aq) and finally diluted 10-fold in 150 mM NaCl (aq). Imaging using phase contrast and fluorescence microscopy confirmed the presence of reactive groups. As a control experiment, beads from Example 22 were treated with the above staining protocol to yield beads that were not visible in fluorescence microscopy.

[0569] Embodiment 24

[0570] Solution 1 (monomer phase): as in Example 17, but AAm was replaced by N-(2-hydroxyethyl)methacrylamide (HEMAAm).

[0571] Solution 2 (stabilizer): as in Example 19.

[0572] Solution 3 (emulsion): as in Example 22.

[0573] Redispersion and analysis: As in Example 17, but finally redispersed in 150 μL and diluted 200-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.2 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.7 μm with CV = 5.8% (main peak).

[0574] Embodiment 25

[0575] Solution 1 (monomer phase): as in Example 17, but with H2 O is replaced by H 2 0.5% methanol in 5% HO.

[0576] Solution 2 (stabilizer): as in Example 19.

[0577] Solution 3 (emulsion): as in Example 22.

[0578] Redispersion and analysis: As in Example 17, but finally redispersed in 150 μL and diluted 200-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.3 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.9 μm with CV = 6.7% (main peak).

[0579] Embodiment 26

[0580] Solution 1 (monomer phase): as in Example 17, except that AAm was replaced by methacrylamide (MAAm).

[0581] Solution 2 (stabilizer): as in Example 19.

[0582] Solution 3 (emulsion): as in Example 22.

[0583] Redispersion and analysis: As in Example 17, but final redispersion in 100 μL and dilution 400-fold in 150 mM NaCl (aq) for microscopy gave a mode diameter of 1.3 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.8 μm with CV = 9.3% (main peak).

[0584] Embodiment 27

[0585] Solution 1 (monomer phase): as in Example 17.

[0586] Solution 2 (stabilizer): as in Example 19.

[0587] Solution 3 (emulsion): As in Example 22, but stirred at 20°C for 1 h instead of overnight.

[0588] Redispersion and analysis: As in Example 17, but finally redispersed in 100 μL and diluted 400-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.1 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.7 μm with CV = 6.1% (main peak).

[0589] Example 28 (Comparative Example)

[0590] Solution 1 (monomer phase): as in Example 17.

[0591] Solution 2 (stabilizer): as in Example 19.

[0592] Solution 3 (emulsion): As Example 17, but using 24 g of solution 1 and 1 g of seed particles from Example 5.

[0593] Redispersion and analysis: As in Example 17, but finally redispersed in 200 μL and diluted 100-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.6 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 3.1 μm with CV = 28% (main peak).

[0594] Example 29 (Comparative Example)

[0595] Solution 1 (monomer phase): as in Example 17.

[0596] Solution 2 (stabilizer): as in Example 19.

[0597] Solution 3 (emulsion): As Example 17, but using the seed particles of Example 5 (instead of the seed particles from Example 4).

[0598] Redispersion and analysis: As in Example 17, but finally redispersed in 200 μL and diluted 100-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.6 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 3.1 μm with CV = 28% (main peak).

[0599] Embodiment 30

[0600] Solution 1 (monomer phase): As Example 17, but AAm was replaced by hydroxyethyl acrylate (HEA).

[0601] Solution 2 (stabilizer): as in Example 19.

[0602] Solution 3 (emulsion): as in Example 22.

[0603] Redispersion and analysis: As in Example 17, but finally redispersed in 100 μL and diluted 10-fold in 150 mM NaCl (aq) for microscopy, giving a mode diameter of 1.2 μm. Characterization by disk centrifugation using CPS method 2 gave a diameter of 1.6 μm with CV = 6.1% (main peak).

[0604] Synthesis of seed particles

[0605] Embodiment 31

[0606] 34.6 g of distilled N,N-dimethylacrylamide, 27.6 g of Kraton G1650, 1.5 g of 2,2'-azobis(2-methylpropionitrile), 747.9 g of heptane, 187.0 g of toluene and 1.2 g of 1-octanethiol were loaded into a 2L jacketed round bottom flask equipped with a mechanical anchor stirrer and condenser. Once all materials were dissolved, the reaction mixture was purged with Ar(g) for 60 min. The reactants were then heated to 71 ° C and heated for 16 h using a temperature-controlled water bath connected to the reactor while stirring at 400 rpm. The resulting dispersion was analyzed by dynamic light scattering to obtain a z-average diameter of 360 nm.

[0607] Highly swellable particles

[0608] Embodiment 32

[0609] Solution 1 (monomer phase): 1.7 g hydroxyethyl acrylamide (HEAAm), 0.02 g acrylamidopropionic acid (AAPA), 0.26 g N,N'-(1,2-dihydroxyethylene)bisacrylamide (DHEBA) and 22.9 g H 2 O. Shake the mixture until everything is dissolved.

[0610] Solution 2 (stabilizer): 1.76 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 24 g Abil WE09, 26 g mineral oil, and 104 g diethylhexyl carbonate (Tegosoft DEC) were added to a 250 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0611] Solution 3 (emulsion): 71 g of solution 2 was added to solution 1 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 3 and 4.17 g of PDMAAm seeds (Example 31) were charged into a 1 L jacketed round bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred at 100 rpm and 20 ° C overnight. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 50 rpm for 7 h.

[0612] Redispersion and analysis: 50 g of the crude product and 150 g of N-methyl-2-pyrrolidone (NMP) were added to a 250 mL centrifuge flask. The flask was shaken for 90 min and then centrifuged at 10,000 rpm for 15 min. The supernatant was removed and the product was washed once more with NMP and washed with H 2O for 3 times and then dispersed in HO. 2 O. The product was analyzed using optical microscopy and disk centrifugation. Microscopy was performed by diluting the redispersed product to a concentration of 0.04 wt % in 150 mM NaCl solution and collecting image statistics from 4 images, resulting in a mode diameter of 1.3 μm. The relative disk centrifugation diameter using CPS method 1 was determined to be 1.6 μm with a CV = 8.0%.

[0613] Transfer to NMP: Dissolve 20 g in H 2 The particle suspension in 0 was divided into 2×50 mL centrifuge tubes, the tubes were filled with NMP and centrifuged at 10000 rpm for 10 min. The supernatant was removed, and then the cells were washed in NMP for another 3 times and finally resuspended in NMP.

[0614] Embodiment 33

[0615] Solution 1 (monomer phase): as in Example 32.

[0616] Solution 2 (stabilizer): as in Example 32.

[0617] Solution 3 (emulsion): as in Example 32.

[0618] Redispersion and analysis: 50 g of the crude product and 150 g of N-methyl-2-pyrrolidone (NMP) were added to a 250 mL centrifuge flask. The flask was shaken for 90 min and then centrifuged at 10,000 rpm for 15 min. The supernatant was removed and the product was washed once more with NMP and washed with H 2 O for 3 times and then dispersed in HO. 2 O. The product was analyzed using optical microscopy and disk centrifugation. Microscopy was performed by diluting the redispersed product to a concentration of 0.05 wt% in 150 mM NaCl solution and collecting image statistics from 25 images, resulting in a mode diameter of 1.6 μm. The relative disk centrifugation diameter using CPS method 1 was determined to be 1.7 μm with a CV = 6.6%.

[0619] Transfer to NMP: as in Example 32.

[0620] Less swellable particles

[0621] Embodiment 34

[0622] Solution 1 (monomer phase): 28.6 g hydroxymethyl acrylamide (HMAAm), 0.95 g acrylamidopropionic acid (AAPA), 19.7 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-1,2-diyl))diacrylamide (EGBEAAm) and 29.4 g HMAAm were placed in a 500 mL Duran flask.2 O. Shake the mixture until everything is dissolved.

[0623] Solution 2 (stabilizer): 3.8 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 48 g Abil WE09, 53 g mineral oil, and 210 g diethylhexyl carbonate (Tegosoft DEC) were added to a 600 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0624] Solution 3 (emulsion): 262 g of solution 2 was added to solution 1 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 3 and 40 g of PDMAAm seeds (Example 31) were charged into a 1 L jacketed round bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred at 100 rpm and 22 ° C overnight. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 64 rpm for 7 h.

[0625] Redispersion and analysis: The crude product was divided into 2 x 250 mL centrifuge flasks and centrifuged at 5000 rpm for 15 min and 7000 rpm for 10 min. The supernatant was removed and the particles were redispersed in isopropanol. The redispersed particles were then divided into a total of 6 x 250 mL centrifuge bottles, washed 4 times with isopropanol, and washed with H 2 O and then dispersed in HO for 6 times. 2 O. The particles were then filtered through three different filter fabrics: Sefar Nitex 03-64 / 32, Sefar Nitex 03-30 / 18 and Sefar Nitex 03-1 / 1. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt% in 150 mM NaCl solution and collecting image statistics from 18 images, resulting in a mode diameter of 0.91 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 0.54 μm with a CV = 6.2%.

[0626] Embodiment 35

[0627] Solution 1 (monomer phase): 27.0 g hydroxymethyl acrylamide (HMAAm), 2.6 g acrylamidopropionic acid (AAPA), 19.7 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 49.3 g HMAAm were placed in a 500 mL Duran flask. 2 O. Shake the mixture until everything is dissolved.

[0628] Solution 2 (stabilizer): as in Example 34.

[0629] Solution 3 (emulsion): as in Example 34.

[0630] Redispersion and analysis: The crude product was divided into 2 × 250 mL centrifuge flasks and centrifuged at 5000 rpm for 25 min. The supernatant was removed and the particles were redispersed in isopropanol. The redispersed particles were then divided into a total of 6 × 250 mL centrifuge bottles, washed 4 times with isopropanol, and washed with H 2 O for 5 times and finally dispersed in HO 2 O. The particles were then filtered through two different filter fabrics: Sefar Nitex 03-30 / 18 and Sefar Nitex 03-1 / 1. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt% in 150 mM NaCl solution and collecting image statistics from 21 images, resulting in a 0.90 μm mode diameter. The relative disk centrifuge diameter using CPS method 3 was determined to be 0.53 μm with a CV = 5.2%.

[0631] Embodiment 36

[0632] Solution 1 (monomer phase): 24.8 g hydroxymethyl acrylamide (HMAAm), 5.0 g acrylamidopropionic acid (AAPA), 19.9 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 49.7 g HMAAm were placed in a 500 mL Duran flask. 2 O. Shake the mixture until everything is dissolved.

[0633] Solution 2 (stabilizer): 3.8 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 52 g Abil WE09, 57 g mineral oil, and 228 g diethylhexyl carbonate (Tegosoft DEC) were added to a 1000 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0634] Solution 3 (emulsion): 284 g of solution 2 was added to solution 1 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 3 and 17 g of PDMAAm seeds (Example 31) were charged into a 1 L jacketed round bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred overnight at 100 rpm and 25 ° C. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 62 rpm for 7 h.

[0635] Redispersion and analysis: The crude product was divided into 2 x 250 mL centrifuge flasks and centrifuged at 3000 rpm for 10 min and 5000 rpm for 20 min. The supernatant was removed and the particles were redispersed in isopropanol. The redispersed particles were then divided into a total of 6 x 250 mL centrifuge bottles, washed 4 times with isopropanol, and washed with H 2 O and then dispersed in HO for 6 times. 2 O. The particles were then filtered through two different filter fabrics: Sefar Nitex 03-30 / 18 and Sefar Nitex 03-1 / 1. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt% in 150 mM NaCl solution and collecting image statistics from 30 images, giving a mode diameter of 1.0 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 0.57 μm with a CV = 6.3%.

[0636] Embodiment 37

[0637] Solution 1 (monomer phase): 1.8 g hydroxymethyl acrylamide (HMAAm), 0.7 g acrylamidopropionic acid (AAPA), 4.9 g N,N-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 17.3 g HMAAm were placed in a 250 mL Duran flask. 2 O. Shake the mixture until everything is dissolved.

[0638] Solution 2 (stabilizer): 2.8 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 35 g Abil WE09, 38 g mineral oil, and 153 g diethylhexyl carbonate (Tegosoft DEC) were added to a 400 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0639] Solution 3 (emulsion): 66 g of solution 2 was added to solution 1 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 3 and 9.9 g of PDMAAm seeds (Example 31) were charged into a 1 L jacketed round bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred at 100 rpm and 19 ° C overnight. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 55 rpm for 7 h.

[0640] Redispersion and analysis: The crude product was added to a 250 mL centrifuge flask and centrifuged at 5000 rpm for 20 min. The supernatant was removed and the particles were redispersed in isopropanol. The redispersed particles were then divided into a total of 2 × 250 mL centrifuge bottles, washed 3 times with isopropanol, and washed with H 2 O and then dispersed in HO for 6 times. 2 O. The particles were then filtered through two different filter fabrics: Sefar Nitex 03-30 / 18 and Sefar Nitex 03-1 / 1. The product was analyzed using light microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt% in 150 mM NaCl solution and collecting image statistics from 21 images, resulting in a mode diameter of 0.84 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 0.41 μm with a CV = 9.5%.

[0641] Embodiment 38

[0642] Solution 1 (monomer phase): 12.3 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 12.4 g H 2 O. Shake the mixture until everything is dissolved.

[0643] Solution 2 (stabilizer): as in Example 37.

[0644] Solution 3 (emulsion): as in Example 37.

[0645] Redispersion and Analysis: As in Example 37. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt % in 150 mM NaCl solution and collecting image statistics from 24 images, yielding a mode diameter of 0.85 μm. The relative disk centrifugation diameter using CPS Method 3 was determined to be 0.50 μm with a CV = 8.7%.

[0646] Embodiment 39

[0647] Solution 1 (monomer phase): 2.1 g hydroxymethyl acrylamide (HMAAm), 0.3 g acrylic acid (AA), 4.9 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 17.3 g HMAAm were placed in a 250 mL Duran flask. 2 O. Shake the mixture until everything is dissolved.

[0648] Solution 2 (stabilizer): as in Example 37.

[0649] Solution 3 (emulsion): as in Example 37.

[0650] Redispersion and Analysis: As in Example 37. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt % in 150 mM NaCl solution and collecting image statistics from 21 images, yielding a 0.85 μm mode diameter. The relative disk centrifugation diameter using CPS Method 3 was determined to be 0.42 μm with a CV = 7.6%.

[0651] 2-stage granules

[0652] Embodiment 40

[0653] Stage 1: Swelling and polymerization of particles in the absence of crosslinking agents

[0654] Solution 1 (12 wt% HMAAm stock solution): 125 g HMAAm monomer (48% solution) and 375 g DI water were mixed until a clear and homogeneous solution was formed.

[0655] Solution 2 (monomer phase): 5 μL 1-thioglycerol was added to 2 g of solution 1 (25 wt% HMAAm stock solution). The solution was then heated to ~40°C to facilitate mixing. Under gentle stirring, 0.08 g azobisdimethylvaleronitrile (V-65) was added to the solution.

[0656] Solution 3 (stabilizer): Weigh 1 g of Hypermer 2296 (stabilizer) and then add 7 g of a 1:1 (volume ratio) mixture of heptane:toluene (hereinafter referred to as solvent or H / T). Stir the stabilizer solution until a homogeneous solution is obtained.

[0657] Solution 4 (emulsion phase): Solutions 2 and 3 were mixed for 1 minute using an Ultraturrax and then sonicated on ice for 3 minutes (6×30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%). After emulsification, 0.81 g of PDMAAm seeds (Example 3) were added to the emulsion and the emulsion containing the seeds was allowed to swell overnight at room temperature (~16 h) under gentle stirring / rotation. After swelling, solution 4 was polymerized at 50° C. with stirring for 7 h.

[0658] Stage 2: Secondary swelling and polymerization of cross-linked particles

[0659] Solution 5 (second stabilizer solution): same as solution 3.

[0660] Solution 6 (second monomer phase): 0.05 g of 1,2-dihydroxybisacrylamide (DHEBA) was added to 8 mL of solution 1 (25 wt% HMAAm stock solution). The solution was then heated to ~40°C to facilitate mixing. 0.05 g of azobisdimethylvaleronitrile (V-65) was added to the solution under gentle stirring.

[0661] Solution 7 (second emulsion phase): Solutions 5 and 6 were mixed for 1 min using an Ultraturrax and then sonicated on ice for 3 min (6 x 30 sec intervals) (Branson digital sonifier 450CE, amplitude 40%).

[0662] Redispersion and analysis: 300 μL polymer emulsion, 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50) were added to 2mL eppendorf tubes. The tube was vortexed and centrifuged. The supernatant was removed and the precipitate was washed three times with 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50). Subsequently, a wash was performed in methanol / deionized water mixture (50:50) and two washes were performed in deionized water, and the precipitate was then resuspended in 150 μL deionized water. The product was analyzed using optical microscopy and disc centrifugation. Bright field microscopy was performed by diluting the redispersed product 10 times in 150mM NaCl solution, and image statistics were collected from 21 images to obtain a mode diameter of 4.0 μm. The relative disc centrifuge diameter using CPS Method 3 was determined to be 0.69 μm with a CV = 3.4%.

[0663] Embodiment 41

[0664] Stage 1: Swelling and polymerization of particles in the absence of crosslinking agents

[0665] Solution 1 (24 wt% HMAAm stock solution): 25 g HMAAm monomer (48% solution) and 25 g DI water were mixed until a clear and homogeneous solution was formed.

[0666] Solution 2 (monomer phase): As in Example 40, but using 20 μL 1-thioglycerol.

[0667] Solution 3 (stabilizer): as in Example 40.

[0668] Solution 4 (emulsion phase): as in Example 40.

[0669] Stage 2: Secondary swelling and polymerization of cross-linked particles

[0670] As Example 40, but using a 50 wt% HMAAm stock solution.

[0671] Redispersion and analysis: 300 μL polymer emulsion, 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50) were added to 2mL eppendorf tubes. The tube was vortexed and centrifuged. The supernatant was removed and the precipitate was washed three times with 300 μL heptane / toluene mixture (50:50) and 1200 μL methanol / deionized water mixture (50:50). Subsequently, a wash was performed in methanol / deionized water mixture (50:50) and two washes were performed in deionized water, and the precipitate was then resuspended in 200 μL deionized water. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product 10 times in 150mM NaCl solution, and image statistics were collected from 21 images to obtain a mode diameter of 3.4 μm. The relative disc centrifuge diameter using CPS Method 3 was determined to be 0.89 μm with a CV = 3.8%.

[0672] Embodiment 42

[0673] Stage 1: Swelling and polymerization of particles in the absence of crosslinking agents

[0674] Solution 1 (monomer phase): 16.0 g hydroxyethyl acrylamide (HEAAm), 0.3 g 1-thioglycerol and 8.3 g H 2 O. Shake the mixture until everything is dissolved.

[0675] Solution 2 (stabilizer): 2.6 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 32 g Abil WE09, 35 g mineral oil, and 139 g diethylhexyl carbonate (Tegosoft DEC) were added to a 250 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0676] Solution 3 (emulsion): 65g of solution 2 was added to solution 1 and then mixed for 1 min using an Ultraturrax. Further emulsification was performed by using an UP 200s from Hielscher Ultrasound Technology with a 0.9 cycle setting and a 40% amplitude setting. In the next step, solution 3 and 10.3g of PDMAAm seeds were loaded into a 250mL three-necked round-bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet, and stirred overnight at 100rpm and 20°C. The flask was finally purged with Ar (g) for 30min and then heated to 70°C while stirring at 53rpm for 7h.

[0677] Stage 2: Secondary swelling and polymerization of cross-linked particles

[0678] Solution 5 (second monomer phase): 7.1 g hydroxyethyl acrylamide (HEAAm), 2.4 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 14.2 g H 2 O. Shake the mixture until everything is dissolved.

[0679] Solution 6 (second stabilizer): 2.6 g of 2,2'-azobis(2-methylbutyronitrile) (AMBN), 34 g AbilWE09, 37 g mineral oil, and 147 g diethylhexyl carbonate (Tegosoft DEC) were added to a 400 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0680] Solution 7 (second emulsion): 69 g of solution 6 was added to solution 5 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 7 and 7.7 g of polymer solution 3 were charged into a 250 mL three-necked round-bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred overnight at 100 rpm and 22 ° C. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 56 rpm for 7 h.

[0681] Redispersion and analysis: The crude product was added to a 250 mL centrifuge flask and centrifuged at 5000 rpm for 30 min. The supernatant was removed and the particles were redispersed in isopropanol. The redispersed particles were then washed twice with isopropanol and washed with H 2 O was washed 14 times and then dispersed in HO 2 O. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.05 wt % in 150 mM NaCl solution and collecting image statistics from 97 images, yielding a mode diameter of 5.6 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 2.0 μm with a CV = 7.5%.

[0682] Embodiment 43

[0683] Stage 1: Swelling and polymerization of particles in the absence of crosslinking agents

[0684] Solution 1 (monomer phase): as in Example 42.

[0685] Solution 2 (stabilizer): 2.6 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 32 g Hypermer 2296, 88 g toluene, and 89 g heptane were added to a 400 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0686] Solution 3 (emulsion): As in Example 42, but using the solution of this example.

[0687] Stage 2: Secondary swelling and polymerization of cross-linked particles

[0688] Solution 5 (second monomer phase): 7.0 g hydroxyethyl acrylamide (HEAAm), 2.3 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide (EGBEAAm) and 14.1 g H 2 O. Shake the mixture until everything is dissolved.

[0689] Solution 6 (second stabilizer): 0.96 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 12 g Hypermer 2296, 34 g toluene and 34 g heptane were added to a 250 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0690] Solution 7 (second emulsion): 67 g of solution 6 was added to solution 5 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 7 and 7.7 g of polymer solution 3 were charged into a 250 mL three-necked round-bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet and stirred overnight at 100 rpm and 22 ° C. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 55 rpm for 7 h.

[0691] Redispersion and analysis: The crude product was added to a 250 mL centrifuge flask and centrifuged at 3000 rpm for 5 min. The supernatant was removed and the particles were redispersed in isopropanol. The redispersed particles were then washed three times with isopropanol and washed with H 2 O was washed 10 times and finally dispersed in HO 2O. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.02 wt% in 150 mM NaCl solution and collecting image statistics from 72 images, yielding a mode diameter of 4.4 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 1.3 μm with a CV = 7.1%.

[0692] Multifunctional crosslinking agent

[0693] Embodiment 44

[0694] Synthesis of N,N-bis(2-acrylamidoethyl)acrylamide (BAAmEAAm).

[0695] Diethylenetriamine (14.63 g; 142 mmol) was dissolved in 200 mL of acetonitrile. Potassium carbonate (64.68 g; 468 mmol) was added and the reaction mixture was cooled to 0°C with an ice bath. Acryloyl chloride (36.3 mL, 447 mmol) was added dropwise over approximately 45 minutes. The ice bath was removed and the reaction was stirred at ambient temperature for 2 hours. The reaction mixture was filtered and the filter cake was washed with 200 mL of CH 2 Cl 2 Rinse. Inhibitor (phenothiazine, 10.1 mg) was added to the filtrate and the volatiles were removed under reduced pressure at 25°C. The crude material was purified by dry flash chromatography on silica using a gradient of methanol in dichloromethane. The fractions containing the product were combined and 9.9 mg of phenothiazine was added and the product was finally dried under vacuum. Yield 12.97 g.

[0696] Embodiment 45

[0697] Solution 1 (monomer phase): 3.1 g hydroxyethyl acrylamide (HEAAm), 0.7 g acrylamidopropionic acid (AAPA), 3.7 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,2-diyl))diacrylamide (EGBEAAm), 0.3 g N,N-bis(2-acrylamidoethyl)acrylamide (BAAmEAAm) and 17 g H 2 O. Shake the mixture until everything is dissolved.

[0698] Solution 2 (stabilizer): 2.6 g 2,2'-azobis(2-methylbutyronitrile) (AMBN), 32 g Abil WE09, 35 g mineral oil, and 140 g diethylhexyl carbonate (Tegosoft DEC) were added to a 250 mL beaker and mixed with a magnetic stir bar until all dissolved.

[0699] Solution 3 (emulsion): 65 g of solution 2 was added to solution 1 and then mixed using an Ultraturrax for 1 min. Further emulsification was performed by ultrasonication using a UP 200s from Hielscher Ultrasound Technology, with a cycle setting of 0.9 and an amplitude setting of 40%. In the next step, solution 3 and 9.87 g of PDMAAm seeds (Example 31) were charged into a 250 mL three-necked round-bottom flask equipped with a condenser, a mechanical stirrer and a gas inlet, and stirred overnight at 100 rpm and 20 ° C. The flask was finally purged with Ar (g) for 30 min and then heated to 70 ° C while stirring at 53 rpm for 7 h.

[0700] Redispersion and analysis: 70 g of crude product was mixed with 500 mL of H 2 O and 2-butanol were added together to a 1000 mL centrifuge flask, followed by shaking for 30 min. The mixture was then centrifuged, and the top 2-butanol phase was removed, followed by another 2×200 ml of 2-butanol for washing. The suspension was then divided into 6×250 mL centrifuge bottles and washed with H 2 O and then dispersed in HO for 6 times. 2 O. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt % in 150 mM NaCl solution and collecting image statistics from 25 images, yielding a mode diameter of 0.82 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 0.43 μm with a CV = 4.6%.

[0701] Embodiment 46

[0702] Solution 1 (monomer phase): 3.0 g hydroxyethyl acrylamide (HEAAm), 0.7 g acrylamidopropionic acid (AAPA), 3.7 g N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2-diyl))diacrylamide (EGBEAAm), 0.2 g 4-arm PEG-acrylamide and 17 g H 2 O. Shake the mixture until everything is dissolved.

[0703] Solution 2 (stabilizer): as in Example 45.

[0704] Solution 3 (emulsion): as in Example 45.

[0705] Redispersion and analysis: 70 g of crude product was mixed with 500 mL of H 2O and 2-butanol were added together to a 1000 mL centrifuge flask, followed by shaking for 60 min. The mixture was then centrifuged and the top 2-butanol phase was removed and then washed once more with 2-butanol. The suspension was then washed with H 2 O for 5 times and finally dispersed in HO 2 O. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt % in 150 mM NaCl solution and collecting image statistics from 11 images, yielding a mode diameter of 0.86 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 0.41 μm with a CV = 6.0%.

[0706] Embodiment 47

[0707] Solution 1 (monomer phase): 1.8 g hydroxyethyl acrylamide (HEAAm), 0.7 g acrylamidopropionic acid (AAPA), 2.5 g N,N-bis(2-acrylamidoethyl)acrylamide (BAAmEAAm) and 20 g H 2 O. Shake the mixture until everything is dissolved.

[0708] Solution 2 (stabilizer): as in Example 45.

[0709] Solution 3 (emulsion): as in Example 45.

[0710] Redispersion and analysis: 70 g of crude product was mixed with 500 mL of H 2 O and 2-butanol were added together to a 1000 mL centrifuge flask, followed by shaking for 60 min. The mixture was then centrifuged and the top 2-butanol phase was removed and then washed once more with 2-butanol. The suspension was then divided into 6 × 250 mL centrifuge bottles and washed with H 2 O for 5 times and finally dispersed in HO 2 O. The product was analyzed using optical microscopy and disk centrifugation. Bright field microscopy was performed by diluting the redispersed product to a concentration of 0.01 wt % in 150 mM NaCl solution and collecting image statistics from 24 images, yielding a mode diameter of 0.67 μm. The relative disk centrifugation diameter using CPS method 3 was determined to be 0.39 μm with a CV = 6.4%.

[0711] Activation of hydrogels containing carboxylate groups.

[0712] Embodiment 48

[0713] 22.6 mg O-(N-succinimidyl)-N,N,N',N'-tetramethyluronium tetrafluoroborate (TSTU), 27 μL tributylamine and NMP were added to a final volume of 7.5 mL to a suspension of 7200 μL of the particles of Example 32 in NMP. After shaking at room temperature for 1 h, the suspension was centrifuged at 15,000 rpm for 50 min. The supernatant was removed from the resulting precipitate, and the precipitate was resuspended in 4 mL of fresh NMP and centrifuged at 15,000 rpm for 1 h. The supernatant was removed from the resulting precipitate containing the NHS ester activated hydrogel. The 4 mL NMP wash / spin was repeated once.

[0714] Embodiment 49

[0715] Example 48 was followed, but using 7300 μL of the suspension of particles from Example 33.

[0716] Conjugation of hydrogels with amine-terminated DNA probes

[0717] Embodiment 50

[0718] The amount is 193.4 μ L 5 '-amine-terminated 30-mer oligonucleotide (for each oligonucleotide phosphate group with tetrabutylammonium counter ion) 5.17mM NMP solution is added to the carboxylic acid NHS ester hydrogel precipitate from Example 48. The suspension is diluted to 9.976mL with NMP. After adding 23.8 microliters of 42mM tributylamine in NMP, the total reaction volume is 10mL, and the reaction vessel is stirred in a 66 ° C thermomixer for 16h. Add 10mL water and cool to room temperature, add 10mL 0.25M NaOH to the mixture. Stir in a thermomixer for 15min at room temperature, and add 1mL 50xTE, then centrifuge for 50min, and remove the supernatant. The obtained precipitate is resuspended in 10 milliliters of 1xTE, then centrifuge for 50min, and remove the supernatant. At this point, the hydrogel pellet was resuspended in 10 mL of 1xTE buffer and heated at 80°C for 1 h; after centrifugation (15,000 rpm for 50 min) and removal of the supernatant, the conjugated hydrogel was washed with 10 mL of 1xTE as described above, followed by centrifugation for 50 min and removal of the supernatant. The resulting pellet was resuspended in 14 mL of deionized water and filtered with a 5 μm syringe filter for subsequent use

[0719] Embodiment 51

[0720] As Example 50, but using the carboxylic acid NHS ester hydrogel precipitate from Example 49.

[0721] Templated with OCP143 library, ChIP loading and sequencing

[0722] Embodiment 52

[0723] For more information, see the User Guide on thermofisher.com, but here are brief instructions. Template the conjugated particles with a 100-120 base pair DNA library by emulsion PCR. TM Reagents and consumables in Automated Ion Chef TM The particles were manually loaded onto the chip and templated on the Ion Proton TM Sequencing was performed on a sequencer. Key indicators for sequencing of the conjugated particles from Example 50: 1.4M total reads, 98.6% raw read accuracy, and 75 base AQ20 average (1% probability of incorrect base reading). Key indicators for sequencing of the conjugated particles from Example 51: 3.0M total reads, 98.7% raw read accuracy, and 83 base AQ20 average

Claims

1. Monodisperse seed particles having a Z-average diameter of 100 nm to 1500 nm, wherein each seed particle comprises a plurality of non-crosslinked oligomers of poly-N,N-dimethylacrylamide, wherein the weight average molecular weight (Mw) of the oligomers is 2,000 Da to 100,000 Da.

2. The seed particle of claim 1, wherein the oligomer has a Mw of 5,000 Da to 70,000 Da. The seed particle of claim 2 , wherein the oligomer has a Mw of 6,000 Da to 40,000 Da. The seed particle of claim 2 , wherein the oligomer has a Mw of 7,000 Da to 50,000 Da. The seed particle of claim 2 , wherein the oligomer has a Mw of 8,000 Da to 40,000 Da.

6. The seed particle of any one of claims 1 to 5, wherein the particle has the characteristics of a seed particle formed by free radical initiated polymerization of N,N-dimethylacrylamide in an organic solvent in the presence of a stabilizer and a chain transfer agent.

7. Use of the seed particles according to any one of claims 1 to 6 for forming monodisperse crosslinked hydrogel polymer particles.

8. The use of claim 7, wherein the monodisperse cross-linked hydrogel polymer particles are cross-linked polyacrylamide particles.

9. The use of claim 7, wherein the monodisperse cross-linked hydrogel polymer particles comprise a polymer formed from: (a)log P oct / wat A hydrophilic vinyl monomer having a (log P) of less than 1; as well as (b) a cross-linking agent comprising at least two vinyl groups, where log P oct / wat (log P) refers to the octanol-water partition coefficient of the compound.

10. The use according to claim 9, wherein the hydrophilic vinyl monomer has a log P of less than 0.

6.

11. The use according to claim 10, wherein the hydrophilic vinyl monomer has a log P of less than 0.

3.

12. The use according to claim 11, wherein the hydrophilic vinyl monomer has a log P of less than 0.

13. The use according to any one of claims 9 to 11, wherein the hydrophilic vinyl monomer has a log P of 0.5 to -2.

14. The use according to claim 13, wherein the hydrophilic vinyl monomer has a log P of 0 to -2.

15. The use according to any one of claims 9 to 11, wherein the hydrophilic vinyl monomer is an acrylamide monomer and / or an acrylate monomer.

16. The use according to any one of claims 9 to 11, wherein the hydrophilic vinyl monomer comprises at least one compound of formula (I): in: R 1 is -H, -CH3 or -CH2CH3; R 2 is -OR 3 or -N(R 4 )R 5 ; R 3 is -H, -C1-C6 alkyl or -C1-C6 alcohol; and R 4 and R 5 Independently selected from -H, -C1-C6 alkyl, -C1-C6 haloalkyl, -C1-C6 alcohol.

17. The use according to claim 16, wherein R 3 and / or R 4 and / or R 5 are each independently substituted by 1 to 5 substituents, each independently selected from the group consisting of: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O)2R a NR a CONR a R a NR a CO2R a , OR a SR a 、S(O)R a 、S(O)2OR a 、S(O)2R a 、S(O)2NR a R a 、CO2R a C(O)R a ,CONR a R a , C1-C4-alkyl, C2-C4-alkenyl, C2-C4-alkynyl, C1-C4-haloalkyl; wherein R a is independently selected at each occurrence from: H and C1-C4 alkyl.

18. The method of claim 16, wherein R 1 It is -H or -CH3.

19. The method of claim 18, wherein R 1 is -H.

20. The method of claim 16, wherein R 2 For-OR 3 .

21. The method of claim 16, wherein R 3 is -H.

22. The method of claim 16, wherein R 4 It is -H or -C1-C6 alkyl.

23. The method of claim 22, wherein R 4 is -H.

24. The method of claim 16, wherein R 5 It can be -H or -C1-C6 alkyl.

25. The method of claim 24, wherein R 5 is -H.

26. The use of any one of claims 9 to 11, wherein the hydrophilic vinyl monomer is selected from or comprises at least one acrylamide monomer, acrylic acid monomer, methacrylamide monomer or methacrylic acid monomer.

27. The use of any one of claims 9 to 11, wherein the hydrophilic vinyl monomer is selected from or comprises acrylamide, hydroxymethyl acrylamide, hydroxyethyl acrylamide, [tris(hydroxymethyl)methyl]acrylamide, 3-acrylamidopropionic acid, methacrylamide, 2-hydroxyethyl methacrylamide, (3-aminopropyl) methacrylamide, or 2-hydroxyethyl acrylate.

28. The use according to any one of claims 9 to 11, wherein the hydrophilic vinyl monomer is selected from or comprises at least one of acrylamide, hydroxymethyl acrylamide, hydroxyethyl acrylamide, [tris(hydroxymethyl)methyl]acrylamide, 2-hydroxyethyl methacrylate and acrylic acid.

29. The use according to any one of claims 9 to 11, wherein the hydrophilic vinyl monomer comprises a primary amide group (-C(O)NH2).

30. The use according to any one of claims 9 to 11, wherein the cross-linking agent is a difunctional, trifunctional or tetrafunctional acrylamide.

31. The use according to claim 30, wherein the crosslinking agent is a difunctional acrylamide.

32. The use according to any one of claims 9 to 11, wherein the crosslinking agent comprises at least one compound of formula (IIa) or (IIb): Where R 6 Selected from -C1-C6 alkyl-, -C1-C6 heteroalkyl-, -C1-C6 cycloalkyl-, -C1-C6 hydroxyalkyl-, -C1-C6 ether- or a polyether containing 2 to 100 C2-C3 ether units; R 7 and R 8 Each is independently selected from -H, -C1-C6 alkyl, -C1-C6 heteroalkyl, -C3-C6 cycloalkyl, -C1-C6 hydroxyalkyl or -C1-C6 ether; R 9 -N(R 11 )C(O)CH=CH2; R 10 Selected from -H and -N(R 12 )C(O)CH=CH2; and R 11 and R 12 Each is independently selected from -H, -C1-C6 alkyl, -C1-C6 heteroalkyl, -C3-C6 cycloalkyl, -C1-C6 hydroxyalkyl or -C1-C6 ether.

33. The use of claim 32, wherein R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 One or more of the following are independently substituted by 1 to 5 substituents, each independently selected from the following: oxo, =NR a , =NOR a , halogen, nitro, cyano, NR a R a NR a S(O)2R a NR a CONR a R a NR a CO2R a , OR a SR a 、S(O)R a 、S(O)2OR a 、S(O)2R a 、S(O)2NR a R a 、CO2R a C(O)R a ,CONR a R a , C1-C4-alkyl, C2-C4-alkenyl, C2-C4-alkynyl, C1-C4-haloalkyl; wherein R a is independently selected at each occurrence from: H, C1-C4 alkyl and C1-C4 alkenyl.

34. The method of claim 32, wherein R 6 Selected from -C1-C6 alkyl-, -C1-C6 hydroxyalkyl- and polyethers containing 2 to 100 C2-C3 ether units.

35. The method of claim 34, wherein R 6 Selected from -C1-C6 alkyl- and -C1-C6 hydroxyalkyl-.

36. The method of claim 35, wherein R 6 It is -C1-C6 hydroxyalkyl-.

37. The method of claim 32, wherein R 6 Selected from -CH2-, -(CH2)2-, -(CH2)3- or -(CH2)4-.

38. The method of claim 37, wherein R 6 It is -(CH2)2-.

39. The method of claim 32, wherein R 6 Selected from -C(OH)H-, -(C(OH)H)2-, -(C(OH)H)3- or -(C(OH)H)4-.

40. The method of claim 39, wherein R 6 It is -(C(OH)H)2-.

41. The method of claim 32, wherein R 6 For (CH2) r (OCH2CH2) n O(CH2) s , wherein r and s are each independently 2 or 3, and n is an integer from 1 to 100.

42. The use of claim 41, wherein r and s are each 2 and n is an integer from 1 to 50.

43. The method of claim 32, wherein R 7 and / or R 8 For H.

44. The use according to any one of claims 9 to 11, wherein the cross-linking agent has a log P value of less than 1.

45. The use of claim 44, wherein the cross-linking agent has a log P value of less than 0.

5.

46. ​​The use of claim 45, wherein the cross-linking agent has a log P value of less than 0.

47. The use of any one of claims 9 to 11, wherein the crosslinking agent is or comprises N,N'-(1,2-dihydroxyethylene)bisacrylamide, N,N'-methylenebis(acrylamide), N,N'-ethylenebis(acrylamide), glycerol 1,3-diglyceride diacrylate, piperazine diacrylamide, N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide, polyethylene glycol diacrylamide, 4-arm PEG-acrylamide and / or N,N-bis(2-acrylamidoethyl)acrylamide.

48. The use of claim 47, wherein the MW of polyethylene glycol diacrylamide is ≤ 2000.

49. The use of claim 47, wherein the MW of 4-arm PEG-acrylamide is ≤ 2000.

50. The use of any one of claims 9 to 11, wherein the cross-linking agent is or comprises 1,2-dihydroxybisacrylamide.

51. The use of any one of claims 9 to 11, wherein the cross-linking agent is or comprises N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide, polyethylene glycol diacrylamide and 4-arm PEG-acrylamide.

52. The use of claim 51, wherein the cross-linking agent is or comprises N,N'-((ethane-1,2-diylbis(oxy))bis(ethane-2,1-diyl))diacrylamide.

53. The use of claim 51, wherein the MW of polyethylene glycol diacrylamide is ≤ 2000.

54. The use of claim 51, wherein the MW of 4-arm PEG-acrylamide is ≤ 2000.

55. The use of any one of claims 9 to 11, wherein the cross-linking agent does not comprise a primary amine, a secondary amine, a hydroxyl group or a carboxylic acid.

56. The use according to any one of claims 9 to 11, wherein the crosslinking level is 1-60 wt% crosslinking agent, wherein the crosslinking level is expressed as a weight percentage of the crosslinking agent contained in the total monomers used for the polymerization.

57. The use of claim 56 wherein the crosslinking level is 1 to 30% by weight of crosslinking agent.

58. The use of claim 56, wherein the crosslinking level is 10-90% by weight of the crosslinking agent.

59. The use of claim 56, wherein the crosslinking level is 25-60% by weight of the crosslinking agent.

60. The use according to any one of claims 9 to 11, wherein the hydrophilic vinyl monomer is a cross-linking agent as defined in any one of claims 30 to 55.

61. The use according to any one of claims 9 to 11, wherein the polymer particles are porous.

62. The use according to any one of claims 9 to 11, wherein the polymer particles have an average diameter of 0.5 μm to 10 μm.

63. The use according to claim 62, wherein the polymer particles have an average diameter of 0.5 μm to 5 μm.

64. The use of any one of claims 9 to 11, wherein the coefficient of variation (CV) is less than 20%.

65. The use of claim 64, wherein the coefficient of variation (CV) is less than 15%.

66. The use of any one of claims 9 to 11, wherein the particle comprises an oligonucleotide attached to the particle.

67. The use of any one of claims 9 to 11, wherein each of the particles comprises a plurality of oligonucleotides attached to the particle.

68. The use of claim 67, wherein the plurality of oligonucleotides are identical for each individual particle.

69. A method of forming monodisperse seed particles according to any one of claims 1 to 6, comprising: dissolving N,N-dimethylacrylamide, a stabilizer, a free radical initiator, and a chain transfer agent in an organic solvent to form a reaction mixture; as well as The reaction mixture is heated to activate the initiator. Thus, monodisperse seed particles are formed.

70. The method of claim 69, wherein the stabilizer is a block copolymer of styrene and a polyolefin.

71. The method of claim 70, wherein the stabilizer is a triblock copolymer consisting of a poly(ethylene-co-butylene) midblock and polystyrene outer blocks.

72. The method of any one of claims 69 to 71, wherein the stabilizer is selected from or comprises Kraton A1535H, Kraton G1650M, Kraton G1652M or Kraton G1657M.

73. The method of any one of claims 69 to 71, wherein the free radical initiator is a peroxide initiator or an azo initiator.

74. The method of any one of claims 69 to 71, wherein the free radical initiator is selected from 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dibenzoyl peroxide.

75. The method of claim 74, wherein the free radical initiator is 2,2'-azobis(2-methylpropionitrile).

76. The method of any one of claims 69 to 71, wherein heating the reaction mixture to activate the initiator comprises heating to at least 40°C.

77. The method of claim 76, wherein heating the reaction mixture to activate the initiator comprises heating to at least 50°C.

78. The method of claim 77, wherein heating the reaction mixture to activate the initiator comprises heating to at least 60°C.

79. The process of any one of claims 69 to 71, wherein the chain transfer agent is a mercaptan or an alkyl halide.

80. The process of claim 79, wherein the chain transfer agent is an alkyl mercaptan.

81. The process of any one of claims 69 to 71, wherein the chain transfer agent is selected from the group consisting of 1-octanethiol, hexanethiol, 6-mercapto-1-hexanol, benzyl mercaptan, carbon tetrachloride, and bromotrichloromethane.

82. The process of any one of claims 69 to 71, wherein the chain transfer agent is 1-octanethiol.

83. The method of any one of claims 69 to 71, wherein the organic solvent comprises a mixture of an alkane component and an aromatic component.

84. The method of claim 83, wherein the alkane component and the aromatic component are present in a weight ratio of alkane component:aromatic component of 0.5:1 to 20:

1.

85. The method of claim 84, wherein the weight ratio of the alkane component:aromatic component is from 1:1 to 10:

1.

86. The process of claim 84 or claim 85, wherein the alkane component is heptane and the aromatic component is toluene.

87. The method of any one of claims 69 to 71, wherein the reaction mixture comprises: N,N-dimethylacrylamide in an amount of 2 to 5 wt %; a stabilizer in an amount of 1 wt % to 5 wt %; a free radical initiator in an amount of 0.01 wt % to 4 wt %; and Chain transfer agents in amounts of 0.05 wt% to 0.25 wt%.

88. The method of claim 87, wherein the weight % of the N,N-dimethylacrylamide is greater than the weight % of the stabilizer.

89. The process of any one of claims 69 to 71, wherein the reaction mixture is purged of oxygen prior to heating the reaction mixture.

90. The method of claim 89, wherein said scavenging oxygen comprises sparging with a chemically inert gas.

91. The method of claim 90, wherein the chemically inert gas is selected from argon, helium, or nitrogen.